A urea-modified iron-nitrogen-carbon supported low-platinum electrocatalyst and its preparation method

By preparing urea-modified iron-nitrogen-carbon supported low-platinum electrocatalysts, the high energy barrier and stability issues of platinum-carbon catalysts in fuel cell cathodes were solved, achieving efficient oxygen reduction reaction and stability, thus promoting the commercial application of fuel cells and metal-air batteries.

CN123120760APending Publication Date: 2026-11-17XINJIANG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510630850.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing platinum-carbon catalysts exhibit high energy barriers and slow kinetics in the oxygen reduction reaction at the cathode of fuel cells, resulting in high costs and insufficient stability, which limits their large-scale application.

Method used

The preparation method of urea-modified iron-nitrogen-carbon supported low platinum electrocatalyst (Pt/Fe-NC-U) is adopted. By forming FeN4 active sites on Fe-NC support and generating strong electronic coupling with Pt NPs, the Pt loading is reduced and the catalytic activity is improved.

Benefits of technology

It achieves high oxygen reduction reaction activity and stability under low Pt loading, reduces costs, and is suitable for fuel cells and metal-air batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention relates to the field of electrocatalyst technology, specifically to a urea-modified iron-nitrogen-carbon supported low-platinum electrocatalyst and its preparation method. This electrocatalyst exhibits excellent oxygen reduction reaction (ORR) catalytic activity and stability, effectively addressing the problem of insufficient activity under low Pt loading and reducing Pt aggregation during long-term operation. The preparation method of the urea-modified iron-nitrogen-carbon supported low-platinum electrocatalyst is as follows: using 2-methylimidazole, urea, zinc nitrate, ferrous sulfate, hexadecyltrimethylammonium bromide (CTAB), chloroplatinic acid, and ethylene glycol as raw materials, an iron-nitrogen-carbon support rich in iron single atoms is obtained through a simple pyrolysis method, and a low-Pt-loaded electrocatalyst (Pt / Fe-NC-U) is obtained through a solvothermal method. The preparation method provided by this invention is safe and controllable, with mild synthesis conditions, effectively reducing the Pt loading while achieving high activity and stability. The electrocatalyst prepared by this method exhibits excellent ORR catalytic activity and can be applied in fuel cells, metal-air batteries, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalyst technology, specifically relating to a urea-modified iron-nitrogen-carbon supported low-platinum electrocatalyst and its preparation method. Background Technology

[0002] Developing renewable and clean energy is crucial for reducing environmental pollution and achieving sustainable development. Proton exchange membrane fuel cells (PEMFCs) have enormous commercial potential in the energy sector due to their environmental friendliness and high energy density. However, the oxygen reduction reaction (ORR) at the fuel cell cathode suffers from a high energy barrier and slow kinetics, hindering the widespread application of this technology. Currently, commercial platinum-carbon (Pt / C) remains the most commonly used ORR catalyst, but its high cost and limited activity restrict its large-scale application. Therefore, developing catalysts with low Pt loading and high activity remains a significant challenge.

[0003] To enhance the ORR activity of platinum-based catalysts, researchers have explored various approaches. One such approach is support enhancement, which involves strong interactions between the support and platinum nanoparticles (Pt NPs). This enhances catalytic activity while reducing Pt dissolution during the catalytic process, thereby improving catalyst stability. Compared to traditional carbon black, metal-nitrogen-carbon materials (MNCs, M = Fe / Co / Ni) exhibit superior catalytic activity and metal anchoring capabilities. Among these, Fe-NCs have attracted widespread attention due to their excellent intrinsic catalytic activity and abundant active sites.

[0004] Loading Pt NPs onto Fe-NC supports results in metal-support interactions that reduce Pt dissolution and enhance catalytic activity. Further research revealed that the FeN4 active sites on the Fe-NC support can form strong electronic coupling with Pt NPs, reducing the *OH protonation barrier and thus improving ORR activity. The study also found that using urea as a second nitrogen source provides more FeN4 sites on the Fe-NC support during pyrolysis. Increasing the FeN4 site density effectively increases the number of active sites, thereby enhancing the electronic interactions between the support and Pt, resulting in high activity even with low Pt loading.

[0005] Therefore, this patent develops a method for preparing a urea-modified iron-nitrogen-carbon supported low-platinum electrocatalyst (Pt / Fe-NC-U), which reduces the Pt loading while ensuring high catalytic activity and long-term stability. This method is of great research significance for promoting the commercial application of fuel cells and metal-air batteries. Summary of the Invention

[0006] The purpose of this invention is to address the problems of decreased activity in the electrocatalytic oxygen reduction reaction (ORR) under low Pt loading and insufficient stability due to Pt agglomeration during long-term operation. This invention provides a method for preparing a urea-modified iron-nitrogen-carbon supported low-platinum electrocatalyst (Pt / Fe-NC-U). The electrocatalyst prepared by this method exhibits excellent ORR catalytic activity and can be applied in fuel cells, metal-air batteries, and other fields. Furthermore, the preparation method provided by this invention offers advantages such as safety, controllability, and mild synthesis conditions.

[0007] Another object of the present invention is to provide a method for preparing high-performance Pt / Fe-NC-U electrocatalysts.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing a Pt / Fe-NC-U electrocatalyst includes the following steps: The first step is to mix 2-methylimidazole and urea in a certain proportion, dissolve them in a certain amount of deionized water, and stir for an appropriate time to obtain a homogeneous solution A. The second step involves mixing zinc nitrate, ferrous sulfate, and CTAB in a certain proportion, dissolving them in a certain amount of deionized water, and then sonicating for an appropriate time to obtain a homogeneous solution B. The third step is to slowly add solution B to solution A, stir for a certain period of time, centrifuge, wash, and dry to obtain precursor precipitate C; The fourth step involves calcining precipitate C at a certain temperature and time under nitrogen protection at a specific heating rate to obtain the Fe-NC-U support. Fifth step: Disperse the Fe-NC-U support and chloroplatinic acid ethylene glycol solution in a certain amount of ethylene glycol solution, stir for a certain time, and then add an appropriate amount of NaOH ethylene glycol solution dropwise to obtain mixed solution D; Step 6: Transfer solution D to a polytetrafluoroethylene-lined autoclave and react at a certain temperature for an appropriate time. After cooling to room temperature, adjust the pH with nitric acid of appropriate concentration and continue stirring for a certain time. After centrifugation, washing, and drying, the Pt / Fe-NC-U electrocatalyst is obtained.

[0009] In the first step, the amount of 2-methylimidazole added is 700-1400 mg, the amount of urea added is 70-140 mg, the amount of deionized water is 60 mL, and the stirring time is 30 min.

[0010] In the second step, the amount of zinc nitrate added is 300-600 mg, ferrous sulfate added is 20-40 mg, CTAB added is 9-18 mg, deionized water is 60 mL, and the ultrasonic time is 30 min.

[0011] In the third step, the stirring time is 6-24 h, the drying temperature is 70 ℃, and the drying time is 8 h.

[0012] In the fourth step, the heating rate is 5 ℃ / min, the calcination temperature is 800-1000 ℃, and the calcination time is 1-3 h.

[0013] In the fifth step, the Fe-NC-U carrier is added in an amount of 100 mg, the concentration of ethylene glycol chloroplatinate solution is 0.0772 M and the amount added is 0.349-1.660 mL, the amount of ethylene glycol solution added is 45 mL, the stirring time is 3 h, the concentration of NaOH ethylene glycol solution is 1 M and the amount of NaOH ethylene glycol solution added is 14 mL.

[0014] In the sixth step, the reaction temperature is 120-180 ℃, the reaction time is 1-4 h, the pH is adjusted to 2-3, the stirring time is 6-12 h, the drying temperature is 70 ℃, and the drying time is 8 h.

[0015] The application of the Pt / Fe-NC-U electrocatalyst in the field of electrochemical catalysis is within the scope of protection of this invention. Preferably, the Pt / Fe-NC-U electrocatalyst is used in the electrocatalytic oxygen reduction reaction (ORR). More preferably, the Pt / Fe-NC-U electrocatalyst of this invention is used in fuel cells and metal-air batteries.

[0016] Compared with existing technologies, this invention has the following advantages: using 2-methylimidazole, urea, zinc nitrate, ferrous sulfate, hexadecyltrimethylammonium bromide (CTAB), chloroplatinic acid, and ethylene glycol as raw materials, an iron-rich support is obtained through a simple pyrolysis method, and a low-Pt-loaded Pt / Fe-NC-U electrocatalyst is obtained through a solvothermal method. This preparation method is safe and controllable, with mild synthesis conditions. While achieving high activity and stability, it effectively reduces the Pt loading, realizing the vision of low-cost preparation of high-efficiency oxygen reduction catalysts, and can be applied in fuel cells and metal-air batteries. Attached Figure Description

[0017] Figure 1 (a) X-ray diffraction (XRD) pattern of Example 1; (b) X-ray photoelectron spectroscopy (XPS) patterns of Pt 4f of Example 1, Comparative Example 1 and Comparative Example 2.

[0018] Figure 2 (a) Transmission electron microscope (TEM) image of Example 1; (b) High-power transmission electron microscope (HRTEM) image of Example 1.

[0019] Figure 3(a) Linear sweep current-voltage (LSV) curves of Examples 1, 2, 3, Comparative Example 1 and Comparative Example 2; (b) Timing current (it) curve of Example 1. Detailed Implementation

[0020] The present invention has been further illustrated with reference to the embodiments, which are for illustrative purposes only and are not intended to limit the scope of the invention.

[0021] The experimental methods used in the examples, unless otherwise specified, are conventional methods; the reagents and materials used, unless otherwise specified, are commercially available. Example 1

[0022] This embodiment provides a Pt / Fe-NC-U electrocatalyst with a Pt loading of 10 wt%, which is prepared by the following method.

[0023] 1400 mg of 2-methylimidazole and 140 mg of urea were dissolved in 60 mL of deionized water and stirred for 30 min to obtain a homogeneous solution A. 600 mg of zinc nitrate, 40 mg of ferrous sulfate, and 18 mg of CTAB were dissolved in 60 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution B. Solution B was slowly added dropwise to solution A and stirred for 24 h. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain precursor precipitate C. Precipitate C was calcined at 910 °C for 2 h under nitrogen protection at a heating rate of 5 °C / min to obtain the Fe-NC-U support.

[0024] 100 mg of the prepared Fe-NC-U support and 0.738 mL of a 0.0772 M H₂PtCl₆·6H₂O ethylene glycol solution were dispersed in 45 mL of ethylene glycol solution. After stirring for 3 h, 14 mL of a 1 M NaOH ethylene glycol solution was added dropwise to obtain mixed solution D. Solution D was transferred to a polytetrafluoroethylene-lined autoclave and reacted at 140 °C for 2 h. After cooling to room temperature, the pH was adjusted to 2 using 0.1 M nitric acid, and stirring was continued for a certain period of time. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain a Pt / Fe-NC-U electrocatalyst with a Pt loading of 10 wt%.

[0025] The results are characterized in the following ways: The phase structure of the Pt / Fe-NC-U electrocatalyst was analyzed using X-ray powder diffraction. Figure 1(a) It can be seen that the sample has a broadened diffraction peak of graphitic carbon at 24.3°, and diffraction peaks of metallic Pt at 39.9°, 46.2°, 67.5°, and 81.3°. The electronic structure of the Pt / Fe-NC-U electrocatalyst was analyzed by X-ray photoelectron spectroscopy. Figure 1 (b) It can be seen that a strong electronic interaction is formed between Pt and the Fe-NC-U support, which optimizes the electronic structure of Pt.

[0026] The microstructure of the Pt / Fe-NC-U electrocatalyst was investigated using transmission electron microscopy. Figure 2 As shown in (a) and (b), the surface of the carbon material contains a large number of spherical particles, among which the lattice fringes (0.226 nm) belong to the metallic Pt. In addition, the curved lattice fringes in the high-resolution TEM image are caused by the high graphitization of the carbon material.

[0027] Linear sweep voltammetry (LSV) was performed using a rotating disk electrode and an electrochemical workstation with a Pt / Fe-NC-U electrocatalyst. Figure 3 As shown in (a), the Pt / Fe-NC-U electrocatalyst exhibited the best oxygen reduction performance, with a half-wave potential of 0.887 V. Furthermore, by optimizing the Pt loading (Examples 1-3), the optimal preparation conditions for the Pt / Fe-NC-U electrocatalyst were obtained, with a Pt loading of 10 wt%. Finally, after a 10-h stability test, as shown... Figure 3 As shown in (b), the Pt / Fe-NC-U electrocatalyst retains 94% of its activity, demonstrating excellent stability. Example 2

[0028] This embodiment provides a Pt / Fe-NC-U electrocatalyst with a Pt loading of 5 wt%, which is prepared by the following method.

[0029] 1400 mg of 2-methylimidazole and 140 mg of urea were dissolved in 60 mL of deionized water and stirred for 30 min to obtain a homogeneous solution A. 600 mg of zinc nitrate, 40 mg of ferrous sulfate, and 18 mg of CTAB were dissolved in 60 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution B. Solution B was slowly added dropwise to solution A and stirred for 24 h. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain precursor precipitate C. Precipitate C was calcined at 910 °C for 2 h under nitrogen protection at a heating rate of 5 °C / min to obtain the Fe-NC-U support.

[0030] 100 mg of the prepared Fe-NC-U support and 0.349 mL of a 0.0772 M H₂PtCl₆·6H₂O ethylene glycol solution were dispersed in 45 mL of ethylene glycol solution. After stirring for 3 h, 14 mL of a 1 M NaOH ethylene glycol solution was added dropwise to obtain mixed solution D. Solution D was transferred to a polytetrafluoroethylene-lined autoclave and reacted at 140 °C for 2 h. After cooling to room temperature, the pH was adjusted to 2 using 0.1 M nitric acid, and stirring was continued for a certain period of time. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain a Pt / Fe-NC-U electrocatalyst with a Pt loading of 5 wt%. Example 3

[0031] This embodiment provides a Pt / Fe-NC-U electrocatalyst with a Pt loading of 20 wt%, which is prepared by the following method.

[0032] 1400 mg of 2-methylimidazole and 140 mg of urea were dissolved in 60 mL of deionized water and stirred for 30 min to obtain a homogeneous solution A. 600 mg of zinc nitrate, 40 mg of ferrous sulfate, and 18 mg of CTAB were dissolved in 60 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution B. Solution B was slowly added dropwise to solution A and stirred for 24 h. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain precursor precipitate C. Precipitate C was calcined at 910 °C for 2 h under nitrogen protection at a heating rate of 5 °C / min to obtain the Fe-NC-U support.

[0033] 100 mg of the prepared Fe-NC-U support and 1.660 mL of a 0.0772 M H₂PtCl₆·6H₂O ethylene glycol solution were dispersed in 45 mL of ethylene glycol solution. After stirring for 3 h, 14 mL of a 1 M NaOH ethylene glycol solution was added dropwise to obtain mixed solution D. Solution D was transferred to a polytetrafluoroethylene-lined autoclave and reacted at 140 °C for 2 h. After cooling to room temperature, the pH was adjusted to 2 using 0.1 M nitric acid, and stirring was continued for a certain period of time. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain a Pt / Fe-NC-U electrocatalyst with a Pt loading of 20 wt%. Comparative Example 1

[0034] This comparative example provides a Pt / Fe-NC electrocatalyst with a Pt loading of 10 wt%, which is prepared by the following method.

[0035] 1400 mg of 2-methylimidazole was dissolved in 60 mL of deionized water and stirred for 30 min to obtain a homogeneous solution A. 600 mg of zinc nitrate, 40 mg of ferrous sulfate, and 18 mg of CTAB were dissolved in 60 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution B. Solution B was slowly added dropwise to solution A and stirred for 24 h. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain precursor precipitate C. Precipitate C was calcined at 910 °C for 2 h under nitrogen protection at a heating rate of 5 °C / min to obtain the Fe-NC support.

[0036] 100 mg of the prepared Fe-NC support and 0.738 mL of a 0.0772 M H₂PtCl₆·6H₂O ethylene glycol solution were dispersed in 45 mL of ethylene glycol solution. After stirring for 3 h, 14 mL of a 1 M NaOH ethylene glycol solution was added dropwise to obtain mixed solution D. Solution D was transferred to a polytetrafluoroethylene-lined autoclave and reacted at 140 °C for 2 h. After cooling to room temperature, the pH was adjusted to 2 using 0.1 M nitric acid, and stirring was continued for a certain period of time. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain a Pt / Fe-NC electrocatalyst with a Pt loading of 10 wt%. Comparative Example 2

[0037] This comparative example provides a Pt / NC-U electrocatalyst with a Pt loading of 10 wt%, which is prepared by the following method.

[0038] 1400 mg of 2-methylimidazole and 140 mg of urea were dissolved in 60 mL of deionized water and stirred for 30 min to obtain a homogeneous solution A. 600 mg of zinc nitrate and 18 mg of CTAB were dissolved in 60 mL of deionized water and sonicated for 30 min to obtain a homogeneous solution B. Solution B was slowly added dropwise to solution A and stirred for 24 h. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain precursor precipitate C. Precipitate C was calcined at 910 °C for 2 h under nitrogen protection at a heating rate of 5 °C / min to obtain the NC-U carrier.

[0039] 100 mg of the prepared NC-U support and 0.738 mL of a 0.0772 M H₂PtCl₆·6H₂O ethylene glycol solution were dispersed in 45 mL of ethylene glycol solution. After stirring for 3 h, 14 mL of a 1 M NaOH ethylene glycol solution was added dropwise to obtain mixed solution D. Solution D was transferred to a polytetrafluoroethylene-lined autoclave and reacted at 140 °C for 2 h. After cooling to room temperature, the pH was adjusted to 2 using 0.1 M nitric acid, and stirring was continued for a certain period of time. After centrifugation and washing, the solution was dried at 70 °C for 8 h to obtain a Pt / NC-U electrocatalyst with a Pt loading of 10 wt%.

[0040] Finally, it should be noted that the above embodiments and comparative examples are only used to illustrate the technical solutions of the present invention, and are intended to help readers understand the present invention, not to limit it. They should be understood that the scope of protection of the present invention is not limited to such specific statements and embodiments. Therefore, those skilled in the art can make modifications according to the technical solutions disclosed in this invention, but these modifications do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this invention.

Claims

1. A urea modified iron-nitrogen-carbon supported low platinum electrocatalyst (Pt / Fe-NC-U) and a method for its preparation, characterized in that, The catalyst exhibits strong electronic interactions between Pt and the Fe-NC-U support, which modulates the electronic structure of Pt. Furthermore, the FeN4 sites abundant in the support firmly anchor the Pt nanoparticles, thereby achieving high catalytic activity and stability in the electrocatalytic oxygen reduction reaction.

2. A method for preparing a Pt / Fe-NC-U electrocatalyst, characterized in that, Includes the following steps: The first step is to mix 2-methylimidazole and urea in a certain proportion, dissolve them in a certain amount of deionized water, and stir for an appropriate time to obtain a homogeneous solution A. The second step involves mixing zinc nitrate, ferrous sulfate, and CTAB in a certain proportion, dissolving them in a certain amount of deionized water, and then sonicating for an appropriate time to obtain a homogeneous solution B. The third step is to slowly add solution B to solution A, stir for a certain period of time, centrifuge, wash, and dry to obtain precursor precipitate C; The fourth step involves calcining precipitate C at a certain temperature and time under nitrogen protection at a specific heating rate to obtain the Fe-NC-U support. Fifth step: Disperse the Fe-NC-U support and chloroplatinic acid ethylene glycol solution in a certain amount of ethylene glycol solution, stir for a certain time, and then add an appropriate amount of NaOH ethylene glycol solution dropwise to obtain mixed solution D; Step 6: Transfer solution D to a polytetrafluoroethylene-lined autoclave and react at a certain temperature for an appropriate time. After cooling to room temperature, adjust the pH with nitric acid of appropriate concentration and continue stirring for a certain time. After centrifugation, washing, and drying, the Pt / Fe-NC-U electrocatalyst is obtained.

3. The preparation method according to claim 2, characterized in that, In the first step, the amount of 2-methylimidazole added is 700-1400 mg, the amount of urea added is 70-140 mg, the amount of deionized water is 60 mL, and the stirring time is 30 min.

4. The preparation method according to claim 2, characterized in that, In the second step, the amount of zinc nitrate added is 300-600 mg, ferrous sulfate added is 20-40 mg, CTAB added is 9-18 mg, deionized water is 60 mL, and the sonication time is 30 min.

5. The method of claim 2, wherein the step of forming the first and second layers is performed by a process selected from the group consisting of: sputtering, evaporation, and chemical vapor deposition. The stirring time in the third step is 6-24 h, the drying temperature is 70 ℃, and the drying time is 8 h.

6. The preparation method according to claim 2, characterized in that, The heating rate in the fourth step is 5 ℃ / min, the calcination temperature is 800-1000 ℃, and the calcination time is 1-3 h.

7. The preparation method according to claim 3, characterized in that, In step 5, the Fe-NC-U carrier was added in an amount of 100 mg, the concentration of chloroplatinic acid ethylene glycol solution was 0.0772 M, the amount added was 0.349-1.660 mL, the amount of ethylene glycol solution added was 45 mL, the stirring time was 3 h, the concentration of NaOH ethylene glycol solution was 1 M, and the amount of NaOH ethylene glycol solution added was 14 mL.

8. The preparation method according to claim 3, characterized in that, In step six, the reaction temperature is 120-180 ℃, the reaction time is 1-4 h, the pH is adjusted to 2-3, the stirring time is 6-12 h, the drying temperature is 70 ℃, and the drying time is 8 h.