A solid-liquid hybrid battery, its preparation method, and its electrical device.

By employing a bilayer structure of niobium oxide-coated lithium titanium aluminum phosphate and a specific orientation in solid-state lithium-ion batteries, combined with improvements in positive and negative electrode materials, the problems of low safety, low energy density, and short cycle life of solid-state lithium-ion batteries have been solved, achieving higher battery performance.

CN123120839APending Publication Date: 2026-11-17HUBEI XINGFA CHEM GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611440159.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing solid-state lithium-ion batteries suffer from problems such as low safety, low energy density, and short cycle life. In particular, side reactions and interfacial impedance at the positive and negative electrode interfaces lead to performance degradation.

Method used

A double-layer solid electrolyte structure of niobium oxide-coated lithium titanium aluminum phosphate is adopted. The first solid electrolyte layer faces the positive electrode and the second solid electrolyte layer faces the negative electrode. A carbon layer and a lithium niobate layer are coated on the positive electrode, and a silicon-carbon-graphite composite material is used for the negative electrode. An electrolyte with a specific ratio and thickness is added.

Benefits of technology

It significantly suppressed side reactions at the positive and negative electrode interfaces, improved conductivity, reduced interface impedance, and enhanced battery safety, energy density, and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application provides a solid-liquid hybrid battery, its preparation method, and an electrical device, relating to the field of solid-state lithium-ion battery technology. By using niobium oxide to coat lithium titanium aluminum phosphate, this application significantly suppresses side reactions at the interface between the solid electrolyte and the positive and negative electrodes, while significantly improving the conductivity of the solid electrolyte. Furthermore, the solid electrolyte is configured as a bilayer structure, with the first solid electrolyte layer coated with polyvinylidene fluoride facing the positive electrode side, and the second solid electrolyte layer coated with polyethylene oxide facing the negative electrode side. This specific orientation significantly reduces the interfacial impedance between the solid electrolyte and the positive and negative electrodes, thereby significantly improving the safety, energy density, and cycle life of the solid-liquid hybrid battery. Therefore, this solid-liquid hybrid battery has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solid-state lithium-ion battery technology, specifically to a solid-liquid hybrid battery and its preparation method and power device. Background Technology

[0002] With the rapid development of electric vehicles and large-scale energy storage systems, the market has placed higher demands on the energy density, safety, and cycle life of lithium-ion batteries. Traditional liquid lithium-ion batteries use organic electrolyte systems, which pose safety hazards such as leakage, flammability, and explosion, and their energy density is nearing its limit. Solid-state batteries use solid electrolytes instead of liquid electrolytes, which can simultaneously solve the two major challenges of "safety" and "high energy density," and are widely regarded as an important development direction for next-generation lithium batteries.

[0003] In solid-state battery cathode systems, lithium manganese iron phosphate (LMFP) is a novel phosphate cathode material formed by doping lithium iron phosphate (LFP) with manganese. It combines the safety advantages of LFP with a higher voltage platform (approximately 4.1V vs. Li / Li). + The specific capacity can reach over 150 mAh / g. However, the inherently low electronic and ionic conductivity of LMFPs limits their rate performance, and Mn content during charge-discharge cycles also increases. 2+ The Jahn-Teller effect, which causes manganese ion dissolution, accelerates interface degradation.

[0004] In terms of solid electrolytes, NASICON-type lithium aluminum titanium phosphate (LATP) stands out due to its high ionic conductivity (approximately 10 Ω·cm at room temperature). -4 The LATP ceramic electrolyte has attracted considerable attention due to its high efficiency (on the order of S / cm), wide electrochemical window (above 4.1V), good air stability, and low cost. However, the instability of the interface between the LATP ceramic electrolyte and the lithium anode, as well as the poor solid-solid contact at the electrode / electrolyte interface, remain prominent issues.

[0005] In terms of anode materials, silicon-carbon materials have advantages such as a theoretical specific capacity of up to about 2400 mAh / g and low operating voltage. However, they undergo significant volume expansion during charging and discharging, which leads to gaps at the interface between the electrode and the solid electrolyte, resulting in rapid capacity decay.

[0006] In view of this, it is necessary to provide a new solid-liquid hybrid battery to address the shortcomings of the existing technology. Summary of the Invention

[0007] In view of the technical problems existing in the background art, this application provides a solid-liquid hybrid battery and its preparation method and power device, aiming to solve the technical problems of low safety, low energy density and short cycle life of existing solid-liquid hybrid batteries.

[0008] In a first aspect, embodiments of this application provide a solid-liquid hybrid battery, including a positive electrode, a solid electrolyte, a negative electrode, and an electrolyte; wherein, the solid electrolyte includes a first solid electrolyte layer and a second solid electrolyte layer; the first solid electrolyte layer includes a first lithium titanium aluminum phosphate layer and a first niobium oxide layer and a polyvinylidene fluoride layer sequentially coated on the surface of the first lithium titanium aluminum phosphate layer; the second solid electrolyte layer includes a second lithium titanium aluminum phosphate layer and a second niobium oxide layer and a polyoxyethylene layer sequentially coated on the surface of the second lithium titanium aluminum phosphate layer; the first solid electrolyte layer faces the positive electrode side, and the second solid electrolyte layer faces the negative electrode side.

[0009] In the technical solution of this application embodiment, by using niobium oxide to coat lithium titanium aluminum phosphate, the side reactions at the interface between the solid electrolyte and the positive and negative electrodes can be significantly suppressed, while the conductivity of the solid electrolyte can be significantly improved. Furthermore, the solid electrolyte is set as a double-layer structure, with the first solid electrolyte layer coated with polyvinylidene fluoride facing the positive electrode side and the second solid electrolyte layer coated with polyethylene oxide facing the negative electrode side. Through this specific orientation setting, the interfacial impedance between the solid electrolyte and the positive and negative electrodes can be significantly reduced, thereby significantly improving the safety, energy density and cycle life of the solid-liquid hybrid battery.

[0010] In some embodiments, the molar ratio of lithium, aluminum, titanium and phosphorus in the first lithium titanium aluminum phosphate layer is (1.2-1.4):(0.2-0.4):(1.6-1.8):(2.9-3.1), and the average particle size of the primary particles in the first lithium titanium aluminum phosphate layer is 300-400 nm; the mass ratio of the first lithium titanium aluminum phosphate layer to the first niobium oxide layer is (9.97-9.99):(0.003-0.008); and the mass ratio of the first lithium titanium aluminum phosphate layer coated with the first niobium oxide layer to the polyvinylidene fluoride layer is (8-10):(0.5-1.5).

[0011] In some embodiments, the molar ratio of lithium, aluminum, titanium and phosphorus in the second lithium titanium aluminum phosphate layer is (1.2-1.4):(0.2-0.4):(1.6-1.8):(2.9-3.1), and the average particle size of the primary particles in the second lithium titanium aluminum phosphate layer is 300-400 nm; the mass ratio of the second lithium titanium aluminum phosphate layer to the second niobium oxide layer is (9.97-9.99):(0.003-0.008); and the mass ratio of the second lithium titanium aluminum phosphate layer coated with the second niobium oxide layer to the polyethylene oxide layer is (7-9):(1-3).

[0012] In some embodiments, the thickness of the first solid electrolyte layer is 10-20 μm, and the thickness of the second solid electrolyte layer is 20-40 μm.

[0013] In some embodiments, the positive electrode includes lithium manganese iron phosphate, which contains doping elements, and the surface of the lithium manganese iron phosphate is sequentially coated with a carbon layer and a lithium niobate layer; wherein the doping elements include at least one of titanium and magnesium; the molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate is (1.05-1.07):(0.6-0.8):(0.2-0.4):(1.02-1.04).

[0014] In some embodiments, the content of titanium is 1600-1800 ppm, the content of magnesium is 1600-1800 ppm, the content of carbon layer is 1-1.5 wt%, and the mass ratio of lithium manganese iron phosphate coated with carbon layer to lithium niobate layer is (9.9-10):(0.005-0.1).

[0015] In some embodiments, the negative electrode sheet comprises a silicon-carbon-graphite composite material, wherein the mass ratio of silicon-carbon to graphite is (10-30):(70-90); wherein the average particle size of silicon particles in the silicon-carbon-graphite composite material is 60-220 nm, the average particle size of carbon matrix is ​​5-8 μm, and the silicon content is 10-15 wt%.

[0016] In some embodiments, the mass of the electrolyte is 4-8 wt% of the mass of the solid-liquid hybrid battery.

[0017] Secondly, embodiments of this application provide a method for preparing a solid-liquid hybrid battery as described above, comprising the following steps: providing doped lithium manganese iron phosphate, and then sequentially coating it with a carbon source and lithium niobate to obtain a positive electrode material; providing a first solid electrolyte layer and a second solid electrolyte layer respectively, and pressurizing the first solid electrolyte layer and the second solid electrolyte layer to obtain a solid electrolyte; providing a silicon-carbon-graphite composite material; preparing the positive electrode material and the silicon-carbon-graphite composite material into a positive electrode sheet and a negative electrode sheet respectively, then placing the solid electrolyte between the positive electrode sheet and the negative electrode sheet, hot-pressing and encapsulating, and adding an electrolyte to obtain a solid-liquid hybrid battery.

[0018] In a third aspect, embodiments of this application provide an electrical device, including any of the solid-liquid hybrid batteries described above or a solid-liquid hybrid battery prepared by the above preparation method.

[0019] Beneficial effects: By using niobium oxide to coat lithium titanium aluminum phosphate, this application can significantly suppress side reactions at the interface between the solid electrolyte and the positive and negative electrodes, while significantly improving the conductivity of the solid electrolyte. Furthermore, by setting the solid electrolyte as a double-layer structure, with the first solid electrolyte layer coated with polyvinylidene fluoride facing the positive electrode side and the second solid electrolyte layer coated with polyethylene oxide facing the negative electrode side, this specific orientation setting can significantly reduce the interfacial impedance between the solid electrolyte and the positive and negative electrodes, thereby significantly improving the safety, energy density, and cycle life of the solid-liquid hybrid battery. Therefore, this solid-liquid hybrid battery has good application prospects.

[0020] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Detailed Implementation

[0021] The embodiments of the technical solution of this application will be described in detail below. The following embodiments are only used to illustrate the technical solution of this application more clearly, and are therefore only examples, and should not be used to limit the scope of protection of this application.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification and claims of this application are intended to cover non-exclusive inclusion.

[0023] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0024] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0025] In the description of the embodiments of this application, the term "and / or" is merely a description of the relationship between related objects, indicating that there can be three relationships. For example, A and / or B can represent three situations: A exists alone, A and B exist simultaneously, and B exists alone.

[0026] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0027] Currently, solid-state batteries use solid electrolytes instead of liquid electrolytes, which can simultaneously solve the two major challenges of "safety" and "high energy density". However, existing solid-liquid hybrid batteries have technical problems such as low safety, low energy density, and short cycle life.

[0028] To address the technical problems of existing solid-liquid hybrid batteries, such as low safety, low energy density, and short cycle life, this application provides a solid-liquid hybrid battery, its preparation method, and an electrical device thereof.

[0029] In a first aspect, this application provides a solid-liquid hybrid battery, including a positive electrode, a solid electrolyte, a negative electrode, and an electrolyte; wherein the solid electrolyte includes a first solid electrolyte layer and a second solid electrolyte layer; the first solid electrolyte layer includes a first lithium titanium aluminum phosphate layer and a first niobium oxide layer and a polyvinylidene fluoride layer sequentially coated on the surface of the first lithium titanium aluminum phosphate layer; the second solid electrolyte layer includes a second lithium titanium aluminum phosphate layer and a second niobium oxide layer and a polyoxyethylene layer sequentially coated on the surface of the second lithium titanium aluminum phosphate layer; the first solid electrolyte layer faces the positive electrode side, and the second solid electrolyte layer faces the negative electrode side.

[0030] In the technical solution of this application embodiment, by using niobium oxide to coat lithium titanium aluminum phosphate, the side reactions at the interface between the solid electrolyte and the positive and negative electrodes can be significantly suppressed, while the conductivity of the solid electrolyte can be significantly improved. Furthermore, the solid electrolyte is set as a double-layer structure, with the first solid electrolyte layer coated with polyvinylidene fluoride facing the positive electrode side and the second solid electrolyte layer coated with polyethylene oxide facing the negative electrode side. Through this specific orientation, the interfacial impedance between the solid electrolyte and the positive and negative electrodes can be significantly reduced, thereby significantly improving the safety, energy density and cycle life of the solid-liquid hybrid battery. Therefore, this solid-liquid hybrid battery has good application prospects.

[0031] Further, in some embodiments, the molar ratio of lithium, aluminum, titanium and phosphorus in the first lithium titanium aluminum phosphate layer is (1.2-1.4):(0.2-0.4):(1.6-1.8):(2.9-3.1), and the average particle size of the primary particles in the first lithium titanium aluminum phosphate layer is 300-400 nm; the mass ratio of the first lithium titanium aluminum phosphate layer to the first niobium oxide layer is (9.97-9.99):(0.003-0.008); and the mass ratio of the first lithium titanium aluminum phosphate layer coated with the first niobium oxide layer to the polyvinylidene fluoride layer is (8-10):(0.5-1.5).

[0032] In this application, by controlling the mass ratio of the first lithium titanium aluminum phosphate layer to the first niobium oxide layer, and the mass ratio of the first lithium titanium aluminum phosphate layer coated with the first niobium oxide layer to the polyvinylidene fluoride layer within a specific range, the side reactions at the interface between the solid electrolyte and the positive electrode can be further significantly suppressed, and the interfacial impedance between the solid electrolyte and the positive electrode can be further significantly reduced, thereby further enhancing the energy density and cycle life of the solid-liquid hybrid battery.

[0033] Specifically, the molar ratio of lithium, aluminum, titanium, and phosphorus in the first lithium titanium aluminum phosphate layer can be, for example, 1.2:0.2:1.6:2.9, 1.3:0.3:1.7:3, 1.4:0.4:1.8:3.1, or other ratios within this range; the average particle size of the primary particles in the first lithium titanium aluminum phosphate layer can be, for example, 300 nm, 320 nm, 350 nm, 370 nm, 400 nm, or other values ​​within this range; the mass ratio of the first lithium titanium aluminum phosphate layer to the first niobium oxide layer can be, for example, 9.97:0.003, 9.97, etc. The mass ratio of the first lithium titanium aluminum phosphate layer coated with the first niobium oxide layer to the polyvinylidene fluoride layer can be, for example, 8:0.5, 8:1, 8:1.5, 9:0.5, 9:1, 9:1.5, 10:0.5, 10:1.5, 10:1.5, or other ratios within this range;

[0034] Further, in some embodiments, the molar ratio of lithium, aluminum, titanium and phosphorus in the second lithium titanium aluminum phosphate layer is (1.2-1.4):(0.2-0.4):(1.6-1.8):(2.9-3.1), and the average particle size of the primary particles in the second lithium titanium aluminum phosphate layer is 300-400 nm; the mass ratio of the second lithium titanium aluminum phosphate layer to the second niobium oxide layer is (9.97-9.99):(0.003-0.008); and the mass ratio of the second lithium titanium aluminum phosphate layer coated with the second niobium oxide layer to the polyethylene oxide layer is (7-9):(1-3).

[0035] In this application, by controlling the mass ratio of the second lithium titanium aluminum phosphate layer to the second niobium oxide layer, and the mass ratio of the second lithium titanium aluminum phosphate layer coated with the second niobium oxide layer to the polyethylene oxide layer within a specific range, the side reactions at the interface between the solid electrolyte and the negative electrode can be further significantly suppressed, and the interfacial impedance between the solid electrolyte and the negative electrode can be further significantly reduced, thereby further enhancing the energy density and cycle life of the solid-liquid hybrid battery.

[0036] Specifically, the molar ratio of lithium, aluminum, titanium, and phosphorus in the second lithium titanium aluminum phosphate layer can be, for example, 1.2:0.2:1.6:2.9, 1.3:0.3:1.7:3, 1.4:0.4:1.8:3.1, or other ratios within this range; the average particle size of the primary particles in the second lithium titanium aluminum phosphate layer can be, for example, 300 nm, 320 nm, 350 nm, 370 nm, 400 nm, or other values ​​within this range; and the mass ratio of the second lithium titanium aluminum phosphate layer to the second niobium oxide layer can be, for example, 9.97:0. 0.003, 9.97:0.005, 9.97:0.008, 9.982:0.003, 9.982:0.005, 9.982:0.008, 9.987:0.003, 9.987:0.005, 9.987:0.008 or other ratios within this range; the mass ratio of the second niobium oxide layer to the polyethylene oxide layer can be, for example, 7:1, 7:2, 7:3, 8:1, 8:2, 8:3, 9:1, 9:2, 9:3 or other ratios within this range.

[0037] Furthermore, in some embodiments, the thickness of the first solid electrolyte layer is 10-20 μm, and the thickness of the second solid electrolyte layer is 20-40 μm.

[0038] In this application, by controlling the thickness of the first solid electrolyte layer and the thickness of the second solid electrolyte layer within a specific range, they work synergistically to significantly reduce the interfacial impedance between the solid electrolyte and the positive and negative electrodes, thereby enhancing the performance of the solid-liquid hybrid battery.

[0039] Specifically, the thickness of the first solid electrolyte layer can be, for example, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm or other values ​​within this range; the thickness of the second solid electrolyte layer can be, for example, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm or other values ​​within this range.

[0040] Furthermore, in some embodiments, the positive electrode includes lithium manganese iron phosphate, which contains doping elements, and the surface of the lithium manganese iron phosphate is sequentially coated with a carbon layer and a lithium niobate layer; wherein the doping elements include at least one of titanium and magnesium; the molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate is (1.05-1.07):(0.6-0.8):(0.2-0.4):(1.02-1.04).

[0041] In this application, by coating the surface of lithium manganese iron phosphate with a carbon layer and a lithium niobate layer, the electronic and ionic conductivity of lithium manganese iron phosphate material can be significantly improved, while side reactions are reduced and the stability of lithium manganese iron phosphate material is improved, thereby significantly improving the performance of solid-liquid hybrid batteries.

[0042] Specifically, the molar ratio of lithium, manganese, iron and phosphorus in lithium manganese iron phosphate can be, for example, 1.05:0.6:0.2:1.02, 1.06:0.7:0.3:1.03, 1.07:0.8:0.4:1.04 or other ratios within this range.

[0043] Furthermore, in some embodiments, the content of titanium is 1600-1800 ppm, the content of magnesium is 1600-1800 ppm, the content of carbon layer is 1-1.5 wt%, and the mass ratio of lithium manganese iron phosphate coated with carbon layer to lithium niobate layer is (9.9-10):(0.005-0.1).

[0044] In this application, by controlling the content of doping elements, the content of carbon layers, and the mass ratio of lithium manganese iron phosphate coated with carbon layers to lithium niobate layers within a specific range, the electronic and ionic conductivity of lithium manganese iron phosphate materials can be further improved, thereby significantly improving the performance of solid-liquid hybrid batteries.

[0045] Specifically, the content of titanium can be, for example, 1600 ppm, 1650 ppm, 1700 ppm, 1750 ppm, 1800 ppm or other values ​​within this range; the content of magnesium can be, for example, 1600 ppm, 1650 ppm, 1700 ppm, 1750 ppm, 1800 ppm or other values ​​within this range; the content of the carbon layer can be, for example, 1 wt%, 1.1 wt%, 1.2 wt%, 1.3 wt%, 1.4 wt%, 1.5 wt% or other values ​​within this range; the mass ratio of lithium manganese iron phosphate coated with carbon layer to lithium niobate layer can be, for example, 9.9:0.005, 9.9:0.05, 9.9:0.1, 9.985:0.005, 9.985:0.05, 9.985:0.1, 10:0.005, 10:0.05, 10:0.1 or other ratios within this range.

[0046] Furthermore, in some embodiments, the negative electrode sheet comprises a silicon-carbon-graphite composite material, wherein the mass ratio of silicon-carbon to graphite is (10-30):(70-90); wherein the average particle size of silicon particles in the silicon-carbon-graphite composite material is 60-220 nm, the average particle size of carbon matrix is ​​5-8 μm, and the silicon content is 10-15 wt%.

[0047] In this application, by using silicon-carbon-graphite composite material as the negative electrode, both the system's energy density and cycle life can be balanced.

[0048] Specifically, the mass ratio of silicon-carbon to graphite can be, for example, 10:70, 10:80, 10:90, 20:70, 20:80, 20:90, 30:70, 30:80, 30:90, or other ratios within this range; the average particle size of silicon particles in the silicon-carbon-graphite composite material can be, for example, 60 nm, 100 nm, 150 nm, 200 nm, 220 nm, or other values ​​within this range; the average particle size of the carbon matrix can be, for example, 5 μm, 6 μm, 7 μm, 8 μm, or other values ​​within this range; and the silicon content can be, for example, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, or other values ​​within this range.

[0049] Furthermore, in some embodiments, the mass of the electrolyte is 4-8 wt% of the mass of the solid-liquid hybrid battery.

[0050] In this application, by adding a specific amount of electrolyte, the solid-solid interface contact can be improved, the conductivity can be increased, and the performance of the solid-liquid hybrid battery can be enhanced.

[0051] Specifically, the mass of the electrolyte can be, for example, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt% of the mass of the solid-liquid hybrid battery, or other values ​​within this range.

[0052] It is understandable that the electrolyte can be selected from conventional electrolytes in the prior art according to actual needs, as long as a high-performance solid-liquid hybrid battery can be assembled. For example, in this invention, the electrolyte includes the following components: LiPF6, LiFSI, EC, EMC, DEC, and VC, and the mass ratio of LiPF6, LiFSI, EC, EMC, DEC, and VC is (15-17):(4-6):(30-32):(34-36):(9-11):(2-4), preferably 16:5:31:35:10:3.

[0053] Secondly, embodiments of this application provide a method for preparing a solid-liquid hybrid battery as described above, comprising the following steps: providing doped lithium manganese iron phosphate, and then sequentially coating it with a carbon source and lithium niobate to obtain a positive electrode material; providing a first solid electrolyte layer and a second solid electrolyte layer respectively, and pressurizing the first solid electrolyte layer and the second solid electrolyte layer to obtain a solid electrolyte; providing a silicon-carbon-graphite composite material; preparing the positive electrode material and the silicon-carbon-graphite composite material into a positive electrode sheet and a negative electrode sheet respectively, then placing the solid electrolyte between the positive electrode sheet and the negative electrode sheet, hot-pressing and encapsulating, and adding an electrolyte to obtain a solid-liquid hybrid battery.

[0054] In the technical solution of this application embodiment, the preparation method is simple, the raw materials used are cheap and readily available, and it is suitable for large-scale production applications.

[0055] Furthermore, in some embodiments, the preparation of the cathode material specifically includes: mixing an iron source, a manganese source, a lithium source, a phosphorus source, a dopant, and a carbon source, and then grinding and calcining the mixture to obtain carbon-coated lithium manganese iron phosphate; mixing the carbon-coated lithium manganese iron phosphate with lithium niobate, and then grinding and annealing the mixture to obtain the cathode material.

[0056] Furthermore, in some preferred embodiments, the iron source includes iron phosphate, the manganese source includes manganese tetroxide, the lithium source includes lithium carbonate, the phosphorus source includes phosphoric acid, and the dopant includes at least one of titanium dioxide and magnesium oxide; the carbon source includes sucrose and PEG, and the mass ratio of sucrose to PEG is (0.5-1.5):(2-4), preferably 1:3; in the step of mixing carbon-coated manganese iron phosphate with lithium niobate, grinding, and annealing, the annealing specifically includes: annealing at a temperature of 300-400°C for 2-4 hours under an inert atmosphere.

[0057] Furthermore, in some embodiments, the preparation of the solid electrolyte in the step of obtaining the solid electrolyte specifically includes: mixing lithium source, aluminum source, titanium source and phosphorus source and grinding them, then calcining and pulverizing them to obtain lithium titanium aluminum phosphate; mixing lithium titanium aluminum phosphate with niobium oxide, then ball milling and annealing to obtain niobium oxide-coated lithium titanium aluminum phosphate; mixing the niobium oxide-coated lithium titanium aluminum phosphate with polyvinylidene fluoride and polyethylene oxide respectively, then drying them to obtain a first solid electrolyte layer and a second solid electrolyte layer, and then pressurizing them to obtain the solid electrolyte.

[0058] Furthermore, in some preferred embodiments, the lithium source includes lithium carbonate, the aluminum source includes aluminum oxide, the titanium source includes titanium dioxide, and the phosphorus source includes ammonium dihydrogen phosphate; in the step of mixing lithium titanium aluminum phosphate with niobium oxide, ball milling, and annealing to obtain niobium oxide-coated lithium titanium aluminum phosphate, the annealing specifically includes annealing at a temperature of 600-700°C for 2-4 hours.

[0059] In a third aspect, embodiments of this application provide an electrical device, including any of the solid-liquid hybrid batteries described above or a solid-liquid hybrid battery prepared by the above preparation method.

[0060] In the technical solution of this application embodiment, since the solid-liquid hybrid battery has good energy density and cycle life, it can be used as a power supply for electrical devices to provide efficient power.

[0061] The following are some specific embodiments. It should be noted that the embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0062] I. Preparation Method Example 1 A solid-liquid hybrid battery includes a positive electrode, a solid electrolyte, a negative electrode, and an electrolyte solution; The positive electrode includes lithium manganese iron phosphate (where the molar ratio of lithium, manganese, iron and phosphorus is 1.06:0.7:0.3:1.03), which is doped with titanium and magnesium (where the content of titanium and magnesium is 1700ppm each), and the surface of the lithium manganese iron phosphate is sequentially coated with a carbon layer and a lithium niobate layer (the content of the carbon layer is 1.4wt%, and the mass ratio of the carbon-coated lithium manganese iron phosphate to the lithium niobate layer is 9.985:0.005). The solid electrolyte comprises a first solid electrolyte layer (15 μm thick, facing the positive electrode) and a second solid electrolyte layer (30 μm thick, facing the negative electrode). The first solid electrolyte layer comprises a first lithium titanium aluminum phosphate layer (where the molar ratio of lithium, aluminum, titanium, and phosphorus is 1.3:0.3:1.7:3, and the average particle size of the primary particles is 350 nm) and a first niobium oxide layer sequentially coated on the surface of the first lithium titanium aluminum phosphate layer (the mass ratio of the first lithium titanium aluminum phosphate layer to the first niobium oxide layer is 9.982:0.008), and a polyvinylidene fluoride layer (coated with the first... The first lithium titanium aluminum phosphate layer of the niobium oxide layer has a mass ratio of 9:1 to the polyvinylidene fluoride layer; the second solid electrolyte layer includes a second lithium titanium aluminum phosphate layer (wherein the molar ratio of lithium, aluminum, titanium and phosphorus is 1.3:0.3:1.7:3, and the average particle size of the primary particles is 350 nm) and a second niobium oxide layer (the mass ratio of the second lithium titanium aluminum phosphate layer to the second niobium oxide layer is 9.982:0.008) and a polyoxyethylene layer (the mass ratio of the second lithium titanium aluminum phosphate layer coated with the second niobium oxide layer to the polyoxyethylene layer is 8:2); The negative electrode sheet comprises a silicon-carbon-graphite composite material with a silicon-carbon to graphite mass ratio of 20:80. The average particle size of the silicon particles in the silicon-carbon-graphite composite material is 150 nm, the average particle size of the carbon matrix is ​​7 μm, and the silicon content is 12 wt%. The electrolyte comprises the following components: LiPF6, LiFSI, EC, EMC, DEC, and VC, and the mass ratio of LiPF6, LiFSI, EC, EMC, DEC, and VC is 16:5:31:35:10:3.

[0063] The preparation of this solid-liquid hybrid battery includes the following steps: 1) Preparation of cathode material: Accurately weigh iron phosphate, manganese tetroxide, phosphoric acid, lithium carbonate, titanium dioxide, magnesium oxide, and carbon source (mass ratio of sucrose to PEG is 1:3) according to the above molar ratio; after grinding and calcining the above raw materials, lithium manganese iron phosphate substrate is prepared; take 9.985 kg of lithium manganese iron phosphate substrate and 0.005 kg of lithium niobate, mix and grind for 6 h, and anneal at 300℃ for 3 h under nitrogen protection to obtain lithium manganese iron phosphate cathode material.

[0064] 2) Solid electrolyte preparation: Lithium carbonate, alumina, titanium dioxide, and ammonium dihydrogen phosphate were accurately weighed according to the above molar ratio, mixed evenly in a sand mill, pre-calcined at 500℃ for 3 hours, sintered at 900℃ for 6 hours, and then pulverized by air jet milling to obtain lithium titanium aluminum phosphate (LATP) substrate; 9.982 kg of lithium titanium aluminum phosphate substrate and 0.008 kg of niobium oxide were mixed and ball-milled for 4 hours, and then annealed at 650℃ for 2 hours to obtain niobium oxide-coated lithium titanium aluminum phosphate material; the coated lithium titanium aluminum phosphate material was then mixed with polyvinylidene fluoride. (PVDF) was mixed at a mass ratio of 9:1 and N-methyl-2-pyrrolidone (NMP) was added. The mixture was then coated and dried to obtain a first solid electrolyte layer (LATP@Nb2O5 / PVDF layer) with a thickness of 15 μm. The coated lithium titanium aluminum phosphate material and polyethylene oxide (PEO) were mixed at a mass ratio of 8:2 and acetonitrile was added. The mixture was then coated and dried to obtain a second solid electrolyte layer (LATP@Nb2O5 / PEO layer) with a thickness of 30 μm. The two layers were then composited and pressed to obtain a solid electrolyte.

[0065] 3) Preparation of negative electrode material: Silicon carbon and graphite are mixed at a mass ratio of 20:80 to obtain silicon carbon-graphite composite material.

[0066] 4) Solid-liquid hybrid battery preparation: The lithium manganese iron phosphate positive electrode material, conductive carbon black, carbon nanotubes, PVDF, and dispersant prepared in step 1) are mixed in a mass ratio of 95.5:1.4:1.0:2.0:0.1 to prepare a positive electrode slurry. This slurry is coated onto aluminum foil, dried at 120°C, and then rolled to obtain the positive electrode sheet. The silicon-carbon-graphite negative electrode material, conductive carbon black, carbon nanotubes, CMC, SBR, and PAA prepared in step 3) are mixed in a mass ratio of 95.4:1.0:0.1:0.3:1.5:1.7 to prepare a negative electrode slurry. The negative electrode sheet is prepared by coating the copper foil, drying it at 100°C, and then rolling it. The solid electrolyte (LATP@Nb2O5 / PVDF layer facing the positive electrode side and LATP@Nb2O5 / PEO layer facing the negative electrode side) prepared in step 2) is placed between the positive and negative electrode sheets. After hot pressing at 80°C and 10MPa for 30 minutes, it is packaged and electrolyte is added (the mass ratio of each component LiPF6:LiFSI:EC:EMC:DEC:VC=16:5:31:35:10:3), and its mass is controlled to account for 8wt% of the battery mass.

[0067] Example 2 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as in Example 1. The difference is that in step 1), 9.9 kg of lithium manganese iron phosphate substrate and 0.1 kg of lithium niobate are taken.

[0068] Example 3 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as those in Example 1. The difference is that in step 1), the battery is annealed at 400°C for 3 hours under nitrogen protection.

[0069] Example 4 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as in Example 1. The difference is that in step 2), 9.987 kg of lithium titanium aluminum phosphate substrate and 0.003 kg of niobium oxide are taken.

[0070] Example 5 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as in Example 1, except that in step 2), annealing is performed at 600°C for 2 hours.

[0071] Example 6 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as in Example 1. The difference is that in step 2), the thickness of the LATP@Nb2O5 / PVDF layer is adjusted to 10μm.

[0072] Example 7 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as in Example 1. The difference is that in step 2), the thickness of the LATP@Nb2O5 / PEO layer is adjusted to 40μm.

[0073] Example 8 In this embodiment, the composition and preparation method of the solid-liquid hybrid battery are basically the same as in Example 1. The difference is that in step 4), the mass ratio of the electrolyte is adjusted to 4wt%.

[0074] Comparative Example 1 In this comparative example, the composition and preparation method of the solid-liquid hybrid battery are basically the same as those in Example 1. The difference is that in step 1), lithium niobate coating is not performed.

[0075] Comparative Example 2 In this comparative example, the composition and preparation method of the solid-liquid hybrid battery are basically the same as those in Example 1. The difference is that in step 2), niobium oxide coating is not performed.

[0076] Comparative Example 3 In this comparative example, the composition and preparation method of the solid-liquid hybrid battery are basically the same as those in Example 1. The difference is that in step 2), the LATP@Nb2O5 / PEO layer is replaced with the LATP@Nb2O5 / PVDF layer, so that the double-layer structure is the LATP@Nb2O5 / PVDF layer.

[0077] Comparative Example 4 In this comparative example, the composition and preparation method of the solid-liquid hybrid battery are basically the same as those in Example 1. The difference is that in step 2), the LATP@Nb2O5 / PVDF layer is replaced with the LATP@Nb2O5 / PEO layer, so that the double-layer structure is the LATP@Nb2O5 / PEO layer.

[0078] Comparative Example 5 In this comparative example, the composition and preparation method of the solid-liquid hybrid battery are basically the same as those in Example 1. The difference is that no electrolyte is added in step 4).

[0079] II. Test Methods and Related Result Analysis 1. Charge and discharge test of solid-liquid hybrid battery The solid-liquid hybrid batteries prepared in Examples 1-8 and Comparative Examples 1-5 were subjected to charge-discharge tests in the voltage range of 2.5~4.3V, and the results are shown in Table 1 below.

[0080] Table 1 Test results of solid-liquid hybrid batteries

[0081] As can be seen from Table 1, the solid-liquid hybrid batteries prepared in Examples 1-8 have good initial efficiency, charge-discharge and cycle stability.

[0082] Comparative Example 1 did not involve lithium niobate coating, and Comparative Example 2 did not involve niobium oxide coating. The results showed that the first-efficiency, charge-discharge, and cycle stability of the prepared solid-liquid hybrid battery decreased significantly. The results indicate that coating the cathode material and solid electrolyte can significantly improve the performance of the solid-liquid hybrid battery.

[0083] In Comparative Example 3, the solid electrolyte bilayer structure was LATP@Nb2O5 / PVDF layer, and in Comparative Example 4, the solid electrolyte bilayer structure was LATP@Nb2O5 / PEO layer. The results showed that the first-time efficiency, charge-discharge, and cycle stability of the prepared solid-liquid hybrid battery decreased to a certain extent. The results indicate that the solid electrolyte adopting a bilayer structure with a specific orientation (LATP@Nb2O5 / PVDF layer facing the positive electrode and LATP@Nb2O5 / PEO layer facing the negative electrode) can significantly improve the performance of the solid-liquid hybrid battery.

[0084] In Comparative Example 5, without the addition of electrolyte, the results showed that the first-efficiency performance, charge-discharge performance, and cycle stability of the prepared solid-liquid hybrid battery decreased significantly. The results indicate that adding a certain amount of electrolyte can significantly improve the performance of the solid-liquid hybrid battery.

[0085] In summary, this application modifies the lithium manganese iron phosphate cathode material by carbon coating and lithium niobate coating, designs the solid electrolyte as a bilayer structure (LATP@Nb2O5 / PVDF layer facing the cathode, LATP@Nb2O5 / PEO layer facing the anode), uses silicon-carbon-graphite composite material as the anode material, adds a certain amount of electrolyte, and adopts an integrated preparation process to synergistically reduce interfacial impedance, suppress electrode volume expansion effect, and improve ion transport efficiency, so that the solid-liquid hybrid battery has high safety, high energy density and long cycle life.

[0086] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.

Claims

1. A solid-liquid hybrid battery, characterized by, It includes positive electrode, solid electrolyte, negative electrode and electrolyte solution; The solid electrolyte includes a first solid electrolyte layer and a second solid electrolyte layer. The first solid electrolyte layer includes a first lithium titanium aluminum phosphate layer and a first niobium oxide layer and a polyvinylidene fluoride layer sequentially coated on the surface of the first lithium titanium aluminum phosphate layer; The second solid electrolyte layer includes a second lithium titanium aluminum phosphate layer and a second niobium oxide layer and a polyethylene oxide layer sequentially coated on the surface of the second lithium titanium aluminum phosphate layer; The first solid electrolyte layer faces the positive electrode, and the second solid electrolyte layer faces the negative electrode.

2. The solid-liquid hybrid battery according to claim 1, wherein The molar ratio of lithium, aluminum, titanium and phosphorus in the first lithium titanium aluminum phosphate layer is (1.2-1.4):(0.2-0.4):(1.6-1.8):(2.9-3.1), and the average particle size of the primary particles in the first lithium titanium aluminum phosphate layer is 300-400 nm; the mass ratio of the first lithium titanium aluminum phosphate layer to the first niobium oxide layer is (9.97-9.99):(0.003-0.008); the mass ratio of the first lithium titanium aluminum phosphate layer coated with the first niobium oxide layer to the polyvinylidene fluoride layer is (8-10):(0.5-1.5).

3. The solid-liquid hybrid battery according to claim 1, wherein The molar ratio of lithium, aluminum, titanium and phosphorus in the second lithium titanium aluminum phosphate layer is (1.2-1.4):(0.2-0.4):(1.6-1.8):(2.9-3.1), and the average particle size of the primary particles in the second lithium titanium aluminum phosphate layer is 300-400 nm; the mass ratio of the second lithium titanium aluminum phosphate layer to the second niobium oxide layer is (9.97-9.99):(0.003-0.008); the mass ratio of the second lithium titanium aluminum phosphate layer coated with the second niobium oxide layer to the polyethylene oxide layer is (7-9):(1-3).

4. The solid-liquid hybrid battery according to claim 1, wherein The thickness of the first solid electrolyte layer is 10-20 μm, and the thickness of the second solid electrolyte layer is 20-40 μm.

5. The solid-liquid hybrid battery of claim 1, wherein, The positive electrode includes lithium manganese iron phosphate, which contains doping elements, and the surface of the lithium manganese iron phosphate is sequentially coated with a carbon layer and a lithium niobate layer. The doping element includes at least one of titanium and magnesium. The molar ratio of lithium, manganese, iron and phosphorus in the lithium manganese iron phosphate is (1.05-1.07):(0.6-0.8):(0.2-0.4):(1.02-1.04).

6. The solid-liquid hybrid battery according to claim 5, characterized in that, The titanium content is 1600-1800 ppm, the magnesium content is 1600-1800 ppm, the carbon layer content is 1-1.5 wt%, and the mass ratio of lithium manganese iron phosphate coated with carbon layer to lithium niobate layer is (9.9-10):(0.005-0.1).

7. The solid-liquid hybrid battery according to claim 1, characterized in that, The negative electrode sheet comprises a silicon-carbon-graphite composite material, wherein the mass ratio of silicon-carbon to graphite is (10-30):(70-90). The silicon-carbon-graphite composite material has an average particle size of 60-220 nm for silicon particles, an average particle size of 5-8 μm for the carbon matrix, and a silicon content of 10-15 wt%.

8. The solid-liquid hybrid battery according to claim 1, characterized in that, The mass of the electrolyte is 4-8 wt% of the mass of the solid-liquid hybrid battery.

9. A method for preparing a solid-liquid hybrid battery as described in any one of claims 1-8, characterized in that, Includes the following steps: Doped lithium manganese iron phosphate is provided, and then coated with carbon source and lithium niobate in sequence to obtain cathode material; A first solid electrolyte layer and a second solid electrolyte layer are provided respectively, and a solid electrolyte is obtained by pressurizing the first solid electrolyte layer and the second solid electrolyte layer. Provide silicon-carbon-graphite composite materials; The positive electrode material and the silicon-carbon-graphite composite material are respectively prepared into positive electrode sheets and negative electrode sheets. Then, the solid electrolyte is placed between the positive electrode sheets and the negative electrode sheets, hot-pressed and sealed, and electrolyte is added to obtain the solid-liquid hybrid battery.

10. An electrical appliance, characterized in that, Includes the solid-liquid hybrid battery according to any one of claims 1-8 or the solid-liquid hybrid battery prepared by the preparation method according to claim 9.