A composite anode material of waste silicon and waste graphite grown in situ by trimetallic synergistic catalysis of carbon nanotubes, its preparation method and application

Carbon nanotubes were generated in situ in lithium-ion battery anode materials by synergistic catalysis of Ca2+-Cu2+-Al3+ trimetallic ions, which solved the problems of volume expansion and conductivity of silicon-based anode materials and achieved efficient self-construction of conductive networks and ultra-long cycle stability.

CN123120697APending Publication Date: 2026-11-17YANCHENG INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611409687.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, silicon-based anode materials for lithium-ion batteries suffer structural damage due to volume expansion during charging and discharging, resulting in poor conductivity. Furthermore, they rely on external carbon nanotubes as conductive additives and lack functional applications for in-situ growth of carbon nanotubes through multi-metal synergistic catalysis.

Method used

A three-metal ion synergistic catalysis method of Ca2+-Cu2+-Al3+ was adopted to generate carbon nanotubes in situ during high-temperature carbonization, constructing a three-dimensional network structure. The synergistic effect of calcium, copper and aluminum was used to construct a conductive pathway, eliminating the dependence on externally added carbon nanotubes.

Benefits of technology

A high-density, uniformly distributed carbon nanotube network was achieved, which improved the battery's conductivity and cycle stability, significantly simplified the process, reduced raw material costs, and maintained excellent capacity retention at high current densities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120697A_ABST
    Figure CN123120697A_ABST
Patent Text Reader

Abstract

This invention relates to a waste silicon and waste graphite composite anode material for in-situ growth of carbon nanotubes via trimetallic synergistic catalysis. The material comprises a three-dimensional structure consisting of a graphite waste framework, porous carbon carbonized with sodium alginate, calcium-copper-aluminum catalyzed carbon nanotubes, and nano-silicon. Preparation: Waste silicon source and graphite are dispersed, copper sulfate and sodium alginate are added, followed by initial cross-linking with calcium chloride, then dense cross-linking with polyaluminum chloride, freeze-drying, and carbonization. The three metals synergistically catalyze the generation of carbon nanotubes. Comparative analysis shows that only Ca... 2+ Carbon nanotubes are sparse, Ca 2+ +Cu 2+ The density increases but is not uniform; only the three metals achieve a high-density, uniform network. Electrochemical performance: half-cell 0.5 A g ‑1 The capacity retention rate is as high as 94.6% after 100 cycles, and the full cell has a capacity of 1 A g. ‑1 The capacity retention rate reaches 94% after 100 cycles. This invention provides a composite anode material preparation scheme for the resource utilization of waste silicon and waste graphite. The preparation method is simple, the performance is excellent, and it has extremely high practical value and commercial prospects.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Technical Field: This invention belongs to the technical field of lithium-ion battery anode materials and industrial solid waste resource utilization, specifically relating to a method for utilizing waste silicon and waste graphite as raw materials, through Ca... 2+ -Cu 2+ -Al 3+ A composite anode material with in-situ growth of carbon nanotubes synergistically catalyzed by three metal ions and hierarchical crosslinking synergistically constructed three-dimensional network structure, as well as the preparation method of the material and its application in lithium-ion batteries. Background Technology

[0002] Lithium-ion batteries, with their high energy density and long cycle life, have become dominant in portable electronic devices, electric vehicles, and renewable energy storage systems. However, as the market demands for higher energy density, faster charge / discharge rates, and longer cycle life, traditional graphite anode materials are limited by their small capacity of only 372 mAh g⁻¹. -1 The theoretical specific capacity of silicon is gradually becoming insufficient to meet the development needs of next-generation high-energy storage systems. Silicon, with its high specific capacity of approximately 4200 mAh g⁻¹, is no longer sufficient. -1 With its theoretical specific capacity, low lithium intercalation potential, and abundant reserves, silicon-based anode material is widely recognized as one of the most promising next-generation lithium-ion battery anode materials. However, the commercial application of silicon-based anodes faces severe technical challenges: silicon undergoes a massive volume expansion of nearly 300% during charging and discharging, leading to silicon particle expansion and breakage, electrode structure damage, and repeated rupture and regeneration of the solid electrolyte interphase (SEI) film. At the same time, silicon itself has poor conductivity, which severely restricts the rate performance and fast charge / discharge capability of the battery.

[0003] To address the aforementioned problems, constructing silicon-carbon composite materials is considered one of the most effective approaches. Sodium alginate, a natural linear polysaccharide extracted from brown algae, contains a large number of carboxyl groups (-COO) in its molecular chain. - Sodium alginate contains hydroxyl groups (-OH) and exhibits good water solubility and ion-complexing ability. When sodium alginate reacts with Ca... 2+ When in contact with polyvalent cations, ionic cross-linking reactions can occur, forming a stable hydrogel network with an "egg box" structure, which can be transformed into a three-dimensional porous carbon skeleton after carbonization.

[0004] Technological progress and unresolved technical problems of existing alginate hydrogel crosslinking systems:

[0005] Category 1: Sodium alginate + Ca 2+ Single-metal crosslinking system. Sodium alginate hydrogels were first reported in 2014 via Ca... 2+ Crosslinking, used as a binder for Si / C anodes, significantly improved electrode cycle stability. Subsequent studies have largely continued this approach, using Ca... 2+Cross-linked sodium alginate acts as a binder to anchor silicon particles. Recent research further utilizes Ca... 2+ Coordination with the carboxyl groups of sodium alginate enhances the bonding strength between silicon nanoparticles and carbon nanotubes, preventing silicon from separating from the carbon nanotube network. However, a key limitation of this approach lies in: Ca 2+ The cross-linked sodium alginate network transforms into amorphous carbon after carbonization, exhibiting poor electronic conductivity, and Ca... 2+ It only serves as a crosslinking node and does not possess the function of catalyzing the graphitization of carbon materials. More importantly, it contains only Ca. 2+ Cross-linked systems cannot generate carbon nanotubes in situ during carbonization and must rely on externally added carbon nanotubes as conductive additives.

[0006] Category 2: Sodium alginate + Al 3+ or Cu 2+ Single-metal crosslinking systems. Al has been reported in the literature. 3+ Cross-linked alginate hydrogels as binders for silicon anodes, and through Cu... 2+ The preparation of self-supporting silicon anodes using sodium alginate aerogel is an enhanced process. However, the aforementioned methods all involve single-metal ion crosslinking, and their functional positioning is limited to improving the mechanical strength of the binder. These disclosed methods primarily focus on the regulation of the alginate network structure, bonding performance, or electrode stability by a single metal ion. A search by the applicant revealed no publicly available method for preparing composite anode materials using waste silicon, waste graphite, and sodium alginate as precursors, and through the sequential introduction of calcium-containing, copper-containing, and aluminum-containing components as described in this application.

[0007] The third category: bimetallic crosslinking systems. In recent years, bimetallic crosslinking systems have also been reported, such as sodium alginate sequentially crosslinked with calcium ions and hyperbranched polyethyleneimine to construct a bi-crosslinked network adhesive. However, these are all two-step sequential introductions, with no clear synergistic division of labor between the metals, and remain limited to the adhesive level.

[0008] Existing technologies for metal-catalyzed carbon nanotube growth. In non-alginate systems, research on transition metal (Fe, Co, Ni) catalytic carbon nanotube growth is relatively mature, usually relying on chemical vapor deposition (CVD) processes, requiring external gaseous carbon sources such as acetylene and methane at 500-800℃ to achieve carbon nanotube growth. In recent years, studies have reported that calcium, as a contaminant, can promote the growth of carbon nanotubes on the carbon fiber surface, aluminum, as a catalyst support or promoter, can enhance catalyst stability and inhibit catalyst particle aggregation, and alumina (Al2O3) supported catalysts have shown high initial growth rates and long activity durations in carbon nanotube synthesis. However, the above studies all have the following limitations: (1) they rely on external carbon sources, rather than utilizing the carbon-containing gas generated in situ during the carbonization process of the system itself; (2) the metal catalyst is introduced as an externally supported catalyst, rather than being uniformly dispersed inside the hydrogel network through ionic crosslinking; (3) there are no reports of synergistic introduction of calcium, copper, and aluminum ions into the same system and utilizing their synergistic catalytic effect to achieve in-situ growth of carbon nanotubes.

[0009] Polyaluminum chloride (PAC), as an inorganic polymeric flocculant, is mainly used in the field of water treatment. The applicant's search revealed no publicly available schemes for using PAC as an aluminum source in the preparation of the waste silicon-waste graphite-sodium alginate composite negative electrode precursor described in this application.

[0010] More importantly, the applicant's search revealed no reports of in-situ carbon nanotube generation in alginate hydrogel systems synergistically catalyzed by metals (Ca-Cu-Al). Existing alginate hydrogel crosslinking systems utilize metal ions primarily for constructing network frameworks through simple ionic crosslinking; no reports have been found of in-situ carbon nanotube growth achieved through the synergistic catalytic effect of multiple metal ions during high-temperature carbonization. This invention is the first to discover that: [The text abruptly ends here, likely due to an incomplete sentence or missing information.] 2+ The cross-linked sample showed sparse carbon nanotube growth after carbonization; it contained only Ca. 2+ +Cu 2+ The bimetallic samples showed increased carbon nanotube density but uneven distribution; only in Ca... 2+ +Cu 2+ +Al 3+ Carbon nanotubes exhibit a high-density, uniformly distributed three-dimensional interwoven network only in systems where three metals coexist. This discovery reveals the irreplaceable synergistic catalytic effect of the Ca-Cu-Al trimetallic trimetallic compounds in the in-situ growth of carbon nanotubes.

[0011] The following technical problems urgently need to be solved in the existing technology:

[0012] (1) The function of trimetallic synergistic catalysis of in-situ carbon nanotube growth has not been recognized or utilized. In existing alginate hydrogel systems, the function of metal ions is limited to ionic crosslinking, and their functional application in synergistic catalysis of in-situ carbon nanotube generation during high-temperature carbonization has not been reported.

[0013] (2) Lack of multi-metal synergistic division of labor design. In the existing technology, metal ion crosslinking is done by a single metal ion or sequentially introduced bimetallic ions. No technical solutions have been reported for the synchronous and synergistic introduction of three metal ions in the same system and the assignment of clear functional division of labor.

[0014] (3) According to the applicant's search, no application of PAC in silicon-carbon anodes has been found. The functions of PAC as an aluminum source and structural densification modifier have not been developed. 3+ The promoting effect of Ca-Cu-Al trimetallic synergistic catalysis has not been recognized.

[0015] (4) There is a lack of integrated solutions for the simultaneous resource utilization and structural optimization of waste silicon and waste graphite.

[0016] (5) Existing preparation methods rely on the addition of carbon nanotubes as conductive additives, rather than the self-construction of conductive networks through in-situ catalytic growth.

[0017] It is particularly noteworthy that in existing research on alginate-based composite materials, the function of metal ions has been strictly limited to ionic crosslinking to construct a network framework, and research on their catalytic behavior during high-temperature carbonization is still lacking. Specifically, the existence and mechanism of synergistic catalytic effects of three metal ions with different chemical properties in the same system are not documented or revealed in existing technologies. Regarding the catalytic growth of carbon nanotubes, while known literature reports the nucleation-promoting effect of Ca, the catalytic activity of Cu, and the support function of Al₂O₃, these studies are all based on independent systems or external catalysts. No research has ever simultaneously introduced Ca, Cu, and Al into the same alginate hydrogel system in situ, nor has it revealed the indispensable synergistic catalytic mechanism among the three. Therefore, the synergistic phenomenon revealed for the first time in this invention through systematic comparative experiments is not a simple combination of existing technologies, but a fundamental breakthrough in the functional design principles of alginate-based composite materials.

[0018] Therefore, developing a composite anode material that enables efficient resource utilization of waste silicon and graphite, achieves in-situ growth of carbon nanotubes through the synergistic catalysis of calcium-copper-aluminum trimetallic elements, and constructs a three-dimensional network structure through hierarchical cross-linking, along with its simple preparation method, is of significant research importance and application value. Summary of the Invention

[0019] The purpose of this invention is to provide a waste silicon and waste graphite-based composite anode material with stable structure and effective buffering of silicon volume expansion, and its preparation method, so as to solve the key technical problems in the prior art, such as poor carbon conductivity, insufficient cycle stability, and dependence on external carbon nanotubes.

[0020] To achieve the above objectives, this invention first provides a waste silicon and waste graphite composite anode material for in-situ growth of carbon nanotubes synergistically catalyzed by three metals. The composite material is characterized by a three-dimensional composite structure consisting of a conductive framework formed from graphite waste, a porous carbon network formed by the carbonization of sodium alginate, a carbon nanotube network synergistically catalyzed by calcium-copper-aluminum trimetallic ions during high-temperature carbonization, and nano-silicon particles uniformly coated and embedded in the conductive framework and porous carbon network. The composite material is simultaneously doped with calcium, copper, and aluminum, which are highly dispersed in the carbon matrix of the composite material, exhibiting spatial overlap in STEM-EDS elemental surface scans and without detected metal or metal oxide impurity diffraction peaks in XRD patterns. The carbon nanotubes are grown using Ca... 2+ -Cu 2+ -Al 3+ The synergistic catalytic effect of the three metal ions during the high-temperature carbonization process generates them in situ, constructing an additional conductive pathway; the molar ratio of the three metal elements calcium, copper, and aluminum is Ca:Cu:Al = (4.8~5.2):(0.9~1.1):(2~5); the XPS full spectrum of the composite material simultaneously contains characteristic peaks of Ca2p, Cu2p, and Al2p; the diameter of the carbon nanotubes is 20-40 nm, and they form a three-dimensional interwoven network.

[0021] Furthermore, the effective molar ratio of the three metal elements calcium, copper, and aluminum is Ca:Cu:Al = 5:1:3.

[0022] Furthermore, the calcium element is Ca 2+ The copper element exists in the form of metallic copper or low-valence copper oxide, serving as a catalytic active center for carbon nanotube growth during carbonization; the aluminum element is derived from PAC, in the form of Al2O3, aluminate, or Al... 3+ The coordination form exists, on the one hand, for use in Ca 2+ On the basis of cross-linked networks, the degree of cross-linking and structural compactness are further enhanced to form a hierarchical cross-linking density structure. On the other hand, it serves as a catalyst support to inhibit the aggregation of copper particles and promote the uniform growth of carbon nanotubes.

[0023] Furthermore, the silicon nanoparticles have a size of 30-50 nm and are coated with a carbon layer with a thickness of 10-20 nm; the composite material has a specific surface area of ​​10-20 m². 2 / g, mainly mesoporous structure, with pore size mainly distributed in the range of 2-20 nm.

[0024] This invention also provides a method for preparing the above-mentioned waste silicon and waste graphite composite anode material, characterized by comprising the following steps:

[0025] (1) Deionized water and anhydrous ethanol were mixed to form a dispersion system, waste silicon source was added, ultrasonic dispersion was performed, and then graphite waste powder treated at high temperature was added and ultrasonic dispersion was continued to obtain a uniform Si-G mixed suspension.

[0026] (2) Add CuSO4 solution and sodium alginate solution to the Si-G mixed suspension obtained in step (1) in sequence, and stir ultrasonically to mix the components thoroughly;

[0027] (3) Stir continuously at room temperature to ensure that the components in the system are uniformly combined;

[0028] (4) Add calcium chloride (CaCl2) solution dropwise to the system in step (3) to induce an ionic cross-linking reaction, which causes sodium alginate to form a stable three-dimensional network structure and promotes gelation and flocculation of the system. 2+ Constructing a primary cross-linking network;

[0029] (5) After the system has formed a preliminary gel, add PAC powder or its aqueous solution, and induce further flocculation and sedimentation of the system under continuous stirring. 3+ In Ca 2+ Based on the network framework, residual carboxyl sites are coordinated to form a secondary dense cross-linked network, thereby constructing a hierarchical cross-linked density structure;

[0030] (6) The solid precipitate was collected by vacuum filtration and freeze-dried to obtain a precursor with a three-dimensional hierarchical cross-linked network structure;

[0031] (7) The precursor obtained in step (6) is subjected to carbonization treatment under an inert atmosphere to convert sodium alginate into a porous carbon network, while Ca 2+ -Cu 2+ -Al 3+ The carbon-containing gas produced by the synergistic catalysis of sodium alginate by three metal ions is one or more of CO, CO2 and CH4. Carbon nanotubes are generated in situ, and the three metal elements calcium, copper and aluminum are retained in situ in a highly dispersed form in the carbon matrix, resulting in a composite anode material of waste silicon and waste graphite.

[0032] Furthermore, in step (1), the volume / mass ratio of the ethanol dispersion containing waste silicon to the graphite waste powder is 8 mL: 4 g. Furthermore, in step (2), the amount of copper sulfate pentahydrate (CuSO4·5H2O) added is 0.1 g; the concentration of sodium alginate solution is 2 wt%, and the amount added is 10 g.

[0033] Furthermore, in step (4), the amount of calcium chloride dihydrate (CaCl2·2H2O) added is 0.3 g; in step (5), the amount of PAC added is 0.204 g.

[0034] Furthermore, the stirring time in step (3) is 5 hours; the freeze-drying temperature in step (6) is -45℃ and the drying time is 48 hours; the carbonization temperature in step (7) is 900℃ and the holding time is 5 hours, and the inert atmosphere is argon or nitrogen.

[0035] A lithium-ion battery, characterized in that it comprises the above-mentioned waste silicon and waste graphite composite negative electrode material or the composite negative electrode material prepared by the above-mentioned preparation method as the negative electrode active material.

[0036] Compared with existing alginate hydrogel crosslinking systems, the present invention has the following outstanding beneficial effects and unexpected technical advantages:

[0037] (1) The in-situ growth of carbon nanotubes in an alginate hydrogel system was discovered and realized for the first time through the synergistic catalysis of calcium-copper-aluminum trimetallic elements. This is the most core creative highlight of this invention. In existing alginate hydrogel crosslinking systems, the function of metal ions is limited to simple ionic crosslinking and adhesion enhancement, and there are no reports of in-situ carbon nanotube generation using multiple metal ions in synergistic catalysis. This invention, through systematic comparative experiments, has for the first time discovered that: carbon nanotubes can be generated in situ using only Ca... 2+ The cross-linked sample showed sparse carbon nanotube growth after carbonization—this confirms the presence of Ca. 2+ Although it possesses some catalytic activity, its catalytic efficiency is limited when used alone; it contains only Ca 2+ +Cu 2+ The bimetallic samples showed increased carbon nanotube density but uneven distribution—indicating that the introduction of Cu enhanced catalytic activity, but growth was uneven without structural regulation; only in Ca… 2+ +Cu 2+ +Al 3+ In systems where three metals coexist, carbon nanotubes exhibit a high-density, uniformly distributed three-dimensional interwoven network. This discovery reveals an irreplaceable synergistic catalytic mechanism among the three metals: Ca... 2+ It is speculated that CaO or CaC2 intermediates are formed during carbonization, providing nucleation sites for carbon nanotube growth; Cu 2+ Reduced to metallic Cu nanoparticles, serving as transition metal catalytic active centers for carbon nanotube growth; Al3+ Existing in the form of Al2O3, it serves as a catalyst support and structure promoter, effectively inhibiting catalyst particle agglomeration and grain growth, and promoting the uniform, high-density growth of carbon nanotubes. The synergistic effect of these three elements enables the efficient conversion of carbon-containing gases such as CO, CO2, and CH4 generated in situ during the carbonization of sodium alginate into carbon nanotubes under mild conditions of 900°C, without the need for any external gaseous carbon source or pre-fabricated carbon nanotubes. This integrated process concept of "tri-metal synergistic catalysis + in-situ carbon source of sodium alginate" has not been reported in any existing literature or patents.

[0038] (2) PAC was introduced into the silicon-carbon anode material preparation system for the first time and Al was realized. 3+ The invention introduces PAC into a silicon-carbon anode material preparation system for the first time, utilizing the dual function of "carrier-densification". PAC is widely used in water treatment, but its application in lithium-ion battery energy storage materials has not been reported. This invention utilizes the Al content within PAC to achieve this dual function. 3+ Achieving dual functions: On the one hand, AI 3+ In Ca 2+ Based on the primary cross-linked network framework, it further coordinates with residual carboxyl sites to form secondary densification cross-links, constructing a hierarchical cross-linked density structure; on the other hand, Al 3+ After carbonization, it transforms into an Al2O3 nano-dispersed phase, which serves as a support for the Cu catalyst, effectively inhibiting the aggregation of Cu nanoparticles and ensuring the uniform growth of carbon nanotubes. This dual-functional design of "structural densification + catalyst support" has not been reported in existing technologies.

[0039] (3) For the first time, a calcium-copper-aluminum trimetallic "hierarchical crosslinking density-synergistic catalytic conductivity" integrated system was constructed in the same system. Existing technologies involve metal ion crosslinking with a single metal ion or sequentially introduced bimetallic ions; there is no technical solution that simultaneously and synergistically introduces three metal ions into the same system and assigns them clear functional roles. This invention utilizes the differences in valence state and chemical properties of the three metal ions to assign them clear functional roles: Ca... 2+ Constructing a primary cross-linked framework and providing nucleation sites for carbon nanotubes; Al 3+ Constructing secondary dense crosslinks and using them as catalyst supports to suppress aggregation; Cu 2+ This provides catalytically active centers for the efficient growth of carbon nanotubes. All three components achieve structural support (Ca) within the same system. 2+ → Densification and toughening (Al) 3+ → Catalytic conductivity (Cu) 0 The integrated synergy of Al2O3 and Al2O3 is a technical concept that has not been disclosed or implied in existing literature and patents.

[0040] (4) Simultaneously achieving nanoscale organic integration of waste silicon and waste graphite with the construction of high-performance anode materials. Existing preparation methods for waste silicon and waste graphite composite materials primarily rely on physical mixing, resulting in weak interfacial bonding between silicon and graphite. This invention utilizes Ca... 2+ And Al 3+ The hierarchical cross-linking process organically integrates waste silicon particles and waste graphite sheets into a three-dimensional hydrogel network at the nanoscale, forming a tightly coupled composite structure after carbonization. STEM-EDS elemental surface scanning shows that C, Si, Ca, Cu, and Al elements exhibit a highly uniform spatial overlapping distribution.

[0041] (5) Eliminating dependence on added carbon nanotubes and achieving self-construction of the conductive network. In the prior art, the preparation of silicon-carbon composite anodes based on alginate aerogel generally relies on added carbon nanotubes as conductive additives. This invention generates carbon nanotubes in situ through trimetallic synergistic catalysis, without adding any added carbon nanotubes to the raw materials, and can self-construct a high-density, uniformly distributed three-dimensional carbon nanotube conductive network during the carbonization process, which significantly simplifies the process and reduces the cost of raw materials.

[0042] (6) Ultra-long cycling stability. Thanks to the multi-scale carbon network and hierarchical crosslinking density structure mentioned above, the composite material prepared in this invention exhibits ultra-long cycling stability: the half-cell maintains stable cycling stability at 0.5 A g. -1 After 100 cycles, the capacity retention rate is as high as 94.6%, and the full cell retains a capacity of 1 A g. -1 After 100 cycles, the capacity retention rate is as high as 94% (the capacity retention rate is calculated as the ratio of the specific capacity of the 100th discharge to the specific capacity of the 1st discharge).

[0043] It should be particularly noted that: although sodium alginate and Ca 2+ Crosslinking systems have been reported (first disclosed in 2014), but their functional positioning has always remained at the level of enhancing the mechanical strength of the binder, and has never involved the use of metal ions to catalyze the in-situ growth of carbon nanotubes. The core distinguishing features of this invention compared with the prior art are: (i) it is the first to discover the phenomenon of trimetallic (Ca-Cu-Al) synergistic catalysis of in-situ carbon nanotube growth, and through systematic comparative experiments (Ca, Ca-Cu, Ca-Cu-Al), it proves that the simultaneous presence of the three metals is an irreplaceable necessary condition—carbon nanotubes grow sparsely in the Ca system, the density is increased but the distribution is uneven in the Ca-Cu system, and only in the Ca-Cu-Al trimetallic system can a high-density uniformly grown carbon nanotube network be achieved; (ii) it is the first to reveal the trimetallic synergistic catalytic mechanism: Ca 2+ Provides nucleation sites, Cu 0 (iii) PAC is introduced into the silicon-carbon anode material system for the first time, providing catalytic active centers and Al2O3 as a support and inhibiting agglomeration; 3+(iv) It achieves the dual function of "structural densification + catalytic support" for the first time; and it realizes the carbon nanotube self-growth process of "trimetallic synergistic catalysis + sodium alginate in-situ carbon source" for the first time, without the need for external carbon nanotubes or gaseous carbon sources. The composite technology effect of "in-situ generation of high-density carbon nanotube network + hierarchical cross-linking densification" brought about by the above distinguishing features is something that cannot be achieved by a single metal system or a bimetallic system, and it has non-obviousness and significant inventiveness. Attached Figure Description

[0044] Figure 1 SEM images (a / b) of the two solid waste raw materials used in Comparative Example 1 and Comparative Example 2 of this invention.

[0045] Figure 2 SEM images of Embodiments 1 and 2 and Comparative Example 5 of the present invention (ac: Embodiment 1; df: Embodiment 2; gi: Comparative Example 5).

[0046] Figure 3 The TEM image (ad) of Embodiment 1 of the present invention shows the particle coating structure and lattice fringes.

[0047] Figure 4 The images shown are STEM image (a) and EDS element distribution map (bh) of Embodiment 1 of the present invention.

[0048] Figure 5 The XRD patterns and Raman spectra of Examples 1, 2, Comparative Example 1, and Comparative Example 2 of the present invention are shown (a: XRD pattern; b: Raman spectrum).

[0049] Figure 6 This is the XPS full spectrum of Embodiment 1 of the present invention.

[0050] Figure 7 This is an XPS fitting image of Embodiment 1 of the present invention.

[0051] Figure 8 The BET curves are those of Embodiment 1, Comparative Example 1, and Comparative Example 2 of the present invention.

[0052] Figure 9 The thermogravimetric analysis curve of Embodiment 1 of the present invention shows its thermal stability and residual mass in an air atmosphere.

[0053] Figure 10 The samples of Example 1, Comparative Example 1, and Comparative Example 2 of this invention were prepared at 0.5 μg. -1 The following is a graph showing the cyclic performance.

[0054] Figure 11 Comparative Example 3 of the present invention was prepared at 0.5A g. -1 The following are the cycle performance graphs (a: Comparative Example 3a; b: Comparative Example 3b; c: Comparative Example 3c).

[0055] Figure 12 Comparative Example 4 of the present invention was prepared at 0.5A g. -1 The following are the cycle performance graphs (a: Comparative Example 4a; b: Comparative Example 4b).

[0056] Figure 13 For embodiments 1-4 of the present invention, at 0.5 A g -1 Cyclic performance comparison chart (a: Example 1; b: Example 2; c: Example 3; d: Example 4).

[0057] Figure 14 For Comparative Example 5 of the present invention, at 0.5 A g -1 Cyclic performance graph.

[0058] Figure 15 For Example 1 and Comparative Example 2 of the present invention, the concentrations were 0.2 to 15 Å g. -1 Rate capability at current density.

[0059] Figure 16 The image shows the EIS impedance fitting diagrams of Embodiment 1 and Comparative Example 1 after 100 cycles.

[0060] Figure 17 The XPS spectrum of Example 1 of the present invention during the first charge and discharge process reveals its surface chemical state and the evolution of interface reaction.

[0061] Figure 18 The following are SEM images showing the structural evolution of the electrodes of Embodiment 1 and Comparative Example 1 before and after cycling (ac: electrode of Comparative Example 1; di: electrode of Embodiment 1), showing the changes in cross-section and surface morphology before and after cycling.

[0062] Figure 19 The electrochemical performance diagrams of the full cell obtained by matching the positive electrode with Example 1 of the present invention are shown in Figure 1 (a: rate performance; b: 1A g). -1 (Lower cycle performance).

[0063] Figure 20 For Example 1 of the present invention, in 2 A g -1 Long-term cycle performance of the full battery.

[0064] Figure 21 This is a SEM image of Comparative Example 4a (Ca+Cu, no Al) of the present invention. Detailed Implementation

[0065] Before detailing the embodiments of the present invention, the source of key raw materials and pretreatment methods are first clarified to ensure that those skilled in the art can repeat the implementation.

[0066] Preparation of waste silicon source: The waste silicon source is derived from waste silicon powder generated during the silicon wafer cutting process in the photovoltaic industry. Its main component is elemental silicon, accompanied by a small amount of silicon carbide and metallic impurities. The waste silicon powder is mixed with anhydrous ethanol at a mass ratio of 1:3 and wet-milled in a ball mill at 400 rpm for 6 hours. After ball milling, the mixture is allowed to stand, and the upper uniform suspension is taken as the "ethanol dispersion containing waste silicon". Testing shows that the solid content of this dispersion is approximately 8 wt%, and the average particle size D50 of the silicon particles is approximately 150 nm.

[0067] Preparation of graphite waste: The graphite waste is cutting waste generated from the machining of graphite parts. First, it is placed in a muffle furnace and calcined at 500°C for 2 hours in air to remove surface oil. After cooling, it is calcined at 900°C for 2 hours under argon atmosphere for high-temperature purification. Finally, the treated lumps are ball-milled and passed through a 300-mesh sieve to obtain graphite waste powder with a carbon content ≥99.5% and a particle size D50 of 15 μm.

[0068] The above-described raw material preparation method is merely illustrative and is not intended to limit the present invention.

[0069] Unless otherwise stated, the calcium source used in this invention is CaCl2·2H2O, the copper source is CuSO4·5H2O, and the aluminum source is PAC (the mass fraction of Al2O3 in PAC is 30.0 wt%, which is subject to the supplier's quality certificate or actual test results). The molar ratios of Ca, Cu, and Al in this document refer to the molar ratio of the effective metal elements fed into each metal source, not the actual residual molar ratio of each element in the composite material after carbonization. The molar numbers of Ca and Cu fed are calculated based on the weighed mass of CaCl2·2H2O and CuSO4·5H2O, respectively; the molar number of Al fed into PAC is calculated according to the following formula:

[0070] n(Al)=2×m(PAC)×w(Al2O3) / M(Al2O3)

[0071] In the formula, n(Al) is the number of moles of Al added, m(PAC) is the weighed mass of PAC, w(Al2O3) is the mass fraction of Al2O3 in PAC, and M(Al2O3) is the molar mass of Al2O3.

[0072] In this embodiment, when the amounts of CaCl2·2H2O, CuSO4·5H2O and PAC added are 0.30 g, 0.10 g and 0.204 g respectively, the effective molar ratio of Ca, Cu and Al is approximately 5:1:3.

[0073] Example 1 (Ca:Cu:Al = 5:1:3, the optimal system of this invention)

[0074] Mix 200 mL of deionized water with 20 mL of anhydrous ethanol, add 8 mL of the ethanol dispersion containing waste silicon prepared above, and ultrasonically disperse for 10 min. Then add 4 g of the graphite waste powder prepared above, and continue ultrasonic dispersion for 10 min. Next, add 0.10 g of CuSO4·5H2O, and ultrasonically stir for 10 min. Add 10 g of sodium alginate solution with a mass concentration of 2 wt%, ultrasonically stir for 5 min, and then magnetically stir at room temperature for 5 h.

[0075] Subsequently, a CaCl2 solution, prepared by dissolving 0.30 g of CaCl2·2H2O in 10 mL of deionized water, was added dropwise to the system, causing the sodium alginate to undergo an ionic cross-linking reaction and form a preliminary gel. After the preliminary gel was formed, 0.204 g of PAC was added, and the system was continuously stirred to induce further flocculation and sedimentation. At this point, the effective molar ratio of Ca, Cu, and Al in the system was 5:1:3.

[0076] The solid was collected by filtration and freeze-dried at -45℃ for 48 h to obtain the composite precursor. The composite precursor was placed in an argon atmosphere and heated to 900℃ at a rate of 5℃ / min and calcined for 5 h to obtain the Si-GC(Ca / Cu / Al) composite material.

[0077] Thermogravimetric analysis showed that the remaining mass of the composite material prepared in this example was approximately 35.36% in an air atmosphere at 800°C.

[0078] SEM / TEM characterization revealed a high-density, uniformly distributed three-dimensional carbon nanotube interwoven network in the composite structure. Figure 2 ac), carbon nanotubes with a diameter of approximately 20-40 nm are interconnected with the carbon layer on the surface of silicon particles ( Figure 3 c). STEM-EDS ( Figure 4 The XRD patterns show that carbon, silicon, calcium, copper, and aluminum elements exhibit a highly uniform spatial distribution throughout the composite structure, and the XRD patterns ( Figure 5 The absence of obvious diffraction peaks for metal or metal oxide impurities in a) confirms the high dispersion of metal elements.

[0079] Electrochemical performance: at 0.5 A g -1 At current density, the initial capacity is stable, and the capacity retention rate is as high as 94.6% after 100 cycles. Figure 10 , Figure 13 a) Coulomb efficiency is close to 99%. Rate test ( Figure 15 This indicates that at 15 Ag -1 It still maintains a high capacity, recovering to 0.2 A g. -1 The capacity rebounded afterward, demonstrating excellent reversibility.

[0080] Example 2 (Ca:Cu:Al = 5:1:2)

[0081] The only difference from Example 1 is that the amount of PAC added is adjusted to 0.136g, so that the molar ratio of Ca:Cu:Al in the system is controlled at 5:1:2. The amounts of other raw materials and all process parameters are exactly the same as in Example 1.

[0082] SEM showed that the silicon particle dispersion was slightly lower than in Example 1, but the overall three-dimensional network structure was still maintained. Electrochemical tests ( Figure 13 b) shows that at 0.5 A g -1 Below this, after 100 cycles, the capacity retention rate is approximately 82%, and the cycle stability is lower than the optimal ratio, indicating that Al... 3+ Insufficient content weakens cross-linking support.

[0083] Example 3 (Ca:Cu:Al = 5:1:4)

[0084] The difference from Example 1 is that the amount of PAC added is adjusted to 0.272 g, so that the molar ratio of Ca:Cu:Al in the system is controlled at 5:1:4. The amounts of other raw materials and all process parameters are exactly the same as in Example 1.

[0085] Electrochemical performance: This electrode at 0.5 A g -1 After 100 laps, the volume retention rate is approximately 86%. Figure 13 c), attributed to Al 3+ The enhanced cross-linking improves structural stability, but the excessive aluminum content leads to a longer ion transport path, resulting in slightly inferior rate performance compared to Example 1.

[0086] Example 4 (Ca:Cu:Al = 5:1:5)

[0087] The difference from Example 1 is that the amount of PAC added is adjusted to 0.340 g, so that the molar ratio of Ca:Cu:Al in the system is controlled at 5:1:5. The amounts of other raw materials and all process parameters are exactly the same as in Example 1.

[0088] Electrochemical performance: This electrode at 0.5 A g -1 After 100 laps, the volume retention rate is approximately 81%. Figure 13 d), although still better than comparative example 5, shows accelerated decay, proving that Al 3+ There exists an optimal window for the content.

[0089] Comparative Example 1 (without any metal ions added)

[0090] Waste silicon powder that has undergone ball milling was used directly as a comparison sample. SEM showed that the waste silicon was in a nanoparticle agglomeration state. Figure 1 a). Electrochemical tests showed that at 0.5 A g -1 Below, after 40 cycles, the capacity retention rate is only about 30%, and after 100 cycles, only about 10% remains. Figure 10 ), with extremely poor structural stability.

[0091] Comparative Example 2 (Graphite waste powder as raw material)

[0092] Graphite waste powder that has undergone high-temperature treatment was directly used. SEM images show a typical layered, folded structure. Figure 1 b). Electrochemical tests show that graphite waste has good cycle stability, but its specific capacity is much lower than that of silicon-based composite materials. Figure 10 ).

[0093] Comparative Example 3 (single metal doping, verifying the necessity of trimetallic synergy)

[0094] The difference from Example 1 is that only a single metal ion is added, without introducing the other two metal ions, in order to examine the structural construction and electrochemical performance of each metal when acting alone.

[0095] Comparative Example 3a (Ca only) 2+ Doping): Without adding CuSO4·5H2O and PAC, only 0.3 g CaCl2 was dissolved in 10 mL of deionized water and added dropwise to the system. The remaining steps were the same as in Example 1. The resulting product was denoted as Si-GC(Ca).

[0096] Comparative Example 3b (Cu only) 2+ Doping): No CaCl2 or PAC were added; only 0.1 g of CuSO4·5H2O was added. The remaining steps were the same as in Example 1. The resulting product was denoted as Si-GC(Cu).

[0097] Comparative Example 3c (Al only) 3+ Doping): No CaCl2·2H2O and CuSO4·5H2O were added; only 0.204 g of PAC was added during the flocculation stage. The remaining steps were the same as in Example 1. The resulting product was denoted as Si-GC(Al).

[0098] Characterization results showed that all three monometal-doped samples could form a certain carbon-coated structure, but SEM and TEM revealed that the silicon particle dispersion was not as uniform as in Example 1, with agglomeration in some areas. XRD retained the characteristic peaks of silicon and graphite, but XPS showed that they corresponded to only a single metal element. Electrochemical tests indicated that the monometal-doped samples at 0.5 A g... -1The cycling stability and capacity retention of the samples were significantly lower than those in Example 1. Specifically, the Ca system showed slightly better stability but insufficient rate performance, the Cu system improved conductivity but had weak structural buffering capacity, and the Al system exhibited enhanced crosslinking but was presumably limited in ion transport. These results validate the necessity of multi-metal synergy; single-metal doping cannot simultaneously achieve a comprehensive improvement in conductive network optimization, structural support, and interface stability.

[0099] Comparative Example 4 (Bimetallic doping, verifying the necessity of trimetallic synergy)

[0100] The difference from Example 1 is that two metal ion combinations were added separately, without introducing a third metal ion, in order to examine the effect of bimetallic synergy on the material structure and properties.

[0101] Comparative Example 4a (Ca 2+ +Cu 2+ (Doping): Without adding PAC, the amount of CuSO4·5H2O added is fixed at 0.10 g, and different amounts of CaCl2·2H2O are added to make the effective Ca:Cu molar ratio approximately 3:1, 5:1, and 7:1, respectively. The corresponding amounts of CaCl2·2H2O added are 0.176 g, 0.294 g, and 0.412 g, respectively. The remaining steps are the same as in Example 1. When the effective Ca:Cu molar ratio is approximately 5:1, the amount of CaCl2·2H2O added is 0.294 g, and the amount of CuSO4·5H2O added is 0.10 g.

[0102] Comparative Example 4b (Ca) 2+ +Al 3+ (Doping): Without adding CuSO4·5H2O, the amount of CaCl2·2H2O added was fixed at 0.294 g. Different amounts of PAC were added to achieve an effective Ca:Al molar ratio of approximately 5:1, 5:2, and 5:3. The amounts of PAC added were 0.068 g, 0.136 g, and 0.204 g, respectively, and the Al2O3 mass fraction of the PAC was 30.0 wt%. The remaining steps were the same as in Example 1.

[0103] Electrochemical testing ( Figure 12 This indicates that the bimetallic system at 0.5 Ag -1 The cycling stability and rate performance of the samples were significantly better than those of the single-metal doped samples. The Ca:Cu=5:1 and Ca:Al=5:2 systems showed better capacity retention, but the overall performance was still lower than that of Example 1 with trimetallic synergy. This confirmed the complementary and synergistic enhancement effects of the three metal ions in terms of structural support, conductivity optimization and crosslinking enhancement.

[0104] Comparative Example 5 (Ca:Cu:Al = 5:1:1)

[0105] The difference from Example 1 is that the amount of PAC added is reduced, so that the molar ratio of Ca:Cu:Al in the system is controlled at 5:1:1. Specifically, after gel formation, the amount of PAC added is approximately 0.068 g. The remaining preparation steps, raw material amounts, and process parameters (such as ultrasonic time, stirring time, calcination temperature, etc.) are exactly the same as in Example 1.

[0106] Electrochemical performance: This electrode at 0.5 A g -1 After 100 laps, the capacity retention rate was only 36%. Figure 14 Although the initial capacity was high, the insufficient cross-linking network strength resulted in extremely limited and severely uneven carbon nanotube formation, failing to form an effective three-dimensional conductive network. This prevented the effective buffering of the large volume effect of silicon during charge and discharge, leading to the pulverization and collapse of the electrode structure in the early stages of cycling. This comparative example demonstrates that Al… 3+ The lack of [certain elements] is the direct cause of the collapse of the mechanical strength of the 3D network, verifying that AI [is involved]. 3+ It plays an indispensable role as a "structural densification and strengthening agent".

[0107] Performance Tests and Results

[0108] The materials obtained in Examples 1-4 and Comparative Examples 1-5 were assembled into CR2025 lithium-ion half-cells for electrochemical testing. The materials from Example 1 were then matched with a positive electrode to assemble full cells for further verification of practical application performance. The half-cells used lithium metal sheets as the counter electrode, and tests included cycle performance, rate performance, CV, GITT, and EIS impedance. The full cells were used to evaluate long-term cycle stability and rate output capability. All specific capacities were calculated based on the total mass of the composite negative electrode active materials.

[0109] 1. Material characterization ( Figure 1-9 , Figure 21 )

[0110] SEM / TEM analysis:

[0111] SEM: Example 1 ( Figure 2 (ac) shows that the composite material exhibits a three-dimensional continuous structure composed of graphite sheets, porous carbon networks, and silicon particles. The silicon particles are uniformly dispersed in the graphite-carbon matrix, and no obvious agglomeration was observed. Example 2 ( Figure 2 (df) shows that a three-dimensional network of carbon nanotubes densely coats the surfaces of graphite and nano-Si, with enhanced cross-linking and good dispersion of silicon particles. Comparative Example 5 ( Figure 2 Although all three metal elements are present, the network is incomplete and the cross-linking network strength is insufficient when the amount of Al is insufficient. Although carbon nanotubes are present, they are not generated uniformly and are not uniformly attached to the surface of nano-silicon and graphite. Figure 21This is a SEM image of Comparative Example 4a (Ca+Cu, no Al) of the present invention. Compared with Example 1 (… Figure 2 Compared to the high-density, uniformly distributed three-dimensional carbon nanotube network in (ac), Figure 21 The microstructures are strikingly different: carbon nanotubes are sparsely distributed in localized clusters, with large areas showing no carbon nanotube coverage. This stark contrast intuitively demonstrates that in the absence of Al... 3+ In this case, Cu catalyst particles agglomerate during high-temperature carbonization, losing their uniform catalytic ability, and carbon nanotubes cannot form a continuous conductive network. This result is corroborated by XRD, BET, and electrochemical performance data, strongly supporting the core invention argument that "trimetallic synergistic catalysis is indivisible."

[0112] TEM:( Figure 3 The results showed that silicon nanoparticles were uniformly embedded and coated within the carbon matrix, with particle sizes mainly distributed in the range of 30-50 nm and a carbon coating thickness of approximately 10-20 nm, forming a typical core-shell structure. HRTEM clearly observed lattice fringes of approximately 0.42 nm and 0.29 nm, corresponding to the (111) crystal plane of crystalline silicon, indicating that the silicon phase maintained good crystal integrity. STEM-EDS ( Figure 4 The results show that carbon, silicon, calcium, copper, and aluminum elements exhibit a highly uniform distribution throughout the composite structure.

[0113] Comparative Example 1 ( Figure 1 a) The waste silicon was found to be agglomerated in nanoscale particles, with uneven particle size distribution and irregular morphology. Comparative Example 2 ( Figure 1 b) The graphite waste is shown to have a layered, folded structure, with the layers stacked on top of each other to form a loose three-dimensional skeleton.

[0114] XRD ( Figure 5 ):

[0115] Example 1 retained both the characteristic diffraction peaks of silicon (2θ ≈ 28.4°, 47.3°, 56.1°, 69.1°, and 76.4°) and the (002) diffraction peak of graphite (2θ ≈ 26.5°). The intensity of the silicon diffraction peak was relatively weakened, which is related to the reduced size of the silicon particles and their coating by the carbon layer. No obvious metal or metal oxide impurity phase diffraction peaks were detected. Comparative Example 1 showed only the characteristic peaks of silicon, and Comparative Example 2 showed only the characteristic peaks of graphite.

[0116] Raman spectroscopy ( Figure 5 b):

[0117] The ID / IG ratio of Example 1 is approximately 0.26, lower than the 0.29 of the original graphite in Comparative Example 2, indicating that the carbon structure has a higher degree of graphitization and a lower defect density. At 500 cm⁻¹ -1Silicon-related characteristic peaks can be observed at this location.

[0118] XPS ( Figure 6 , Figure 7 ):

[0119] The XPS full spectrum of Example 1 shows characteristic signals such as C1s, O1s, Si2p, Cu2p, Al2p, and Ca2p, with C atoms accounting for 32.61% and Si atoms accounting for 9.00%. The main peak at 284.8 eV in the C1s spectrum is attributed to the C-C bond; in the Si2p spectrum, 100.24 eV corresponds to the dominant Si-Si bond, and 101.77 eV is attributed to the Si-C bond (proving a stable chemical bond between silicon and carbon); characteristic peaks of Cu 2p3 / 2 and Cu 2p1 / 2 appear at approximately 932.6 eV and 952.8 eV, respectively, in the Cu2p spectrum; and characteristic peaks of Al2p appear at 75.24 eV. 3+ Characteristic peaks: The Ca2p spectrum shows characteristic peaks at 347.06 eV and 350.64 eV corresponding to Ca 2p3 / 2 and Ca 2p1 / 2, respectively. XPS analysis of Comparative Examples 3a, 3b, and 3c detected only the corresponding single metal element, while Comparative Examples 4a and 4b detected the corresponding two metal elements. No metal element signals were detected in Comparative Examples 1-2.

[0120] BET Figure 8 ):

[0121] The specific surface area of ​​Example 1 is 15.25 m². 2 / g, pore volume 0.02 cm³ 3 Based on the approximate relationship between the average pore size and the g, the average pore size is approximately 5.25 nm. The pore size distribution results show that the pore size is mainly concentrated in the range of 2-20 nm, and the isotherm exhibits typical type IV isothermal adsorption characteristics.

[0122] TGA ( Figure 9 ):

[0123] Example 1 showed a significant decrease in mass in the range of 500°C to 750°C, which was attributed to the high-temperature oxidative decomposition of the carbon component. The final remaining mass was 35.36%, corresponding to SiO2 generated by silicon oxidation and oxides of metal elements such as calcium, copper, and aluminum.

[0124] 2. Electrochemical performance testing

[0125] 0.5A g -1 Cyclic performance under ( Figure 10 ,11):

[0126] Example 1: at 0.5A g -1During the initial cycle, the capacity quickly stabilizes and then maintains a steady trend, with the overall coulombic efficiency remaining at approximately 99%.

[0127] Comparative Example 1 (waste silicon): After 40 cycles, the capacity retention rate is only about 30%, and after 100 cycles, it is only about 10%.

[0128] Comparative Example 2 (waste graphite): Although it showed better cycle stability, its specific capacity was much lower than that of Example 1.

[0129] Single metal doping ( Figure 11 ):

[0130] Comparative Example 3a (Ca only): The cycle performance was optimal when the amount of CaCl2 added was 0.3 g, and the capacity change was relatively stable, but the rate performance was insufficient.

[0131] Comparative Example 3b (Cu only): The cycling stability was the best when the amount of CuSO4·5H2O added was 0.3 g, but the structural buffering capacity was weak.

[0132] Comparative Example 3c (Al only): The capacity change was relatively stable when the amount of PAC added was 0.1 g, but it is speculated that ion transport was limited.

[0133] Bimetallic doping optimization ( Figure 12 ):

[0134] Comparative Example 4a (Ca+Cu): Ca:Cu=5:1 exhibited better cycle stability.

[0135] Comparative Example 4b (Ca+Al): Ca:Al=5:3 showed better cycle stability.

[0136] Three-metal synergistic optimization Figure 13-14 ):

[0137] Example 1 ( Figure 13 a) It exhibits the best cycling trend and the highest capacity retention rate, indicating that the three metal ions achieve functional complementarity and synergistic enhancement in terms of structural support, conductivity optimization and cross-linking enhancement.

[0138] Example 2 ( Figure 13 b) Exhibited good cycling stability (0.5 A g) -1 (The retention rate after 100 laps is approximately 82%), but the overall performance is slightly inferior to the optimal ratio, indicating that Al 3+ Insufficient Ca content weakens the degree of cross-linking in the system, leading to a decrease in the supporting force of the three-dimensional network structure and a reduction in its volume expansion buffering capacity. However, it is still superior to most bimetallic systems, indicating that Ca... 2+ With Cu 2+ The synergistic effect can still provide basic electrical conductivity and structural protection.

[0139] Example 3 ( Figure 13 c) It exhibits good cycling stability (0.5 A g) -1 (The retention rate after 100 laps is about 86%), indicating that appropriately increasing the Al 3+ The ratio helps enhance the structural stability and anti-expansion ability of the cross-linked network, but excessively high Al content... 3+ The increased content of Al slightly prolonged the ion transport path, resulting in a minor impact on rate performance, confirming that Al... 3+ There exists an optimal window for its effect.

[0140] Example 4 ( Figure 13 d) Exhibits high initial capacity but rapid cycling decay (0.5 A g) -1 The retention rate after 100 laps was approximately 81%, indicating that excessive Al... 3+ Excessive cross-linking leads to shrinkage of the three-dimensional network, decreased electrolyte wettability, and increased interfacial impedance, indicating that Al 3+ The content needs to be precisely controlled to achieve a balance between structural compactness and ion accessibility.

[0141] Comparative Example 5 ( Figure 14 It exhibits high initial capacity but significantly insufficient cycling stability (0.5A g). -1 The retention rate over the next 100 laps is only about 36%, indicating that Al 3+ The severe lack of Ca leads to an incomplete cross-linking network, which cannot effectively suppress the volume effect and structural pulverization of silicon during repeated charge and discharge processes, but Ca... 2+ With Cu 2+ The synergistic effect of the components still makes its performance superior to undoped or single-metal doped systems, further confirming the synergistic mechanism that each component in the trimetallic system is indispensable.

[0142] By comparing the results of Comparative Example 3 (single metal), Comparative Example 4 (bimetal), and Examples 1-4 (trimetal), the following patterns can be identified:

[0143] Although bimetallic systems outperform monometallic systems in some performance indicators, their improvement effect is characterized by "partial superposition but with structural shortcomings".

[0144] Ca 2+ +Cu 2+ System: Electrical conductivity is improved (Cu) 2+ (catalytic effect), but due to the lack of dispersion effect of Al2O3 support, Cu 2+ The particles agglomerate during the high-temperature carbonization process, resulting in a severe uneven distribution of carbon nanotubes ("island effect"), and the overall electrode structure uniformity and cycle stability are still insufficient.

[0145] Ca 2+ +Al3+ System: It has a dense structure and good mechanical strength (Ca). 2+ And Al 3+ (hierarchical crosslinking), but due to the lack of Cu 2 + The catalytic active center has a limited growth density of carbon nanotubes, resulting in an incomplete conductive network and limited rate performance.

[0146] Only when all three metals are present, Ca 2+ Nucleation function of Cu 2+ Catalytic function and Al 3+ Only through the dispersion of the carrier's functions can a complete closed-loop synergistic chain be formed, achieving a simultaneous leap in conductivity and structural stability. This result strongly confirms that the trimetallic synergistic effect is indivisible—the absence of any metal element leads to the breakage of the synergistic chain, resulting in a "cliff-like" drop in performance rather than a non-linear decay. This is an important indicator of the existence of the synergistic effect. This discovery strongly refutes the argument that "trimetallic synergy is merely a simple combination of known functions," confirming that the trimetallic synergistic effect is not self-evident.

[0147] Rate performance (0.2-15 Ag) -1 , Figure 15 ):

[0148] Example 1 at 0.2 A g -1 It exhibits a high reversible specific capacity; as the current density is gradually increased to 0.5, 1, 2, 5, 10 and 15 A g, it shows a high reversible specific capacity. -1 The specific capacity decreases in a stepwise manner, but even at 15 A g... -1 It can maintain stable capacity output even under high current density; when the current density recovers to 0.2 A g -1 When the capacity recovers significantly, it demonstrates excellent rate reversibility.

[0149] EIS analysis ( Figure 16 ):

[0150] Quantitative analysis was performed using an equivalent circuit model constructed based on the interface characteristics of silicon-based anodes. In Example 1, the charge transfer impedance R_ct in the mid-to-high frequency region was significantly lower than that of the comparative example and the system without added metal ions. This is due to the Cu... 2+ Catalytic effect on localized ordering of carbon structure and Ca 2+ And Al 3+ The constructed three-dimensional network structure. As the cycle progresses, the semicircle in the high-frequency region gradually shrinks, while the slope of the straight line in the low-frequency region gradually increases. After 100 cycles, Example 1 still maintains a relatively stable impedance curve shape. Figure 16 The interface structure did not deteriorate significantly.

[0151] Structural evolution analysis of charging and discharging process (corresponding) Figure 17 )

[0152] C1s spectrum ( Figure 17 a) The display shows that when discharged to 0.5 V, the CC bond ratio is 63%, CO / CS is 12%, and CN is 11%; when discharged to 0.01 V, the CC ratio rises to 72%, and CO / CS drops to 7%; when charged to 2 V, the CC ratio drops to 72%, and CO / CS rises back to 15%. N1s spectrum ( Figure 17 b) shows that the ratio of pyrrole nitrogen to pyridine nitrogen undergoes a reversible change during cycling. Si2p spectrum ( Figure 17 c) The display shows that when discharged to 0.01 V, SiO2 decreases to 16%, and SiO2... x The percentages increased to 54%, SiO2 decreased to 30%, and were 19%, 40%, and 41% respectively when charged to 2 V. (Cu2p spectrum) Figure 17 d) Al2p spectrum ( Figure 17 e) and Ca2p spectrum ( Figure 17 f) shows that the three metal ions remain stable at all voltage levels.

[0153] Post-cycle electrode structure analysis (corresponding) Figure 18 )

[0154] Comparative Example 1 (pure silicon) had a cross-sectional thickness of approximately 9.4 µm before cycling. Figure 18 a), after 100 cycles ( Figure 18 (b) and (c) the cross-section expands to 61.1 µm, the surface is rough and porous, and accompanied by obvious pulverization. In Example 1, the cross-sectional thickness before cycling was approximately 15.0 µm. Figure 18 d), after repeating 100 times ( Figure 18 e) The cross-section expanded to 39.5 µm, which was significantly less than that of Comparative Example 1, and the surface microporous structure remained uniform and intact. Figure 18 (h, i), no obvious cracks or powdering. After 20 cycles ( Figure 18 f, g) The surface structure maintains good integrity.

[0155] Full battery performance (corresponding) Figure 19 ,20)

[0156] Ratio performance ( Figure 19 a) Displays from 0.2 A g -1 Gradually increase to 15A g -1 The specific capacitance decreases gradually in a stepwise manner, until the current density recovers to 0.2 A g. -1 The capacity can recover significantly. At 1 A g -1 Down( Figure 19(b) After 100 stable cycles of the full battery, the capacity retention rate is approximately 94% or higher. At 2A g -1 Down( Figure 20 The full battery retains over 80% of its capacity after 100 stable cycles. The full battery exhibits stable long-cycle performance.

[0157] Overall Conclusion

[0158] This invention uses photovoltaic waste silicon and graphite processing waste as raw materials. Through systematic experimental exploration, it has for the first time observed Ca... 2 + -Cu 2+ -Al 3+ Three metal ions can synergistically catalyze the in-situ growth of carbon nanotubes during high-temperature carbonization. The results of the control experiment clearly show that only when these three metal ions are present simultaneously and in appropriate proportions can a high-density, uniformly interwoven carbon nanotube network spontaneously form inside the material. The absence of any one of them or an imbalance in the proportions will significantly reduce the growth density and uniformity of the carbon nanotubes.

[0159] In this system, the three metal ions each have their own function: Ca 2+ Responsible for building the primary gel framework and participating in nucleation during subsequent carbonization; Cu 2+ It is the catalytic core for carbon nanotube growth; while Al from PAC 3+ This plays a dual role—it strengthens the network structure during the gelation stage and transforms into an Al2O3 support after carbonization, effectively preventing the aggregation of Cu particles and ensuring the uniform growth of carbon nanotubes. It is this division of labor and cooperation of "skeleton support-dense structure-catalytic conductivity" that enables the entire composite material to construct a complete conductive and buffering network without the need for an external carbon source or carbon nanotubes.

[0160] Waste silicon and waste graphite, two types of industrial solid waste, were simultaneously integrated into a high-performance composite anode material through this simple process. The prepared material exhibited excellent cycle stability in both half-cell and full-cell tests, providing a feasible technical path for the resource utilization of industrial solid waste in the energy storage field.

Claims

1. A composite anode material of waste silicon and waste graphite grown in situ using trimetallic synergistic catalysis of carbon nanotubes, comprising a conductive framework of waste graphite, a sodium alginate carbonized porous carbon network, and nano-silicon particles, characterized in that... The composite material also includes a carbon nanotube network grown in situ through the synergistic catalysis of calcium-copper-aluminum trimetallic ions, forming a three-dimensional composite structure. This three-dimensional composite structure has a primary network formed by calcium ion crosslinking and a secondary densified network formed by further crosslinking of aluminum ions on top of the primary network, creating a hierarchical crosslinking density structure. The carbon matrix of the composite material is uniformly doped with calcium, copper, and aluminum, without any metal or metal oxide agglomerates or impurities. The carbon nanotubes are composed of Ca... 2+ -Cu 2+ -Al 3+ High temperature synergistic catalysis generates and constructs a three-dimensional additional conductive pathway in situ, and the surface of the composite material contains characteristic signals of Ca, Cu and Al elements.

2. The composite anode material made from waste silicon and waste graphite according to claim 1, characterized in that, The molar ratio of the three metallic elements calcium, copper, and aluminum is Ca:Cu:Al = (4.8–5.2):(0.9–1.1):(2–5); preferably, the molar ratio is Ca:Cu:Al = 5:1:

3.

3. The composite anode material made from waste silicon and waste graphite according to claim 1, characterized in that, The carbon nanotubes have a diameter of 20-40 nm and form a three-dimensional interwoven network; the silicon nanoparticles have a size of 30-50 nm and are coated with a carbon layer with a thickness of 10-20 nm; the composite material has a specific surface area of ​​10-20 m². 2 / g, mainly mesoporous structure, with pore size mainly distributed in the range of 2-20 nm.

4. The composite anode material made from waste silicon and waste graphite according to claim 1, characterized in that, The calcium element is Ca 2+ The copper element exists in the form of metallic copper or low-valence copper oxide, serving as a catalytic active center for carbon nanotube growth during carbonization; the aluminum element is derived from polyaluminum chloride, in the form of alumina, aluminate, or Al. 3+ The coordination form exists, on the one hand, for use in Ca 2+ On the basis of cross-linked networks, the degree of cross-linking and structural compactness are further enhanced to form a hierarchical cross-linking density structure. On the other hand, it serves as a catalyst support to inhibit the aggregation of copper particles and promote the uniform growth of carbon nanotubes.

5. A method for preparing a composite negative electrode material of waste silicon and waste graphite as described in any one of claims 1 to 4, characterized in that, Includes the following steps: (1) Deionized water and anhydrous ethanol were mixed to form a dispersion system, waste silicon source was added, ultrasonic dispersion was performed, and then graphite waste powder treated at high temperature was added and ultrasonic dispersion was continued to obtain a uniform Si-G mixed suspension. (2) Add copper sulfate solution to the Si-G mixed suspension obtained in step (1), then add sodium alginate solution, and stir ultrasonically to mix the components thoroughly. (3) Stir continuously at room temperature to ensure that the components in the system are uniformly combined; (4) After the stirring in step (3) is completed, add calcium chloride solution dropwise to the system so that sodium alginate reacts with Ca. 2+ An ionic cross-linking reaction occurs, forming a preliminary gel with a primary cross-linking network structure; (5) After the system has formed a preliminary gel, add PAC powder or its aqueous solution, and under continuous stirring, use Al 3+ With Ca 2+ The residual carboxyl sites on the primary network are coordinated to form a secondary compacted cross-linking network, thereby constructing a hierarchical cross-linking density structure; (6) The solid precipitate was collected by vacuum filtration and freeze-dried to obtain a precursor with a three-dimensional hierarchical cross-linked network structure; (7) The precursor obtained in step (6) is subjected to carbonization treatment under an inert atmosphere to convert sodium alginate into a porous carbon network, while Ca 2+ -Cu 2+ -Al 3+ The carbon-containing gas produced by the carbonization and decomposition of sodium alginate by the synergistic catalysis of three metal ions generates carbon nanotubes in situ. The three metal elements calcium, copper and aluminum are retained in situ in a highly dispersed form in the carbon matrix, resulting in a composite anode material of waste silicon and waste graphite.

6. The preparation method according to claim 5, characterized in that, The waste silicon source mentioned in step (1) is an ethanol dispersion containing waste silicon after the silicon wafer cutting waste in the photovoltaic industry is ball-milled. The graphite waste is the powder obtained after high-temperature treatment of the waste generated during the processing of graphite products. The volume / mass ratio of the ethanol dispersion containing waste silicon to the graphite waste powder is 8 mL: 4 g.

7. The preparation method according to claim 5, characterized in that, In step (2), the amount of copper sulfate pentahydrate added is 0.1 g; the concentration of sodium alginate solution is 2 wt%, and the amount added is 10 g.

8. The preparation method according to claim 5, characterized in that, In step (4), the amount of calcium chloride dihydrate added is 0.3 g; in step (5), the amount of polyaluminum chloride added is 0.204 g.

9. The preparation method according to claim 5, characterized in that, The stirring time in step (3) is 5 hours; the freeze-drying temperature in step (6) is -45℃ and the drying time is 48 hours; the carbonization temperature in step (7) is 900℃ and the holding time is 5 hours, and the inert atmosphere is argon or nitrogen.

10. A lithium-ion battery, characterized in that, The lithium-ion battery comprises the composite negative electrode material according to any one of claims 1-4 or the composite negative electrode material prepared by any one of claims 5-9 as the negative electrode active material, and the lithium-ion battery is suitable for power batteries or energy storage batteries.