A low-temperature resistant halide solid electrolyte, its preparation method and application
By using a multiphase structure composed of nanocrystalline cores and amorphous phases, and combined with La3+, Zr4+ and O2- modification, a low-temperature resistant halide solid electrolyte was prepared, which solved the problems of low ionic conductivity and unstable crystal phase of halide electrolytes at low temperatures, and achieved high conductivity and stability in extremely cold environments.
Patent Information
- Application Number
- CN202611436037.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing halide solid electrolytes exhibit significantly reduced ionic conductivity, unstable crystal structure, and high interfacial impedance at low temperatures, making them unsuitable for long-term use in extremely cold environments.
An electrolyte with high ion conductivity and a stable crystalline phase was prepared by using a multiphase structure composed of a nanocrystalline core and an amorphous phase, through La3+ replacing Y3+ to expand the lattice, Zr4+ introducing lithium vacancies, and O2- replacing Cl- to weaken bond energy, combined with low-temperature annealing and ice-water quenching processes.
It maintains high ion conductivity and stable crystal structure over a wide low-temperature range, reduces interfacial impedance, and is suitable for long-term use in extremely cold environments, thus solving the problem of rapid performance degradation of traditional halide electrolytes at low temperatures.
Smart Images

Figure CN123120846A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of all-solid-state lithium battery electrolyte technology, and in particular to a low-temperature resistant halide solid electrolyte, its preparation method and application. Background Technology
[0002] Solid-state electrolytes, as the core component of all-solid-state batteries, directly determine the battery's ion conductivity, interfacial stability, and wide-temperature adaptability. Currently, solid-state electrolytes that have been studied on a large scale are mainly divided into four major systems: polymer, oxide, sulfide, and halide. Polymer solid-state electrolytes have good processability, but at low temperatures, the polymer chain segments freeze and crystallize, closing the ion conduction channels and resulting in extremely poor low-temperature ion conductivity. Oxide solid-state electrolytes have a wide electrochemical window and stable structure, but the material has high hardness, poor solid-solid interface contact, and a sharp increase in grain boundary impedance at low temperatures, making them unsuitable for cold pressing. Sulfide solid-state electrolytes have room-temperature ion conductivity close to that of liquid electrolytes, but they have poor chemical stability, are prone to decomposition in water, releasing toxic gases, and have insufficient compatibility with high-voltage cathodes, making it difficult to guarantee low-temperature cycle stability.
[0003] Halide solid electrolytes, based on alkali metal halides and rare earth halides, possess advantages such as high ionic conductivity, wide electrochemical window, compatibility with high-voltage cathodes, strong plasticity, and good interfacial adhesion. They exhibit excellent compatibility with high-nickel ternary cathodes and lithium metal anodes, making them one of the most promising solid electrolyte systems for industrialization. Conventional commercially available halide electrolytes such as Li3YCl6 and Li3InCl6 show a 1-2 order of magnitude decrease in ionic conductivity at -20℃ compared to room temperature, resulting in severe polarization during low-temperature charge and discharge and extremely low capacity retention. Furthermore, some halide crystal phases undergo low-temperature phase transitions, transforming from highly conductive phases to less conductive or even insulating impurities, directly blocking lithium-ion transport channels and making them unsuitable for long-term stable use under extremely cold conditions.
[0004] To optimize the performance of halide electrolytes, various modification methods have been developed. Introducing elements such as In, Y, and Zr to regulate lattice vacancies can optimize bulk ion conduction to some extent, but it cannot reduce the low-temperature conduction barrier at grain boundaries, resulting in limited improvement in low-temperature performance. Inorganic oxide surface coating processes can improve the water vapor stability of materials and avoid hydrolysis failure, but they cannot optimize the lattice structure or reduce the ion transition barrier, thus having no significant effect on improving low-temperature conductivity. Polymer composite modification, which combines halide powder with a polymer matrix to improve interfacial contact, can lead to hardening and crystallization of the polymer matrix at low temperatures, which can block the ion transport channels of the composite system and further reduce the overall low-temperature conductivity of the electrolyte. In addition, at low temperatures, the thermal expansion coefficients of the electrolyte and the lithium metal anode and cathode are mismatched, leading to increased interfacial gaps, contact failure, and a sharp increase in interfacial impedance. At the same time, halides are prone to side reactions with the lithium anode at low temperatures, generating a high-resistance passivation interfacial layer, which exacerbates cell polarization. Conventional interface modification layers are prone to cracking and falling off at low temperatures, making it impossible to stabilize the interface for a long time. This results in rapid low-temperature cycle degradation and short service life of all-solid-state batteries.
[0005] In summary, there is an urgent need to develop a low-temperature resistant halide solid electrolyte that can maintain high ion conductivity, stable crystal structure, and low interface impedance over a wide low-temperature range, in order to meet the usage requirements of all-solid-state lithium batteries in extremely cold environments. Summary of the Invention
[0006] To address at least one of the aforementioned technical problems and to develop a solid electrolyte that maintains high ion conductivity, stable crystal structure, and low interfacial impedance over a wide low-temperature range, this application provides a low-temperature resistant halide solid electrolyte, its preparation method, and its application.
[0007] On the one hand, this application provides a low-temperature resistant halide solid electrolyte, wherein the solid electrolyte is composed of a nanocrystalline core and an amorphous phase coated on the outer surface of the nanocrystalline core: the nanocrystalline core is a Y / La / Zr mixed metallic chloride octahedral crystal phase, and the amorphous phase is a Li-Cl-O disordered phase;
[0008] The general chemical formula is: Li 3+a Y 1-x-z La x Zr z Cl 6-b O b ;
[0009] Where: a = 0.08~0.22;
[0010] x = 0.05~0.15;
[0011] z = 0.02~0.08;
[0012] b = 0.03~0.10.
[0013] The technical solution of this application is approved by La. 3+ Large radius replacement of Y 3+ It expands the octahedral framework of metal halide, structurally suppressing low-temperature lattice contraction and preserving ion migration space; Zr 4+ Heterovalent substitution can artificially introduce controllable lithium vacancies, increasing lithium-ion transport sites; O 2- Partially replaces Cl - It can weaken lattice bond energy and reduce the activation energy of lithium-ion transition, thereby improving the low-temperature ion conductivity from the intrinsic level of the material. The nanocrystalline core provides long-range ordered high-speed ion channels in the bulk phase, while the outer amorphous phase acts as a low-resistance flexible conductive layer across grain boundaries, avoiding the common problem of grain boundary impedance surge at low temperatures in pure crystalline electrolytes, and achieving low-temperature high conductivity across the entire bulk-grain boundary domain.
[0014] Optionally, the chemical formula of the solid electrolyte is: Li 3.15 Y 0.85 La 0.10 Zr 0.05 Cl 5.94 O 0.06 .
[0015] This ratio provides relatively better lattice opening, lithium vacancy concentration, and anion bond energy weakening effect. It ensures a low octahedral cavity shrinkage rate at extremely low temperatures of -60℃, while avoiding lattice distortion caused by excessive vacancies and excessive amorphous layer that reduces overall conductivity. It can reduce the lithium-ion migration activation energy to as low as 0.27eV, thereby improving low-temperature conductivity and structural stability.
[0016] Optionally, the grain size of the nanocrystalline core is 20~40nm, and the cell space group is P63 / mmc; the coating thickness of the amorphous phase is 3~8nm.
[0017] A grain size of 20-40 nm strikes a balance between bulk conductivity and grain boundary quantity: if the grains are too small, the grain boundary ratio will be too high, increasing impedance; if the grains are too large, the amorphous layer cannot completely cover the grain boundaries. An amorphous coating thickness of 3-8 nm can completely cover the grain boundaries, eliminating the grain boundary conductivity barrier, while not slowing down the overall ion conduction rate due to an excessively thick amorphous layer. The P63 / mmc space group corresponds to a highly conductive hexagonal crystal structure, providing a stable three-dimensional transport framework for lithium ions, ensuring the bulk ion conduction rate, and avoiding the formation of insulating impurities due to crystal phase transitions at low temperatures.
[0018] Optionally, after the solid electrolyte is pressed into an electrolyte sheet, the thickness of the electrolyte sheet is 120~300μm, and the interior is a three-dimensional interconnected porous structure in which crystalline and amorphous phases are interlocked, with a closed pore rate of ≤6% and an open pore connectivity of ≥89%.
[0019] A sheet thickness of 120~300μm balances ion transport distance and mechanical strength: excessive thickness results in a long ion conduction path and increased polarization, while insufficient thickness leads to insufficient mechanical strength and susceptibility to lithium dendrite penetration. The three-dimensional interconnected structure of intercalated crystalline and amorphous phases forms a fully continuous ion-conducting network after pressing; an open-pore connectivity rate of ≥89% ensures continuous and uninterrupted ion pathways, while a closed-pore rate of ≤6% reduces ineffective porosity, lowers overall contact impedance, and improves the uniformity of ion conduction at low temperatures.
[0020] Secondly, this application also provides a method for preparing the above-mentioned solid electrolyte, comprising the following steps:
[0021] S1. Weigh lithium chloride, yttrium chloride, lanthanum chloride, zirconium chloride and zirconium dioxide raw materials according to the molar ratio of the general chemical formula. The raw materials are pre-vacuum dried to remove water.
[0022] S2. Place the raw materials into the ball mill jar, evacuate the jar, and then backfill with argon gas. Mix the materials at a low speed first, and then perform high-energy ball milling.
[0023] S3. Vacuum seal the ball-milled powder in a tube, perform low-temperature annealing, and then remove it for ice water cooling.
[0024] S4. The product after quenching is crushed, ground, and sieved to obtain solid electrolyte powder.
[0025] By adopting the above technical solution, mechanical solid-state synthesis is used to replace high-temperature melting and sintering, and cation doping and anion substitution are completed in situ at low temperature, avoiding the stoichiometric shift caused by high-temperature volatilization of halides. At the same time, amorphous nanocrystal-coated composite structures can be directly generated.
[0026] The combined process of vacuum low-temperature annealing and ice-water quenching can stabilize the crystal phase structure while quickly locking the size of the lattice lithium vacancies and octahedral cage cavity, preventing vacancy closure and cage cavity contraction during slow cooling, and maximizing the preservation of low-temperature ion conduction channels.
[0027] The entire process is prepared using a dry method, avoiding the low-temperature hydrolysis failure caused by residual solvents and moisture in the liquid phase method, thus ensuring the low-temperature stability and cycle life of the electrolyte.
[0028] Optionally, in S2, the argon pressure inside the ball mill is 0.12 MPa; the speed of low-speed mixing is 120 r / min and the duration is 90 min; the speed of high-energy ball milling is 450~650 r / min and the duration is 12~22 h.
[0029] Low-speed mixing enables homogeneous dispersion of raw materials, eliminates local agglomeration, ensures uniform distribution of subsequent doping elements, and avoids uneven conductivity caused by local component deviations. Limiting the rotation speed and time of high-energy ball milling provides sufficient mechanical force to induce solid-state reactions, achieving in-situ doping of the crystal lattice and generation of amorphous phases; at the same time, controlling the reaction intensity avoids excessive grain growth and imbalance of the amorphous phase ratio.
[0030] The slightly positive pressure environment of argon can isolate water vapor and oxygen, preventing the halide raw materials from hydrolyzing and oxidizing during ball milling, thus generating insulating impurities.
[0031] Optionally, in S3, the vacuum degree of the vacuum-sealed tube is ≤0.08Pa; the heating rate of the low-temperature annealing is 2.5℃ / min, the temperature is 280~360℃, and the holding time is 12~20h; after annealing, the furnace is cooled to 60℃, and then rapidly cooled to room temperature with ice water.
[0032] Low-temperature annealing at 280~360℃ can eliminate the internal stress introduced by ball milling, promote the ordering of crystal phases, and at the same time, it will not cause grain coarsening or the disappearance of amorphous layers, thus ensuring the stability of the multiphase structure; the high vacuum environment avoids the oxidation and hydrolysis of raw materials at high temperatures.
[0033] A gentle heating rate can reduce thermal stress shock and prevent powder particles from cracking and structural damage; the holding time ensures that the crystal phase is fully stable and defects are evenly distributed.
[0034] Rapid cooling with ice water can freeze lattice vacancies and cage size at high temperatures to room temperature, avoiding lithium vacancy recombination and cage shrinkage during slow cooling, thus preserving sufficient low-temperature ion transport sites.
[0035] Optionally, in S4, after crushing, the powder is ball-milled at 300 r / min for 4 h and passed through a 300-mesh sieve to obtain a finished powder with a median particle size D50 = 1.8 μm.
[0036] Low-speed, short-time grinding can break annealed blocks into uniform particle sizes without damaging the core-shell multiphase structure of individual particles. The uniform fine powder results in higher packing density and tighter interparticle contact during subsequent tableting, effectively reducing interfacial contact resistance after tableting. A 300-mesh sieve removes large particle agglomerates, preventing defects such as pinholes and cracks after compression molding, ensuring the density and insulation consistency of the electrolyte tablets.
[0037] Optionally, it also includes: S5, placing solid electrolyte powder into a mold and pressing it into an electrolyte sheet, with a pressure of 220~380MPa and a holding time of 5~12min.
[0038] A pressure range of 220~380MPa allows the powder particles to undergo sufficient plastic deformation and close adhesion, forming a continuous three-dimensional conductive network. Simultaneously, excessive pressure prevents the nanocrystalline structure of the particle core from breaking down or the amorphous coating from failing. Holding the pressure allows for sufficient powder densification, ensuring that the open-pore connectivity and closed-pore ratio meet standards, improving the mechanical strength and ion conduction uniformity of the electrolyte sheet, and reducing interfacial polarization at low temperatures.
[0039] Thirdly, this application also provides the application of the above-mentioned solid electrolyte in the field of all-solid-state lithium batteries. The all-solid-state lithium batteries are used in polar exploration power supply, high-altitude base station energy storage, military special power supply or low-temperature energy storage scenarios for new energy vehicles, with an operating temperature range of -60℃ to 75℃.
[0040] The solid electrolyte of this application exhibits stable high ionic conductivity, excellent interfacial stability, and safety performance over a wide temperature range of -60℃ to 75℃. It solves the problems of viscosity spikes, rapid capacity decay, flammability, and leakage of traditional liquid electrolytes at low temperatures, and overcomes the defects of conventional solid electrolytes such as high grain boundary impedance and easy phase transition at low temperatures. It can meet the long-term reliable power supply requirements of extreme low-temperature scenarios such as polar exploration, high-altitude base stations, and special power supply for military applications.
[0041] In summary, the technical solution of this application is achieved through La 3+ Large radius replacement of Y 3+ It expands the octahedral framework of metal halide, structurally suppressing low-temperature lattice contraction and preserving ion migration space; Zr 4+ Heterovalent substitution can artificially introduce controllable lithium vacancies, increasing lithium-ion transport sites; O 2- Partially replaces Cl - It can weaken lattice bond energy and reduce the activation energy of lithium-ion transition, thereby improving the low-temperature ion conductivity from the intrinsic level of the material. The nanocrystalline core provides long-range ordered high-speed ion channels in the bulk phase, while the outer amorphous phase acts as a low-resistance flexible conductive layer across grain boundaries, avoiding the common problem of grain boundary impedance surge at low temperatures in pure crystalline electrolytes, and achieving low-temperature high conductivity across the entire bulk-grain boundary domain. Detailed Implementation
[0042] The present application will be further described in detail below with reference to the embodiments.
[0043] Unless otherwise specified, the main components involved in the following embodiments of this application are all purchased from commercially available products. Specific Implementation
[0044] Example 1
[0045] This application prepares a low-temperature resistant halide solid electrolyte with the chemical formula Li. 3.15 Y 0.85 La 0.10 Zr 0.05 Cl5.9 4O 0.06 The specific preparation method is as follows.
[0046] Based on the preparation of 10g of finished product: anhydrous LiCl 4.12g, anhydrous YCl3 4.05g, anhydrous LaCl3 0.48g, anhydrous ZrCl4 0.22g, ZrO2 0.13g; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0047] The entire preparation process is carried out in an argon glove box with water ≤1ppm and oxygen ≤1ppm.
[0048] All raw materials were placed into a zirconia ball mill jar in a glove box with a ball-to-material mass ratio of 4.2:1. The jar was filled with argon gas to 0.12 MPa. The mixture was mixed at a low speed of 120 r / min for 90 min and then ball-milled at a high energy speed of 550 r / min for 18 h. The temperature rise inside the jar was controlled to be ≤45℃. The jar was cooled to room temperature and discharged under an argon atmosphere through a 200-mesh sieve to remove large agglomerated powder particles.
[0049] Take 8g of the sieved powder and place it into a quartz crucible. Then, load it into a quartz vacuum tube, evacuate it to 0.08Pa using a vacuum tube sealing machine, and then flame seal the quartz tube.
[0050] The room temperature was raised at a uniform rate of 2.5℃ / min until it reached 320℃, and then kept at that temperature for 16 hours.
[0051] After the natural furnace cools down to 60°C, the quartz tube is removed and rapidly cooled to room temperature with ice water.
[0052] The annealed block was removed from the broken quartz tube, ball-milled at 300 r / min for 4 h in an argon atmosphere, and passed through a 300-mesh sieve to obtain solid electrolyte powder with a median particle size D50 = 1.8 μm.
[0053] Take 0.18g of finished powder and place it into a Φ12mm hard alloy mold; pressurize it at a uniform speed to 300MPa, hold it for 8min, and release it at a rate of 5MPa / s; obtain a circular low-temperature resistant halide solid electrolyte sheet with a thickness of 180μm, a smooth surface, no cracks, and a closed-pore rate of ≤6%.
[0054] Example 2
[0055] This application prepares a low-temperature resistant halide solid electrolyte with the chemical formula Li. 3.08 Y 0.93 La 0.05 Zr 0.02 Cl 5.9 7O 0.03 The specific preparation method is as follows.
[0056] Based on the preparation of 10g of finished product: anhydrous LiCl 4.02g, anhydrous YCl3 5.59g, anhydrous LaCl3 0.38g, anhydrous ZrCl4 0.04g, ZrO2 0.06g; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0057] The entire preparation process is carried out in an argon glove box with water ≤1ppm and oxygen ≤1ppm.
[0058] All raw materials were placed into a zirconia ball mill jar in a glove box with a ball-to-material mass ratio of 4.2:1. The jar was filled with argon gas to 0.12 MPa. The mixture was mixed at a low speed of 120 r / min for 90 min and then ball-milled at a high energy speed of 550 r / min for 18 h. The temperature rise inside the jar was controlled to be ≤45℃. The jar was cooled to room temperature and discharged under an argon atmosphere through a 200-mesh sieve to remove large agglomerated powder particles.
[0059] Take 8g of the sieved powder and place it into a quartz crucible. Then, load it into a quartz vacuum tube, evacuate it to 0.08Pa using a vacuum tube sealing machine, and then flame seal the quartz tube.
[0060] The room temperature was raised at a uniform rate of 2.5℃ / min until it reached 320℃, and then kept at that temperature for 16 hours.
[0061] After the natural furnace cools down to 60°C, the quartz tube is removed and rapidly cooled to room temperature with ice water.
[0062] The annealed block was removed from the broken quartz tube, ball-milled at 300 r / min for 4 h in an argon atmosphere, and passed through a 300-mesh sieve to obtain solid electrolyte powder with a median particle size D50 = 1.8 μm.
[0063] Take 0.18g of finished powder and place it into a Φ12mm hard alloy mold; pressurize it at a uniform speed to 300MPa, hold it for 8min, and release it at a rate of 5MPa / s; obtain a circular low-temperature resistant halide solid electrolyte sheet with a thickness of 180μm, a smooth surface, no cracks, and a closed-pore rate of ≤6%.
[0064] Example 3
[0065] This application prepares a low-temperature resistant halide solid electrolyte with the chemical formula Li. 3.22 Y 0.77 La 0.15 Zr 0.08 Cl 5.9 0O 0.10 The specific preparation method is as follows.
[0066] Based on the preparation of 10g of finished product: anhydrous LiCl 4.14g, anhydrous YCl3 4.56g, anhydrous LaCl3 1.12g, anhydrous ZrCl4 0.21g, ZrO2 0.19g; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0067] The entire preparation process is carried out in an argon glove box with water ≤1ppm and oxygen ≤1ppm.
[0068] All raw materials were placed into a zirconia ball mill jar in a glove box with a ball-to-material mass ratio of 4.2:1. The jar was filled with argon gas to 0.12 MPa. The mixture was mixed at a low speed of 120 r / min for 90 min and then ball-milled at a high energy speed of 550 r / min for 18 h. The temperature rise inside the jar was controlled to be ≤45℃. The jar was cooled to room temperature and discharged under an argon atmosphere through a 200-mesh sieve to remove large agglomerated powder particles.
[0069] Take 8g of the sieved powder and place it into a quartz crucible. Then, load it into a quartz vacuum tube, evacuate it to 0.08Pa using a vacuum tube sealing machine, and then flame seal the quartz tube.
[0070] The room temperature was raised at a uniform rate of 2.5℃ / min until it reached 320℃, and then kept at that temperature for 16 hours.
[0071] After the natural furnace cools down to 60°C, the quartz tube is removed and rapidly cooled to room temperature with ice water.
[0072] The annealed block was removed from the broken quartz tube, ball-milled at 300 r / min for 4 h in an argon atmosphere, and passed through a 300-mesh sieve to obtain solid electrolyte powder with a median particle size D50 = 1.8 μm.
[0073] Take 0.18g of finished powder and place it into a Φ12mm hard alloy mold; pressurize it at a uniform speed to 300MPa, hold it for 8min, and release it at a rate of 5MPa / s; obtain a circular low-temperature resistant halide solid electrolyte sheet with a thickness of 180μm, a smooth surface, no cracks, and a closed-pore rate of ≤6%.
[0074] Example 4
[0075] This application prepares a low-temperature resistant halide solid electrolyte with the chemical formula Li. 3.15 Y 0.85 La 0.10 Zr 0.05 Cl 5.9 4O 0.06 The specific preparation method is as follows.
[0076] Based on the preparation of 10g of finished product: anhydrous LiCl 4.12g, anhydrous YCl3 4.05g, anhydrous LaCl3 0.48g, anhydrous ZrCl4 0.22g, ZrO2 0.13g; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0077] The entire preparation process is carried out in an argon glove box with water ≤1ppm and oxygen ≤1ppm.
[0078] All raw materials were placed into a zirconia ball mill jar in a glove box with a ball-to-material mass ratio of 4.2:1. The jar was filled with argon gas to 0.12 MPa. The mixture was mixed at a low speed of 120 r / min for 90 min and then ball-milled at a high energy speed of 450 r / min for 22 h. The temperature rise inside the jar was controlled to be ≤45℃. The jar was cooled to room temperature and discharged under an argon atmosphere through a 200-mesh sieve to remove large agglomerated powder particles.
[0079] Take 8g of the sieved powder and place it into a quartz crucible. Then, load it into a quartz vacuum tube, evacuate it to 0.08Pa using a vacuum tube sealing machine, and then flame seal the quartz tube.
[0080] The room temperature was raised at a uniform rate of 2.5℃ / min until it reached 280℃, and then kept at that temperature for 20 hours.
[0081] After the natural furnace cools down to 60°C, the quartz tube is removed and rapidly cooled to room temperature with ice water.
[0082] The annealed block was removed from the broken quartz tube, ball-milled at 300 r / min for 4 h in an argon atmosphere, and passed through a 300-mesh sieve to obtain solid electrolyte powder with a median particle size D50 = 1.8 μm.
[0083] Take 0.18g of finished powder and place it into a Φ12mm hard alloy mold; pressurize it at a uniform speed to 220MPa, hold it for 12min, and release it at a rate of 5MPa / s; to obtain a circular low-temperature resistant halide solid electrolyte sheet with a thickness of 180μm, a smooth surface, no cracks, and a closed-cell rate of ≤6%.
[0084] Comparative Example 1
[0085] This comparative example provides a solid electrolyte with the chemical formula Li3YCl6. Anhydrous LiCl and anhydrous YCl3 are weighed at a molar ratio of 3:1.
[0086] After mixing, the mixture was ball-milled at 550 r / min for 18 h, annealed at 500℃ for 12 h, and then naturally cooled in the furnace; the remaining environment and tableting conditions were the same as in Example 1.
[0087] The product has a pure crystalline phase structure with no amorphous coating layer and a grain size of approximately 200 nm.
[0088] Comparative Example 2
[0089] This comparative example provides a solid electrolyte, doped only with La / Zr cations and without O anion modification. Its chemical formula is Li. 3.15 Y 0.85 La 0.10 Zr 0.05 Cl 6.1 .
[0090] Based on the preparation of 10g of finished product: 3.98g of anhydrous LiCl, 4.94g of anhydrous YCl3, 0.73g of anhydrous LaCl3, and 0.35g of anhydrous ZrCl4; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0091] After mixing, the mixture was ball-milled at 550 r / min for 18 h, annealed at 500℃ for 12 h, and then naturally cooled in the furnace; the remaining environment and tableting conditions were the same as in Example 1.
[0092] The product structure is a pure crystalline phase doped structure with no amorphous coating layer.
[0093] Comparative Example 3
[0094] This comparative example prepares a low-temperature resistant halide solid electrolyte with the chemical formula Li. 3.15 Y 0.85 La 0.10 Zr 0.05 Cl 5.9 4O 0.06 The specific preparation method is as follows.
[0095] Based on the preparation of 10g of finished product: anhydrous LiCl 4.12g, anhydrous YCl3 4.05g, anhydrous LaCl3 0.48g, anhydrous ZrCl4 0.22g, ZrO2 0.13g; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0096] The entire preparation process is carried out in an argon glove box with water ≤1ppm and oxygen ≤1ppm.
[0097] All raw materials were placed into a zirconia ball mill jar in a glove box with a ball-to-material mass ratio of 4.2:1. The jar was filled with argon gas to 0.12 MPa. The mixture was mixed at a low speed of 120 r / min for 90 min and then ball-milled at a high energy speed of 550 r / min for 18 h. The temperature rise inside the jar was controlled to be ≤45℃. The jar was cooled to room temperature and discharged under an argon atmosphere through a 200-mesh sieve to remove large agglomerated powder particles.
[0098] Take 8g of the sieved powder and place it into a quartz crucible. Then, load it into a quartz vacuum tube, evacuate it to 0.08Pa using a vacuum tube sealing machine, and then flame seal the quartz tube.
[0099] The room temperature was raised at a uniform rate of 2.5℃ / min until it reached 450℃, and then kept at that temperature for 12 hours.
[0100] After annealing, the furnace is allowed to cool naturally to room temperature without being opened or subjected to quenching.
[0101] The annealed block was removed from the broken quartz tube, ball-milled at 300 r / min for 4 h in an argon atmosphere, and passed through a 300-mesh sieve to obtain solid electrolyte powder with a median particle size D50 = 2.2 μm.
[0102] Take 0.18g of the finished powder and place it into a Φ12mm cemented carbide mold; pressurize it at a uniform speed to 300MPa, hold it for 8min, and release it at a rate of 5MPa / s to obtain a solid electrolyte sheet.
[0103] The product structure is dominated by pure crystalline phase, with a low proportion of amorphous phase and a significantly reduced lithium vacancy concentration.
[0104] Comparative Example 4
[0105] This comparative example provides a polymer composite modified halide electrolyte, which uses pure Li3YCl6 powder from Comparative Example 1 combined with PEO polymer. The specific preparation method is as follows.
[0106] Based on the preparation of 10g of pure inorganic powder: anhydrous LiCl 3.94g, anhydrous YCl3 6.06g; all raw materials have a purity ≥99.99% and a water content ≤20ppm, and are vacuum dried at 80℃ for 12h in advance.
[0107] The entire preparation process is carried out in an argon glove box with water ≤1ppm and oxygen ≤1ppm.
[0108] All raw materials were placed into a zirconia ball mill jar in a glove box with a ball-to-material mass ratio of 4.2:1. The jar was filled with argon gas to 0.12 MPa. The mixture was mixed at a low speed of 120 r / min for 90 min and then ball-milled at a high energy speed of 550 r / min for 18 h. The temperature rise inside the jar was controlled to be ≤45℃. The jar was cooled to room temperature and discharged under an argon atmosphere through a 200-mesh sieve to remove large agglomerated powder particles.
[0109] After sieving, the powder is placed into a quartz crucible, a quartz vacuum tube is inserted, a vacuum sealing machine is used to evacuate the quartz tube to 0.08 Pa, and the quartz tube is then flame-sealed.
[0110] The room temperature was raised at a uniform rate of 2.5℃ / min until it reached 500℃, and then kept at that temperature for 12 hours.
[0111] After annealing, the quartz tube was naturally cooled to room temperature in the furnace and then removed. The quartz tube was broken into pieces and passed through a 300-mesh sieve under argon atmosphere to obtain Li3YCl6 electrolyte powder.
[0112] Based on a total mass of 10g of composite electrolyte: weigh 7.00g of the above Li3YCl6 powder and 3.00g of PEO, place them in a zirconia ball mill jar, and dry mix at 150r / min for 2h under an argon atmosphere to obtain a uniformly dispersed mixed powder.
[0113] Take 0.26g of mixed powder and place it into a Φ12mm hard alloy mold. Use hot pressing to form the mold: heat the mold to 60℃, press it at a uniform speed to 200MPa, hold the pressure for 10min, release the pressure and then cool it naturally to room temperature to obtain polymer composite halide electrolyte sheet.
[0114] All samples were pressed into electrolyte sheets with a diameter of 12 mm and a thickness of 180 ± 5 μm under the same testing conditions. The samples were then tested, and the results are shown in Table 1.
[0115]
[0116] Comparative Examples 1, 2, and 1 show that cation doping alone can improve conductivity to a certain extent, but cannot reduce the ion transition energy barrier; introducing O 2- After anion modification, the lattice bond energy is weakened, and the activation energy for migration decreases from 0.41 eV to 0.27 eV. Combined with La... 3+ The lattice expansion effect effectively solves the problem of low-temperature lattice shrinkage and improves ionic conductivity.
[0117] Comparative Example 3 and Example 1 show that, with the same composition, the sample without a multiphase structure exhibits a significantly greater decrease in low-temperature conductivity. The amorphous coating layer eliminates the grain boundary conduction barrier, preventing a sharp increase in grain boundary impedance at low temperatures in pure crystalline electrolytes, thus achieving low-temperature conductivity across the entire bulk-grain boundary domain.
[0118] As can be seen from Comparative Example 3 and Example 1, high-temperature natural cooling will lead to lithium vacancy recombination, cage shrinkage, and a significant decrease in low-temperature performance. The ice-water quenching process used in this application can freeze the vacancies and cage size at high temperatures, maximize the preservation of low-temperature ion transport channels, and ensure no phase change in a wide temperature range.
[0119] Comparative Example 4 and Example 1 show that when polymer composite systems crystallize at low temperatures, ion channels close, resulting in even worse low-temperature performance. The dry, anhydrous, and oxygen-free process of this invention avoids solvent residue and hydrolysis side reactions. After long-term standing at low temperatures, the conductivity retention rate is far greater than that of existing systems, and the cycle stability is relatively better.
[0120] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.
Claims
1. A low-temperature resistant halide solid electrolyte, characterized in that, The solid electrolyte is composed of a nanocrystalline core and an amorphous phase coated on the outer surface of the nanocrystalline core: the nanocrystalline core is a mixed metallic chloride octahedral crystal phase of Y, La, and Zr, and the amorphous phase is a disordered Li-Cl-O phase. The general chemical formula is: Li 3+a Y 1-x-z La x Zr z Cl 6-b O b ; Where: a = 0.08~0.22; x=0.05~0.15; z=0.02~0.08; b=0.03~0.10。 2. The solid electrolyte according to claim 1, characterized in that, The chemical formula of the solid electrolyte is: Li 3.1 5Y 0.85 La 0.10 Zr 0.05 Cl 5.94 O 0.06 .
3. The solid electrolyte according to claim 1, characterized in that, The nanocrystalline core has a grain size of 20~40nm and a unit cell space group of P63 / mmc; the coating thickness of the amorphous phase is 3~8nm.
4. The solid electrolyte according to claim 1, characterized in that, After the solid electrolyte is pressed into an electrolyte sheet, the thickness of the electrolyte sheet is 120~300μm. The interior is a three-dimensional interconnected porous structure in which crystalline and amorphous phases are interlocked, with a closed pore rate of ≤6% and an open pore connectivity of ≥89%.
5. A method for preparing a solid electrolyte according to claim 1, characterized in that, Includes the following steps: S1. Weigh lithium chloride, yttrium chloride, lanthanum chloride, zirconium chloride and zirconium dioxide raw materials according to the molar ratio of the general chemical formula. The raw materials are pre-vacuum dried to remove water. S2. Place the raw materials into the ball mill jar, evacuate the jar, and then backfill with argon gas. Mix the materials at a low speed first, and then perform high-energy ball milling. S3. Vacuum seal the ball-milled powder in a tube, perform low-temperature annealing, and then remove it for ice water cooling. S4. The product after quenching is crushed, ground, and sieved to obtain solid electrolyte powder.
6. The preparation method according to claim 5, characterized in that, In S2, the argon pressure inside the ball mill jar is 0.12 MPa; the speed of low-speed mixing is 120 r / min for 90 min; and the speed of high-energy ball milling is 450~650 r / min for 12~22 h.
7. The preparation method according to claim 5, characterized in that, In S3, the vacuum degree of the vacuum-sealed tube is ≤0.08Pa; the heating rate of the low-temperature annealing is 2.5℃ / min, the temperature is 280~360℃, and the holding time is 12~20h; after annealing, the furnace is cooled to 60℃, and then rapidly cooled to room temperature with ice water.
8. The preparation method according to claim 5, characterized in that, In S4, after crushing, the powder is ball-milled at 300 r / min for 4 h and passed through a 300 mesh sieve to obtain a finished powder with a median particle size D50 = 1.8 μm.
9. The preparation method according to claim 5, characterized in that, It also includes S5, placing solid electrolyte powder into a mold and pressing it into an electrolyte sheet, with a pressure of 220~380MPa and a holding time of 5~12min.
10. An application of the solid electrolyte of claim 1 in the field of all-solid-state lithium batteries, wherein the all-solid-state lithium battery is used in polar exploration power supply, high-altitude base station energy storage, military special power supply or low-temperature energy storage scenarios for new energy vehicles, and the operating temperature range is -60℃ to 75℃.