A temperature-sensitive system functional current collector and a preparation method thereof, pole piece and battery

By employing a three-layer sandwich structure and a graded protection mechanism in the current collector of lithium-ion batteries, the problems of slow response speed and insufficient safety of batteries under abnormal operating conditions in existing technologies are solved, achieving fast current protection and efficient current transmission, which is applicable to consumer electronics and new energy vehicles.

CN123120740APending Publication Date: 2026-11-17JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611018207.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery current collectors lack a fast-response current protection mechanism under abnormal conditions such as overcharging and external short circuits. Traditional protection technologies cannot balance safety and battery performance, and external protection circuits have slow response speeds and occupy space, failing to meet the needs of consumer electronics and power batteries.

Method used

A polymer base film is used as the support layer, and the surface is coated with a silane coupling agent. Metal current collection layers are set at both ends, and the middle array of through holes is filled with temperature-sensitive material to form a three-layer sandwich structure with metal. It is divided into early warning, current limiting and cut-off zones. Reversible and irreversible temperature-sensitive materials are used to realize dynamic conductivity-insulation switching and build a multi-level protection mechanism.

Benefits of technology

It achieves efficient current transmission at room temperature and rapid current cut-off at high temperature, preventing battery fires and explosions, thus improving battery safety and reliability. It is suitable for consumer electronics and new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120740A_ABST
    Figure CN123120740A_ABST
Patent Text Reader

Abstract

This invention discloses a temperature-sensitive functional current collector, its preparation method, electrode, and battery, comprising: a polymer material base film as a support layer; the polymer material base film contains antioxidants and ultraviolet absorbers in its material composition, and the surface of the polymer material base film has a silane coupling agent coating; current collector layers, which are metal layers respectively disposed on the upper and lower sides of the left and right ends of the polymer material base film; an array of through holes distributed in the polymer material base film between the left and right current collector layers, the through holes being filled with temperature-sensitive material and metal, forming a three-layer sandwich structure of temperature-sensitive material-metal-temperature-sensitive material. The current collector of this invention achieves a balance between high-efficiency conductivity at room temperature and high-temperature protection through the three-layer sandwich structure containing a temperature-sensitive material system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to a temperature-sensitive functional current collector and its preparation method, as well as an electrode and a battery. Background Technology

[0002] Lithium-ion batteries, due to their high energy density and long cycle life, are widely used in new energy vehicles, mobile phones, energy storage devices, and other fields. However, significant safety hazards still exist in actual use: when the battery is under abnormal conditions such as overcharging, external short circuits, or punctures, a large amount of heat is generated internally. Once the temperature exceeds the safety threshold, the electrolyte is prone to decomposition, and the positive and negative electrode materials may experience thermal runaway, leading to safety accidents such as fires and explosions. The current collectors of lithium-ion batteries (including positive electrode aluminum foil and negative electrode copper foil) are the core carriers for current transmission, and their safety performance directly determines the overall reliability of the battery.

[0003] Current protection technologies have several shortcomings: First, coating the current collector surface with temperature-sensitive materials only relies on the increase in resistance at high temperatures to increase the battery's internal resistance, lacking the ability to dynamically switch between conductivity and insulation, and failing to meet the dynamic current transmission requirements of the current collector. Second, external protection circuits (such as PTC thermistors) have slow response speeds, requiring heat to be conducted to the outside of the battery to activate protection, and occupying external battery space, making them unsuitable for small consumer electronics or highly integrated power batteries. Third, internal flame-retardant additives can only slow down the rate of thermal runaway, failing to fundamentally cut off current conduction and reducing battery energy density. Fourth, traditional materials can only achieve irreversible blocking, failing to meet the differentiated needs of reusable consumer electronics batteries and high-reliability protection for single-use power batteries. Summary of the Invention

[0004] The purpose of this invention is to effectively solve the problems of the prior art by providing a current collector and its preparation method, an electrode and a battery, which have a current protection structure that is integrated inside the battery, has a fast response speed, high blocking reliability and does not affect the normal performance of the battery.

[0005] To achieve the above objectives, the technical solution provided by the present invention is as follows: The first aspect of this application provides a temperature-sensitive system functional current collector, comprising: A polymeric material base film serves as a support layer; the polymeric material base film contains antioxidants and ultraviolet absorbers in its material composition, and the surface of the polymeric material base film has a silane coupling agent coating. The current collection layer is a metal current collection layer set on the upper and lower sides of the left and right ends of the polymer material base film, respectively; An array of through-holes is distributed in the polymer material base film between the left and right current collector layers. The through-holes are filled with temperature-sensitive material and metal, forming a three-layer sandwich structure of temperature-sensitive material-metal-temperature-sensitive material.

[0006] To optimize the above technical solution, the specific limitations also include: The polymer base film contains 0.4-0.6% by mass of antioxidant and 0.2-0.4% by mass of ultraviolet absorber.

[0007] Furthermore, the thickness of the silane coupling agent coating is 0.1~0.3μm; the upper and lower surfaces of the three-layer sandwich structure filling the through-hole are basically flush with the upper and lower surfaces of the polymer material base film, and the basically flush means that the flatness error is ≤0.02mm; in the three-layer sandwich structure, the height ratio of the temperature-sensitive material-metal-temperature-sensitive material is 0.8~1.2:1:0.8~1.2.

[0008] Furthermore, the temperature-sensitive material includes reversible and irreversible temperature-sensitive materials; the polymer base film is divided into three functional regions: a warning region, a current-limiting region, and a cutoff region, with corresponding area percentages of 25-35%, 45-55%, and 15-25%, respectively. The temperature-sensitive material in the warning zone is a reversible temperature-sensitive material; the temperature-sensitive material in the current-limiting zone is a mixture of reversible and irreversible temperature-sensitive materials, with a mass ratio of 4~6:4~6; the temperature-sensitive material in the cutting-off zone is an irreversible temperature-sensitive material.

[0009] Furthermore, the polymer material base film is divided into zones by dividing it into segments sequentially from one side to the other, or by dividing it in concentric circles from the outside to the inside in a U-shape, or by dividing it in a checkerboard pattern; the warning zone, the flow restriction zone, and the cut-off zone are distributed in different zones.

[0010] Furthermore, the temperature-sensitive material is composed of a temperature-sensitive polymer matrix, conductive particles, and functional additives; the conductive particles account for 12-20% of the mass fraction of the temperature-sensitive material, and the functional additives account for 1-3% of the mass fraction of the temperature-sensitive material. In the reversible thermosensitive material described above, the thermosensitive polymer matrix is ​​a mixture of poly(N-isopropylacrylamide) and polyoxyethylene copolymer in a mass ratio of 6 to 8:3, the conductive particles are at least one of carbon black and graphene, and the functional additives are crosslinking agents and antioxidants. In the aforementioned irreversible thermosensitive material, the thermosensitive polymer matrix is ​​a mixture of epoxy-modified phenolic resin and low-melting-point polyamide in a mass ratio of 5~7:4, the conductive particles are at least one of nano-silver powder and carbon nanotubes, and the functional additives are curing agents and coupling agents.

[0011] The second aspect of this application provides a method for preparing a temperature-sensitive functional current collector, comprising the following steps: S1: Prepare the raw materials of the polymer, add antioxidants and ultraviolet absorbers, melt and mix them, and then extrude and stretch them into a film. S2: After ultrasonic cleaning and drying, the polymer material base film is coated with a silane coupling agent on its surface; S3: Use a perforation device to process an array of through holes on a polymer material base film; S4: Use plasma cleaning to clean the through holes and remove debris from the hole walls; S5: The areas without through-holes on the surface of the polymer base film are masked, leaving only the through-hole locations exposed. Then, an electroplating process is used to deposit metal into the through-holes. Pulsed electroplating and controlled plating current are employed to reduce the discharge effect at the tip of the through-hole opening, allowing the metal to preferentially and uniformly deposit and grow in the center of the through-hole. S6: Inject temperature-sensitive material into both ends of the metal deposited in the through hole; S7: Scrape and smooth the surface of the polymer base film; S8: Metal current collectors are respectively set on the upper and lower sides of both ends of the polymer material base film.

[0012] Further, in step S5, a masking film is attached to the surface of the polymer material base film or a positioning fixture is installed, and the masking film or fixture has clearance openings corresponding to the through holes; the metal current collector layer mentioned in step S8 is prepared by magnetron sputtering process, and the other parts of the surface of the polymer material base film are masked before sputtering.

[0013] A third aspect of this application provides an electrode comprising the aforementioned temperature-sensitive system functional current collector.

[0014] A fourth aspect of this application provides a battery comprising the aforementioned electrode.

[0015] Compared with the prior art, the beneficial effects of the present invention are: The current collector of this invention uses a polymer material base film containing antioxidants and ultraviolet absorbers as a support layer. The surface of the base film is coated with a silane coupling agent. Metal current collector layers are respectively provided on the upper and lower sides of both ends of the base film. An array of through holes is distributed in the middle region. The through holes are filled with temperature-sensitive material and metal, forming a three-layer sandwich structure of temperature-sensitive material-metal-temperature-sensitive material. The metal layer undertakes the main current transmission function at room temperature, ensuring efficient and smooth current conduction. The temperature-sensitive material layers on both sides are responsible for sensing temperature changes. At room temperature, they maintain a conductive state and conduct electricity in conjunction with the metal layer. At high temperatures, they achieve a switching between conductivity and insulation through phase change or chemical reaction, quickly activating the protection function. This balances safety and performance, achieving a balance between efficient conductivity at room temperature and high-temperature protection.

[0016] Furthermore, to achieve graded protection, the base film is divided into three functional zones: a warning zone, a current-limiting zone, and a cut-off zone. Each zone is distributed according to a certain area ratio and uses different types of temperature-sensitive materials: the warning zone uses reversible temperature-sensitive materials, the current-limiting zone uses a combination of reversible and irreversible temperature-sensitive materials, and the cut-off zone uses irreversible temperature-sensitive materials. This constructs a multi-level protection mechanism corresponding to the stepped damage process of the current collector, solving the shortcomings of traditional single-threshold protection technology. This multi-level protection mechanism for the current collector matches the damage process of the current collector from local overheating to oxidation and then to near melting through graded responses of warning, current-limiting, and cut-off. In the warning stage, it can promptly remind users to take cooling measures; in the current-limiting stage, it can reduce Joule heat accumulation and delay thermal runaway; and in the cut-off stage, it can quickly and completely block the current, timely avoiding safety accidents such as battery fire and explosion, and significantly improving the reliability of the battery under abnormal conditions such as overcharging and external short circuits.

[0017] This current collector can be widely adapted to the needs of different fields such as consumer electronics, new energy vehicles, and energy storage equipment, providing a brand-new solution for lithium-ion battery safety protection technology. Attached Figure Description

[0018] Figure 1 : A schematic diagram of the structure of the temperature-sensitive functional current collector of the present invention.

[0019] In the figure: 1-Polymer base film, 2-Current collector layer, 3-Thermosensitive material, 4-Metal, 5-Electrode active material. Detailed Implementation

[0020] The present invention will be further described in detail below through specific embodiments, but it should not be construed as limiting the scope of the subject matter of the present invention to the following embodiments. All technologies implemented based on the above content of the present invention fall within the scope of the present invention.

[0021] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, and the reagents, methods and equipment used are conventional reagents, methods and equipment in this technical field.

[0022] This invention provides a functional current collector for a temperature-sensitive system, such as... Figure 1 As shown, it includes: A polymer base film serves as a support layer; the polymer base film contains antioxidants and ultraviolet absorbers in its material composition, and the surface of the polymer base film has a silane coupling agent coating; The current collection layer is a metal current collection layer set on the upper and lower sides of the left and right ends of the polymer material base film, respectively; An array of through-holes is distributed in the polymer material base film between the left and right current collector layers. The through-holes are filled with temperature-sensitive material and metal, forming a three-layer sandwich structure of temperature-sensitive material-metal-temperature-sensitive material.

[0023] This invention constructs an integrated functional current collector with a three-layer sandwich structure of polymer material base film, current collector layer, and through-hole, solving the problem of the inability to simultaneously achieve current collection conductivity and safety protection. Unlike traditional current collectors that only focus on conductivity or rely solely on external protection, this invention solves the problems of easy delamination and aging failure between the protective structure and the base film through the synergy of base film modification and silane coupling agent coating. The three-layer sandwich structure of temperature-sensitive material-metal-temperature-sensitive material achieves dynamic and reversible switching between high-efficiency conductivity at room temperature and insulation at high temperature, breaking the limitations of traditional single-fill structure with large conductivity loss or delayed protection response. It constructs an active protection system from inside the battery without occupying external space, adapting to various scenarios and integrating safety protection into the current collector.

[0024] The three-layer sandwich structure's metal layer bears the main current transmission function at room temperature, ensuring efficient and smooth current conduction. The temperature-sensitive material layers on both sides are responsible for sensing temperature changes, maintaining a conductive state at room temperature and conducting electricity in conjunction with the metal layer. At high temperatures, it achieves a switching between conductivity and insulation through phase change or chemical reaction, quickly activating the protection function.

[0025] The polymer base film contains 0.4-0.6% antioxidant and 0.2-0.4% UV absorber by mass.

[0026] A properly formulated antioxidant can effectively inhibit the oxidative degradation of the base film under high temperature and electrolyte conditions, reducing the performance degradation of the base film; an appropriate amount of ultraviolet absorber can block the erosion of the base film by external ultraviolet rays, avoiding problems such as embrittlement and cracking of the base film, and further extending the service life of the base film and the entire protective structure.

[0027] The thickness of the silane coupling agent coating is 0.1~0.3μm; the upper and lower surfaces of the three-layer sandwich structure filling the through-hole are basically flush with the upper and lower surfaces of the polymer material base film, and the flatness error is ≤0.02mm; in the three-layer sandwich structure, the height ratio of temperature-sensitive material-metal-temperature-sensitive material is 0.8~1.2:1:0.8~1.2. Preferably, the diameter of the through-hole can be 0.3~0.8mm, and the center-to-center distance between adjacent holes is 1~5mm.

[0028] The defined height ratio of each layer in the three-layer sandwich structure allows for a more rational combination of the temperature-sensitive material and the metal layer. This ensures that the metal layer can fully exert its conductivity at room temperature, while the temperature-sensitive material can respond quickly and switch between conductivity and insulation at high temperatures. This avoids problems such as delayed protection response or insufficient conductivity caused by improper layer thickness ratios, further improving the response accuracy and conductivity reliability of the protection structure.

[0029] Thermosensitive materials include reversible and irreversible thermosensitive materials; the polymer base film is divided into three functional zones: a warning zone, a current-limiting zone, and a cutoff zone, with corresponding area proportions of 25-35%, 45-55%, and 15-25%, respectively. The temperature-sensitive material in the warning zone is a reversible temperature-sensitive material; the temperature-sensitive material in the current-limiting zone is a mixture of reversible and irreversible temperature-sensitive materials, with a mass ratio of 4~6:4~6; the temperature-sensitive material in the cutting-off zone is an irreversible temperature-sensitive material.

[0030] The polymer base film is divided into sections from one side to the other, or in a concentric circle from the outside to the inside in a U-shape, or in a checkerboard pattern; the warning zone, the flow restriction zone and the cut-off zone are distributed in different sections.

[0031] This invention constructs a graded protection mechanism by clearly defining the two systems of the temperature-sensitive material and the functional partitions and area ratios of the base film. This mechanism matches the stepped damage process of the current collector, overcoming the shortcomings of existing technologies such as single-threshold protection and lack of graded response. The differentiated use of reversible and irreversible temperature-sensitive materials allows the functional current collector to adapt to the needs of different application scenarios, breaking the limitation of traditional single temperature-sensitive materials that cannot simultaneously achieve reusability and high-reliability protection. The division into three functional partitions makes the protection response more hierarchical and targeted. The warning zone, serving as the first line of defense, employs reversible temperature-sensitive materials. Utilizing the temperature response characteristics of these materials, it provides users with emergency response time when the current collector experiences localized overheating but has not yet reached the level of oxidation damage, and the temperature reaches the warning threshold. The current-limiting zone, acting as an intermediate buffer, uses a mixture of reversible and irreversible temperature-sensitive materials. When the temperature continues to rise and the current collector shows slight oxidation or corrosion, the reversible material switches to an insulating state, while the irreversible material begins a curing reaction. This dual action significantly reduces the total current, decreases Joule heat accumulation in the current collector, delays the thermal runaway process, and provides sufficient time for subsequent cut-off protection. The cut-off zone, serving as the final safety line, uses irreversible temperature-sensitive materials. When the current collector temperature rises to a critical threshold near melting and structural failure, the irreversible material rapidly undergoes a curing or carbonization reaction, permanently destroying the conductive network and completely cutting off the current throughout the entire area, preventing thermal runaway at its source.

[0032] Preferably, the functional partitioning allows the current to be evenly distributed on the base film, avoiding localized overheating of the current collector caused by localized current concentration.

[0033] Among them, the segmented division method is simple to operate, facilitates large-scale industrial production, and is suitable for current collectors of conventional sizes; the zigzag layer division method can achieve gradient protection from the inside out, with the heat of the cell mostly concentrated in the center of the electrode, and the inner layer prioritizes temperature rise detection to initiate graded protection, and from the inside out, it sequentially provides early warning, current limiting, and cut-off; the checkerboard grid division method can make the three functional areas evenly and staggered, further optimizing the current distribution, avoiding local current concentration, and at the same time ensuring that when an abnormal temperature occurs in any area, the corresponding level of protection response can be quickly triggered.

[0034] In some embodiments, the temperature-sensitive material is composed of a temperature-sensitive polymer matrix, conductive particles, and functional additives; the conductive particles account for 12-20% of the mass fraction of the temperature-sensitive material, and the functional additives account for 1-3% of the mass fraction of the temperature-sensitive material. Reversible temperature-sensitive materials use a specific copolymer as a matrix, exhibiting a swollen state at room temperature with uniformly dispersed conductive particles, possessing excellent conductivity. When the temperature rises to the phase transition threshold, the matrix shrinks, the conductive particles agglomerate and separate, losing their conductivity. When the temperature drops below the threshold, the matrix returns to a swollen state, the conductive particles redisperse, and conductivity is restored, enabling multiple repeated protection-recovery cycles. Irreversible temperature-sensitive materials use modified resin as the main matrix, exhibiting a viscous state at room temperature with an intact conductive network. At high temperatures, the matrix undergoes a curing or carbonization reaction, permanently destroying the conductive network and completely losing its conductivity, achieving one-time irreversible and highly efficient blocking, meeting the requirements for high-reliability protection.

[0035] Specific examples of material selection are as follows: In the reversible thermosensitive material, the thermosensitive polymer matrix is ​​a mixture of poly(N-isopropylacrylamide) and polyoxyethylene copolymer in a mass ratio of 6 to 8:3, the conductive particles are at least one of carbon black and graphene, and the functional additives are crosslinking agents and antioxidants. In the irreversible thermosensitive material, the thermosensitive polymer matrix is ​​a mixture of epoxy-modified phenolic resin and low-melting-point polyamide in a mass ratio of 5~7:4, the conductive particles are at least one of nano-silver powder and carbon nanotubes, and the functional additives are curing agents and coupling agents.

[0036] This invention also provides a method for preparing a temperature-sensitive functional current collector, comprising the following steps: S1: Prepare the raw materials of the polymer, add antioxidants and ultraviolet absorbers, melt and mix them, and then extrude and stretch them into a film. S2: After ultrasonic cleaning and drying, the polymer material base film is coated with a silane coupling agent on its surface; S3: Use a perforation device to process an array of through holes on a polymer material base film; S4: Use plasma cleaning to clean the through holes and remove debris from the hole walls; S5: The areas without through-holes on the surface of the polymer base film are masked, leaving only the through-hole locations exposed. Then, an electroplating process is used to deposit metal into the through-holes. Pulsed electroplating and controlled plating current are employed to reduce the discharge effect at the tip of the through-hole opening, allowing the metal to preferentially and uniformly deposit and grow in the center of the through-hole. S6: Inject temperature-sensitive material into both ends of the metal deposited in the through hole; S7: Scrape and smooth the surface of the polymer base film; S8: Metal current collectors are respectively set on the upper and lower sides of both ends of the polymer material base film.

[0037] In step S5, a masking film is attached to the surface of the polymer material base film or a positioning fixture is installed. The masking film and the fixture are provided with clearance openings corresponding to the through holes. In step S8, the metal current collector layer is prepared by magnetron sputtering. Before sputtering, the other parts of the surface of the polymer material base film are masked.

[0038] The present invention also provides an electrode comprising the above-described temperature-sensitive system functional current collector.

[0039] The present invention also provides a battery comprising the above-described electrode.

[0040] The electrode incorporating the functional current collector of this invention not only possesses the current transmission function of conventional electrodes, but also achieves graded protection under abnormal temperature conditions, delaying electrode damage and preventing electrode failure due to overheating, oxidation, or melting. Simultaneously, it reduces electrode resistance loss, improving charge / discharge efficiency and cycle life. The battery incorporating this electrode achieves internal current regulation and safety protection without requiring additional external protection devices, saving internal battery space, increasing battery energy density, and avoiding the drawbacks of slow response and poor adaptability of external protection circuits.

[0041] The technical solution of the present invention will be further described in detail below with reference to specific embodiments: Example 1 The specific preparation steps are as follows: S1: Prepare PET raw materials, add 0.5% antioxidant (1010) and 0.3% UV absorber (UV-531) by mass, melt and mix them, and then extrude and stretch them into a 12μm thick base film (base film glass transition temperature 75℃, thermal decomposition temperature >300℃).

[0042] S2: The base film was ultrasonically cleaned (300W, 10min) with ethanol-deionized water (1:1 volume ratio) and dried at 60℃, and then coated with 0.2μm of silane coupling agent KH560.

[0043] S3: Using an ultraviolet laser drilling machine (wavelength 355nm, pulse frequency 70kHz, power 3.5W), an array of through holes (hole diameter 0.5mm, hole depth 12μm, consistent with the thickness of the base film) are processed on the base film. The functional areas are divided into a checkerboard grid with an area ratio of 30% for the warning zone, 50% for the current limiting zone, and 20% for the cutting zone.

[0044] S4: Use argon plasma to clean the through hole (power 100W, time 5min, vacuum degree -0.09MPa) to remove debris from the hole wall and make the hole wall roughness Ra=0.25μm.

[0045] S5: A masking film (with clearance openings corresponding to the through-holes) is attached to the surface of the base film, exposing only the through-hole locations. 99.99% high-purity copper is deposited into the through-holes using a selective electroplating process. Pulse electroplating is employed with controlled plating current to reduce the discharge effect at the hole tip, ensuring that the metal is preferentially and uniformly deposited in the middle of the through-hole, forming the middle metal layer of a three-layer sandwich structure within the hole.

[0046] S6: At both ends of the metal layer inside the through hole, the temperature-sensitive material corresponding to the functional area is injected to form a three-layer sandwich structure inside the hole (temperature-sensitive material-metal-temperature-sensitive material) with a height ratio of 1:1:1; the two ends of the through hole in the warning zone are injected with a reversible system temperature-sensitive material (PNIPAM:PEO=7:3 mass ratio, with 16% carbon black and 2% crosslinking agent + antioxidant added); the two ends of the through hole in the flow-limiting zone are injected with a mixed material of reversible and irreversible temperature-sensitive materials in a mass ratio of 5:5 (the irreversible system is EPN:PA612=6:4 mass ratio, with 16% nano silver powder and 2% curing agent + coupling agent added); the two ends of the through hole in the cutting-off zone are injected with an irreversible system temperature-sensitive material.

[0047] S7: Use a PTFE scraper (pressure 0.15MPa) to scrape and smooth the surface of the base film, ensuring that the sandwich structure inside the hole is flush with the upper and lower surfaces of the base film (flatness error ≤0.02mm).

[0048] S8: The base film is shielded except at both ends. A metal current collector layer is prepared on the upper and lower sides of both ends of the base film using magnetron sputtering to complete the preparation of the temperature-sensitive functional current collector.

[0049] Battery fabrication: The temperature-sensitive functional current collector prepared in Example 1 was selected as the positive electrode current collector. Lithium iron phosphate was selected as the positive electrode active material, conductive carbon black SP was selected as the conductive agent, and PVDF binder was selected as the binder. The positive electrode slurry was prepared by adding NMP solvent and stirring according to the mass ratio of lithium iron phosphate, conductive carbon black SP, and PVDF binder of 96:2:2. The positive electrode slurry was coated on the surface of the functional current collector and then pre-dried, gradient dried, rolled, slit, and die-cut to obtain the positive electrode sheet. The negative electrode used conventional copper foil current collector and artificial graphite was selected as the negative electrode active material. It was combined with conventional conductive agent and CMC-SBR aqueous binder and prepared conventional negative electrode sheet by slurry preparation, coating, drying, rolling, and cutting. Combined with polypropylene separator and conventional lithium battery electrolyte, the cell stacking, aluminum-plastic film encapsulation, electrolyte injection, room temperature wetting, formation, capacity testing, and aging processes were completed to finally obtain the finished soft pack battery.

[0050] Example 2 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S2: After cleaning and drying the base film, coat it with 0.1μm of silane coupling agent KH560.

[0051] Example 3 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S2: After cleaning and drying the base film, coat it with 0.3μm of silane coupling agent KH560.

[0052] Example 4 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S5 and S6: Adjust the electroplating and potting processes to make the height ratio of the sandwich structure inside the hole 0.8:1:0.8, and the flatness error after filling is 0.018mm.

[0053] Example 5 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S5 and S6: Adjust the electroplating and potting processes to make the height ratio of the sandwich structure inside the hole 1.2:1:1.2, and the flatness error after filling is 0.016mm.

[0054] Example 6 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S3: After drilling, the functional areas are divided into a checkerboard grid pattern according to the area ratio of 25% for the warning zone, 45% for the flow restriction zone, and 15% for the cut-off zone.

[0055] S6: The temperature-sensitive material in the current-limiting zone is a mixture of reversible and irreversible systems in a 4:6 mass ratio.

[0056] Example 7 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S3: After drilling, the functional areas are divided into a checkerboard grid pattern according to the area ratio of 35% for the warning zone, 55% for the current restriction zone, and 25% for the cut-off zone.

[0057] S6: The temperature-sensitive material in the current-limiting zone is a mixture of reversible and irreversible systems in a 6:4 mass ratio.

[0058] Example 8 Compared with Example 1, only step S3 is adjusted, while the other steps are the same: S3: After perforation, the base film is divided into functional zones (early warning zone → current limiting zone → cut-off zone) from one end to the other, with an area ratio of 30%, 50%, and 20%, respectively.

[0059] Example 9 Compared with Example 1, only step S3 is adjusted, while the other steps are the same: S3: After perforation, with the center of the base film as the origin, the functional areas are divided into concentric circles from the outside to the inside in a U-shape (outer layer cutting area, middle layer current limiting area, inner layer early warning area), with an area ratio of 20%, 50%, and 30%, respectively.

[0060] Example 10 Compared with Example 1, only step S6 is adjusted, while the other steps remain the same: S6: In the reversible temperature-sensitive material system, PNIPAM:PEO=6:3; in the irreversible temperature-sensitive material system, EPN:PA612=5:4; the composition and addition amount of the remaining temperature-sensitive materials are the same as in Example 1.

[0061] Example 11 Compared with Example 1, only step S6 is adjusted, while the other steps remain the same: S6: In the reversible temperature-sensitive material system, PNIPAM:PEO=8:3; in the irreversible temperature-sensitive material system, EPN:PA612=7:4; the composition and addition amount of the remaining temperature-sensitive materials are the same as in Example 1.

[0062] Comparative Example 1 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S2: After the base film is cleaned and dried, no silane coupling agent is coated.

[0063] Comparative Example 2 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: Steps S3 (drilling), S4 (hole wall cleaning), S5 (through-hole metal deposition), and S6 (temperature-sensitive material injection) are omitted, and the base film has no through-holes or sandwich structure.

[0064] S8: Metal layers are sputtered directly onto the top and bottom sides of both ends of the base film, relying solely on the metal layers for conductivity.

[0065] Comparative Example 3 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S5, S6: Adjust the electroplating and potting processes to make the height ratio of the sandwich structure inside the hole 0.7:1:0.7.

[0066] Comparative Example 4 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S7: Insufficient leveling of the coating; the flatness error between the sandwich structure inside the hole and the base film is 0.03mm.

[0067] Comparative Example 5 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S3: After drilling, the functional areas are divided according to the area ratio of 20% for the warning zone, 60% for the flow restriction zone, and 20% for the cut-off zone.

[0068] S6: The current-limiting zone uses only irreversible temperature-sensitive materials.

[0069] Comparative Example 6 Compared with Example 1, only the following steps are adjusted, while the rest of the steps are the same: S3: After drilling, no functional zones are defined; the hole density is 150 holes / cm². 2 .

[0070] S6: All through holes are filled with a single irreversible temperature-sensitive material.

[0071] Comparative Example 7 Compared with Example 1, only step S6 is adjusted, while the other steps remain the same: S6: In reversible temperature-sensitive materials, PNIPAM:PEO = 5:3; in irreversible temperature-sensitive materials, EPN:PA612 = 4:4.

[0072] Comparative Example 8 Compared with Example 1, only step S6 is adjusted, while the other steps remain the same: S6: In the reversible temperature-sensitive material system, PNIPAM:PEO=9:3; in the irreversible temperature-sensitive material system, EPN:PA612=8:4; the composition and addition amount of the remaining temperature-sensitive materials are the same as in Example 1.

[0073] Comparative Example 9 Compared with Example 1, only step S6 is adjusted, while the other steps remain the same: S6: The temperature-sensitive material contains no conductive particles, only a temperature-sensitive polymer matrix and functional additives.

[0074] Table 1

[0075] Table 2

[0076] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent substitutions, and improvements made by those skilled in the art to the above embodiments without departing from the scope of the technical solution of the present invention, based on the technical essence of the present invention, shall still fall within the protection scope of the technical solution of the present invention.

Claims

1. A temperature-sensitive functional current collector, characterized in that, include: A polymeric material base film serves as a support layer; the polymeric material base film contains antioxidants and ultraviolet absorbers in its material composition, and the surface of the polymeric material base film has a silane coupling agent coating. The current collection layer is a metal current collection layer set on the upper and lower sides of the left and right ends of the polymer material base film, respectively; An array of through-holes is distributed in the polymer material base film between the left and right current collector layers. The through-holes are filled with temperature-sensitive material and metal, forming a three-layer sandwich structure of temperature-sensitive material-metal-temperature-sensitive material.

2. The temperature-sensitive system functional current collector according to claim 1, characterized in that: The polymer base film contains 0.4-0.6% by mass of antioxidant and 0.2-0.4% by mass of ultraviolet absorber.

3. The temperature-sensitive system functional current collector according to claim 1, characterized in that: The thickness of the silane coupling agent coating is 0.1~0.3μm; the upper and lower surfaces of the three-layer sandwich structure filled in the through hole are basically flush with the upper and lower surfaces of the polymer material base film, and the basically flush means that the flatness error is ≤0.02mm; in the three-layer sandwich structure, the height ratio of the temperature-sensitive material-metal-temperature-sensitive material is 0.8~1.2:1:0.8~1.

2.

4. The temperature-sensitive system functional current collector according to claim 1, characterized in that: The temperature-sensitive material includes reversible and irreversible temperature-sensitive materials; the polymer base film is divided into three functional zones: a warning zone, a current-limiting zone, and a cutoff zone, with corresponding area proportions of 25-35%, 45-55%, and 15-25%, respectively. The temperature-sensitive material in the warning zone is a reversible temperature-sensitive material; the temperature-sensitive material in the current-limiting zone is a mixture of reversible and irreversible temperature-sensitive materials, with a mass ratio of 4~6:4~6; the temperature-sensitive material in the cutting-off zone is an irreversible temperature-sensitive material.

5. The temperature-sensitive system functional current collector according to claim 4, characterized in that: The polymer base film is divided into sections from one side to the other, or in a concentric circle from the outside to the inside in a U-shape, or in a checkerboard pattern; the warning zone, the flow restriction zone and the cut-off zone are distributed in different sections.

6. The temperature-sensitive system functional current collector according to claim 4, characterized in that: The temperature-sensitive material is composed of a temperature-sensitive polymer matrix, conductive particles, and functional additives; the conductive particles account for 12-20% of the mass fraction of the temperature-sensitive material, and the functional additives account for 1-3% of the mass fraction of the temperature-sensitive material. In the reversible thermosensitive material described above, the thermosensitive polymer matrix is ​​a mixture of poly(N-isopropylacrylamide) and polyoxyethylene copolymer in a mass ratio of 6 to 8:3, the conductive particles are at least one of carbon black and graphene, and the functional additives are crosslinking agents and antioxidants. In the aforementioned irreversible thermosensitive material, the thermosensitive polymer matrix is ​​a mixture of epoxy-modified phenolic resin and low-melting-point polyamide in a mass ratio of 5~7:4, the conductive particles are at least one of nano-silver powder and carbon nanotubes, and the functional additives are curing agents and coupling agents.

7. A method for preparing a temperature-sensitive functional current collector according to any one of claims 1 to 6, characterized in that, Includes the following steps: S1: Prepare the raw materials of the polymer, add antioxidants and ultraviolet absorbers, melt and mix them, and then extrude and stretch them into a film. S2: After ultrasonic cleaning and drying, the polymer material base film is coated with a silane coupling agent on its surface; S3: Use a perforation device to process an array of through holes on a polymer material base film; S4: Use plasma cleaning to clean the through holes and remove debris from the hole walls; S5: The areas without through-holes on the surface of the polymer base film are masked, leaving only the through-hole locations exposed. Then, an electroplating process is used to deposit metal into the through-holes. Pulsed electroplating and controlled plating current are employed to reduce the discharge effect at the tip of the through-hole opening, allowing the metal to preferentially and uniformly deposit and grow in the center of the through-hole. S6: Inject temperature-sensitive material into both ends of the metal deposited in the through hole; S7: Scrape and smooth the surface of the polymer base film; S8: Metal current collectors are respectively set on the upper and lower sides of both ends of the polymer material base film.

8. The method for preparing the temperature-sensitive functional current collector according to claim 1, characterized in that: In step S5, a masking film is attached to the surface of the polymer material base film or a positioning fixture is installed. The masking film or fixture has clearance openings corresponding to the through holes. The metal current collector layer in step S8 is prepared by magnetron sputtering. Before sputtering, other parts of the surface of the polymer material base film are masked.

9. An electrode sheet, characterized in that: The thermosensitive system functional current collector includes the method described in any one of claims 1 to 6 or the method described in any one of claims 7 and 8.

10. A battery, characterized in that: It includes the electrode sheet as described in claim 9.