Electrodes based on coated solid electrolytes and nanofibers, their preparation methods and applications

By using polyether polyol-nano silica hybrid coating to encapsulate solid electrolyte and nanofiber toughening agent in lithium battery electrodes, a synergistic lithium-ion transport and flexible support network is formed, solving the problems of easy agglomeration and poor compatibility of solid electrolyte in electrode slurry, and improving the cycle stability and mechanical properties of lithium battery.

CN123120632APending Publication Date: 2026-11-17HUBEI XINGSHUN NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611537483.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, solid electrolyte particles tend to agglomerate in the electrode slurry and have poor compatibility with electrode active materials and binders, resulting in increased interfacial impedance, increased cyclic polarization, and significant increase in impedance after cycling, as well as insufficient electrode structural stability and mechanical flexibility.

Method used

A solid electrolyte is coated with a polyether polyol-nano silica hybrid and combined with a nanofiber toughening agent to form an electrode that coats the solid electrolyte and nanofibers. By forming a lithium-ion transport auxiliary network and a flexible support network in the positive electrode slurry, the dispersion stability and interfacial compatibility are improved, and the limitation of ion transport paths and local stress concentration are alleviated.

Benefits of technology

This study achieves a synergistic improvement in ion transport capability and structural stability of high-voltage positive electrodes, reduces capacity decay and impedance growth during cycling, and enhances the cycling stability and mechanical flexibility of the electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
  • Figure SMS_8
    Figure SMS_8
Patent Text Reader

Abstract

This invention relates to an electrode based on a coated solid electrolyte and nanofibers, its preparation method, and its application. The electrode comprises a substrate and a positive electrode material attached to the substrate. The positive electrode material comprises, by mass percentage: 2.0%-5.0% coated solid electrolyte, 0.20%-0.80% nanofiber toughening agent, 1.0%-2.0% conductive agent, 1.0%-1.8% binder, 0.10%-0.30% dispersant, with the balance being active material. The coated solid electrolyte comprises a solid electrolyte and a nano-SiO2 and polyether polyol modification layer on the surface of the solid electrolyte. This invention achieves a synergistic effect through the "coated solid electrolyte ion transport auxiliary network" and the "nanofiber entanglement toughening network," reducing the risk of inorganic ceramic particle agglomeration, debinding, and crushing under rolling pressure, and improving the structural retention ability of the positive electrode material under bending, cutting, and cyclic stacking pressure changes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery technology, specifically to an electrode based on a solid electrolyte and nanofiber coating, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries, with their advantages of high energy density, high operating voltage, and long cycle life, have been widely used in consumer electronics, electric vehicles, and energy storage. However, with the increasing demands for battery energy density and cycle life, problems such as increased polarization, impedance growth, and decreased structural stability of electrodes during cycling are becoming increasingly prominent. Especially in thick electrodes, high areal loading electrodes, or electrodes using high-capacity active materials, factors such as volume changes in the active material, interfacial side reactions, and repeated growth and damage of the SEI film during cycling can lead to obstruction of ion transport channels within the electrode and a continuous increase in interfacial impedance, resulting in increased cyclic polarization, accelerated capacity decay, and deteriorated electrode stability.

[0003] To improve ion transport performance within electrodes, existing technologies typically incorporate solid electrolytes as ion conductors. Solid electrolytes, such as lithium aluminum titanium phosphate (LATP), garnet-type (LLZO), and lithium aluminum germanium phosphate (LAGP), possess high ionic conductivity and a wide electrochemical window, which can enhance the electrode's ion conduction capacity to some extent. However, directly mixing solid electrolyte particles into the electrode slurry presents challenges, including particle agglomeration, poor compatibility with electrode active materials and binders, and difficulty in suppressing interfacial side reactions. During cycling, the interfacial impedance between the solid electrolyte and the electrode active material tends to increase continuously, leading to increased cyclic polarization and a significant increase in impedance after cycling.

[0004] Surface coating is a common method to improve the interfacial stability and dispersibility of solid electrolytes. Existing technologies have reported the use of metal oxides or non-metal oxides to modify the surface of solid electrolytes to form core-shell structures, such as using Al₂O₃ and Li₂O₂B₂O₃ (LBO) to surface-coat LATP. However, such surface modifications are mostly used to improve the air stability, lithium metal stability, or ionic conductivity of solid electrolyte sheets, composite electrolyte membranes, or separator coatings. The application system is usually an electrolyte layer or separator layer, rather than an electrode slurry system. Furthermore, in existing technologies, solid electrolytes mostly exist as additive phases or are used as coating layers on the surface of electrode active materials. There are few methods that use a solid electrolyte as the core and inorganic particles as the shell to form a coating structure, and then formulate it together with toughening fibers, electrode active materials, binders, conductive agents, and dispersants to prepare a slurry for lithium electrode fabrication. Summary of the Invention

[0005] The purpose of this invention is to improve the dispersion stability, wetting compatibility and pressure interface stability of solid electrolytes by coating them with polyether polyol-nano silica hybrid coating, while introducing flexible nanofibers to construct a support network. This ensures the ion transport capacity of the high-pressure positive electrode while improving the structural stability of the electrode, thereby reducing capacity decay and impedance growth during cycling.

[0006] To achieve the above-mentioned technical objectives, the present invention provides an electrode based on a solid electrolyte and nanofibers, comprising a matrix and a positive electrode material attached to the matrix. The positive electrode material comprises, by mass percentage, 2.0%-5.0% solid electrolyte, 0.20%-0.80% nanofiber toughening agent, 1.0%-2.0% conductive agent, 1.0%-1.8% binder, 0.10%-0.30% dispersant, and the balance being active material. The coated solid electrolyte includes a solid electrolyte and a nano-SiO2 and polyether polyol modification layer on the surface of the solid electrolyte.

[0007] Furthermore, the method for preparing the coated solid electrolyte includes, Solid electrolyte, nano-SiO2, polyether polyol and coating solvent are mixed in a mass ratio of 150-200:1-3:2-8:200-250 to obtain coated solid electrolyte.

[0008] Furthermore, the D50 particle sizes of the solid electrolyte and the nano-SiO2 are 0.5-2 μm and 15-50 nm, respectively; The mixing and stirring are carried out at a temperature of 45-65℃ for 1-3 hours.

[0009] Furthermore, the nanofiber toughening agent is composed of polyurethane nanofibers and carboxylated cellulose nanofibers in a mass ratio of 1-4:1; The diameter and length of the polyurethane nanofibers and the carboxylated cellulose nanofibers are 30-150 nm and 3-15 μm, respectively.

[0010] This invention also provides the above-mentioned method for preparing electrodes based on coated solid electrolytes and nanofibers, characterized in that it includes, The binder is dissolved in the dispersion solvent, then the dispersant and conductive agent are added for dispersion, the active material and the coated solid electrolyte are added and mixed, and then the nanofiber toughening agent is added and mixed evenly to obtain the positive electrode slurry; The positive electrode slurry is coated onto the substrate surface and pre-dried to obtain the initial sheet; The initial sheet is rolled and heat-treated to obtain an electrode based on a solid electrolyte and nanofiber coating.

[0011] Furthermore, the solid content of the positive electrode slurry is 68%-75%, and the viscosity is 4000-6500 mPa·s.

[0012] Furthermore, the surface loading of the positive electrode slurry on one side is 18-22 mg / cm². 2 ; The pre-drying process is carried out at a temperature of 80-110℃ for 30-120 seconds.

[0013] Furthermore, the rolling parameters include a temperature of 40-70℃, a pressure of 80-180MPa, and a speed of 1-6m / min; The heat treatment is carried out at a temperature of 90-120℃ and a vacuum degree of -0.10 to -0.08MPa for 4-12 hours.

[0014] Furthermore, the compacted density of the initial sheet after roll pressing reaches 3.60-3.70 g / cm³. 3 .

[0015] The present invention also provides the application of the above-mentioned electrode based on coated solid electrolyte and nanofiber in lithium batteries.

[0016] Compared with the prior art, the beneficial effects of the present invention include: (1) This invention does not rely solely on solid electrolytes to improve ion conduction or on nanofiber toughening agents to improve electrode toughness. Instead, it achieves a synergistic effect through a "solid electrolyte-coated ion transport auxiliary network" and a "nanofiber entanglement toughening network." On the one hand, the solid electrolyte particles are distributed on the surface of the active material and in the pores between the particles, providing lithium-ion transport auxiliary sites inside the high-pressure positive electrode, thus alleviating the problems of limited ion transport paths and concentration polarization caused by high pressure. The polyether polyol-nano silica hybrid coating layer on the surface of the solid electrolyte improves its dispersion stability and interfacial compatibility in the slurry system, reducing the risk of inorganic ceramic particle agglomeration, debinding, and crushing during rolling.

[0017] (2) The nanofiber toughening agent is dispersed inside the cathode material to form an interwoven and entangled flexible support network. This network can buffer local stress concentration during rolling, slitting and cycling, and improve the structural retention ability of the cathode material under bending, slitting and cycling stacking pressure changes.

[0018] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the invention; the terms “comprising” and “having” and any variations thereof in the specification and claims of this invention are intended to cover non-exclusive inclusion.

[0021] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0022] Adding toughening fibers to electrode slurry can improve the mechanical flexibility of the electrode and suppress cracking and powdering during the coating and drying process. However, it is still difficult to simultaneously ensure the dispersibility and interfacial compatibility between the fibers and the solid electrolyte, inorganic particles, electrode active materials, conductive agents, and binders. If the components are not dispersed uniformly, it can easily lead to slurry agglomeration, uneven coating, and localized stress concentration on the electrode, which in turn affects the ion / electron transport network of the electrode, resulting in the inability to effectively solve the problems of cyclic polarization and impedance growth.

[0023] Lithium electrodes still suffer from the following problems during cycling: unstable ion transport channels inside the electrode, leading to a gradual increase in cyclic polarization; significant increases in interfacial impedance and charge transfer impedance after cycling; insufficient structural stability and mechanical flexibility, resulting in cracking and powder shedding; and poor interfacial stability due to direct contact between the solid electrolyte and the electrode active material, which easily triggers side reactions. There is a lack of electrode slurries and electrode solutions that can effectively synergize the ion conduction effect of the solid electrolyte, the interfacial stabilization effect of the inorganic shell, and the mechanical reinforcement effect of the toughening fibers.

[0024] Therefore, this invention is proposed.

[0025] On one hand, the present invention provides an electrode based on a solid electrolyte and nanofibers, comprising a matrix and a positive electrode material attached to the matrix, wherein the positive electrode material comprises, by mass percentage, 2.0%-5.0% solid electrolyte, 0.20%-0.80% nanofiber toughening agent, 1.0%-2.0% conductive agent, 1.0%-1.8% binder, 0.10%-0.30% dispersant, and the balance being active material; The coated solid electrolyte includes a solid electrolyte and a nano-SiO2 and polyether polyol modification layer on the surface of the solid electrolyte.

[0026] This invention does not strictly limit the types of solid electrolytes, conductive agents, binders, dispersants, active materials, and matrices; all are conventional raw materials in the art. Exemplarily, the solid electrolyte can be at least one of LISICON-type solid electrolytes, NASICON-type solid electrolytes, perovskite-type solid electrolytes, garnet-type solid electrolytes, sulfide-type solid electrolytes, etc. The conductive agent can be carbon black SUPER. P, conductive graphite KS 6. At least one of the following: carbon nanofibers, carbon nanotubes (CNTs), acetylene black, graphene, Ketjen carbon, metallic silver, metallic gold, etc. The binder may be polyvinylidene fluoride, styrene-butadiene latex, styrene-acrylic latex, polyvinyl alcohol, ethylene... Vinyl acetate, polymethyl methacrylate Butyl acrylate, ethylene The material can be at least one of vinyl acetate copolymer, polyvinyl acetate, polyurethane, polyacrylamide, polyethylene oxide, and polytetrafluoroethylene. The dispersant can be at least one of hydroxyethyl cellulose, sodium alginate, methyl hydroxyethyl cellulose, sodium carboxymethyl cellulose, polyacrylamide, and polyvinylpyrrolidone. The active material can be at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium manganese iron phosphate, and lithium nickel cobalt manganese oxide. The matrix can be a current collector formed from at least one of aluminum foil, porous aluminum foil, carbon-coated aluminum foil, and porous carbon-coated aluminum foil.

[0027] This invention fixes the proportion of the coated solid electrolyte in the electrode material to be 2.0%-5.0%. On the one hand, this avoids obstruction of the ion transport path inside the electrode, reduces ohmic resistance, and ensures that the active material has an appropriate content and the electrode slurry has an appropriate viscosity, thereby improving the coating performance of the slurry. On the other hand, it ensures the physical support of the coated solid electrolyte for the electrode, thereby improving the cycle stability of the electrode.

[0028] Furthermore, this invention has verified the effect of nano-SiO2 and / or polyether polyol coating on the performance of solid electrolyte electrode materials through a large number of experiments. The results show that only when nano-SiO2 and polyether polyol are used together to coat the solid electrolyte does the resulting electrode have a lower initial impedance, while ensuring effective support performance during cyclic use.

[0029] In this invention, the proportion of nanofiber toughening agent in the electrode material is selected to be 0.20%-0.80%. On the one hand, it can form a continuous reinforcing skeleton that runs through the electrode, enabling the electrode to resist the mechanical stress caused by the volume change of the active material during cycling; on the other hand, it will not block the ion transport channels, allowing lithium ions to be transported effectively.

[0030] In some preferred embodiments, the method for preparing the coated solid electrolyte includes: Solid electrolyte, nano-SiO2, polyether polyol and coating solvent are mixed in a mass ratio of 150-200:1-3:2-8:200-250 to obtain coated solid electrolyte.

[0031] In some preferred embodiments, the D50 particle sizes of the solid electrolyte and the nano-SiO2 are 0.5-2 μm and 15-50 nm, respectively; The mixing and stirring are carried out at a temperature of 45-65℃ for 1-3 hours.

[0032] In this invention, the type of coating solvent is not strictly limited. For example, it can be at least one of water, ethanol, acetone, isopropanol, ethylene glycol, etc. Preferably, it is an inexpensive solvent that can effectively disperse nano-SiO2 and dissolve polyether polyol.

[0033] In some preferred embodiments, the nanofiber toughening agent is composed of polyurethane nanofibers and carboxylated cellulose nanofibers in a mass ratio of 1-4:1. The diameter and length of the polyurethane nanofibers and the carboxylated cellulose nanofibers are 30-150 nm and 3-15 μm, respectively.

[0034] On the other hand, the present invention also provides the above-mentioned method for preparing electrodes based on coated solid electrolytes and nanofibers, including, The binder is dissolved in the dispersion solvent, then the dispersant and conductive agent are added for dispersion, the active material and the coated solid electrolyte are added and mixed, and then the nanofiber toughening agent is added and mixed evenly to obtain the positive electrode slurry; The positive electrode slurry is coated onto the substrate surface and pre-dried to obtain the initial sheet; The initial sheet is rolled and heat-treated to obtain an electrode based on a solid electrolyte and nanofiber coating.

[0035] The viscosity of the slurry directly affects the coating effect and the drying process. In some preferred embodiments, the solid content of the positive electrode slurry is 68%-75%, and the viscosity is 4000-6500 mPa·s.

[0036] In some preferred embodiments, the surface loading of the positive electrode slurry on one side is 18-22 mg / cm². 2 ; The pre-drying process is carried out at a temperature of 80-110℃ for 30-120 seconds.

[0037] In some preferred embodiments, the rolling parameters include a temperature of 40-70°C, a pressure of 80-180 MPa, and a speed of 1-6 m / min; The heat treatment is carried out at a temperature of 90-120℃ and a vacuum degree of -0.10 to -0.08MPa for 4-12 hours.

[0038] In some preferred embodiments, the compaction density of the initial sheet after roll pressing reaches 3.60-3.70 g / cm³. 3 .

[0039] The present invention will be further described in detail below through specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or in accordance with the product instructions. Reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0040] Preparation Example 1 A method for preparing a coated solid electrolyte includes the following steps: 2.5g of nano-SiO2 with a D50 particle size of 20nm and 7.5g of polyether polyol with a molecular weight of 2000 (the mass ratio of nano-SiO2 to polyether polyol is 1:3) were added to 220g of anhydrous ethanol and ultrasonically dispersed for 30min to form a uniform coating solution. Then, 190g of LATP powder with a D50 particle size of 1.0μm was added and stirred at 55℃ for 2h for coating. After centrifugation / filtration, vacuum drying at 80℃, and sieving, the coated solid electrolyte was obtained.

[0041] Preparation Example 2 Compared with Preparation Example 1, the difference is that LATP powder was replaced with garnet-type LLZO of the same size.

[0042] Preparation Example 3 The difference compared to Preparation Example 1 is that no polyether polyol was added and the amount of nano-SiO2 used was 10g.

[0043] Preparation Example 4 The difference compared to Preparation Example 1 is that no nano-SiO2 was added and the amount of polyether polyol used was 10g.

[0044] Preparation Example 5 Compared with Preparation Example 1, the difference is that the amount of nano-SiO2 and polyether polyol used is 5g, and the mass ratio of nano-SiO2 to polyether polyol is 1:1.

[0045] Preparation Example 6 Compared with Preparation Example 1, the difference is that the amounts of nano-SiO2 and polyether polyol used are 1.67 g and 8.33 g, respectively, and the mass ratio of nano-SiO2 to polyether polyol is approximately 1:5.

[0046] Example 1 A method for preparing an electrode based on a solid electrolyte and nanofibers includes the following steps: (1) Preparation of positive electrode slurry: 65g of polyvinylidene fluoride was added to N-methylpyrrolidone and stirred at 50°C for 3h to fully dissolve and form a homogeneous gel. 10g of polyvinylpyrrolidone, 46.2g of conductive carbon black and 28.8g of carbon nanotubes were added to the obtained gel and dispersed at 1500rpm for 45min to achieve uniform dispersion of the conductive agent in the liquid phase slurry. Then, 4675g of active material NCM811 and 150g of the coated solid electrolyte obtained in Example 1 were added and stirred at 800rpm for 2h to make the coated solid electrolyte uniformly distributed between NCM811 particles and in the conductive agent dispersion system. Finally, 25g of nanofiber toughening agent, which is a mixture of polyurethane nanofibers and carboxylated cellulose nanofibers in a mass ratio of 2:1, was added. The diameter and length of the polyurethane nanofibers and carboxylated cellulose nanofibers were 90nm and 9μm, respectively. The mixture was stirred at 800rpm for 60min to obtain a homogeneous positive electrode slurry. The obtained positive electrode slurry, by solid mass percentage, comprises: 93.5% active material, 3.0% coated solid electrolyte, 0.5% nanofiber toughening agent, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone. The obtained positive electrode slurry has a solid content of 71.5% and a viscosity of 5051 mPa·s.

[0047] (2) Coating and pre-drying: The positive electrode slurry obtained in step (1) is uniformly coated onto the surface of the aluminum foil current collector, and the coating surface loading on one side is controlled to be 20 mg / cm². 2 The film was then pre-dried using a hot air oven at 95°C for 75 seconds to obtain the initial film.

[0048] (3) High-pressure compaction: The initial sheet obtained in step (2) is subjected to low-temperature compaction treatment, wherein the compaction temperature is set to 55℃, the compaction pressure is set to 130MPa, and the compaction speed is set to 3m / min. The compaction density of the initial sheet after compaction is controlled to be 3.65g / cm³. 3 .

[0049] (4) Post-processing: The initial sheet obtained in step (3) after rolling is subjected to vacuum heat treatment to remove residual solvent and moisture, and an electrode based on coated solid electrolyte and nanofiber is obtained.

[0050] Example 2 Compared to Example 1, the active material was replaced with lithium cobalt oxide, and the coated solid electrolyte replaced the hybrid coated LLZO solid electrolyte obtained in Preparation Example 2. The resulting cathode slurry, by solids mass percentage, comprised: 93.5% lithium cobalt oxide, 3.0% hybrid coated LLZO solid electrolyte, 0.5% nanofiber toughening agent, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone. The resulting cathode slurry had a solid content of 69.7% and a viscosity of 4720 mPa·s. The single-sided coating surface loading was 20 mg / cm². 2 Pre-dry at 100℃ for 70 seconds; roll pressing temperature 55℃, pressure 130MPa, speed 3m / min; compacted density after roll pressing 3.65g / cm³. 3 Vacuum heat treatment at 105℃ for 7 hours; the remaining preparation steps are the same as in Example 1.

[0051] Example 3 Compared with Example 1, the proportions of each group and some process parameters were adjusted; the resulting positive electrode slurry, by solid mass percentage, comprised: 94.0% active material, 2.5% coated solid electrolyte, 0.3% nanofiber toughening agent, 1.0% conductive carbon black, 0.4% carbon nanotubes, 1.4% polyvinylidene fluoride, and 0.4% polyvinylpyrrolidone; the resulting positive electrode slurry had a solid content of 69% and a viscosity of 4400 mPa·s. The single-sided coating surface loading was 19 mg / cm². 2 Pre-dry at 90℃ for 90 seconds; roll pressing temperature 50℃, pressure 110MPa, speed 2m / min; compacted density after roll pressing 3.65g / cm³. 3 Vacuum heat treatment at 100℃ for 8 hours; the remaining preparation steps are the same as in Example 1.

[0052] Comparative Example 1 Compared with Example 1, the difference is that: no solid electrolyte coating or nanofiber toughening agent is added in step (1); the obtained positive electrode slurry, by solid mass percentage, includes: 96.5% active material, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.8% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 72.6% and a viscosity of 5310 mPa·s.

[0053] Comparative Example 2 Compared with Example 1, the difference is that in step (1), LATP powder with a D50 particle size of 1.0 μm is used to replace the coating solid electrolyte, and no nanofiber toughening agent is added; the resulting positive electrode slurry, by solid mass percentage, includes: 94.0% active material, 3.0% solid electrolyte, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the solid content of the resulting positive electrode slurry is 70.9%, and the viscosity is 5214 mPa·s.

[0054] Comparative Example 3 Compared with Example 1, the difference is that: no nanofiber toughening agent is added in step (1); the obtained positive electrode slurry, by solid mass percentage, includes: 94.0% active material, 3.0% coated solid electrolyte, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 70.9% and a viscosity of 5214 mPa·s.

[0055] Comparative Example 4 Compared with Example 1, the difference is that no coated solid electrolyte is added in step (1); the obtained positive electrode slurry, by solid mass percentage, includes: 96.5% active material, 0.5% nanofiber toughening agent, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 70.9% and a viscosity of 5214 mPa·s.

[0056] Comparative Example 5 Compared with Example 1, the difference is that in step (1), LATP powder with a D50 particle size of 1.0 μm is used to replace the coating solid electrolyte; the resulting positive electrode slurry, by solid mass percentage, includes: 93.5% active material, 3.0% solid electrolyte, 0.5% nanofiber toughening agent, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the solid content of the resulting positive electrode slurry is 73.5%, and the viscosity is 5510 mPa·s.

[0057] Comparative Example 6 Compared with Example 1, the difference is that the amount of solid electrolyte coating is reduced in step (1), and the reduced amount is made up by active material; the obtained positive electrode slurry, by solid mass percentage, includes: 95.5% active material, 1.0% solid electrolyte, 0.5% nanofiber toughening agent; 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 70.3% and a viscosity of 4895 mPa·s.

[0058] Comparative Example 7 Compared with Example 1, the difference is that the amount of solid electrolyte coating is increased in step (1), and the amount of active material added is reduced; the obtained positive electrode slurry, by solid mass percentage, includes: 91.0% active material, 5.5% solid electrolyte, 0.5% nanofiber toughening agent, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 71.7% and a viscosity of 5815 mPa·s.

[0059] Comparative Example 8 Compared with Example 1, the difference is that the amount of nanofiber toughening agent is increased in step (1), and the amount of active material added is reduced; the obtained positive electrode slurry, by solid mass percentage, includes: 92.8% active material, 3.0% solid electrolyte, 1.2% nanofiber toughening agent; 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 72.3% and a viscosity of 5611 mPa·s.

[0060] Comparative Example 9 Compared with Example 1, the difference is that: in step (1), the coated solid electrolyte obtained in Preparation Example 3 is used, and no nanofiber toughening agent is added; the obtained positive electrode slurry, by solid mass percentage, includes: 94.0% active material, 3.0% solid electrolyte, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 70.7% and a viscosity of 5441 mPa·s.

[0061] Comparative Example 10 Compared with Example 1, the difference is that: in step (1), the coated solid electrolyte obtained in Preparation Example 4 is used, and no nanofiber toughening agent is added; the obtained positive electrode slurry, by solid mass percentage, includes: 94.0% active material, 3.0% solid electrolyte, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 70.0% and a viscosity of 5125 mPa·s.

[0062] Comparative Example 11 Compared with Example 1, the difference is that: in step (1), the coated solid electrolyte obtained in Preparation Example 5 is used, and no nanofiber toughening agent is added; the obtained positive electrode slurry, by solid mass percentage, includes: 94.0% active material, 3.0% solid electrolyte, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 71.2% and a viscosity of 5368 mPa·s.

[0063] Comparative Example 12 Compared with Example 1, the difference is that: in step (1), the coated solid electrolyte obtained in Preparation Example 6 is used, and no nanofiber toughening agent is added; the obtained positive electrode slurry, by solid mass percentage, includes: 94.0% active material, 3.0% solid electrolyte, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone; the obtained positive electrode slurry has a solid content of 71.0% and a viscosity of 5246 mPa·s.

[0064] Comparative Example 13 Compared with Example 1, the difference is that the order of adding slurry in step (1) is changed. After the binder is dissolved, the dispersant and nanofiber toughening agent are added first and stirred for 60 minutes. Then the conductive agent, active material and coated solid electrolyte are added to complete the mixing. The resulting positive electrode slurry, by solid mass percentage, includes: 93.5% active material, 3.0% coated solid electrolyte, 0.5% nanofiber toughening agent, 0.924% conductive carbon black, 0.576% carbon nanotubes, 1.3% polyvinylidene fluoride, and 0.2% polyvinylpyrrolidone. The solid content of the resulting positive electrode slurry is 71.1%, and the viscosity is 6330 mPa·s.

[0065] Comparative Example 14 Compared to Example 2, the difference is that the hybrid coated LLZO solid electrolyte is replaced with an LLZO solid electrolyte.

[0066] In all the above Examples 1-3 and Comparative Examples 1-14, the compaction density of the initial sheet was controlled to be 3.65 g / cm³ through roller pressing. 3 .

[0067] Table 1 summarizes the composition of the positive electrode slurry of Examples 1-3 and Comparative Examples 1-14, in wt.%. Hybrid coating refers to the co-coating of solid electrolyte (LATP or LLZO) with nano-SiO2 and polyether polyol. Unless otherwise specified, the active material is NCM811.

[0068]

[0069] The industry-standard quantitative macroscopic mechanical indicators are used to evaluate the flexibility and structural retention of the electrode sheets. The specific test methods are as follows: (1) Bending powder loss rate: Weigh the positive electrode sample m0 before the test, bend it back and forth 20 times with a 6mm diameter round bar and shake off the free powder, and weigh the mass m1. Calculate the bending powder loss rate η according to the formula η=(m0-m1) / m0×100%. The lower the value, the better the coating bonding stability.

[0070] (2) 180° peel strength: The positive electrode sheet is cut into strips with a width of 20 mm. The average peel force between the positive electrode coating and the aluminum foil current collector is tested at a peel speed of 50 mm / min using the 180° peel test method. The value is converted into peel strength per unit width. The higher the value, the stronger the interlayer adhesion stability.

[0071] The test results of bending powder loss rate and 180° peel strength of Examples 1-3 and Comparative Examples 1-14 are shown in Table 2.

[0072] Table 2

[0073] The electrode sheets obtained in Examples 1-3 and Comparative Examples 1-14 were matched with corresponding active material systems and assembled with silicon-carbon anodes to form soft-pack lithium-ion batteries for testing. The silicon-based material in the silicon-carbon anode sheet accounted for 10% of the total mass of the anode active material. The electrochemical performance of Examples 1-3 and Comparative Examples 1-14 was tested, and the results are shown in Table 3. DCIR refers to the initial DC internal resistance.

[0074] Table 3

[0075] As shown in Table 3, the coating solid electrolyte and the composite nanofiber toughening system have a synergistic effect on improving the cycle stability of the high voltage solid electrode.

[0076] First, Comparative Example 1 shows that under high-compaction conditions, the electrode without the introduced solid electrolyte coating and flexible toughening network exhibits poor cycling stability, with a capacity retention of only 62.8% after 500 cycles and a DCIR increase rate of 86% after cycling. This indicates that the limited ion transport and structural degradation caused by high-compaction are important factors affecting cycling performance. Second, combined with the control experiments of Comparative Examples 2, 3, 9, 10, 11, and 12, it is evident that the introduction of hybrid solid electrolyte coating can reduce the initial impedance of the electrode, and the organic-inorganic hybrid coating of polyether polyol nano-silica has a significant synergistic modification effect on LATP. Although uncoated LATP (Comparative Example 2) can reduce the initial DCIR, the rigid inorganic particles have poor bonding stability with the electrode system, resulting in a DCIR increase rate of up to 95% after cycling and a capacity retention rate of only 60.5%. Single nano-silica inorganic coating (Comparative Example 9) can only slightly optimize the surface state of LATP. Due to the poor compatibility between the inorganic phase and the organic slurry, the coating layer is prone to failure during cycling, resulting in limited performance improvement. Single polyether polyol organic coating (Comparative Example 10) can improve particle interfacial adhesion, but lacks ion conduction channels constructed by inorganic components, resulting in a high initial impedance.

[0077] The ratio of nano-silica to polyether polyol significantly affects the coating modification effect: at a mass ratio of 1:1 (Comparative Example 11, where the polyether polyol ratio is lower than the preferred ratio), the organic compatibility component in the coating layer is insufficient, resulting in poor affinity between LATP and the slurry interface. This leads to easy peeling of the coating layer during rolling and cycling, increased electrode powder shedding, and accelerated growth in cycling impedance. At a mass ratio of 1:5 (Comparative Example 12, where the polyether polyol ratio exceeds the preferred ratio), excessive polyether polyol forms an overly thick organic coating layer, increasing the lithium-ion interfacial transport resistance and causing an increase in initial DC impedance. Only when the mass ratio is controlled within the 1:2-4 range specified in the claims can the organic-inorganic components be matched, allowing the coating layer to simultaneously achieve excellent ion conductivity and interfacial compatibility. In Comparative Example 3, using a hybrid coating of LATP within this range, the capacity retention rate after 500 cycles increased to 73.6%, confirming that the organic-inorganic hybrid coating can effectively improve the dispersibility of LATP particles and enhance the structural stability during cycling.

[0078] Furthermore, Comparative Example 4 shows that adding the compound nanofiber toughening agent alone can significantly improve the mechanical properties of the electrode, reducing the bending powder loss rate from 0.48% to 0.12% and increasing the peel strength from 17.5 N / m to 29.5 N / m. However, due to the lack of ion transport enhancement components, the improvement in cycling performance is limited, with a capacity retention rate of only 74.8% after 500 cycles. Further, Comparative Examples 5-8 show that there are optimization ranges for both the LATP coating content and the compound nanofiber content. Although the combination of uncoated LATP and nanofibers can improve the structural stability of the electrode, the cycling performance is still lower than that of the LATP-coated system. When the LATP content is too low, the ion transport enhancement effect is insufficient; when the LATP content is too high, the increase in rigid ceramic particles leads to a decrease in the structural stability of the electrode; and excessive nanofibers will affect the stability and electrochemical performance of the slurry system. Furthermore, as can be seen from Comparative Example 13, the order of slurry addition also affects the performance of the electrode. If the nanofiber toughening agent is added in advance, pre-entanglement is likely to occur, which will disrupt the uniform dispersion of the conductive agent, resulting in increased internal resistance and deterioration of mechanical and cycling performance of the electrode. This proves that the order of adding the nanofiber toughening agent last in this application can ensure the uniform dispersion of the conductive agent and toughening fiber components. After the slurry is coated and dried to remove the solvent, the uniformly dispersed conductive agent particles come into contact with each other and finally form a continuous conductive network inside the electrode, so that the two networks can work together.

[0079] In contrast, Example 1 used 3.0% polyether polyol. The synergistic regulation of LATP coated with nano-silica and 0.5% compounded nanofiber toughening agent achieved a 91.2% capacity retention rate after 500 cycles while maintaining a low initial DCIR (29.8 mΩ), and reduced the DCIR growth rate after cycles to 24%. Simultaneously, the electrode bending powder shedding rate remained at 0.09%, and the 180° peel strength reached 30.2 N / m.

[0080] Furthermore, compared to the electrode obtained in Comparative Example 14, the electrode of Example 2 exhibits a peel strength that is more than 100% higher, and a capacity retention rate that increases from approximately 60% to nearly 90% after 500 cycles at 1C. This also demonstrates that the silica and polyether polyol hybrid coating of the present invention is suitable for various solid electrolyte systems.

[0081] Compared to Example 1, Example 3 showed a slight decrease in performance, with a powder shedding rate of 0.12% after 20 bends and a peel strength of 29.1 N / m at 180°, and a capacity retention rate of 89.9% after 500 cycles at 1C, still meeting the usage requirements. This also demonstrates that within the raw material ratio range defined in this invention, the obtained electrode sheets all exhibit good performance.

[0082] In summary, this invention utilizes polyether polyols... Nano-silica organic hybrid coating modifies the solid electrolyte, constructing a continuous lithium-ion transport auxiliary network. On the other hand, composite nanofibers form a flexible structural support network, and a reasonable feeding sequence prevents nanofibers from interfering with the construction of the conductive network. These two networks work together to give the high-density positive electrode both excellent ion transport capability and structural stability, effectively reducing impedance growth and capacity decay during cycling and improving the long-term cycle stability of the lithium-ion battery.

[0083] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. An electrode based on a coated solid electrolyte and nanofibers, characterized in that, The material includes a matrix and a positive electrode material attached to the matrix. The positive electrode material comprises, by mass percentage, 2.0%-5.0% of a solid electrolyte coating, 0.20%-0.80% of a nanofiber toughening agent, 1.0%-2.0% of a conductive agent, 1.0%-1.8% of a binder, 0.10%-0.30% of a dispersant, and the balance being an active material. The coated solid electrolyte includes a solid electrolyte and a nano-SiO2 and polyether polyol modification layer on the surface of the solid electrolyte.

2. The electrode based on coated solid electrolyte and nanofibers according to claim 1, characterized in that, The preparation method of the coated solid electrolyte includes, Solid electrolyte, nano-SiO2, polyether polyol and coating solvent are mixed in a mass ratio of 150-200:1-3:2-8:200-250 to obtain coated solid electrolyte.

3. The electrode based on coated solid electrolyte and nanofibers according to claim 2, characterized in that, The solid electrolyte and the nano-SiO2 have D50 particle sizes of 0.5-2 μm and 15-50 nm, respectively; The mixing and stirring are carried out at a temperature of 45-65℃ for 1-3 hours.

4. The electrode based on coated solid electrolyte and nanofibers according to claim 1, characterized in that, The nanofiber toughening agent is composed of polyurethane nanofibers and carboxylated cellulose nanofibers in a mass ratio of 1-4:

1. The diameter and length of the polyurethane nanofibers and the carboxylated cellulose nanofibers are 30-150 nm and 3-15 μm, respectively.

5. A method for preparing an electrode based on a coated solid electrolyte and nanofibers as described in any one of claims 1-4, characterized in that, include, The binder is dissolved in the dispersion solvent, then the dispersant and conductive agent are added for dispersion, the active material and the coated solid electrolyte are added and mixed, and then the nanofiber toughening agent is added and mixed evenly to obtain the positive electrode slurry; The positive electrode slurry is coated onto the substrate surface and pre-dried to obtain the initial sheet; The initial sheet is rolled and heat-treated to obtain an electrode based on a solid electrolyte and nanofiber coating.

6. The method for preparing an electrode based on a coated solid electrolyte and nanofibers according to claim 5, characterized in that, The positive electrode slurry has a solid content of 68%-75% and a viscosity of 4000-6500 mPa·s.

7. The method for preparing an electrode based on a coated solid electrolyte and nanofibers according to claim 5, characterized in that, The surface loading of the positive electrode slurry on one side is 18-22 mg / cm². 2 ; The pre-drying process is carried out at a temperature of 80-110℃ for 30-120 seconds.

8. The method for preparing an electrode based on a coated solid electrolyte and nanofibers according to claim 5, characterized in that, The roller pressing parameters include a temperature of 40-70℃, a pressure of 80-180MPa, and a speed of 1-6m / min. The heat treatment is carried out at a temperature of 90-120℃ and a vacuum degree of -0.10 to -0.08MPa for 4-12 hours.

9. The method for preparing an electrode based on a coated solid electrolyte and nanofibers according to claim 5, characterized in that, The compacted density of the initial sheet after roller pressing reaches 3.60-3.70 g / cm³. 3 .

10. The application of an electrode based on a solid electrolyte and nanofibers as described in any one of claims 1-4 in a lithium battery.