A cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material, its preparation method and application
By in-situ growing ZIF-8 nanoparticles in cotton-based ZIF-8 porous carbon and constructing a hierarchical pore structure, the problem of easy loss of iodine species in zinc-iodine batteries was solved, achieving high specific capacity, excellent rate performance and long cycle stability, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202611377171.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-07
- Publication Date
- 2026-11-17
AI Technical Summary
In existing zinc-iodine battery cathode materials, iodine species are easily lost during charging and discharging, leading to severe self-discharge and low coulombic efficiency. Furthermore, polyiodide ions chemically corrode the zinc metal surface, forming insulating byproducts that hinder uniform zinc stripping and electroplating, resulting in rapid capacity decay and reduced rate performance of the battery.
Cotton-based ZIF-8 porous carbon was used as the positive electrode material. ZIF-8 nanoparticles were grown in situ on the fiber surface through hydrothermal treatment. Combined with KOH activation, a microporous-mesoporous hierarchical pore structure and abundant polar active sites were constructed to achieve physical confinement and chemical adsorption of iodine species, thereby enhancing the material's ability to fix iodine.
It improves the specific capacity and cycle stability of zinc-iodine batteries, suppresses the shuttle effect of polyiodide ions, exhibits excellent rate performance and long cycle life, and has a simple preparation process and low cost, making it suitable for industrial applications.
Smart Images

Figure CN123120695A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nanofiltration membrane technology, specifically to a cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material, its preparation method, and its application. Background Technology
[0002] As portable energy storage devices face increasing demands for cost, safety, and capacity, zinc-iodine batteries are considered a highly promising energy storage system due to their rich elemental composition, rapid reversible electrochemical performance, and good safety. However, during the charging and discharging process of zinc-iodine batteries, the redox reaction of iodine at the positive electrode is accompanied by the release of soluble polyiodide ions (such as I3). - The formation of polyiodide ions is a significant issue. These polyiodide ions readily shuttle from the positive electrode to the negative electrode, leading to continuous loss of active material, severe self-discharge, and low coulombic efficiency. Simultaneously, the polyiodide ions shuttling to the negative electrode chemically corrode the zinc metal surface, forming insulating byproducts and inducing disordered zinc dendrite growth, hindering uniform zinc stripping / plating. Ultimately, this results in rapid capacity decay, reduced rate performance, and shortened cycle life. Therefore, developing positive electrode carrier materials capable of efficiently immobilizing iodine species and suppressing polyiodide ion shuttle has become crucial for improving the performance of zinc-iodine batteries.
[0003] Currently, porous carbon materials are widely used as cathode materials for zinc-iodine batteries due to their excellent electronic conductivity, high specific surface area, and tunable pore structure. For example, hierarchical porous carbon obtained from ginkgo biomass activated with KOH has a specific surface area of 1176 m². 2 ·g -1 When used as a positive electrode carrier in zinc-iodine batteries, at 100 mA·g -1 It still maintains 100 mAh·g after 150 cycles at current density. -1 The discharge capacity indicates that the hierarchical porous structure can alleviate the shuttle effect, but its iodine storage mechanism mainly depends on physical confinement (Junwei Xu, Wenqing Ma, Linheng Ge, Manman Ren, Xiaoxia Cai, Weiliang Liu, Jinshui Yao, Changbin Zhang, Hui Zhao, Confining iodine into a biomass-derived hierarchically porous carbon as cathode material for highperformance zinc–iodine battery, Journal of Alloys and Compounds, Volume 912, 2022, 165151).
[0004] In addition, the pyrolysis char of cotton is at 0.1 A·g -1 The specific capacity at the current density is 145.8 mAh·g. -1 Although in 2A·g -1 It can still retain 88% of its capacity after 10,000 cycles, but it has the problem of relatively low specific capacity (LishanWei, Xue Li, Jinsong Peng, Chunxia Chen, Zhuo Li, Gongyuan Zhao, Greensynthesis of renewable biomass-derived porous carbon hosts for superioraqueous zinc-iodine batteries, Inorganic Chemistry Communications, Volume 170, Part 3, 2024, 113489).
[0005] It is evident that biomass porous char can effectively increase iodine loading and improve electron and ion transport, but its iodine storage mechanism still mainly relies on the physical confinement effect generated by the pore structure. The polar sites on the surface of the char material are limited, and there is a lack of sufficient chemical interaction with polyiodide ions. Under long-term cycling and high-rate conditions, it is still difficult to completely suppress the continuous dissolution of polyiodide ions, and the capacity decay problem still exists, making it difficult to meet practical needs.
[0006] To further enhance the immobilization capacity of iodine species, researchers have begun to introduce metal-organic frameworks (MOFs). Among them, ZIF-8, due to its regular pore structure, abundant Zn-N coordination sites, and excellent thermal stability, has become one of the most widely studied MOF materials in recent years. Through strategies such as ZIF-8-derived carbon, MOF-derived hierarchical porous carbon, and defect engineering, the chemisorption capacity and redox kinetics of iodine species can be improved to some extent, thereby enhancing the electrochemical performance of zinc-iodine batteries. However, existing technologies generally rely on complex MOF designs, single-atom loading, or bimetallic modulation strategies, resulting in cumbersome preparation processes, high costs, and problems such as uneven distribution and insufficient interfacial bonding in some MOF particles, which are not conducive to large-scale applications. Therefore, how to utilize natural biomass to construct a stable three-dimensional carbon framework, achieve in-situ uniform growth of ZIF-8 on a carbon substrate, and simultaneously construct a hierarchical pore structure, a continuous conductive network, and abundant polar active sites by combining KOH activation, thereby achieving synergistic enhancement of the physical confinement, chemisorption, and redox kinetics of iodine species, remains a key technical problem that urgently needs to be solved.
[0007] Therefore, there is an urgent need to develop an iodine-loaded carbon-based cathode material with a stable structure, abundant pore structure, and both physical confinement and efficient chemical adsorption and conversion capabilities for iodine species, which is the key to breaking through the bottlenecks in cycle life and rate performance of zinc-iodine batteries. Summary of the Invention
[0008] This invention aims to address the problems of weak chemical interaction and poor physical confinement durability of pure carbon carriers and iodine species in existing aqueous zinc-iodine battery cathode materials, while conventional MOF post-loading composite methods suffer from unstable bonding and easy detachment and deactivation. The invention provides a cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material, its preparation method, and its application.
[0009] The present invention achieves the above objectives through the following technical solutions: As a first aspect of the present invention, a cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material is provided, comprising cotton-based ZIF-8 porous carbon and active iodine loaded in the pores of the cotton-based ZIF-8 porous carbon. The cotton-based ZIF-8 porous carbon is based on a three-dimensional carbon skeleton formed by hydrothermal carbonization of cotton fibers. On its surface, a cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles is generated in situ. After the cotton-based ZIF-8 precursor is pre-carbonized and carbonized, it is then activated to form pores, thus forming an integrated porous carbon with a microporous-mesoporous hierarchical pore structure.
[0010] As a further optimization of the present invention, the micropore size of the cotton-based ZIF-8 porous carbon is concentrated below 2 nm, and the mesopore size of the cotton-based ZIF-8 porous carbon is distributed in the range of 2-50 nm.
[0011] As a further optimization of the present invention, the mass ratio of the cotton-based ZIF-8 porous carbon to active iodine is 1:3.
[0012] As a second aspect of the present invention, a method for preparing the cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material as described in any one of the above claims is also provided, comprising the following steps: (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse the pretreated cotton in deionized water, place it in a reaction vessel and hydrothermally react at 200-230 °C for 12-24 h. After natural cooling, filter and wash to obtain cotton hydrothermal carbon. (3) Disperse the hydrothermal carbon of cotton in zinc nitrate hexahydrate solution and stir to adsorb, then slowly add it to 2-methylimidazole solution, stir to react and let stand to obtain cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers. (4) The cotton-based ZIF-8 precursor was heated to 350 ℃ at a rate of 5-10 ℃ / min under an inert protective gas atmosphere and held for 1-2 h for pre-carbonization. Then, it was heated to 900 ℃ at the same heating rate and held for 2 h for carbonization treatment to obtain cotton-based ZIF-8 activated carbon. (5) Mix cotton-based ZIF-8 activated carbon with KOH evenly, heat to 800 ℃ at a rate of 5 ℃ / min under an inert protective gas atmosphere, and maintain for 1-2 h to activate and form pores. Wash the obtained activated product until neutral and then dry it to obtain cotton-based ZIF-8 porous carbon. (6) Mix and grind cotton-based ZIF-8 porous carbon with elemental iodine, heat under closed conditions to sublimate the iodine and diffuse it into the porous carbon channels, and then heat in an open manner to remove excess iodine from the surface to obtain cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material.
[0013] As a further optimization of the present invention, in step (3), the zinc nitrate hexahydrate solution is prepared by dissolving zinc nitrate hexahydrate in methanol to form a solution with a concentration of 10-50 g / L; the 2-methylimidazole solution is prepared by dissolving 2-methylimidazole in methanol to form a solution with a concentration of 50-100 g / L.
[0014] As a further optimization of the present invention, in step (5), the preparation method of the cotton-based ZIF-8 precursor is specifically as follows: the cotton hydrothermal carbon is first dispersed in a zinc nitrate hexahydrate solution and stirred at 25 ℃ for 8-12 h to allow Zn²⁺ to form a soluble Zn²⁺ precipitate. + After complete adsorption, add the solution dropwise to a 2-methylimidazole solution, stir for 20-60 min, and then let stand for 6-12 h.
[0015] As a further optimization of the present invention, in step (5), the mass ratio of cotton-based ZIF-8 activated carbon to KOH is 1:(0.5-3), the activation temperature is increased to 800 ℃ at a rate of 5℃ / min, and the holding time is 1-2 h.
[0016] As a further optimization of the present invention, in step (6), cotton-based ZIF-8 porous carbon and elemental iodine are mixed at a mass ratio of 1:2-4, anhydrous ethanol is added and ground evenly, and the iodine is sublimated under sealed conditions at 150-170 ℃ for 2-3 h, and then the surface free iodine is removed under open conditions at 80-90 ℃ for 1-2 h.
[0017] As a second aspect of the present invention, a zinc-iodine battery is also provided, comprising a positive electrode, a negative electrode and an electrolyte; wherein the positive electrode is a cotton-based ZIF-8 porous carbon-supported iodine zinc-iodine battery positive electrode material as described in any of the preceding claims, the negative electrode is zinc foil, and the electrolyte is an aqueous solution of ZnSO4.
[0018] As a further optimization of the present invention, the preparation method of the positive electrode is as follows: cotton-based ZIF-8 porous carbon-supported iodine positive electrode material, conductive carbon black and binder are mixed in a mass ratio of 8:1:1, deionized water is added and the mixture is ground into a uniform slurry, coated on a stainless steel current collector, vacuum dried at 60-90 ℃ for 6-12 h and then cut into electrode sheets; the areal density of the active material in the positive electrode sheet is 1.0-2.0 mg / cm²; the electrolyte is a 2 mol / L ZnSO4 aqueous solution.
[0019] The technical principle of this invention lies in using waste cotton fibers as a biomass template and carbon source. Oxygen-containing functional groups are introduced onto the fiber surface through hydrothermal treatment, inducing ZIF-8 nanoparticles to be uniformly and firmly anchored to the fiber skeleton in situ. Subsequent carbonization and KOH activation treatment yields cotton-based ZIF-8 porous carbon with a microporous-mesoporous hierarchical pore structure, high specific surface area, and abundant active sites. When used as an iodine carrier, the micropores provide effective physical confinement for iodine species, the mesopores promote electrolyte wetting and provide rapid ion diffusion channels, and the nitrogen-containing carbon derived from ZIF-8 and the activated defect sites provide abundant polar active sites, enhancing the material's chemical adsorption capacity for iodine species. These three factors work synergistically to effectively suppress the shuttle effect of polyiodide ions. The zinc-iodine battery cathode prepared in this manner exhibits a high specific surface area of 0.2 A·g⁻¹. -1 The specific capacity reaches 198 mAh·g -1 1 A·g -1 The capacity retention rate is as high as 97.8% after 1300 cycles, demonstrating excellent rate performance and long-cycle stability.
[0020] The beneficial effects of this invention are as follows: (1) The cotton-based hydrothermal carbon of the present invention provides a large number of oxygen-containing functional groups, which induces ZIF-8 in-situ nucleation growth and anchoring, so that MOF-derived carbon and cotton carbon skeleton form an integrated structure by chemical bonding, which solves the problems of weak binding force, uneven distribution and easy shedding during cycling of the post-loaded MOF.
[0021] (2) This invention constructs a microporous-mesoporous hierarchical pore structure, wherein the micropores provide effective physical confinement for iodine species, and the mesopores facilitate full electrolyte wetting and provide rapid ion diffusion channels; the defect sites formed by the nitrogen-containing carbon derived from ZIF-8 and activated by KOH construct abundant polar active sites, enhancing the material's chemical adsorption capacity for iodine species and promoting the reversible redox reaction of iodine species, thereby improving the utilization rate of active materials. The synergistic effect of physical confinement, rapid mass transfer, and chemical adsorption gives the cathode material of this invention a high specific capacity, excellent rate performance, and good cycle stability.
[0022] (3) The positive electrode material obtained in this invention exhibits high specific capacity, excellent rate performance and long cycle stability in zinc-iodine batteries due to the synergy of its structure and function, and effectively suppresses self-discharge and zinc anode corrosion.
[0023] (4) This invention uses waste cotton as raw material, which is widely available and inexpensive. The preparation process is mild and controllable, taking into account both economic efficiency and environmental friendliness, and has the potential for industrial application. Attached Figure Description
[0024] Figure 1 The N2 isothermal adsorption-desorption curves are shown for the cotton-based ZIF-8 porous carbon prepared in Example 1 of this invention and the pure ZIF-8 derived carbon prepared in Comparative Example 1.
[0025] Figure 2 The pore size distribution diagrams are shown for the cotton-based ZIF-8 porous carbon prepared in Example 1 of this invention and the pure ZIF-8 derived carbon prepared in Comparative Example 1.
[0026] Figure 3 Cyclic voltammetry curves of a zinc-iodine battery prepared using the cathode material of Example 1 at different scan rates.
[0027] Figure 4 Schematic diagram of the rate performance of zinc-iodine batteries prepared using the cathode materials of Examples 1 and Comparative Examples 1-7 of the present invention at different current densities.
[0028] Figure 5 Zinc-iodine batteries prepared using the cathode materials of Examples 1 and Comparative Examples 1-7 of this invention were tested at 1 A·g -1 Cycle lifetime and coulombic efficiency at current density. Detailed Implementation
[0029] The present application will now be described in further detail with reference to the accompanying drawings. It should be noted that the following specific embodiments are only used to further illustrate the present application and should not be construed as limiting the scope of protection of the present application. Those skilled in the art can make some non-essential improvements and adjustments to the present application based on the above application content.
[0030] The present invention achieves the following technical solution through at least one typical embodiment: The cotton-based ZIF-8 porous carbon provided by this invention is prepared by the following method: (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse the pretreated cotton in 150 mL of deionized water, transfer it to a 300 mL reaction vessel lined with para-polystyrene (PPL), and continue the reaction in a forced-air drying oven. After natural cooling, filter and wash to obtain cotton hydrothermal carbon. The amount of pretreated cotton can be any number between 2 g, 4 g, 6 g, 8 g or 2-8 g. The temperature of the forced-air drying oven can be any number between 200℃, 210℃, 220℃, 230℃ or 200-230℃. The reaction time can be any number between 12 h, 14 h, 16 h, 18 h, 20 h, 24 h or 12-24 h. (3) Disperse cotton hydrothermally in a zinc nitrate hexahydrate solution and stir at 25 °C for a period of time. The stirring time can be any number between 8 h, 10 h, 12 h, or 8-12 h to ensure that Zn 2+ Ions are fully adsorbed onto the oxygen-containing functional groups of hydrothermal carbon in cotton, providing anchoring sites for the uniform nucleation of ZIF-8. Then, they are slowly added to a 2-methylimidazole solution, stirred for a period of time, and then allowed to stand to obtain a cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers. The stirring time can be any number between 20 min, 30 min, 40 min, 50 min, 60 min, or 20-60 min, and the standing time can be any number between 6 h, 8 h, 10 h, 12 h, or 6-12 h. Furthermore, the zinc nitrate hexahydrate solution is prepared by dissolving zinc nitrate hexahydrate in methanol to form a solution of a certain concentration, which can be any number between 15 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, or 15-50 g / L; the 2-methylimidazole solution is prepared by dissolving 2-methylimidazole in methanol to form a solution of a certain concentration, which can be any number between 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L, 100 g / L, or 50-100 g / L. (4) Place the cotton-based ZIF-8 precursor in a tube furnace and heat it to 350 ℃ at a certain heating rate under an inert protective gas atmosphere. The heating rate can be any number between 5 ℃ / min, 10 ℃ / min or 5-10 ℃ / min. Hold it for a period of time for pre-carbonization. The holding time can be any number between 1 h, 2 h or 1-2 h. Then heat it to 900 ℃ at the same heating rate and hold it for 2 h for carbonization treatment to obtain cotton-based ZIF-8 activated carbon. (5) Mix cotton-based ZIF-8 activated carbon and KOH in a certain ratio and place them in a tube furnace. The mixing ratio (w:w) can be any number between 1:0.5, 1:1, 1:2, 1:3 or 1:(0.5-3). Under an inert protective gas atmosphere, heat the mixture to 800℃ at a rate of 5℃ / min and keep it for a period of time to activate and form pores. The holding time is any number between 1 h, 2 h or 1-2 h. The activated product is washed alternately with deionized water and anhydrous ethanol until the pH of the filtrate is neutral. The product is then dried to obtain cotton-based ZIF-8 porous carbon.
[0031] The cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material provided by this invention comprises porous carbon derived from a cotton-based in-situ grown ZIF-8 metal-organic framework compound and active iodine. The preparation method is as follows: The cotton-based ZIF-8 porous carbon prepared above is mixed with elemental iodine at any mass ratio between 1:2, 1:3, or 1:4. A small amount of anhydrous ethanol is added and the mixture is ground evenly. The mixture is placed in a sealed container and kept at any temperature between 150 ℃, 160 ℃, 170 ℃, or 150-170 ℃ for 2 h, 3 h, or 2-3 h, allowing the iodine to sublimate and diffuse into the pores of the porous carbon. Then, the mixture is transferred to an open container and kept at any temperature between 80 ℃, 90 ℃, or 80-90 ℃ for 1 h, 2 h, or 1-2 h, allowing the iodine adhering to the surface of the porous carbon to volatilize and remove excess iodine, thus obtaining the cotton-based ZIF-8 porous carbon iodine-loaded cathode material.
[0032] This invention provides a zinc-iodine battery, which is assembled using the cotton-based ZIF-8 porous carbon-supported iodine positive electrode material prepared above as the positive electrode, zinc foil as the negative electrode, and 2 mol / L ZnSO4 solution as the electrolyte.
[0033] Furthermore, the preparation method of the positive electrode is as follows: cotton-based ZIF-8 porous carbon-supported iodine positive electrode material, conductive carbon black, and binder are mixed in a mass ratio of 8:1:1, deionized water is added, and the mixture is ground into a uniform slurry. This slurry is then coated onto a 400-mesh stainless steel mesh and vacuum-dried at any temperature between 60℃, 70℃, 80℃, 90℃, or 60-90℃ for a period of time. After drying, the material is cut into electrode sheets, with drying times of any number between 6 h, 8 h, 10 h, 12 h, or 6-12 h. The surface area mass of the active material in the prepared positive electrode sheet is controlled to be 1.0-2.0 mg / cm². 2 Specifically, it is 1.0 mg / cm³. 2 1.5 mg / cm 2 2.0 mg / cm 2 Or 1.0-2.0 mg / cm 2 Any number between 0 and 1.
[0034] The present invention will be described below through specific embodiments. It should be noted that the specific embodiments below are for illustrative purposes only and do not limit the scope of the present invention in any way. In addition, unless otherwise specified, methods that do not specifically describe conditions or steps are conventional methods, and the reagents and materials used can be obtained commercially.
[0035] Example 1 This embodiment provides a method for preparing a cotton-based ZIF-8 porous carbon-supported iodine cathode material, including the following steps: 1.1 Preparation of cotton-based ZIF-8 porous carbon (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse 2 g of pretreated cotton in 150 mL of deionized water, transfer it to a 300 mL reaction vessel lined with para-polystyrene (PPL), and continue to react in a 200 °C drying oven for 24 h. After natural cooling, filter and wash to obtain hydrothermal carbon of cotton. (3) Dissolve 2 g of zinc nitrate hexahydrate in 130 mL of methanol to obtain solution A; dissolve 2.29 g of 2-methylimidazole in 40 mL of methanol to obtain solution B; disperse 2 g of hydrothermal carbon of cotton in solution A and stir at 25 °C for 8 h; then slowly add it to solution B, stir for 20 min, and let it stand for 12 h to obtain cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers; (4) Place the cotton-based ZIF-8 precursor in a tube furnace and heat it to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere. Hold it for 1 h for pre-carbonization. Then heat it to 900 °C at the same heating rate and hold it for 2 h for carbonization treatment to obtain cotton-based ZIF-8 derived carbon. (5) Mix cotton-based ZIF-8 derived carbon and KOH in a mass ratio of 1:1, place them in a tube furnace, heat them to 800 ℃ at a rate of 5 ℃ / min under an inert protective gas atmosphere, and maintain the temperature for 2 h to activate and form pores; wash the activated product alternately with deionized water and anhydrous ethanol until the pH of the filtrate is neutral, and dry it to obtain cotton-based ZIF-8 porous carbon.
[0036] 1.2 Preparation of cotton-based ZIF-8 porous carbon-supported iodine cathode material 150 mg of cotton-based ZIF-8 porous carbon was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the cotton-based ZIF-8 porous carbon iodine-loaded cathode material.
[0037] Comparative Example 1 This comparative example provides a method for preparing a pure ZIF-8 derived carbon-supported iodine cathode material, including the following steps: 1.1 Preparation of pure ZIF-8 derived carbon (1) Dissolve 2 g of zinc nitrate hexahydrate in 130 mL of methanol to obtain solution A; dissolve 2.29 g of 2-methylimidazole in 40 mL of methanol to obtain solution B; slowly add solution A to solution B, stir for 20 min, and let stand for 12 h to obtain ZIF-8 particles; (2) The ZIF-8 particle precursor was placed in a tube furnace and heated to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere and held for 1 h for pre-carbonization. Then, it was heated to 900 °C at the same heating rate and held for 2 h for carbonization treatment to obtain pure ZIF-8 derived carbon. 1.2 Preparation of pure ZIF-8 derived carbon-supported iodine cathode material 150 mg of pure ZIF-8 derived carbon was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining pure ZIF-8 derived carbon iodine-loaded cathode material.
[0038] Comparative Example 2 This comparative example provides a method for preparing a pure cotton activated carbon iodine-supported cathode material, including the following steps: 1.1 Preparation of pure cotton activated carbon (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) The pretreated cotton was placed in a tube furnace and heated to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere and held for 1 h for pre-carbonization. Then, the temperature was increased to 900 °C at the same heating rate and held for 2 h for carbonization treatment to obtain cotton carbon. (3) Mix cotton carbon and KOH in a mass ratio of 1:1, place them in a tube furnace, heat them to 800 ℃ at a rate of 5 ℃ / min under an inert protective gas atmosphere, and keep them for 2 h to activate and create pores; wash the activated product alternately with deionized water and anhydrous ethanol until the pH of the filtrate is neutral, and dry it to obtain pure cotton activated carbon.
[0039] 1.2 Preparation of pure cotton activated carbon iodine-supported cathode material 150 mg of pure cotton activated carbon was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the pure cotton activated carbon iodine-loaded cathode material.
[0040] Comparative Example 3 This comparative example provides a method for preparing a cotton-based hydrothermal activated carbon-supported iodine cathode material, comprising the following steps: 1.1 Preparation of cotton-based hydrothermal activated carbon (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse 2 g of pretreated cotton in 150 mL of deionized water, transfer it to a 300 mL reaction vessel lined with para-polystyrene (PPL), and continue to react in a 200 °C drying oven for 24 h. After natural cooling, filter and wash to obtain hydrothermal carbon of cotton. (3) Mix cotton hydrothermal activated carbon and KOH in a mass ratio of 1:1, place them in a tube furnace, heat them to 800 ℃ at a rate of 5 ℃ / min under an inert protective gas atmosphere, and maintain the temperature for 2 h to activate and create pores; wash the activated product alternately with deionized water and anhydrous ethanol until the pH of the filtrate is neutral, and dry it to obtain cotton-based hydrothermal activated carbon.
[0041] 1.2 Preparation of cotton-based hydrothermal activated carbon iodine-supported cathode material 150 mg of cotton-based hydrothermal activated carbon was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the cotton-based hydrothermal activated carbon iodine-loaded cathode material.
[0042] Comparative Example 4 This comparative example provides a method for preparing a cotton-based, non-in-situ grown ZIF-8 derived carbon-supported iodine cathode material, including the following steps: 1.1 Preparation of cotton-based non-in-situ grown ZIF-8 derived charcoal (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse 2g of pretreated cotton in 150 mL of deionized water, transfer it to a 300 mL reaction vessel lined with para-polystyrene (PPL), and continue to react in a 200 °C drying oven for 24 h. After natural cooling, filter and wash to obtain cotton hydrothermal carbon. (3) Dissolve 2 g of zinc nitrate hexahydrate in 130 mL of methanol to obtain solution A; dissolve 2.29 g of 2-methylimidazole in 40 mL of methanol to obtain solution B; slowly add solution A to solution B, stir for 20 min, and let stand for 12 h to obtain ZIF-8 particles; add 2 g of cotton hydrothermal carbon, stir for 2 h to obtain cotton non-in-situ growth ZIF-8 precursor; (4) The cotton non-in-situ ZIF-8 precursor was placed in a tube furnace and heated to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere and held for 1 h for pre-carbonization. Then, the temperature was increased to 900 °C at the same heating rate and held for 2 h for carbonization treatment to obtain cotton-based non-in-situ ZIF-8 derived carbon.
[0043] 1.2 Preparation of cotton-based non-in-situ grown ZIF-8 derived carbon-supported iodine cathode material 150 mg of cotton-based non-in-situ grown ZIF-8 derivative carbon was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the cotton-based non-in-situ grown ZIF-8 derivative carbon iodine-loaded cathode material.
[0044] Comparative Example 5 This comparative example provides a method for preparing a cotton-based ZIF-8 derived carbon ① iodine-supported cathode material, including the following steps: 1.1 Preparation of cotton-based ZIF-8 derived char (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse 2g of pretreated cotton in 150mL of deionized water, transfer it to a 300mL reaction vessel lined with para-polystyrene (PPL), and continue to react in a 200℃ drying oven for 24h. After natural cooling, filter and wash to obtain cotton hydrothermal carbon. (3) Dissolve 2g of zinc nitrate hexahydrate in 130mL of methanol to obtain solution A; dissolve 2.29g of 2-methylimidazole in 40mL of methanol to obtain solution B; disperse 2g of hydrothermal carbon of cotton in solution A and stir at 25℃ for 8h; then slowly add it to solution B, stir for 20min, and let it stand for 12h to obtain cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers; (4) The cotton-based ZIF-8 precursor was placed in a tube furnace and heated to 350°C at a rate of 5°C / min under an inert protective gas atmosphere and held for 1 hour for pre-carbonization. Then, the temperature was increased to 900°C at the same rate and held for 2 hours for carbonization treatment to obtain cotton-based ZIF-8 derived carbon ①.
[0045] 1.2 Preparation of cotton-based ZIF-8 derived carbon ① iodine-loaded cathode material 150 mg of cotton-based ZIF-8 derived carbon ① was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the cotton-based ZIF-8 derived carbon ① iodine-loaded cathode material.
[0046] Comparative Example 6 This comparative example provides a method for preparing a cotton-based ZIF-8 derived carbon ② iodine-supported cathode material, including the following steps: 1.1 Preparation of cotton-based ZIF-8 derived char ② (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse 2g of pretreated cotton in 150mL of deionized water, transfer it to a 300mL reaction vessel lined with para-polystyrene (PPL), and continue to react in a 200℃ drying oven for 12h. After natural cooling, filter and wash to obtain cotton hydrothermal carbon. (3) Dissolve 2g of zinc nitrate hexahydrate in 130mL of methanol to obtain solution A; dissolve 2.29g of 2-methylimidazole in 40mL of methanol to obtain solution B; disperse 2g of hydrothermal carbon of cotton in solution A and stir at 25℃ for 8h; then slowly add it to solution B, stir for 20min, and let it stand for 12h to obtain cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers; (4) The cotton-based ZIF-8 precursor was placed in a tube furnace and heated to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere and held for 1 h for pre-carbonization. Then, the temperature was increased to 900 °C at the same heating rate and held for 2 h for carbonization treatment to obtain cotton-based ZIF-8 derived carbon ②.
[0047] 1.2 Preparation of cotton-based ZIF-8 derived carbon ② iodine-loaded cathode material 150 mg of cotton-based ZIF-8 derived carbon ② was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the cotton-based ZIF-8 derived carbon ② iodine-loaded cathode material.
[0048] Comparative Example 7 This comparative example provides a method for preparing a cotton-based pre-carbonized carbon-based ZIF-8 porous carbon-supported iodine cathode material, including the following steps: 1.1 Preparation of cotton pre-carbonized carbon-based ZIF-8 derived carbon (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Place the pretreated cotton in a tube furnace and heat it to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere, and keep it for 1 h to carry out cotton pre-carbonization. (3) Dissolve 2 g of zinc nitrate hexahydrate in 130 mL of methanol to obtain solution A; dissolve 2.29 g of 2-methylimidazole in 40 mL of methanol to obtain solution B; disperse 2 g of cotton pre-carbonized carbon in solution A and stir at 25 °C for 8 h; then slowly add it to solution B, stir for 20 min, and let it stand for 12 h to obtain cotton pre-carbonized carbon-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers; (4) The cotton pre-carbonized carbon-based ZIF-8 precursor was placed in a tube furnace and heated to 350 °C at a rate of 5 °C / min under an inert protective gas atmosphere and held for 1 h for pre-carbonization. Then, the temperature was increased to 900 °C at the same heating rate and held for 2 h for carbonization treatment to obtain cotton pre-carbonized carbon-based ZIF-8 derived carbon. (5) Mix cotton precarbonized carbon-based ZIF-8 derived carbon with KOH at a mass ratio of 1:1, place in a tube furnace, heat to 800 ℃ at a rate of 5 ℃ / min under an inert protective gas atmosphere, and maintain for 2 h to activate and form pores; wash the activated product alternately with deionized water and anhydrous ethanol until the pH of the filtrate is neutral, and dry to obtain cotton precarbonized carbon-based ZIF-8 porous carbon.
[0049] 1.2 Preparation of cotton-based pre-carbonized carbon-based ZIF-8 porous carbon-supported iodine cathode material 150 mg of cotton-based pre-carbonized carbon-based ZIF-8 porous carbon was mixed with 450 mg of elemental iodine, and a small amount of anhydrous ethanol was added and ground evenly. The mixture was placed in a sealed high-pressure container and kept at 150 °C for 3 h to allow the iodine to sublimate and diffuse into the pores of the porous carbon. Then, it was transferred to an open container and kept at 90 °C for 2 h to volatilize the iodine adhering to the surface of the porous carbon and remove excess iodine, thus obtaining the cotton-based pre-carbonized carbon-based ZIF-8 porous carbon iodine-loaded cathode material.
[0050] Verification test 1. To evaluate the specific surface area and pore size distribution of cotton-based ZIF-8 porous carbon materials, nitrogen adsorption / desorption isotherm analysis was performed on the cotton-based ZIF-8 porous carbon prepared in Example 1 and the pure ZIF-8 derived carbon prepared in Comparative Example 1, respectively. The N2 isotherm adsorption-desorption curves are shown below. Figure 1 As shown; and based on the isothermal adsorption-desorption curves, the pore size distribution was analyzed, as follows. Figure 2 As shown.
[0051] Depend on Figure 1 As can be seen, the cotton-based ZIF-8 porous carbon of Example 1 exhibits a steep adsorption increase in the extremely low relative pressure region (P / P0 < 0.01), indicating that there are a large number of micropores within the material generated by the ZIF-8 carbonized framework micropores and KOH-activated etching. These micropores constitute physically confined iodine species and polyiodide ions (such as I3). - I5 - The main space of the membrane can suppress the shuttle effect at its source. Within the relative pressure range of 0.01–0.8, the adsorption curve shows a gradual and continuous rise, reflecting the transition from monolayer to multilayer adsorption, indicating that the existence of the mesoporous structure provides channels for electrolyte penetration and ion diffusion. When the relative pressure exceeds 0.9, the adsorption amount increases sharply, confirming that the carbon skeleton of cotton fiber forms a rich mesoporous network after carbonization shrinkage and activation pore expansion.
[0052] The cotton-based ZIF-8 porous carbon in Example 1 has a specific surface area as high as 1443 m². 2 / g, higher than the 917 m of pure ZIF-8 derived carbon in Comparative Example 1. 2The micropores and mesopores form a continuous, interconnected hierarchical pore system. This structural feature provides direct structural evidence for the synergistic function of strong micropore confinement and fast mesopore transport in cotton-based ZIF-8 porous carbon materials.
[0053] Depend on Figure 2 The pore size distribution curves (DFT model) of the cotton-based ZIF-8 porous carbon in Example 1 and the pure ZIF-8 derived carbon in Comparative Example 1 show that the sample in Example 1 exhibits a typical multi-peak distribution: sharp, narrow peaks exist in the <2 nm micropore region, attributed to the inherent micropores of the ZIF-8 carbonization framework and newly created micropores generated by KOH activation etching. These micropores provide high-density physical constraint sites, serving as the first barrier to inhibit polyiodide ion shuttle. Broad peaks appear in the 2–5 nm and >10 nm regions, originating from the carbonization retention of the natural structure of cotton fibers and the mesoporous channels formed by activation and pore expansion, providing a low-resistance backbone network for electrolyte wetting and rapid ion transport. In contrast, the pore size distribution of the pure ZIF-8 derived carbon in Comparative Example 1 is concentrated in the <2 nm micropore region, with an extremely low proportion of mesopores, exhibiting an overall single-peak narrow distribution characteristic and lacking effective ion transport channels. A comparison of the two demonstrates that this invention, using cotton fiber as a biomass template, successfully integrates the microporous confinement advantage of ZIF-8 derived carbon with the mesoporous transport function of the cotton carbon skeleton, forming a hierarchical porous structure with a micropore-mesopore gradient. This structure, on the one hand, achieves strong physical confinement of iodine species through abundant micropores, and on the other hand, accelerates electrolyte penetration and ion migration through mesopores, ensuring efficient utilization of active sites inside the electrode. The single microporous structure in Comparative Example 1 cannot achieve this effect.
[0054] 2. Electrochemical performance testing The positive electrode materials prepared in Example 1 and Comparative Examples 1-7 were mixed with conductive carbon black and binder in a mass ratio of 8:1:1, and 2 mL of deionized water was added to grind them into a uniform slurry. The slurry was coated on a 400-mesh stainless steel mesh, vacuum dried at 80°C for 8 hours, and then cut into electrode sheets. The electrode sheets were then used as the positive electrode, zinc foil as the negative electrode, and 2 mol / L ZnSO4 solution as the electrolyte to assemble a zinc-iodine battery.
[0055] (1) Cyclic Voltammetry (CV) Test The zinc-iodine battery prepared using the cathode material of Example 1 was subjected to cyclic voltammetry testing.
[0056] like Figure 3 As shown, the zinc-iodine battery prepared using the cathode material of Example 1 exhibits stable cyclic voltammetry curves at different scan rates. The redox peaks in the figure correspond to continuous oxidation and reduction reactions, indicating that it has good electrochemical reversibility.
[0057] (2) Ratio performance test Zinc-iodine batteries prepared using the cathode materials of Example 1 and Comparative Examples 1-7 were subjected to rate performance tests at current densities of 0.2 A / g, 0.4 A / g, 0.6 A / g, 0.8 A / g, 1 A / g, 2 A / g, 5 A / g, and 0.2 A / g, respectively. The results are shown in Table 1 below. Figure 4 As shown.
[0058] Table 1. Specific capacity of zinc-iodine batteries in the examples and comparative examples at different current densities, based on rate performance tests. ; According to Table 1 and Figure 4 The rate performance test results show that: The zinc-iodine battery prepared using the cathode material of Example 1 exhibited significantly higher specific capacity at all tested current densities (0.2–5 A / g) than the zinc-iodine batteries prepared using the cathode materials of Comparative Examples 1–7. In particular, when the current density increased from 0.2 A / g to 5 A / g (a 25-fold increase), the capacity retention of Example 1 reached 73.7% (146 mAh·g). -1 / 198mAh·g -1 The capacity of the example was superior to that of Comparative Example 1 (68.1%), Comparative Example 2 (29.5%), Comparative Example 3 (51.2%), Comparative Example 4 (55.0%), Comparative Example 5 (64.9%), Comparative Example 6 (60.1%), and Comparative Example 7 (56.5%). When the current returned to 0.2 A / g, the capacity of the example recovered to 197 mAh·g. -1 The recovery rate is as high as 99.5%, proving that its structure has no irreversible damage after high current impact.
[0059] The superior rate performance is primarily attributed to the synergistic effect of the hierarchical porous structure and interfacial active sites constructed in this invention. The micropores are mainly composed of micropores formed by ZIF-8 carbonization and micropores generated by KOH activation etching, effectively confining iodine and polyiodide ions and suppressing the rapid dissolution of active materials during high-rate charge and discharge. The mesopores originate from the skeletal structure retained after cotton fiber carbonization and the channels formed by further activation and expansion with KOH, providing low-torsion diffusion channels for sufficient electrolyte wetting and rapid ion transport, significantly reducing mass transfer resistance and concentration polarization. Simultaneously, the nitrogen-doped carbon layer derived from ZIF-8 and the abundant defect sites introduced by KOH activation jointly construct a polar active interface, which can promote I3 under high current density conditions. - / I -The redox reaction kinetics accelerate the reversible transformation of polyiodide ions, reducing their accumulation within the pores and thus further improving the utilization rate of the active material. The synergistic effect of the hierarchical pore structure, continuous conductive network, and polar active sites collectively endows the examples with superior rate performance compared to the comparative examples.
[0060] In contrast, Comparative Example 1 has only a single microporous structure and lacks efficient ion transport channels, limiting mass transfer efficiency under high-rate conditions; Comparative Examples 2 and 3 lack ZIF-8-derived polar active sites, resulting in insufficient chemisorption and redox kinetics for polyiodide ions; Comparative Example 4 uses an in-situ growth method to load ZIF-8, resulting in weak interfacial bonding between MOF particles and the cotton substrate, limiting the uniformity and utilization of active sites, making it difficult to form a stable interfacial synergistic effect; Comparative Example 5 was not activated with KOH, failing to form a rich hierarchical pore structure and activation defect sites, leading to decreased electrolyte wetting ability and ion transport efficiency; Comparative Example 6, due to shortened hydrothermal treatment time, resulted in insufficient generation of oxygen-containing functional groups and in-situ nucleation sites on the cotton surface, leading to a reduced degree of in-situ growth of ZIF-8; Comparative Example 7 uses pre-carbonized carbon as a precursor, which reduces its surface active sites, making it difficult to achieve tight interfacial coupling between ZIF-8 and the carbon substrate, resulting in decreased utilization of active sites, ultimately failing to achieve the synergistic enhancement effect of physical confinement, chemisorption, and redox kinetics constructed in this invention.
[0061] (3) Galvanostatic Charge-Discharge Cycling (GCD Cycling) For zinc-iodine batteries prepared using the cathode materials of Example 1 and Comparative Examples 1-7, respectively, at 1 A·g -1 Constant current charge-discharge cycle test was performed at current density.
[0062] Cycle life and coulombic efficiency curves are as follows Figure 5 As shown, the initial discharge specific capacity of Example 1 is 187 mAh·g. -1 After 1300 consecutive charge-discharge cycles, the capacity remained stable at 183 mAh·g. -1 The capacity retention rate was as high as 97.8%, and the average decay rate per cycle was only 0.0016%; at the same time, the coulombic efficiency remained stable between 99.8% and 100%, indicating that the electrode has excellent cycle stability and reversibility. In contrast, the capacity retention rates of Comparative Examples 1 to 7 were only 89%, less than 70%, about 90%, 92%, 80%, 75%, and 93%, respectively, all lower than that of Example 1.
[0063] The results show that the in-situ growth of ZIF-8 combined with KOH activation can effectively improve the cycling stability of the electrode material, significantly reduce capacity decay, and enable the zinc-iodine battery to maintain more stable electrochemical performance during long-term cycling.
[0064] It should be noted that, Figure 5 1A·g -1 The initial capacity (187mAh·g) -1 Slightly higher than the value in Table 1 for the rate test at the same current (176 mAh·g) -1 This is because the two tests are conducted independently. The rate test involves a gradual increase in current, resulting in accumulated polarization and a slight irreversible capacity loss; while... Figure 4 The cyclic test is performed directly at 1 A·g in the first lap. -1 Under normal operating conditions, with sufficient electrolyte wetting and electrode activation, the active sites are utilized more fully. This difference does not affect the comparative conclusion of the intrinsic properties of the material; both consistently demonstrate the superiority of the cathode material of this invention.
[0065] The embodiments described above are merely examples of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these modifications and improvements all fall within the scope of protection of the present invention.
Claims
1. A cotton-based ZIF-8 porous carbon zinc-iodine battery anode material, characterized in that, Includes cotton-based ZIF-8 porous carbon and active iodine supported in the pores of the cotton-based ZIF-8 porous carbon; The cotton-based ZIF-8 porous carbon is based on a three-dimensional carbon skeleton formed by hydrothermal carbonization of cotton fibers. On its surface, regular octahedral ZIF-8 nanoparticles are generated in situ. After the cotton-based ZIF-8 precursor is pre-carbonized and carbonized, it is then activated to form an integrated porous carbon with a microporous-mesoporous hierarchical pore structure.
2. The cotton-based ZIF-8 porous carbon zinc-iodine battery anode material of claim 1, wherein, The micropore size of the cotton-based ZIF-8 porous carbon is concentrated below 2 nm, and the mesopore size of the cotton-based ZIF-8 porous carbon is distributed in the range of 2-50 nm.
3. The cotton-based ZIF-8 porous carbon zinc-iodine battery anode material of claim 1, wherein, The mass ratio of cotton-based ZIF-8 porous carbon to activated iodine is 1:2-4.
4. A method for preparing the cotton-based ZIF-8 porous carbon zinc iodine battery anode material according to any one of claims 1-3, characterized in that, Includes the following steps: (1) Tear the cotton into pieces, wash and dry it to obtain pretreated cotton; (2) Disperse the pretreated cotton in deionized water, place it in a reaction vessel and hydrothermally react at 200-230 °C for 12-24 h. After natural cooling, filter and wash to obtain cotton hydrothermal carbon. (3) Disperse the hydrothermal carbon of cotton in zinc nitrate hexahydrate solution and stir to adsorb, then slowly add it to 2-methylimidazole solution, stir to react and let stand to obtain cotton-based ZIF-8 precursor with octahedral ZIF-8 nanoparticles grown in situ on cotton fibers. (4) The cotton-based ZIF-8 precursor was heated to 350°C at a rate of 5-10°C / min under an inert protective gas atmosphere and held for 1-2 h for pre-carbonization. Then, it was heated to 900°C at the same heating rate and held for 2 h for carbonization treatment to obtain cotton-based ZIF-8 activated carbon. (5) Mix cotton-based ZIF-8 activated carbon with KOH evenly, heat to 800 ℃ at a rate of 5 ℃ / min under an inert protective gas atmosphere, and maintain for 1-2 h to activate and form pores. Wash the obtained activated product until neutral and then dry it to obtain cotton-based ZIF-8 porous carbon. (6) Mix and grind cotton-based ZIF-8 porous carbon with elemental iodine, heat under closed conditions to sublimate the iodine and diffuse it into the porous carbon channels, and then heat in an open manner to remove excess iodine from the surface to obtain cotton-based ZIF-8 porous carbon zinc-iodine battery cathode material.
5. The preparation method according to claim 4, characterized in that, In step (3), the zinc nitrate hexahydrate solution is prepared by dissolving zinc nitrate hexahydrate in methanol to form a solution with a concentration of 10-50 g / L; the 2-methylimidazole solution is prepared by dissolving 2-methylimidazole in methanol to form a solution with a concentration of 50-100 g / L.
6. The preparation method according to claim 4, characterized in that, In step (5), the preparation method of the cotton-based ZIF-8 precursor is specifically as follows: the cotton hydrothermal carbon is first dispersed in a zinc nitrate hexahydrate solution, stirred at 25 ℃ for 8-12 h to make Zn² + After being fully adsorbed, it is added dropwise into a 2-methylimidazole solution, stirred for 20-60 min, and then left to stand for 6-12 h.
7. The preparation method according to claim 4, characterized in that, In step (5), the mass ratio of cotton-based ZIF-8 activated carbon to KOH is 1:(0.5-3), the activation temperature is increased to 800 ℃ at a rate of 5 ℃ / min, and the holding time is 1-2h.
8. The preparation method according to claim 4, characterized in that, In step (6), cotton-based ZIF-8 porous carbon and elemental iodine are mixed at a mass ratio of 1:2-4, anhydrous ethanol is added and ground evenly, and the iodine is sublimated under sealed conditions at 150-170 ℃ for 2-3 h, and then the surface free iodine is removed under open conditions at 80-90 ℃ for 1-2 h.
9. A zinc-iodine cell characterized in that, The application relates to a zinc-iodine battery positive electrode material, which comprises a positive electrode, a negative electrode and an electrolyte; the positive electrode is a cotton-based ZIF-8 porous carbon loaded iodine zinc-iodine battery positive electrode material according to any one of claims 1-3, the negative electrode is a zinc foil, and the electrolyte is a ZnSO4 aqueous solution.
10. The zinc-iodine cell of claim 9, wherein, The preparation method of the positive electrode is as follows: cotton-based ZIF-8 porous carbon loaded iodine positive electrode material, conductive carbon black and a binder are mixed according to a mass ratio of 8:1:1, deionized water is added to grind into a uniform slurry, the slurry is coated on a stainless steel current collector, vacuum drying is carried out at 60-90 DEG C for 6-12 h, and then the positive electrode sheet is cut; the surface density of the active material in the positive electrode sheet is 1.0-2.0 mg / cm2; and the electrolyte is a 2mol / L ZnSO4 aqueous solution.