Anode materials and their preparation methods, anode sheets and secondary batteries
By depositing a deoxygenated carbon layer, a SiCN layer, and a carbon coating layer on a porous carbon framework, a three-dimensional conductive network is constructed, which solves the shortcomings of silicon-carbon materials in terms of high initial efficiency and cycle performance, and realizes an anode material with high initial efficiency, low expansion, and long cycle life.
Patent Information
- Application Number
- CN202611459575.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silicon-carbon materials struggle to balance high initial efficiency and good cycle performance, primarily due to irreversible lithium loss caused by oxygen-containing functional groups on the porous carbon framework surface and the formation of high-resistivity SiC from the reaction of silicon and carbon, which affects battery capacity and lifespan.
A deoxygenated carbon layer, a SiCN layer, and a carbon coating layer are sequentially deposited on the surface of a porous carbon framework. By constructing a three-dimensional conductive network, direct contact between silicon and carbon is isolated, irreversible lithium consumption and SiC formation are reduced, and volume expansion is buffered.
A negative electrode material with high initial efficiency, low expansion, and long cycle life has been achieved, improving the energy density and cycle stability of lithium-ion batteries.
Smart Images

Figure CN123120701A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and more specifically, to a negative electrode material and its preparation method, a negative electrode sheet, and a secondary battery. Background Technology
[0002] With the increasing demands for battery energy density from fields such as electric vehicles and high-end consumer electronics, developing next-generation high-capacity anode materials has become an industry consensus. Silicon (Si) boasts a theoretical specific capacity of up to 4200 mAh / g, more than 10 times that of traditional graphite anodes, and is considered one of the most promising anode materials. However, silicon undergoes a dramatic volume expansion of over 300% during charge and discharge, leading to a series of problems such as active particle pulverization, repeated rupture and regeneration of the solid electrolyte interphase (SEI) film, and electrical contact failure. Ultimately, this results in rapid capacity decay and short cycle life.
[0003] To address these issues, current approaches primarily employ nanotechnology, carbon composites, and porous structure design. Among these, silicon-carbon composites prepared by chemical vapor deposition (CVD) are widely recognized as the mainstream technology for the future. Silicon-carbon composites utilize the dispersion and internal space of the carbon framework to buffer the volume expansion of silicon by depositing nano-silicon within a porous carbon framework. Currently, CVD-deposited silicon-carbon materials achieve capacities of 1800–2100 mAh / g and initial efficiency of 91–94%. However, these approaches still suffer from the following problems: First, the numerous oxygen-containing functional groups (such as -COOH and -OH) within the porous carbon framework undergo irreversible side reactions with lithium ions during the first charge-discharge cycle, permanently consuming active lithium and hindering further improvements in initial efficiency. Second, during high-temperature carbon coating deposition, silicon readily reacts with the carbon source to form silicon carbide (SiC). Silicon carbide is electrochemically inert and has poor conductivity, leading to the loss of active material and causing long-term capacity decay.
[0004] Therefore, developing a novel silicon-based anode material that can reduce irreversible lithium loss from the material itself and establish a stable non-SiC generation interface is crucial for promoting the large-scale application of silicon anodes. Summary of the Invention
[0005] The main objective of this invention is to provide a negative electrode material and its preparation method, a negative electrode sheet, and a secondary battery, so as to solve the problem that silicon-carbon materials in the prior art are difficult to achieve both high initial efficiency and good cycle performance.
[0006] To achieve the above objectives, according to one aspect of the present invention, a negative electrode material is provided, comprising a porous carbon skeleton and a composite layer coated on the surface of the porous carbon skeleton, wherein the composite layer comprises, in a direction away from the porous carbon skeleton, a deoxidized carbon layer, a deposited silicon layer, a SiCN layer and a carbon coating layer in sequence.
[0007] Furthermore, the thickness of the deoxidized carbon layer is 10~50nm; and / or the thickness of the SiCN layer is 5~20nm; and / or the loading of deposited silicon is 80~150wt% of the weight of the porous carbon framework; and / or the thickness of the carbon coating layer is 2~86nm.
[0008] Furthermore, the pores of the porous carbon framework include first-type pores and second-type pores. The pore size of the first-type pores is 0.7~3nm, and the pore size of the second-type pores is <0.7nm. The pore volume of the first-type pores accounts for 75~90% of the total pore volume of the porous carbon framework; and / or the pore volume of the second-type pores accounts for 10~20% of the total pore volume of the porous carbon framework; and / or the total pore volume of the porous carbon framework is 0.65~1.24cc / g; and / or the particle size Dv50 of the porous carbon framework is 3~13.5μm; and / or the compressive strength of the porous carbon framework is 300~840MPa, and the compressive modulus is 15~66Gpa.
[0009] Furthermore, the specific surface area of the negative electrode material is 0.8~3.5m². 2 / g; and / or the particle size Dv50 of the negative electrode material is 4.0~13.4μm; and / or the true density of the negative electrode material is 1.95~2.15g / cc; and / or the conductivity of the negative electrode material at 10MPa pressure is 0.04~0.5S / cm.
[0010] The above-mentioned method for preparing the negative electrode material includes the following steps: Step S1, introducing a first deposition material and performing a first CVD deposition on porous carbon under a protective atmosphere to deposit a deoxygenated carbon layer on the surface of the porous carbon framework formed by the porous carbon, thereby obtaining a first intermediate; the first deposition material includes a first carbon source; Step S2, introducing a second deposition material and performing a second CVD deposition on the first intermediate to deposit silicon on the surface of the deoxygenated carbon layer, thereby obtaining a second intermediate; the second deposition material includes a first silicon source and a first dilution gas; Step S3, introducing a third deposition material... The second intermediate is subjected to plasma-enhanced atomic layer deposition to deposit a SiCN layer on the silicon surface, resulting in a third intermediate. The third deposition raw materials include a second silicon source, a nitrogen source, a second carbon source, and a second dilution gas. The deposition temperature of the plasma-enhanced atomic layer deposition is 400~600℃. In step S4, a fourth deposition raw material is introduced to perform a third CVD deposition on the third intermediate to deposit a carbon coating layer on the SiCN layer surface until the pores of the porous carbon framework are filled, resulting in a negative electrode material. The fourth deposition raw material includes a third carbon source and a third dilution gas.
[0011] Further, by volume percentage, the first dilution gas, the second dilution gas, or the third dilution gas comprises 1-5% H2 and 95-99% carrier gas, wherein the carrier gas is N2 or Ar; and / or the first carbon source, the second carbon source, or the third carbon source comprises one or more of CH4, C2H2, and toluene; and / or the first silicon source or the second silicon source comprises one or more of silane and chlorosilane; and / or in step S3, the nitrogen source comprises one or more of NH3 and urea; and / or in step S1, the protective atmosphere comprises one or more of argon atmosphere, nitrogen atmosphere, and helium atmosphere.
[0012] Further, in step S1, the flow rate of the first CVD deposition is: 80~120 sccm of first deposition material per 20g of porous carbon; and / or in step S1, the temperature of the first CVD deposition is 550~750℃, the pressure is 120~1500Pa, and the time is 40~120min; and / or in step S2, the volume ratio of the first silicon source to the first dilution gas is 1:(18~50); and / or in step S2, the second CVD deposition is carried out in a fluidized bed, and the volume concentration of the first silicon source in the fluidized bed is 2~5%; and / or in step S2, the flow rate of the second CVD deposition is: 100~300 sccm of second deposition material per 20g of the first intermediate; and / or in step S2, the temperature of the second CVD deposition is 400℃~550℃, the pressure is 100~500Pa, and the time is 1~4h.
[0013] Further, in step S3, the volume ratio of the second silicon source, nitrogen source, and second carbon source is 1:(2~6):(0.15~0.3); and / or in step S3, the second dilution gas accounts for 70~85% of the total flow rate of the third deposition material; and / or in step S3, the flow rate of plasma-enhanced atomic layer deposition is: 20~80 sccm of the third deposition material per 100g of the second intermediate; and / or in step S3, the plasma power of plasma-enhanced atomic layer deposition is 50~200W; and / or in step S3, the temperature of plasma-enhanced atomic layer deposition is 40°C. The temperature ranges from 0 to 500℃, the pressure from 100 to 500 Pa, and the time from 5 to 30 min; and / or in step S4, the volume ratio of the third carbon source to the third dilution gas is 1:(5 to 10); and / or in step S4, the third CVD deposition is carried out in a fluidized bed, and the volume concentration of the third carbon source in the fluidized bed is 10 to 20%; and / or in step S4, the flow rate of the third CVD deposition is: 100 to 300 sccm of fourth deposition material per 10 g of the third intermediate; and / or in step S4, the temperature of the third CVD deposition is 450℃ to 550℃, and the pressure is 10 min. 3 ~10 4 Pa, time is 5~45min.
[0014] According to another aspect of the present invention, a negative electrode sheet is provided, comprising a negative electrode current collector and a negative electrode material active layer disposed on at least one side of the negative electrode current collector, wherein the negative electrode material active layer comprises the aforementioned negative electrode material, or comprises a negative electrode material obtained according to the aforementioned method for preparing the negative electrode material.
[0015] According to another aspect of the present invention, a secondary battery is provided, comprising the aforementioned negative electrode.
[0016] By applying the technical solution of this invention, an ultra-stable interface is established based on existing silicon-carbon materials, thereby simultaneously achieving high initial efficiency, low expansion, and long cycle life. The dense deoxidized carbon layer on the surface of the porous carbon framework strengthens the structure, simultaneously achieving deep deoxidation, reducing irreversible consumption of active lithium, and improving initial efficiency. Simultaneously, the introduction of a dense and highly resilient SiCN layer isolates the deposited silicon from direct contact with the outer carbon coating layer, avoiding the formation of high-resistivity SiC byproducts at high temperatures. This dual mechanism of internal buffering and external confinement suppresses volume expansion, improving long-term cycle capacity retention. Attached Figure Description
[0017] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:
[0018] Figure 1 SEM images of the negative electrode material according to Embodiment 1 of the present invention are shown;
[0019] Figure 2 A TEM image of the negative electrode material according to Embodiment 1 of the present invention is shown;
[0020] Figure 3 The EDS spectrum of the negative electrode material according to Embodiment 1 of the present invention is shown. Detailed Implementation
[0021] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0022] As described in the background section of this invention, existing technologies suffer from the problem that silicon-carbon materials cannot simultaneously achieve high initial efficiency and good cycle performance. To address this issue, in a typical embodiment of this invention, a negative electrode material is provided, comprising a porous carbon framework and a composite layer coated on the surface of the porous carbon framework. The composite layer, in a direction away from the porous carbon framework, sequentially comprises a deoxidized carbon layer, deposited silicon, a SiCN layer, and a carbon coating layer.
[0023] This invention establishes an ultra-stable interface based on existing silicon-carbon materials, thereby simultaneously achieving high initial efficiency, low expansion, and long cycle life.
[0024] Porous carbon frameworks possess abundant pore structures and exhibit high compressive strength and modulus, providing support and space for composite layer deposition. However, the presence of numerous oxygen-containing functional groups on the surface can lead to reduced initial efficiency. Depositing a dense deoxidized carbon layer on the surface of the porous carbon framework strengthens the structure, suppresses radial deformation caused by silicon expansion through mechanical confinement, and significantly reduces the number of oxygen-containing functional groups on the surface after deposition, achieving deep deoxidation and reducing irreversible consumption of active lithium. Depositing silicon within the pores of the porous carbon framework (nearly filling them) improves the utilization rate of silicon active anode materials and enhances initial efficiency.
[0025] Simultaneously, a dense and highly resilient SiCN layer is introduced on top of the deposited silicon. Located between the deposited silicon and the carbon coating layer, it effectively isolates the direct contact between the deposited silicon and the outer carbon coating layer, preventing the formation of high-resistivity SiC byproducts at high temperatures. The SiCN layer combines high fracture toughness with good conductivity, maintaining electrical contact between the deposited silicon and the outer carbon layer while buffering shear stress. Combined with the amorphous carbon deposited on the outer layer, it forms a three-dimensional conductive network of "carbon skeleton-silicon-SiCN-carbon encapsulation," enabling the material to maintain high conductivity even under high pressure. Furthermore, as the substrate for the artificial solid electrolyte interphase (SEI) film, the SiCN layer effectively suppresses direct side reactions between the electrolyte and silicon, promoting the formation of a thin and dense natural SEI film, significantly reducing irreversible lithium consumption during cycling. The carbon coating layer provides additional conductive network and mechanical constraint, further buffering volume expansion and stabilizing the entire electrode structure.
[0026] The material of this invention forms a three-dimensional conductive network comprising a porous carbon framework, deoxygenated carbon, deposited silicon, SiCN, and a carbon coating layer. This significantly improves the structural integrity of the electrode during cycling, suppresses interfacial cracking and irreversible consumption of active lithium to enhance first-efficiency, and suppresses volume expansion through a dual mechanism of internal buffering and external confinement, thereby improving long-term cycling capacity retention.
[0027] In a preferred embodiment, the thickness of the deoxidized carbon layer is 10-50 nm. Controlling the deoxidized carbon layer within this range achieves a balance between structural strengthening and deoxidation efficiency, effectively constraining the radial stress induced by silicon expansion, while avoiding excessive occupation of the effective electrode volume and reducing energy density.
[0028] In a preferred embodiment, the SiCN layer has a thickness of 5-20 nm. These conditions are more conducive to isolating the high-temperature reaction between silicon and the carbon layer, suppressing SiC formation, and reducing the problem of increased lithium-ion diffusion resistance due to excessive thickness. The SiCN layer has better fracture toughness than traditional carbon layers, significantly improving its buffering capacity against silicon expansion shear stress and maintaining electrical contact stability. Its good conductivity also helps to cooperate with the outer carbon coating to construct a low-resistance conductive network, further improving the material's conductivity. These conditions facilitate a thinner and more stable SEI film, reduce active lithium consumption, and improve the initial efficiency of the anode material, which is beneficial for further improving the energy density and cycle life of lithium-ion batteries, achieving synergistic optimization of high initial efficiency, low expansion, and long cycle life.
[0029] The deposited silicon, uniformly distributed on the inner and outer surfaces of the porous carbon framework with a high loading, significantly improves the specific capacity of the material, fully leveraging the high theoretical capacity of silicon. Simultaneously, the confined space of the porous carbon framework and the mechanical constraint of the deoxidized carbon layer effectively mitigate structural damage caused by silicon expansion. In a preferred embodiment, the loading of deposited silicon is 80-150 wt% of the porous carbon framework; and / or the thickness of the carbon coating layer is 2-86 nm. The carbon coating layer forms a continuous, dense conductive protective shell on the surface of the SiCN layer. Its suitable thickness enhances the overall conductivity network and mechanical stability while reducing ion transport obstruction and energy density reduction caused by excessive thickness. This helps maintain the structural integrity, stable electrical contact, and controllable interfacial reactions of the anode material during cycling.
[0030] In a preferred embodiment, the porous carbon framework comprises a first type of pore and a second type of pore, wherein the pore size of the first type of pore is 0.7~3 nm, and the pore size of the second type of pore is <0.7 nm; wherein the pore volume of the first type of pore accounts for 75~90% of the total pore volume of the porous carbon framework; and / or the pore volume of the second type of pore accounts for 10~20% of the total pore volume of the porous carbon framework; and / or the total pore volume of the porous carbon framework is 0.65~1.24 cc / g; and / or the particle size Dv50 of the porous carbon framework is 3~13.5 μm; and / or the compressive strength of the porous carbon framework is 300~840 MPa, and the compressive modulus is 15~66 GPa.
[0031] The hierarchical pore structure of the porous carbon framework is more conducive to balancing efficient confined deposition of silicon and rapid electrolyte wetting after the deoxygenated carbon layer is coated, thereby improving the utilization rate of active materials and ion transport efficiency. The moderate total pore volume and high compressive strength and modulus characteristics help form a robust and stable mechanical support, restraining structural damage caused by silicon expansion. The optimized particle size distribution helps improve the fluidization and coating performance of the material, enhancing electrode uniformity. The aforementioned porous carbon framework can synergistically enhance the "hooking" effect of the deoxygenated carbon layer, the interfacial isolation effect of the SiCN layer, and the conductive network of the carbon coating layer, significantly improving the structural stability and interfacial integrity of the anode material, thereby improving the battery's initial efficiency, cycle stability, and rate performance.
[0032] In a preferred embodiment, the specific surface area of the negative electrode material is 0.8~3.5m². 2 / g; and / or the particle size Dv50 of the anode material is 4.0~13.4μm; and / or the true density of the anode material is 1.95~2.15g / cc; and / or the conductivity of the anode material at 10MPa pressure is 0.04~0.5S / cm. A suitable specific surface area of the anode material can more effectively balance the exposure of active sites and electrolyte side reactions, promoting the formation of a stable SEI film; a suitable particle size Dv50 is beneficial for providing excellent slurry dispersibility and electrode compaction performance, improving coating uniformity and electrode density; controlling the true density within the above range is preferable, as it helps the material maintain good volume utilization even under high silicon loading. The high conductivity originates from the synergistic effect of the three-dimensional conductive network of the carbon skeleton, silicon, SiCN, and carbon coating layer, which can significantly enhance electron transport capability and interfacial contact stability.
[0033] In another typical embodiment of the present invention, a method for preparing the above-mentioned negative electrode material of the present invention is also provided, comprising the following steps: Step S1, introducing a first deposition material and performing a first CVD deposition on porous carbon under a protective atmosphere to deposit a deoxygenated carbon layer on the surface of the porous carbon framework formed by the porous carbon, thereby obtaining a first intermediate; the first deposition material includes a first carbon source; Step S2, introducing a second deposition material and performing a second CVD deposition on the first intermediate to deposit silicon on the surface of the deoxygenated carbon layer, thereby obtaining a second intermediate; the second deposition material includes a first silicon source and a first dilution gas; Step S3, Introduce the third deposition material and perform plasma-enhanced atomic layer deposition on the second intermediate to deposit a SiCN layer on the silicon surface to obtain the third intermediate; the third deposition material includes a second silicon source, a nitrogen source, a second carbon source, and a second dilution gas, and the deposition temperature of plasma-enhanced atomic layer deposition is 400~600℃; In step S4, Introduce the fourth deposition material and perform third CVD deposition on the third intermediate to deposit a carbon coating layer on the SiCN layer surface until the pores of the porous carbon framework are filled to obtain the anode material; the fourth deposition material includes a third carbon source and a third dilution gas.
[0034] Porous carbon is first placed in a tube furnace, heated under a protective atmosphere, and a carbon source is introduced for short-term carbon deposition. The carbon source reacts with oxygen-containing groups inside the porous carbon framework to generate CO2 and CO, achieving deep deoxidation and depositing a deoxidized carbon layer on the surface of the porous carbon framework. Simultaneously, a dense pyrolytic carbon layer accumulates on the inner surface of the porous carbon framework, acting as an "outer shell." This dense surface layer provides a "binding" effect, limiting overall volume expansion and resisting radial stress generated by silicon expansion. After the reaction is complete, the framework is cooled to room temperature under a protective atmosphere to obtain the pretreated porous carbon framework, i.e., the first intermediate.
[0035] Then, in a fluidized bed apparatus, a silicon source and dilution gas are introduced to deposit silicon as nanoparticles or thin layers onto the inner and outer surfaces of the porous carbon framework, thereby depositing silicon on the surface of the deoxidized carbon layer to obtain the second intermediate. CVD deposition is used to lower the temperature below the initiation temperature of a significant solid-state reaction between silicon and carbon (typically <550°C), thus avoiding reaction between silicon and the porous carbon framework or the deoxidized carbon layer.
[0036] Subsequently, silicon, nitrogen, carbon, and dilution gases are introduced. Plasma-enhanced atomic layer deposition (PEALD) is used on the surface of the deposited silicon material to achieve conformal and nanoscale control of the SiCN thin film, encapsulating a dense, continuous, and conductive SiCN layer (thin film) as a barrier to prevent silicon-carbon reaction during subsequent carbon deposition, resulting in a third intermediate. During the SiCN deposition process, a trace amount of carbon source is introduced to form a ternary amorphous SiCN layer. The SiCN thin film exhibits high fracture toughness and slightly improved conductivity, making it more resistant to shear stress generated by silicon expansion.
[0037] The deposition temperature of the SiCN layer is 400~600℃, far lower than the temperature at which silicon and carbon can react significantly (typically >600℃). Plasma can dissociate nitrogen source molecules into active nitrogen atoms, allowing them to react and form SiCN at low temperatures, achieving high-quality film deposition at low temperatures. Furthermore, the low deposition temperature of plasma-enhanced atomic layer deposition does not damage the existing deposited silicon structure, making it particularly suitable for covering deposited silicon particles inside porous materials. Too low a deposition temperature will result in poor film quality, while too high a temperature may promote the reaction between Si and C. High-quality deposition can only be achieved within the aforementioned temperature range.
[0038] Finally, a carbon source and dilution gas are introduced to deposit an amorphous carbon coating layer on the surface of the SiCN layer, filling the pores of the porous carbon framework to obtain the anode material. At this point, the SiCN layer is present and can withstand higher temperatures than the first CVD deposition to obtain a high-quality carbon layer. Furthermore, because a dense SiCN layer is immediately coated onto the silicon surface as an insulating layer after silicon deposition, subsequent carbon coating layer deposition (even at higher temperatures) occurs on the SiCN layer surface, not on the silicon surface, thus physically blocking the direct contact reaction between silicon and the carbon source at high temperatures.
[0039] This invention employs a sequential deposition structure of "silicon, SiCN, and carbon coating." Through carbon framework pretreatment, silicon deposition, low-temperature SiCN deposition, and carbon coating, the material composition and interface are controlled at the molecular / atomic scale to obtain a multilayer deposition anode material. The porous carbon framework, after carbon deposition pretreatment, forms a dense pyrolytic carbon shell, which significantly improves the framework's compressive strength and achieves radial constraint on silicon expansion. Silicon is deposited on the inner and outer surfaces of the porous carbon framework pores, followed by plasma-enhanced atomic layer deposition to form an in-situ SiCN isolation layer on the silicon surface. This layer possesses both high fracture toughness and conductivity, blocking the high-temperature reaction path between silicon and subsequent carbon layers and inhibiting SiC formation. Finally, an amorphous carbon coating layer is deposited to construct a continuous conductive network. This multilayer composite structure can buffer the expansion stress of silicon and maintain the conductive network, while simultaneously solving the problems of silicon volume expansion, electrical contact, and direct reaction with carbon (SiC formation). This material can significantly reduce the irreversible consumption of active lithium and the formation of SiC, and suppress volume expansion through a dual mechanism of internal buffering and external confinement. At the same time, it establishes an ultra-stable interface, thereby simultaneously achieving high initial efficiency, low expansion and long cycle life.
[0040] The dilution gas uses high-purity hydrogen (H2) and a carrier gas. H2 helps clean the surface and inhibit gas-phase nucleation, while its addition is controlled in trace amounts to reduce the potential effect of reducing carbon. In a preferred embodiment, the first, second, or third dilution gas, by volume percentage, comprises 1-5% H2 and 95-99% carrier gas, wherein the carrier gas is N2 or Ar; and / or the first, second, or third carbon source comprises one or more of CH4, C2H2, and toluene; and / or the first or second silicon source comprises one or more of silane and chlorosilane; and / or in step S3, the nitrogen source comprises one or more of NH3 and urea; and / or in step S1, the protective atmosphere comprises one or more of argon, nitrogen, and helium atmospheres. The above-mentioned carbon sources are abundant and have moderate pyrolysis temperatures. The above-mentioned silicon sources have higher reactivity, which is beneficial for low-temperature deposition. The nitrogen source is a plasma-activated nitrogen source.
[0041] In a preferred embodiment, in step S1, the flow rate of the first CVD deposition is: 80-120 sccm of first deposition material per 20g of porous carbon; and / or in step S1, the temperature of the first CVD deposition is 550-750℃, the pressure is 120-1500Pa, and the time is 40-120min. The above deposition flow rate facilitates the full penetration of the carbon source into the porous carbon framework, efficiently removes oxygen-containing functional groups, achieves deep deoxidation, and significantly reduces irreversible lithium consumption during the first charge-discharge cycle. Controlling the deposition temperature and time within the above range is preferable, as it synergistically promotes the uniform coating of a dense pyrolytic carbon layer, forming a strong and tough outer shell, enhancing the stability of the framework structure, and ensuring a tight bond between the deoxidized carbon layer and the framework, providing a stable substrate for the subsequent uniform deposition of silicon.
[0042] To further promote uniform diffusion and deep deposition of the silicon source within the porous carbon framework, achieving highly consistent silicon deposition both inside and outside the pores, in a preferred embodiment, in step S2, the volume ratio of the first silicon source to the first dilution gas is 1:(18~50); and / or in step S2, the flow rate of the second CVD deposition is: 100~300 sccm of second deposition material per 20g of the first intermediate; and / or in step S2, the temperature of the second CVD deposition is 400℃~550℃, the pressure is 100~500Pa (approximately 1~5 Torr), and the time is 1~4h. A higher dilution ratio is beneficial for promoting sufficient diffusion of the silicon source into the pores and removing reaction byproducts (such as H2). The total gas flow rate can be adjusted according to the size of the reaction chamber and the amount of powder to ensure stable fluidization. A lower deposition temperature is beneficial for further reducing side reactions between silicon and the carbon substrate, and a low-pressure environment can promote gas diffusion within the micropores, improving deposition uniformity. A suitable deposition time can ensure sufficient silicon loading, guaranteeing high capacity and enabling high-quality, low-damage in-situ deposition of silicon.
[0043] Preferably, the second CVD deposition is carried out in a fluidized bed, and the volume concentration of the first silicon source in the fluidized bed is 2-5%. A low concentration helps silicon to be deposited uniformly in the channels and reduces the problem of excessively rapid clogging at the orifices. Here, the volume concentration of the first silicon source in the fluidized bed refers to the concentration of the first silicon source during deposition in the fluidized bed equipment, and is not entirely consistent with the gas flow rate.
[0044] In a preferred embodiment, in step S3, the volume ratio of the second silicon source, nitrogen source, and second carbon source is 1:(2~6):(0.15~0.3); and / or the second dilution gas accounts for 70~85% of the total flow rate of the third deposition material; and / or in step S3, the flow rate of plasma-enhanced atomic layer deposition is: 20~80 sccm of the third deposition material per 100g of the second intermediate; and / or the plasma power of plasma-enhanced atomic layer deposition is 50~200W; and / or in step S3, the temperature of plasma-enhanced atomic layer deposition is 400~500℃, the pressure is 100~500Pa, and the time is 5~30min.
[0045] The above conditions facilitate the synergistic construction of a high-toughness, high-conductivity SiCN layer during plasma activation. Its dense, continuous structure effectively blocks direct contact between silicon and carbon, inhibiting SiC formation. Appropriate dilution of the silicon, nitrogen, and carbon sources using dilution gas promotes uniform diffusion into the porous structure, achieving conformal coating. The total gas flow rate can be adjusted according to the reaction chamber size and powder quantity to maintain stable fluidization. A moderate total flow rate and plasma power help balance the deposition rate and film quality, stimulating the decomposition of the deposition raw materials (precursors), promoting Si-NC formation, and achieving high-quality film formation at low temperatures without damaging existing deposited silicon. Low pressure facilitates gas diffusion within the porous structure. Controlling the temperature, pressure, and time of plasma-enhanced atomic layer deposition within the above ranges is beneficial for synergistically promoting high-quality SiCN layer formation and uniform coverage at the nanoscale, enhancing interfacial electrical contact and stress buffering capacity, and giving the SiCN layer both structural stability and conductivity. As an SEI substrate, it significantly suppresses side reactions, constructs an efficient and stable conductive network for the anode material, and improves the battery's initial efficiency and cycle stability.
[0046] Hydrogen helps form a denser carbon coating layer, further promoting the full decomposition of the carbon source and forming a dense, continuous, and highly conductive amorphous carbon coating layer. Simultaneously, to regulate the deposition rate, in a preferred embodiment, in step S4, the volume ratio of the third carbon source to the third dilution gas is 1:(5~10); and / or in step S4, the flow rate of the third CVD deposition is: 100~300 sccm of fourth deposition material per 10g of the third intermediate; and / or in step S4, the temperature of the third CVD deposition is 450℃~550℃, and the pressure is 10... 3 ~10 4 Pa, time is 5~45min.
[0047] In the third CVD deposition process, the total gas flow rate can be adjusted according to the reaction chamber size and powder amount to maintain stable fluidization and improve coating uniformity. Due to the protection of the SiCN layer, silicon does not come into contact with the carbon generated by high-temperature decomposition, avoiding SiC formation. Therefore, the third CVD deposition can use higher temperatures, allowing for sufficient carbon source decomposition at high temperatures, which is beneficial for forming amorphous carbon with good conductivity. A suitable deposition temperature can promote a moderate increase in the graphitization degree of the carbon layer under the protection of the SiCN layer, enhancing conductivity and mechanical strength. Operation in atmospheric to low-pressure environments is simpler and suitable for mass production. Combined with appropriate deposition time, this facilitates control of the carbon layer thickness, fully encapsulating the silicon system while reducing impedance rise. Without damaging the inner structure, it constructs a highly efficient conductive network and a tough outer shell, significantly improving the electrical contact stability and expansion buffering capacity of the anode material, thereby enhancing the battery's cycle life, initial efficiency, and rate performance.
[0048] Preferably, the third CVD deposition is carried out in a fluidized bed, and the volume concentration of the third carbon source in the fluidized bed is 10-20%, preferably 10-16%, which is higher than the volume concentration of the silicon source in the fluidized bed during the second CVD deposition process, because the carbon layer needs a certain thickness and continuity. The volume concentration of the third carbon source in the fluidized bed refers to the concentration of the third carbon source during deposition in the fluidized bed equipment, and is not entirely consistent with the gas flow rate.
[0049] In another typical embodiment of the present invention, a negative electrode sheet is also provided, comprising a negative electrode current collector and a negative electrode material active layer disposed on at least one side of the negative electrode current collector. The negative electrode material active layer comprises the negative electrode material described above in the present invention, or comprises a negative electrode material obtained by the preparation method of the negative electrode material described above in the present invention, which has significantly improved first-efficiency and cycle performance.
[0050] In some embodiments, the preparation method of the negative electrode sheet includes the following steps: kneading the negative electrode active material, a portion of the conductive agent, a portion of the binder, and the solvent (water) for 0.5 to 3 hours; then adding the remaining conductive agent, the remaining binder, and the solvent (water) and stirring for 0.5 to 3 hours, controlling the solid content to be 30 to 55%; then adding the solvent (water) and stirring to obtain a negative electrode slurry. Preferably, the solid content of the negative electrode slurry is 25 to 48%, and the slurry fineness is ≤45 μm. The negative electrode slurry is coated onto a negative electrode current collector (foil), dried to remove the solvent, rolled, cut, dried again, and die-cut to obtain the negative electrode sheet. Preferably, the areal density of the negative electrode sheet is 0.003 to 0.015 g / cm³. 2 The thickness is 45~195μm. The negative electrode active material includes the negative electrode material described above in this invention, and may also include artificial graphite negative electrode material. In the negative electrode slurry, the weight ratio of negative electrode active material, conductive agent and binder is (86~98.6):(0.2~10):(1.2~8).
[0051] In another typical embodiment of the present invention, a secondary battery is also provided, comprising the negative electrode sheet described above.
[0052] In some embodiments, the preparation method of the secondary battery includes the following steps: kneading the positive electrode material, a portion of the conductive agent, binder, and solvent (NMP) for 0.5-3 hours; then adding the remaining conductive agent, solvent (NMP), and electrolyte and stirring for 0.5-3 hours, controlling the solid content to be 65-85%; then adding solvent (NMP) and stirring for 0.5-3 hours to obtain a positive electrode slurry. Preferably, the solid content of the positive electrode slurry is 60-80%, and the slurry fineness is ≤45μm. The positive electrode slurry is coated onto a positive electrode current collector (foil), dried to remove the solvent, rolled, dried again, and die-cut to obtain a positive electrode sheet. Preferably, the areal density of the positive electrode sheet is 0.012-0.027 g / cm³. 2The thickness is 60~210μm. In the positive electrode slurry, the weight ratio of positive electrode material, conductive agent, and binder is (94~99.4):(0.5~10):(0.05~0.8). The positive electrode sheet, separator, and negative electrode sheet are stacked, and the tabs are welded, the casing is installed, the electrolyte is injected, formation is performed, and capacity is tested to obtain a secondary battery.
[0053] In some embodiments, the conductive agent includes one or more of conductive carbon black, conductive Ketjen black, conductive acetylene black, conductive graphene, single-walled carbon nanotubes, and multi-walled carbon nanotubes; and / or the binder includes one or more of lithium polyacrylate, polymethyl methacrylate, polyethyl ethyl acrylate, lithium polyacrylate-methacrylate, lithium polyacrylate-acrylonitrile, sodium polyacrylate-acrylonitrile, carboxymethyl cellulose, and polyvinylidene fluoride; and / or the electrolyte includes one or more of lithium lanthanum zirconate, lithium lanthanum tantalate, lithium lanthanum zirconate-tantalate, lithium titanium aluminum phosphate, lithium germanium aluminum phosphate, polyoxyethylene, polyacrylonitrile, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polymethyl methacrylate, lithium indium chloride, lithium yttrium chloride, lithium yttrium bromide, lithium chlorosulfur phosphorus, and lithium sulfur phosphorus germanium; and / or the cathode material includes any one of lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium nickel cobalt manganese aluminum oxide, lithium-rich manganese-based oxide, lithium iron phosphate, lithium manganese phosphate, lithium iron manganese phosphate, lithium manganese oxide, lithium cobalt oxide, and lithium nickel manganese oxide.
[0054] Typical, but not limiting, thickness of the deoxygenated carbon layer is 10 nm, 20 nm, 30 nm, 40 nm, 50 nm or any two of these values.
[0055] Typical, but not limited, SiCN layer thicknesses are 5 nm, 10 nm, 12 nm, 15 nm, 20 nm, or any combination of two of these values.
[0056] Typically, but not limitingly, the loading of deposited silicon is 80 wt%, 100 wt%, 120 wt%, 140 wt%, 150 wt% of the weight of the porous carbon framework, or a range of any two of these values.
[0057] Typical, but not limiting, carbon coating thicknesses are 2 nm, 20 nm, 38 nm, 56 nm, 74 nm, 86 nm, or any combination of two of these values.
[0058] Typically, but not limitingly, in step S3, the deposition temperature for plasma-enhanced atomic layer deposition is 400°C, 450°C, 500°C, 550°C, 600°C, or a range of any two of these values.
[0059] Typically, but not limitingly, in step S1, the flow rate of the first CVD deposition is: for every 20g of porous carbon, a first deposition feedstock is introduced at a value within the range of 80 sccm, 90 sccm, 100 sccm, 110 sccm, 120 sccm, or any two of these values.
[0060] Typically, but not limitingly, in step S1, the temperature of the first CVD deposition is 550°C, 600°C, 650°C, 700°C, 750°C or any two of these values; the pressure is 120 Pa, 400 Pa, 700 Pa, 1000 Pa, 1300 Pa, 1500 Pa or any two of these values; and the time is 40 min, 60 min, 80 min, 100 min, 120 min or any two of these values.
[0061] Typically, but not limitingly, in step S2, the second CVD deposition is carried out in a fluidized bed, and the volume concentration of the first silicon source in the fluidized bed is 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, or any two of these values.
[0062] Typically, but not limitingly, in step S2, the flow rate of the second CVD deposition is: for every 20g of the first intermediate, a second deposition feedstock is introduced at a flow rate of 100 sccm, 150 sccm, 200 sccm, 250 sccm, 300 sccm, or any two of these values.
[0063] Typically, but not limitingly, in step S2, the temperature of the second CVD deposition is 400°C, 420°C, 450°C, 480°C, 500°C, 520°C, 550°C, or any two of these values; the pressure is 100 Pa, 200 Pa, 300 Pa, 400 Pa, 500 Pa, or any two of these values; and the time is 1 h, 2 h, 3 h, 4 h, or any two of these values.
[0064] Typically, but not limitingly, in step S3, the flow rate of plasma-enhanced atomic layer deposition is: for every 100g of the second intermediate, a third deposition feedstock is introduced at a flow rate of 20 sccm, 35 sccm, 50 sccm, 65 sccm, 80 sccm, or any two of these values.
[0065] Typically, but not limitingly, in step S3, the plasma power for plasma-enhanced atomic layer deposition is a range of 50 W, 80 W, 100 W, 150 W, 200 W, or any two of these values.
[0066] Typically, but not limitingly, in step S3, the temperature for plasma-enhanced atomic layer deposition is 400°C, 425°C, 450°C, 475°C, 500°C or any two of these values; the pressure is 100 Pa, 200 Pa, 300 Pa, 400 Pa, 500 Pa or any two of these values; and the time is 5 min, 10 min, 15 min, 20 min, 25 min, 30 min or any two of these values.
[0067] Typically, but not limitingly, in step S4, the third CVD deposition is carried out in a fluidized bed, and the volume concentration of the third carbon source in the fluidized bed is 10%, 12%, 14%, 16%, 18%, 20%, or any two of these values.
[0068] Typically, but not limitingly, in step S4, the flow rate of the third CVD deposition is: for every 10g of the third intermediate, a fourth deposition feedstock is introduced at a flow rate of 100 sccm, 150 sccm, 200 sccm, 250 sccm, 300 sccm, or any two of these values.
[0069] Typically, but not limitingly, in step S4, the temperature of the third CVD deposition is 450°C, 475°C, 500°C, 525°C, 550°C or any two of these values, and the time is 5 min, 15 min, 25 min, 35 min, 45 min or any two of these values.
[0070] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.
[0071] Example 1
[0072] The preparation parameters are detailed in Tables 1 to 4.
[0073] Step S1: CH4 is introduced and heated at a rate of 5℃ / min under an argon atmosphere to perform a first CVD deposition on porous carbon, so as to deposit a deoxygenated carbon layer on the surface of the porous carbon framework to obtain the first intermediate.
[0074] In step S2, SiH4 and dilution gas (2% H2 + 98% Ar) are introduced to perform a second CVD deposition on the first intermediate to deposit silicon on the surface of the deoxygenated carbon layer, thereby obtaining the second intermediate.
[0075] In step S3, SiH4, NH3, C2H2 and dilution gas (2%H2+98%Ar) are introduced to perform plasma-enhanced atomic layer deposition on the second intermediate to deposit a SiCN layer on the silicon surface, thus obtaining the third intermediate.
[0076] Step S4: C2H2 and dilution gas (2%H2+98%Ar) are introduced to perform a third CVD deposition on the third intermediate to deposit a carbon coating layer on the surface of the SiCN layer until the pores of the porous carbon framework are filled, thus obtaining the anode material.
[0077] Examples 2 to 17
[0078] The difference from Example 1 is that the preparation parameters are different, as detailed in Tables 1 to 4.
[0079] Comparative Example 1
[0080] The difference from Example 1 is that the deoxygenated carbon layer deposition in step S1 was not performed.
[0081] Comparative Example 2
[0082] The difference from Example 1 is that the SiCN layer deposition in step S3 was not performed.
[0083] Comparative Example 3
[0084] The difference from Example 1 is that in step S3, the temperature of plasma-enhanced atomic layer deposition is 350°C.
[0085] Comparative Example 4
[0086] The difference from Example 1 is that in step S3, the temperature of plasma-enhanced atomic layer deposition is 650°C.
[0087] Performance testing:
[0088] The negative electrode materials prepared in the above embodiments and comparative examples were analyzed and tested as follows, and the results are shown in Tables 5 and 6.
[0089] 1. Porous carbon (skeleton)
[0090] Pore distribution and total pore volume: measured using the N2 / CO2 gas adsorption method.
[0091] Particle size Dv50: Measured using a laser particle size analyzer; dispersant: water; refractive index: 2.0; absorptivity: 0.8; medium refractive index: 1.33; stirring speed: 2000 rpm; power: 30 W.
[0092] Compressive strength: Measured on a nanoindenter. Porous carbon particles were dispersed in ethanol, and then fixed onto a substrate with UV adhesive. The radius d of the porous carbon particles was measured (the cross-sectional area of the particles was calculated as πd). 2 The "Nano Compression" module was selected to measure the pressure P received during particle pressure loss. M Compressive strength = P M / πd 2Thirty porous carbon particles were tested, and the average value was taken as the compressive strength.
[0093] Compression modulus: Measured on a nanoindenter. Porous carbon particles were dispersed in ethanol, and then fixed to a substrate using UV adhesive. The "nanocompression" loading segment was selected. Loading rate setting: Displacement control was used, with the rate kept as low as possible (8 nm / s). Maximum displacement setting: Set to 20% of the particle size to ensure a sufficiently long elastic segment without one-time crushing. Loading to 80 nm and then unloading can be performed first, and elastic recovery observed to calculate the compression modulus (avoiding particle damage). The entire loading-unloading linear elastic segment was recorded, along with the engineering stress 'a' and engineering strain 'b'. The highest slope of the linear elastic segment, E=A / b, was calculated as the compression modulus.
[0094] 2. Sedimentary layer
[0095] The thicknesses of the deoxygenated carbon layer, SiCN layer, and carbon coating layer were calculated using TEM images.
[0096] The percentage of silicon loading relative to the porous carbon framework: Measure the total mass before and after silicon deposition, and calculate the silicon loading as follows: (Total mass after silicon deposition - Total mass before silicon deposition) ÷ Total mass before silicon deposition × 100%.
[0097] 3. Negative electrode material
[0098] Specific surface area: Measured using a specific surface area analyzer, referring to GB / T 38823-2020 "Silicon Carbon".
[0099] Particle size Dv50: Measured using a laser particle size analyzer, referring to GB / T 38823-2020 "Silicon Carbon".
[0100] True density: Measured using a true density meter, referring to GB / T 24533-2019 "Graphite Anode Materials for Lithium-ion Batteries".
[0101] 10MPa conductivity: Measured using a powder resistance meter, referring to GB / T 47091-2026 "Determination of conductivity of metal powders".
[0102] 4. Electrochemical performance
[0103] 4.1 First-efficiency and negative electrode interface
[0104] The negative electrode materials obtained in the above embodiments and comparative examples were used to prepare coin cells for testing according to the following method: A negative electrode material:SP:CMC:SBR was mixed in a weight ratio of 94.5:1.5:1.5:2.5, and water was added to achieve a solid content of 40%. The weighed material was placed in a homogenizer, homogenized, and defoamed. The slurry was then coated onto a negative electrode sheet. In a glove box, the negative electrode shell was placed on clean paper, a nickel mesh was placed inside, and the brushed lithium sheet was placed on top. One drop of electrolyte (1M LiPF6, EC:EMC=3:7, 10% FEC) was added. The separator was placed in the middle of the lithium sheet, one drop of electrolyte was added, and the negative electrode sheet was placed directly above the lithium sheet. The positive electrode shell was then covered. All operations were performed on clean paper. The assembled coin cell was placed flat in the lower mold groove with the positive electrode facing down and the negative electrode facing up. It was sealed using a sealing machine (600kg pressure electric sealing machine / 60psi pneumatic sealing machine), and then removed with insulated tweezers and placed back in the original order. Charge the button cell to 2V at a rate of 0.1C, let it stand for 5 minutes, and the capacity is a; let it stand for 5 hours, discharge it to 0.005V at a rate of 0.05C, discharge it to 0.005V at a constant current of 0.05mA, let it stand for 5 minutes, and discharge it to 0.005V at a constant current of 0.01mA, and the capacity is b.
[0105] First-efficacy: First-efficacy = b / a × 100%.
[0106] Negative electrode interface: Disassemble the tamper and observe the negative electrode interface.
[0107] 4.2 Cyclic Performance
[0108] The negative electrode materials obtained in the above embodiments and comparative examples were used to prepare negative electrode sheets and secondary batteries for testing according to the following methods:
[0109] (1) The negative electrode active material includes artificial graphite and newly prepared negative electrode material in a weight ratio of 15:85; the conductive agent includes conductive carbon black and single-walled carbon nanotubes in a weight ratio of 60:40; the binder includes lithium polyacrylate, lithium polyacrylate-methacrylate and carboxymethyl cellulose in a weight ratio of 25:50:25; the solvent is water. The weight ratio of negative electrode active material, conductive agent and binder is 94:1.3:4.7. The conductive agent and negative electrode active material are premixed; half of the lithium polyacrylate, half of the lithium polyacrylate-methacrylate, half of the carboxymethyl cellulose and solvent are added and kneaded for 1 hour; the remaining lithium polyacrylate, the remaining lithium polyacrylate-methacrylate, the remaining carboxymethyl cellulose, the remaining conductive agent and solvent are added and mixed and stirred for 2.5 hours to control the solid content at 53%; the solvent is added and stirred for 1.5 hours to control the solid content at 47% and the fineness ≤45μm to obtain the negative electrode slurry.
[0110] (2) The cathode material is lithium nickel cobalt manganese oxide; the conductive agent includes conductive carbon black, single-walled carbon nanotubes and multi-walled carbon nanotubes, with a weight ratio of 60:20:20; the binder is polyvinylidene fluoride; the electrolyte is lithium titanium aluminum phosphate; and the solvent is NMP. The weight ratio of cathode material, conductive agent, binder and electrolyte is 98.5:0.9:0.6. The conductive agent and cathode material are premixed, and the binder and solvent are added and kneaded for 1 hour; then the conductive agent, solvent and electrolyte are added and stirred for 1.5 hours to control the solid content at 85%, and then the solvent NMP is added and stirred for 1 hour to control the solid content at 74% and the fineness ≤45μm to obtain the cathode slurry.
[0111] (3) Coat the negative electrode paste onto the copper foil, controlling the areal density to be 0.008 g / cm³. 2 The process involves drying to remove solvent, rolling, cutting, drying again, and die-cutting to obtain a negative electrode sheet with a thickness of 120 μm.
[0112] (4) Coat the positive electrode paste onto aluminum foil, controlling the areal density to be 0.023 g / cm³. 2 The positive electrode sheet is obtained by drying to remove solvent, rolling, drying, and die cutting, with a thickness of 116μm.
[0113] (5) Stack the positive electrode, separator (polypropylene), and negative electrode, and prepare the electrolyte (13% LiPF6, 18.2% solvent (EC:EMC=3:7, v / v), 10% FEC, 25% PP, 24% EP, 8.0% PC, 0.55% DTD, 1.0% PS, 0.25% LITFSI). LiPF6 refers to lithium hexafluorophosphate, EC refers to ethylene carbonate, EMC refers to ethyl methyl carbonate, FEC refers to fluoroethylene carbonate, PP refers to 1,3-propanesulfonyl lactone, EP refers to propylene oxide, PC refers to propylene carbonate, DTD refers to lithium bis(oxalato)borate, PS refers to 1,3-propanesulfonyl lactone, and LITFSI refers to lithium bis(trifluoromethanesulfonyl)imide. Weld the tabs, install the casing, fill with electrolyte, form, and perform capacity testing to obtain a secondary battery.
[0114] After the prepared secondary battery was left to stand at 25°C for 2 days, it was first discharged at 0.5C to 2.80V, left to rest for 5 minutes, charged at a constant current of 0.5C to 4.35V, charged at a constant voltage of 4.35V until the current < 0.05C, and discharged at 0.5C to 2.80V. This charging and discharging process was repeated until the discharge capacity was 80% of the initial value. The number of cycles was recorded as the cycle life.
[0115] During the cycle, the battery in each group is taken for 100 cycles for cycle expansion calculation. The 100-cycle cycle expansion growth = 100-cycle battery full charge thickness ÷ initial battery full charge thickness × 100%.
[0116] 100-turn DC internal resistance: The DC internal resistance meter measures the internal resistance of the battery cell at 1KHz.
[0117] Table 1
[0118]
[0119] Table 2
[0120]
[0121] Table 3
[0122]
[0123] Table 4
[0124]
[0125] Table 5
[0126]
[0127] Table 6
[0128]
[0129]
[0130] SEM image of the negative electrode material in Example 1 is shown below. Figure 1 As can be seen, the negative electrode material is spherical. A TEM image of the negative electrode material in Example 1 is shown below. Figure 2 As can be seen, the negative electrode material is spherical with a dense surface and no pores. The EDS spectrum of the negative electrode material in Example 1 is shown below. Figure 3 It can be seen that the negative electrode material contains silicon, carbon, and nitrogen, with silicon and carbon being the most abundant and nitrogen the least abundant.
[0131] As can be seen from the above, compared with the comparative examples, the embodiments of the present invention establish an ultra-stable interface based on existing silicon-carbon materials, thereby simultaneously achieving high initial efficiency, low expansion, and long cycle life. The dense deoxidized carbon layer on the surface of the porous carbon framework can strengthen the structure, simultaneously achieve deep deoxidation, reduce irreversible consumption of active lithium, and improve initial efficiency. At the same time, the introduction of a dense and highly resilient SiCN layer isolates the direct contact between the deposited silicon and the outer coated carbon layer, avoiding the formation of high-resistivity SiC byproducts at high temperatures. Through the dual mechanism of internal buffering and external confinement, volume expansion is suppressed, improving long-term cycle capacity retention.
[0132] Furthermore, it can be seen that the overall effect is better when all process parameters are within the preferred range of the present invention.
[0133] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A negative electrode material, characterized in that, It includes a porous carbon skeleton and a composite layer covering the surface of the porous carbon skeleton. In the direction away from the porous carbon skeleton, the composite layer sequentially includes a deoxidized carbon layer, a deposited silicon layer, a SiCN layer and a carbon coating layer.
2. The negative electrode material according to claim 1, characterized in that, The negative electrode material satisfies at least one of the following conditions: (1) The thickness of the deoxidized carbon layer is 10~50 nm; (2) The thickness of the SiCN layer is 5~20nm; (3) The loading of the deposited silicon is 80-150 wt% of the weight of the porous carbon framework; (4) The thickness of the carbon coating layer is 2~86nm.
3. The negative electrode material according to claim 1 or 2, characterized in that, The negative electrode material satisfies at least one of the following conditions: (1) The porous carbon framework has pores of a first type and a second type, wherein the pore diameter of the first type of pore is 0.7~3nm and the pore diameter of the second type of pore is <0.7nm; wherein the pore volume of the first type of pore accounts for 75~90% of the total pore volume of the porous carbon framework; and / or the pore volume of the second type of pore accounts for 10~20% of the total pore volume of the porous carbon framework; (2) The total pore volume of the porous carbon framework is 0.65~1.24cc / g; (3) The particle size Dv50 of the porous carbon skeleton is 3~13.5μm; (4) The compressive strength of the porous carbon skeleton is 300~840 MPa and the compressive modulus is 15~66 GPa.
4. The negative electrode material according to claim 1 or 2, characterized in that, The negative electrode material satisfies at least one of the following conditions: (1) The specific surface area of the negative electrode material is 0.8~3.5m². 2 / g; (2) The particle size Dv50 of the negative electrode material is 4.0~13.4μm; (3) The true density of the negative electrode material is 1.95~2.15 g / cc; (4) The conductivity of the negative electrode material at a pressure of 10 MPa is 0.04~0.5 S / cm.
5. The method for preparing the negative electrode material according to any one of claims 1 to 4, characterized in that, Includes the following steps: Step S1: Introduce a first deposition material and perform a first CVD deposition on porous carbon under a protective atmosphere to deposit a deoxygenated carbon layer on the surface of the porous carbon framework formed by the porous carbon, thereby obtaining a first intermediate; the first deposition material includes a first carbon source. Step S2: Introduce a second deposition material to perform a second CVD deposition on the first intermediate to deposit silicon on the surface of the deoxygenated carbon layer, thereby obtaining a second intermediate; the second deposition material includes a first silicon source and a first dilution gas; Step S3: Introduce a third deposition material and perform plasma-enhanced atomic layer deposition on the second intermediate to deposit a SiCN layer on the silicon surface to obtain the third intermediate; the third deposition material includes a second silicon source, a nitrogen source, a second carbon source, and a second dilution gas, and the deposition temperature of the plasma-enhanced atomic layer deposition is 400~600℃; Step S4: Introduce a fourth deposition material to perform a third CVD deposition on the third intermediate to deposit a carbon coating layer on the surface of the SiCN layer until the pores of the porous carbon framework are filled, thereby obtaining the anode material; the fourth deposition material includes a third carbon source and a third dilution gas.
6. The method for preparing the negative electrode material according to claim 5, characterized in that, The method for preparing the negative electrode material satisfies at least one of the following conditions: (1) By volume percentage, the first dilution gas, the second dilution gas, or the third dilution gas comprises 1-5% H2 and 95-99% carrier gas, wherein the carrier gas is N2 or Ar; (2) The first carbon source, the second carbon source, or the third carbon source includes one or more of CH4, C2H2, and toluene; (3) The first silicon source or the second silicon source includes one or more of silane and chlorosilane; (4) In step S3, the nitrogen source includes one or more of NH3 and urea; (5) In step S1, the protective atmosphere includes one or more of argon atmosphere, nitrogen atmosphere and helium atmosphere.
7. The method for preparing the negative electrode material according to claim 5, characterized in that, The method for preparing the negative electrode material satisfies at least one of the following conditions: (1) In step S1, the flow rate of the first CVD deposition is: 80~120 sccm of the first deposition raw material is introduced for every 20g of the porous carbon; (2) In step S1, the temperature of the first CVD deposition is 550~750℃, the pressure is 120~1500Pa, and the time is 40~120min; (3) In step S2, the volume ratio of the first silicon source to the first dilution gas is 1:(18~50). (4) In step S2, the second CVD deposition is carried out in a fluidized bed, and the volume concentration of the first silicon source in the fluidized bed is 2-5%; (5) In step S2, the flow rate of the second CVD deposition is: for every 20g of the first intermediate, 100~300sccm of the second deposition material is introduced; (6) In step S2, the temperature of the second CVD deposition is 400℃~550℃, the pressure is 100~500Pa, and the time is 1~4h.
8. The method for preparing the negative electrode material according to claim 5, characterized in that, The method for preparing the negative electrode material satisfies at least one of the following conditions: (1) In step S3, the volume ratio of the second silicon source, the nitrogen source and the second carbon source is 1:(2~6):(0.15~0.3). (2) In step S3, the second dilution gas accounts for 70-85% of the total flow rate of the third deposition raw material; (3) In step S3, the flow rate of the plasma-enhanced atomic layer deposition is: for every 100g of the second intermediate, 20~80sccm of the third deposition material is introduced; (4) In step S3, the plasma power of the plasma-enhanced atomic layer deposition is 50~200W; (5) In step S3, the temperature of plasma-enhanced atomic layer deposition is 400~500℃, the pressure is 100~500Pa, and the time is 5~30min; (6) In step S4, the volume ratio of the third carbon source to the third dilution gas is 1:(5~10). (7) In step S4, the third CVD deposition is carried out in a fluidized bed, and the volume concentration of the third carbon source in the fluidized bed is 10~20%; (8) In step S4, the flow rate of the third CVD deposition is: for every 10g of the third intermediate, 100~300sccm of the fourth deposition raw material is introduced; (9) In step S4, the temperature of the third CVD deposition is 450℃~550℃, and the pressure is 10. 3 ~10 4 Pa, time is 5~45min.
9. A negative electrode sheet, comprising a negative electrode current collector and a negative electrode material active layer disposed on at least one side of the negative electrode current collector, characterized in that, The active layer of the negative electrode material comprises the negative electrode material according to any one of claims 1 to 4, or the negative electrode material obtained by the preparation method of the negative electrode material according to any one of claims 5 to 8.
10. A secondary battery, characterized in that, Includes the negative electrode sheet as described in claim 9.