A composite solid electrolyte membrane and its preparation method, and a solid-state lithium battery
By employing a bidirectional continuous gradient distribution of ternary components and a three-dimensional porous framework filling structure in the solid electrolyte membrane, the problems of high interfacial impedance and easy delamination failure in existing solid electrolyte systems are solved, achieving performance improvement of all-solid-state batteries with high conductivity, wide electrochemical window and long cycle life.
Patent Information
- Application Number
- CN202611466621.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing solid electrolyte systems present a trade-off between high conductivity, wide electrochemical window, mechanical strength, and interfacial stability, leading to problems such as high interfacial impedance, easy delamination failure, and difficulty in suppressing lithium dendrites.
By employing a bidirectional continuous gradient distribution of ternary components and a three-dimensional porous framework filling structure, and through the composite of halides, sulfides and anti-reduction components, antioxidant, high-conductivity and anti-reduction functional zones are formed. Combined with a self-healing polymer framework and lithium-affinity precursor, low-impedance ion transport and mechanical integrity without discrete interfaces are achieved.
It achieves a synergistic improvement in wide electrochemical window, low interfacial impedance, high critical current density and long cycle life, and solves the performance bottleneck of electrolyte membrane in all-solid-state batteries.
Smart Images

Figure CN123120848A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid-state secondary battery technology, specifically a composite solid-state electrolyte membrane and its preparation method, and a solid-state lithium battery. Background Technology
[0002] With the increasing demands for battery energy density and safety in the electric vehicle and energy storage sectors, all-solid-state lithium batteries, which use non-flammable solid electrolytes and are matched with high-specific-capacity lithium metal anodes (theoretical specific capacity 3860 mAh / g) and high-voltage cathodes (such as high-nickel ternary NMC811, lithium-rich manganese-based, etc.), are considered an important direction for the next generation of batteries.
[0003] However, existing solid-state electrolyte systems all have inherent limitations that are difficult to overcome individually. Sulfide electrolytes (such as Li6PS5Cl, silver-germanium sulfide, Li...) 10 GeP2S 12 High ionic conductivity at room temperature (10) -3 ~10 -2 S / cm), soft texture, easy to cold press and mold, but its electrochemical window is narrow: it is easily reduced by lithium metal at low potentials and at high potentials (>2.5 V vs. Li / Li). + It is easily oxidized by the positive electrode and releases H2S upon contact with water. Oxide electrolytes (such as garnet-type Li7La3Zr2O) 12 Lithium sulfide (LLZO) electrolytes are relatively stable to lithium metal and high voltage, and have a wide electrochemical window. However, they are brittle and hard, and lithium dendrites can easily penetrate the grain boundaries. Furthermore, their contact with the electrode is a rigid-rigid point contact with extremely high interfacial impedance, requiring high-temperature sintering and making thin-film and large-scale production difficult. Halogen electrolytes (such as Li3InCl6, Li2ZrCl6, and Li3YCl6) have excellent oxidation resistance and good compatibility with high-voltage cathodes, but poor reduction stability to lithium metal, and cannot directly contact the lithium anode when used alone. Polymer electrolytes (such as PEO-based electrolytes) have good flexibility and good interfacial contact, but low room-temperature conductivity, a narrow electrochemical window, and insufficient mechanical strength to suppress lithium dendrites.
[0004] To achieve the aforementioned performance, existing technologies often employ discrete multilayer structures, where different electrolytes are deposited and stacked on the positive, intermediate, and negative electrode sides. However, this approach presents three major new problems: First, the internal heterogeneous interface impedance is high, with clear physical interfaces forming between the discrete layers. Ions must cross multiple hard interfaces, leading to superimposed interfacial contact resistance and an increase in overall impedance. Second, delamination failure is prone to occur during charge-discharge cycles due to the mismatch between the thermal expansion coefficients and volume changes of different materials, resulting in stress concentration at the interfaces during cycling, leading to cracking and delamination. Third, lithium dendrite formation on the negative electrode side remains difficult to suppress, lacking active control over lithium deposition morphology, and the critical current density (CCD) is generally below 1 mA / cm². 2 It is difficult to meet the requirements of fast charging and high surface capacity. Summary of the Invention
[0005] In view of this, the present invention provides a composite solid electrolyte membrane and its preparation method, as well as a solid lithium battery. Through the integrated structure of bidirectional continuous gradient distribution of ternary components and three-dimensional porous framework filling, the all-solid electrolyte membrane simultaneously achieves functional partitioning of the positive electrode side for anti-oxidation, high bulk conductivity, and negative electrode side for anti-reduction, as well as low-impedance ion transport without discrete interfaces, and ensures the mechanical integrity of the membrane with the help of framework support.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: In a first aspect, the present invention discloses a composite solid electrolyte membrane, which is divided along its thickness direction into a positive electrode facing region, an ion-conducting main region, and a negative electrode facing region with continuous component transition, wherein: The electrolyte membrane is composed of a halide solid electrolyte component, a sulfide solid electrolyte component, and an anti-reduction component. The electrolyte membrane is permeated with a three-dimensional continuous porous polymer nanofiber framework, and the halide solid electrolyte component, sulfide solid electrolyte component and anti-reduction component fill the pores of the nanofiber framework.
[0007] As a further aspect of the present invention: the mass fraction of the halide component decreases monotonically from the positive electrode region to the negative electrode region along the thickness direction of the composite solid electrolyte membrane; the mass fraction of the sulfide component reaches its maximum value in the ion conduction host region; and the mass fraction of the anti-reduction component increases monotonically from the positive electrode region to the negative electrode region along the thickness direction of the composite solid electrolyte membrane.
[0008] As a further aspect of the present invention: the anti-reduction component is at least one of a nitrogen-containing component and a fluorine-containing component.
[0009] As a further aspect of the present invention: a lithium-affinity metal or its compound nanoparticle precursor is dispersed in the negative electrode facing region, wherein the lithium-affinity metal is selected from at least one of Mg, Ag, Zn, Au, Sn, Al, and Bi. The nanoparticle precursor is used to generate an interfacial phase with both ion-conducting and electronically insulating properties in situ upon contact with lithium metal.
[0010] As a further aspect of the present invention: the three-dimensional porous polymer nanofiber framework comprises at least one self-healing polymer having dynamic reversible bonds; the self-healing polymer contains at least one of borate ester dynamic bonds, imine bonds, or a reversible hydrogen bond network.
[0011] As a further aspect of the present invention: the halide solid electrolyte component is selected from at least one of Li3InCl6, Li2ZrCl6, Li3YCl6, Li3YBr6, and Li3ScCl6; and / or, The sulfide solid electrolyte component is selected from Li6PS5Cl, Li6PS5Br, and Li 10 GeP2S 12 Li7P3S 11 At least one of Li3PS4; and / or, The anti-reduction component is selected from at least one of Li3N, Li3N-doped silver-germanium sulfide, LiF, and Li2O-modified sulfides.
[0012] As a further aspect of the present invention: the anti-reduction component in the negative electrode facing region is a composite of Li3N and an electronic insulating component, wherein the electronic insulating component is selected from at least one of LiF and Li2O modified sulfides, and the overall electronic conductivity of the negative electrode facing region is less than 10. -8 S / cm. Due to the high electronic conductivity of Li3N (approximately 10 S / cm). -3 ~10 -4 If used alone as the negative electrode facing region, it would form a continuous electronic pathway within the film, triggering continuous reduction and self-discharge of lithium metal through this pathway. Therefore, this invention combines Li3N in the negative electrode facing region with electronically insulating LiF (and / / or Li2O-modified sulfides). LiF forms an electron-blocking phase between the ion-conducting phases of Li3N; simultaneously, the dispersed lithium-affinity metal nanoparticle precursor transforms in situ into an alloy interface phase with both ion-conducting and electronically insulating properties upon contact with lithium, further cutting off the electron permeation path. The synergistic effect of these two factors allows the negative electrode facing region to maintain high lithium-ion conductivity while reducing electronic conductivity to 10. -8 With a value below S / cm, self-discharge is suppressed and the negative electrode interface is stabilized.
[0013] As a further aspect of the present invention: the reduction potential of the negative electrode facing region to lithium metal is less than 0.1 V vs. Li / Li + Given that the equilibrium potential for lithium metal deposition / stripping is 0 V vs. Li / Li + The negative electrode facing material must maintain electrochemical stability in a strong reducing environment close to 0V, that is, its reduction decomposition potential must be below 0.1 V; if it is higher than this value, the material will be continuously reduced by lithium, resulting in increased interfacial impedance and uneven lithium deposition.
[0014] As a further aspect of the present invention: the three-dimensional porous polymer nanofiber skeleton is prepared by electrospinning, with a fiber diameter of 50-800 nm and a porosity of 60%-90%.
[0015] As a further aspect of the present invention: the total thickness of the composite solid electrolyte membrane is 15-80 μm, wherein the thickness of the positive electrode facing region is 5-30 μm, the thickness of the ion conduction main region is 5-40 μm, and the thickness of the negative electrode facing region is 3-20 μm.
[0016] As a further aspect of the present invention: the composite solid electrolyte membrane has an ionic conductivity of 1×10⁻⁶ at 25°C. -3 ~1×10 -2 S / cm, and the interfacial impedance with the lithium metal anode is less than 15 Ω·cm. 2 The critical current density is not less than 3 mA / cm². 2 .
[0017] Secondly, the present invention discloses a method for preparing a composite solid electrolyte membrane as described above, comprising the following steps: S1: Prepare halide electrolyte slurry, sulfide electrolyte slurry and anti-reduction component slurry respectively, and add lithium affinity metal nanoparticle precursor to the anti-reduction component slurry; S2: Provides a three-dimensional porous polymer nanofiber framework and places it on a cast substrate; S3: The halide electrolyte slurry, sulfide electrolyte slurry and anti-reduction component slurry are mixed in real time according to a continuously varying ratio along the film thickness direction, and then co-cast and impregnated into the pores of the nanofiber skeleton to form a continuous component gradient skeleton composite filled with the mixed slurry. S4: The skeleton composite filled with the mixed slurry is subjected to solvent evaporation treatment to obtain a dry gradient composite membrane; S5: The gradient composite membrane is subjected to thermal and pressure densification treatment under an inert atmosphere to obtain the integrated composite solid electrolyte membrane.
[0018] As a further aspect of the present invention: In step S3, a multi-channel gradient ratio pump is used to achieve co-cast slurry. By controlling the instantaneous flow ratio of each channel pump, the mass fraction of each component is made to have a linear or S-shaped continuous transition curve along the thickness direction, and the mass fraction change rate of adjacent micro-areas is not greater than 5% / μm.
[0019] As a further aspect of the present invention: the casting speed of the co-casting process is 0.3 to 0.8 m / min, the doctor blade gap is 30 to 120 μm, and the substrate temperature is 20 to 40 °C.
[0020] Furthermore, the solid content of the halide slurry, sulfide slurry, and anti-reduction component slurry is 20-35 wt%; the pressure of the warm-press densification treatment is 100-500 MPa, and the temperature is 80-200 ℃; the halide slurry, sulfide slurry, and anti-reduction component slurry are each independently dispersed in an inert organic solvent and a polymer binder is added to each.
[0021] Thirdly, the present invention discloses a solid-state lithium battery, comprising a positive electrode, a negative electrode, and a solid electrolyte located between the positive electrode and the negative electrode, wherein the solid electrolyte is the aforementioned composite solid electrolyte membrane.
[0022] Compared with the prior art, the beneficial effects of the present invention are: This invention utilizes a bidirectional continuous gradient distribution of halide, sulfide, and anti-reduction components along the film thickness direction. This allows the same electrolyte membrane to spontaneously form functional zones for oxidation resistance, high conductivity, and anti-reduction on the positive, middle, and negative sides, respectively. Furthermore, because the components transition continuously rather than physically stacked, internal discrete interfaces are eliminated, significantly reducing interfacial resistance to ion transport within the membrane and mitigating the risk of delamination failure due to differences in thermal expansion or volume changes between different functional layers. A three-dimensional continuous porous polymer nanofiber framework runs throughout the membrane, providing flexible support for the brittle inorganic electrolyte, inhibiting crack propagation, and ensuring the structural integrity of the membrane during cycling. Meanwhile, the lithium affinity precursor pre-placed on the negative side utilizes the anti-reduction component environment enriched in this region of the gradient distribution to form a stable interfacial protective layer in situ upon contact with lithium metal. The chemical gradient ensures intrinsic compatibility across regions, the framework ensures mechanical integrity, and the precursor ensures interfacial dynamic stability. These three elements are interdependent in function: the gradient provides a basis for the compositional distribution of the framework, the framework provides a confined reaction space for precursor conversion, and the precursor conversion products further suppress the mechanical impact of lithium dendrites on the framework. Thus, at the full-cell level, a synergistic improvement in wide electrochemical window, low interfacial impedance, high critical current density, and long cycle life is achieved simultaneously. Attached Figure Description
[0023] Figure 1 This is a continuous gradient distribution curve of each component along the thickness direction in the solid electrolyte membrane of Embodiment 1 of the present invention; Figure 2 This is a schematic diagram of the multi-channel gradient co-casting and skeleton impregnation process. Detailed Implementation
[0024] To facilitate understanding of the present invention, a more comprehensive description will be given below with reference to specific embodiments. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a more thorough and complete understanding of the disclosure of the present invention.
[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. Unless otherwise specified, all operations described below are performed in an argon glove box or drying room with a dew point below -60 °C.
[0026] In addition, unless otherwise specified, the preparation processes in the following embodiments are all conventional methods in the prior art, and therefore will not be described in detail; unless otherwise specified, the parts in the following embodiments refer to parts by weight.
[0027] The preparation method of the self-healing polymer (PVA-boronate network) containing dynamic borate bonds used in Example 1 is as follows: (1) Weigh the raw materials: 10 parts of polyvinyl alcohol (PVA, degree of alcoholysis 98%, degree of polymerization about 1700); 1 part of sodium tetraborate decahydrate (borax, Na2B4O7·10H2O); 115 parts of deionized water.
[0028] (2) Add 10 parts of PVA to 100 parts of deionized water and stir mechanically at 90 °C for 2 h until completely dissolved to obtain a transparent PVA aqueous solution (about 9 wt%). Cool to room temperature.
[0029] (3) Dissolve 1 part of borax in 15 parts of deionized water to prepare a borax aqueous solution.
[0030] (4) Under vigorous stirring (500 r / min), the borax aqueous solution was slowly added dropwise to the PVA aqueous solution. The mass ratio of PVA to borax was 10:1. After the addition was complete, the mixture was stirred at 60°C for 2 h to allow the 1,2-diol side chain of PVA to undergo esterification crosslinking with borate to form a dynamic covalent network of borate ester (B–O).
[0031] (5) Dialyze the product in deionized water for 48 h (changing the water every 8 h) to remove unreacted borax, then Freeze-dry at 50 °C for 48 h to obtain a white, spongy PVA-boronate network.
[0032] The preparation method of the self-healing polymer (polyether diamine-terephthalaldehyde polyimide) containing dynamic imine bonds used in Example 2 is as follows: (1) Weigh the raw materials: 100 parts of polyether diamine (Jeffamine D2000, amino-terminated polypropylene glycol, Mn≈2000); 10 parts of terephthalaldehyde (the molar ratio of polyether diamine to terephthalaldehyde is about 1:1); 220 parts of anhydrous tetrahydrofuran (THF).
[0033] (2) Under nitrogen protection, 10 parts of terephthalaldehyde were dissolved in 120 parts of anhydrous THF and stirred at room temperature until clear to obtain an aldehyde solution.
[0034] (3) Dissolve 100 parts of polyether diamine in 100 parts of anhydrous THF and slowly add it dropwise into the above aldehyde solution. Stir at room temperature (25 °C) for 6 h. The terminal amino group and the aldehyde group undergo condensation (Schiff base reaction) to generate imine bonds (–CH=N–), forming a polyimide dynamic network. The solution can be observed to gradually turn into a light yellow viscous state.
[0035] (4) Most of the THF was removed by rotary evaporation under reduced pressure at 40 °C, and then the solvent and water generated by condensation were completely removed by vacuum drying at 50 °C for 12 h, to obtain light yellow elastomer polyether diamine-terephthalaldehyde polyimide.
[0036] The preparation method of the self-healing polymer (UPy-terminated polycarbonate / polyether) containing a dynamic hydrogen bond network used in Example 3 is as follows: (1) Weigh the raw materials: Step 1 (Synthesis of UPy-NCO intermediate): 13 parts of 2-amino-4-hydroxy-6-methylpyrimidine; 44 parts of isophorone diisocyanate (IPDI); 150 parts of anhydrous chloroform.
[0037] Step 2 (end-capping): 100 parts of polytetrahydrofuran diol (PTMEG, Mn≈2000); 0.1 parts of dibutyltin dilaurate (catalyst); 200 parts of anhydrous chloroform.
[0038] (2) Synthesis of UPy-isocyanate intermediate: Under nitrogen atmosphere, 13 parts of 2-amino-4-hydroxy-6-methylpyrimidine were added to 44 parts of excess IPDI, and stirred at 100 °C for 16 h. The pyrimidinone amino group reacted with the isocyanate at one end of IPDI to generate a ureidopyrimidinone intermediate (UPy-NCO) containing free –NCO. After cooling, excess IPDI was removed by washing with anhydrous n-hexane, and the product was dried under vacuum to obtain a white UPy-NCO solid.
[0039] (3) End-hydroxyl capping: Dissolve 100 parts of PTMEG in 200 parts of anhydrous chloroform, add 0.1 parts of catalyst, and then add UPy-NCO (at a PTMEG end-hydroxyl:NCO molar ratio of 1:1, approximately equivalent to the product of the previous step); reflux and stir at 60 °C for 8 h to allow the PTMEG end-hydroxyl group to react with UPy-NCO, thereby capping the UPy quadruple hydrogen bond unit at both ends of the polyether chain.
[0040] (4) The reaction solution was poured into n-hexane to precipitate, filtered, and dried under vacuum at 50 °C for 24 h to obtain UPy end-capped self-healing polymer (elastic solid) containing a quadruple hydrogen bond network.
[0041] Example 1 S1. Preparation of three-dimensional self-healing framework: 3 parts of PVA-boronate network and 7 parts of polyamic acid were dissolved in 90 parts of N,N-dimethylformamide (DMF) and mixed evenly. The mixture was electrospun (voltage 18 kV, receiving distance 15 cm) to obtain a three-dimensional porous nanofiber framework with a fiber diameter of about 300 nm, a porosity of about 82%, and a thickness of about 50 μm. The framework was then imidized at 280℃ for 2 h for later use.
[0042] S2, Gradient Slurry Preparation: Halogenated slurry: Weigh Li2ZrCl6, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP) and nitrile rubber (NBR), mix them in a mass ratio of 93:3:4, add anhydrous toluene / isobutyl isobutyrate (mass ratio 1:1) to form a slurry with a total solid content of 27wt%, and then mix it with planetary stirring for 4 h and ball milling for 2 h before use.
[0043] Sulfide slurry: Weigh Li6PS5Cl and PVDF-HFP, mix them at a mass ratio of 95:5, add anhydrous toluene / ethyl acetate (mass ratio 3:2) to form a slurry with a total solid content of 30 wt%, and set aside after planetary stirring for 5 h and vacuum degassing for 30 min.
[0044] Anti-reduction component slurry: Li3N, LiF, PVA-boronate network, and Ag nanoparticles were weighed and mixed in a mass ratio of 46:44:5:5, wherein the average particle size of the Ag nanoparticles was approximately 20 nm. The Ag nanoparticles were first ultrasonically dispersed in anhydrous acetonitrile in 5 times their mass for 20 min. Then, Li3N and LiF powders and the PVA-boronate network were added, followed by anhydrous acetonitrile / DMF (mass ratio 1:1) to form a slurry with a total solids content of 24 wt%. After magnetic stirring for 4 h, the slurry was degassed and ready for use.
[0045] S3. Lay the three-dimensional porous skeleton flat on an inert substrate, and use a three-channel precision metering pump and a gradient co-casting device to cast regions A, B, and C (e.g., Figure 1(As shown) The slurry was simultaneously cast and impregnated into the pores of the substrate. The mass ratio of each component along the film thickness direction changed continuously according to the following program: Positive electrode side initial end (0–10 μm): Li₂ZrCl₆: Li₆PS₅Cl: C region component = 80:20:0; Transition zone I (10–22 μm): continuously transitioning to 45:50:5; Middle zone (22–45 μm): continuously transitioning to 10:85:5; Negative electrode side end (45–55 μm): continuously transitioning to 0:25:75. The casting parameters were: casting speed 0.40 m / min; doctor blade gap 95 μm; substrate temperature 28 ℃; single channel flow rate 0.5–1.2 mL / min; gradient change mode adopted S-type continuous program control; the component change rate between adjacent micro-regions ≤5% / μm. After film formation, the film is first allowed to stand at room temperature for 30 minutes, then pre-dried at 40°C for 2 hours, and finally vacuum dried at 60°C for 8 hours to obtain a pre-dried film.
[0046] S4. The pre-dried membrane is pre-pressed at 150 ℃ and 80 MPa for 5 min under Ar atmosphere, and then pressed at 300 MPa for 10 min. After hot pressing, the pressure is maintained and cooled to 40 ℃ before depressurization to obtain an integrated continuous gradient electrolyte membrane with a total thickness of about 55 μm (A region about 22 μm, B region about 23 μm, C region about 10 μm).
[0047] S5. This film is used to assemble an all-solid-state lithium metal battery. The positive electrode is prepared from NMC811, Li2ZrCl6, Super P, and PTFE in a mass ratio of 72:18:5:5, with a positive electrode surface capacity of 4.2 mAh / cm². 2 The negative electrode is a 50 μm thick lithium metal foil. A stacking pressure of 10 MPa is applied during assembly. The test temperature is 25 °C, and the voltage window is 2.8–4.3 V.
[0048] It should be noted that the aforementioned gradient co-casting process falls under the category of continuous co-casting molding of functionally graded materials. The key lies in transforming the ratio control of the three slurries from the traditional offline, portioned preparation and layer-by-layer coating to online, real-time mixing and single-port co-casting. Specifically, as... Figure 2As shown, halide slurry, sulfide slurry, and anti-reduction component slurry are respectively loaded into three independent precision metering pumps. The three slurries are transported through pipelines to the same static mixer or micro-mixing chamber for confluence. After thorough mixing, they flow out from a single casting blade nozzle. The instantaneous flow rate ratio f1(t):f2(t):f3(t) of the three pumps is adjusted in real time by a programmable logic controller, so that the instantaneous composition of the slurry at the mixing chamber outlet changes continuously with time. Since the casting substrate advances at a constant linear velocity, the position of the casting head relative to the substrate is proportional to time. Therefore, the continuous change of slurry composition with time is recorded as a continuous composition gradient along the film thickness direction—the time axis is directly mapped to the thickness axis. When the flow rate ratio changes linearly with time, the resulting composition-thickness curve is a straight line segment; when the flow rate ratio changes according to a sigmoid or logistic function, the resulting composition-thickness curve is a smooth S-shape with a small slope at both ends, which can avoid internal stress on both sides of the film due to excessively rapid composition changes. Figure 1 As shown, in the integrated solid electrolyte membrane obtained using the above-mentioned S-type continuous program control, the mass fraction of the halide component decreases smoothly and continuously from the positive electrode side to the negative electrode side; the sulfide component reaches its peak in the ion conduction main region and then decreases smoothly to both sides; and the mass fraction of the nitrogen-containing / fluorine-containing anti-reduction component increases smoothly and continuously from the positive electrode side to the negative electrode side. All three curves are continuous and smooth curves, without step-like jumps or plateau regions, proving that the rate of change of mass fraction of each component between adjacent micro-regions is continuous and there are no discrete physical interfaces with abrupt component changes. It should be particularly noted that the present invention adopts a real-time mixing and single-port co-casting method, that is, the three slurries are combined into a single slurry with a continuously changing instantaneous ratio in the mixing chamber, and then coated and impregnated into the pores of the nanofiber skeleton in one go through a single doctor blade, rather than stacking and casting three layers of slurries with different ratios sequentially. This process feature results in an electrolyte membrane without interlayer physical interfaces in the thickness direction, fundamentally different from the traditional discrete multilayer laminated structure.
[0049] In the following examples and comparative examples, the casting process was carried out in accordance with the method described in Example 1. Only the specific parameters such as casting speed, doctor blade gap, and gradient change method were adjusted according to the target film thickness and gradient form. Other operations will not be described again.
[0050] Example 2 S1. Preparation of three-dimensional self-healing framework: 5.4 parts of polyether diamine-terephthalaldehyde polyimide and 6.6 parts of polyacrylonitrile (PAN) were dissolved in 100 parts of DMF / THF solvent (mass ratio 7:3). Electrospinning (voltage 16 kV, receiving distance 14 cm) was used to prepare a three-dimensional porous nanofiber framework with a fiber diameter of about 220 nm, a porosity of about 85%, and a thickness of about 42 μm. The framework was then vacuum dried for later use.
[0051] S2, Gradient Slurry Preparation: Halogenated slurry: Li3InCl6, PVDF-HFP and NBR were weighed and mixed evenly according to a mass ratio of 92:4:4. Anhydrous ethyl acetate / anhydrous toluene (mass ratio 3:2) was used as solvent to obtain a slurry with a solid content of 28 wt%. The slurry was stirred by planetary stirring for 4 h and ball milled for 2 h before use.
[0052] Sulfide slurry: Weigh Li 10 GeP2S 12 PVDF-HFP were mixed at a mass ratio of 95:5, and anhydrous toluene / isobutyl isobutyrate (mass ratio 1:1) was used as solvent to obtain a slurry with a solid content of 30 wt%. The slurry was then subjected to planetary stirring for 5 h and vacuum degassing for 30 min before use.
[0053] Anti-reduction component slurry: Li3N, LiF, polyether diamine-terephthalaldehyde polyimide and Mg nanoparticles (average particle size about 50 nm) were weighed in a mass ratio of 48:42:6:4. First, the Mg nanoparticles were ultrasonically dispersed in anhydrous acetonitrile in 5 times their mass for 20 min. Then, Li3N and LiF powders and polyether diamine-terephthalaldehyde polyimide were added. Anhydrous acetonitrile / toluene (mass ratio 1:1) was added to form a slurry with a total solid content of 25 wt%. After magnetic stirring for 4 h, the slurry was degassed and ready for use.
[0054] S3. The three-dimensional porous framework is laid flat on an inert substrate. A three-channel precision metering pump and a gradient co-casting device are used to simultaneously cast and impregnate the slurries of regions A, B, and C into the pores of the framework. The mass ratio of each component along the film thickness direction changes continuously according to the following program: Positive electrode side starting end (0-15 μm): Li3InCl6 : Li10GeP2S12 : C region component = 78 : 22 : 0; Transition zone I (15-25 μm): continuously transitions to 45 : 50 : 5; Middle zone (25-35 μm): continuously transitions to 15 : 75 : 10; Negative electrode side end (35-48 μm): continuously transitions to 0 : 28 : 72. The casting parameters were as follows: casting speed 0.45 m / min; doctor blade gap 85 μm; substrate temperature 28 ℃; single-channel flow rate 0.5–1.2 mL / min; gradient change mode controlled by S-type continuous program; component change rate between adjacent micro-regions ≤4.5% / μm. After film formation, the film was first allowed to stand at room temperature for 20 min, then slowly dried at 40 ℃ for 3 h, and finally vacuum dried at 60 ℃ for 8 h to obtain a pre-dried film.
[0055] S4. The pre-dried membrane is pre-pressed at 140 ℃ and 50 MPa for 5 min under Ar atmosphere, and then pressed at 250 MPa for 20 min. After hot pressing, the pressure is maintained and cooled to 40 ℃ before depressurization to obtain an integrated continuous gradient electrolyte membrane with a total thickness of about 48 μm (A region about 15 μm, B region about 20 μm, and C region about 13 μm).
[0056] S5. This film was used to assemble an all-solid-state lithium metal battery. The positive electrode was prepared from NMC811, Li3InCl6, Super P, and PTFE in a mass ratio of 70:20:5:5, with a positive electrode surface capacity of 4.0 mAh / cm². The negative electrode was a 50 μm thick lithium metal foil. A stacking pressure of 12 MPa was applied during assembly. The test temperature was 25 °C, and the voltage window was 2.8–4.3 V.
[0057] Example 3 S1. Preparation of three-dimensional self-healing framework: 3.5 parts of UPy-terminated polycarbonate / polyether and 6.5 parts of PVDF-HFP were dissolved in 100 parts of DMF / acetone (mass ratio 6:4) and mixed evenly. The mixture was electrospun (voltage 14 kV, receiving distance 13 cm) to obtain a three-dimensional porous nanofiber framework with a fiber diameter of about 180 nm, a porosity of about 80%, and a thickness of about 26 μm. The framework was then vacuum dried for later use.
[0058] It should be noted that although UPy and imine bonds may not be completely stable on the negative electrode side, their total content in the electrolyte membrane is very low (only 5-8 wt%). Even if they decompose partially, they will not significantly affect the overall ionic conductivity and mechanical integrity of the membrane. At the same time, a small amount of decomposition products (such as nitrogen-containing / fluorine-containing fragments) may actually be beneficial to the lithium metal interface.
[0059] S2, Gradient Slurry Preparation: Halogenated slurry: Weigh Li2ZrCl6 and PVDF-HFP at a mass ratio of 9:1 and mix them. Add anhydrous toluene / isobutyl isobutyrate (mass ratio 1:1) to form a slurry with a total solid content of 27 wt%. Stir the slurry planetarily for 4 h and ball mill it for 2 h before use.
[0060] Sulfide slurry: Weigh Li6PS5Cl and PVDF-HFP at a mass ratio of 95:5 and mix them. Add anhydrous toluene / ethyl acetate (mass ratio 3:2) to form a slurry with a total solid content of 30 wt%. Stir the slurry planetarily for 5 h and then degas it under vacuum for 30 min before use.
[0061] Anti-reduction component slurry: Li3N, LiF, UPy-terminated polycarbonate / polyether, Ag nanoparticles (average particle size approximately 20 nm), and Li2O-modified sulfide (Li2O was used to modify the sulfide electrolyte Li3PS4 to obtain the oxysulfide glass-ceramic system xLi2O·Li3PS4, in which the molar doping of Li2O in the system was approximately 10%) were weighed out. First, Ag nanoparticles were ultrasonically dispersed in anhydrous acetonitrile in 5 times their mass for 20 min. Then, Li3N and LiF powders, UPy-terminated polycarbonate / polyether, and Li2O-modified sulfide were added. Anhydrous acetonitrile / toluene (mass ratio 1:1) was added to form a slurry with a total solid content of 24 wt%. After magnetic stirring for 4 h, the slurry was degassed and ready for use.
[0062] S3. The three-dimensional porous framework is laid flat on an inert substrate. A three-channel precision metering pump and a gradient co-casting device are used to simultaneously cast and impregnate the slurry of regions A, B, and C into the pores of the framework. The mass ratio of each component along the film thickness direction changes continuously according to the following program: Positive electrode side starting end (0 μm): Li2ZrCl6: Li6PS5Cl: C region component = 75:25:0; Transition zone I (10 μm): continuously transitions to 45:50:5; Middle zone (20 μm): continuously transitions to 15:65:20; Negative electrode side end (30 μm): continuously transitions to 0:30:70. The casting parameters were as follows: casting speed 0.60 m / min; doctor blade gap 45 μm; substrate temperature 28 ℃; single-channel flow rate 0.5–1.2 mL / min; gradient change mode controlled by linear continuous program; component change rate between adjacent micro-regions ≤5% / μm. After film formation, the film was first allowed to stand at room temperature for 10 min, then pre-dried at 35 ℃ for 1 h, and finally vacuum dried at 60 ℃ for 6 h to obtain a pre-dried film.
[0063] S4. The pre-dried membrane is pressed at 130 ℃ and 320 MPa for 8 min under Ar atmosphere. After hot pressing, the pressure is maintained and cooled to 40 ℃ before depressurization to obtain an integrated continuous gradient electrolyte membrane with a total thickness of about 30 μm (A region about 12 μm, B region about 12 μm, C region about 6 μm).
[0064] S5. This film is used to assemble an all-solid-state lithium metal battery. The positive electrode is prepared from NMC811, Li2ZrCl6, Super P, and PTFE in a mass ratio of 72:18:5:5, with a positive electrode surface capacity of 4.5 mAh / cm². 2 The negative electrode is a 40 μm thick lithium metal foil. A stacking pressure of 15 MPa is applied during assembly. The test temperature is 25 °C, and the voltage window is 2.8–4.3 V.
[0065] Comparative Example 1 S1. Refer to Example 1.
[0066] S2. Slurry preparation: Refer to Example 1.
[0067] S3. Separate casting: The halide slurry, sulfide slurry, and anti-reduction component slurry are cast separately onto three independent three-dimensional porous nanofiber frameworks. After drying, the positive electrode facing region membrane (about 20 μm), the ion conduction host region membrane (about 20 μm), and the negative electrode facing region membrane (about 15 μm) are obtained.
[0068] S4. Stacking and forming: Stack the above three membranes in the order of positive electrode side layer / intermediate layer / negative electrode side layer, and press them at 150 ℃ and 300 MPa for 15 min to obtain an electrolyte membrane with a total thickness of about 55 μm (positive electrode facing area about 20 μm, ion conduction main area about 20 μm, and negative electrode facing area about 15 μm).
[0069] S5. Refer to Example 1.
[0070] Comparative Example 2 A method for preparing a solid electrolyte membrane includes the following steps: S1. Preparation of three-dimensional self-healing skeleton: Refer to Example 1.
[0071] S2. Slurry preparation: Refer to Example 1 and prepare only the sulfide slurry.
[0072] S3. The three-dimensional porous framework is laid flat on an inert substrate. The sulfide slurry is cast and impregnated into the pores of the framework using a single-channel precision metering pump and a casting device to form a homogeneous film. After film formation, it is first allowed to stand at room temperature for 30 min, then pre-dried at 40 ℃ for 2 h, and finally vacuum dried at 60 ℃ for 8 h to obtain a pre-dried film.
[0073] S4. The pre-dried membrane is pre-pressed at 150 °C and 80 MPa for 5 min under Ar atmosphere, then pressed at 300 MPa for 10 min. After hot pressing, the pressure is maintained and cooled to 40 °C before depressurization to obtain a homogeneous electrolyte membrane with a total thickness of about 55 μm.
[0074] S5. Refer to Example 1.
[0075] Comparative Example 3 A method for preparing a solid electrolyte membrane includes the following steps: S1. Preparation of three-dimensional self-healing skeleton: Refer to Example 1.
[0076] S2. Slurry preparation: Refer to Example 1 and prepare only the halide slurry.
[0077] S3. The three-dimensional porous framework is laid flat on an inert substrate. A single-channel precision metering pump and a casting device are used to cast and impregnate the halide slurry into the pores of the framework to form a homogeneous film. After film formation, the film is first allowed to stand at room temperature for 30 minutes, then pre-dried at 40°C for 2 hours, and finally vacuum-dried at 60°C for 8 hours to obtain a pre-dried film.
[0078] S4. The pre-dried membrane is pre-pressed at 150 ℃ and 80 MPa for 5 min under Ar atmosphere, then pressed at 300 MPa for 10 min. After hot pressing, the pressure is maintained and cooled to 40 ℃ before depressurization to obtain a homogeneous electrolyte membrane with a total thickness of about 55 μm.
[0079] S5. Refer to Example 1.
[0080] Comparative Example 4 A method for preparing a solid electrolyte membrane includes the following steps: S1. Preparation of three-dimensional self-healing skeleton: Refer to Example 1.
[0081] S2. Slurry preparation: Refer to Example 1 and prepare only the anti-reduction component slurry.
[0082] S3. The three-dimensional porous framework is laid flat on an inert substrate. The anti-reduction component slurry is cast and impregnated into the pores of the framework using a single-channel precision metering pump and a casting device to form a homogeneous film. After film formation, it is first allowed to stand at room temperature for 30 minutes, then pre-dried at 40°C for 2 hours, and finally vacuum dried at 60°C for 8 hours to obtain a pre-dried film.
[0083] S4. The pre-dried membrane is pre-pressed at 150 ℃ and 80 MPa for 5 min under Ar atmosphere, then pressed at 300 MPa for 10 min. After hot pressing, the pressure is maintained and cooled to 40 ℃ before depressurization to obtain a homogeneous electrolyte membrane with a total thickness of about 55 μm.
[0084] S5. Refer to Example 1.
[0085] Comparative Example 5 A method for preparing a composite solid electrolyte membrane includes the following steps: S1. Gradient slurry preparation: Prepare halide slurry, sulfide slurry and anti-reduction component slurry according to Example 1.
[0086] S2. A three-channel precision metering pump and a gradient co-casting device are used to simultaneously cast the slurry from zones A, B, and C onto an inert substrate. The mass ratio of each component along the film thickness direction is continuously varied according to the following program: Positive electrode side initial end (0–10 μm): Li₂ZrCl₆: Li₆PS₅Cl: Zone C component = 80:20:0; Middle zone: 10:85:5; Negative electrode side end (45–55 μm): continuously transitioning to 0:25:75. Casting parameters are: casting speed 0.40 m / min; doctor blade gap 90 μm; substrate temperature 28 ℃; single-channel flow rate 0.5–1.2 mL / min; gradient variation using S-type continuous program control; component change rate between adjacent micro-zones ≤5% / μm. After film formation, the film is first allowed to stand at room temperature for 30 minutes, then pre-dried at 40°C for 2 hours, and finally vacuum dried at 60°C for 8 hours to obtain a pre-dried film.
[0087] S3. The pre-dried membrane is pre-pressed at 150 ℃ and 80 MPa for 5 min under Ar atmosphere, and then pressed at 300 MPa for 10 min. After hot pressing, the pressure is maintained and cooled to 40 ℃ before depressurization to obtain an integrated continuous gradient electrolyte membrane with a total thickness of about 55 μm (A region about 22 μm, B region about 23 μm, C region about 10 μm).
[0088] S4. Refer to Example 1.
[0089] Test case The electrochemical performance of the electrolyte membranes obtained in the above embodiments and comparative examples was tested using a CR2025 coin cell configuration. All assembly operations were carried out in an argon glove box with a dew point below -60 °C.
[0090] The assembly sequence for the full cell is as follows: negative electrode shell → lithium sheet (12 mm in diameter, 50 μm in thickness) → electrolyte membrane (16 mm in diameter) → positive electrode sheet (10 mm in diameter) → gasket → spring sheet → positive electrode shell; the assembly sequence for the Li|electrolyte|Li symmetric cell is as follows: negative electrode shell → lithium sheet (12 mm in diameter) → electrolyte membrane (16 mm in diameter) → lithium sheet (12 mm in diameter) → gasket → spring sheet → positive electrode shell; the ionic conductivity test uses a stainless steel blocked electrode symmetric cell, and the assembly sequence is as follows: negative electrode shell → stainless steel gasket → electrolyte membrane (16 mm in diameter) → stainless steel gasket → spring sheet → positive electrode shell. The button cell is sealed using a hydraulic sealing machine at 50 MPa. After sealing, the battery is placed in a specially designed external pressure fixture, and a constant stacking pressure of 10 MPa is applied and maintained throughout the electrochemical testing process.
[0091] Ionic conductivity was measured by AC impedance spectroscopy in the frequency range of 1 MHz to 10 mHz with an amplitude of 10 mV, and calculated using the formula σ = L / (R·S), where L is the electrolyte film thickness, R is the bulk resistance, and S is the electrode area. The lithium-electrolyte interface impedance was obtained by fitting the AC impedance spectrum of a Li-electrolyte-Li symmetric cell. The critical current density was determined by a constant current increment method, starting at 0.1 mA / cm² and increasing by 0.1 mA / cm² every 10 min. 2 The voltage drops sharply or a short circuit occurs. The full-cell cycle test is performed at 25 °C with constant current charge and discharge at a rate of 0.5C, with a voltage range of 2.8–4.3 V. The AC impedance spectrum of the full cell is tested before and after the cycle to analyze the impedance change.
[0092] The test results are shown in Table 1-3.
[0093] Table 1
[0094] Table 2
[0095] Table 3
[0096] Results analysis: 1. As shown in Tables 1 and 3, the lithium-electrolyte interface impedances of Examples 1-3 are 9 Ω·cm², 11 Ω·cm², and 7 Ω·cm², respectively, all significantly lower than the 48 Ω·cm² of Comparative Example 1. This indicates that, when using similar functional materials, the continuous composition gradient integrated structure of this invention can effectively avoid the ion transport barriers caused by clear interlayer interfaces in traditional discrete multilayer systems, thereby significantly reducing the overall interface impedance. In particular, although Comparative Example 1 also includes a positive electrode protective layer, an intermediate high-conductivity layer, and a negative electrode protective layer, the three layers are physically stacked at an interface. During cycling, interface peeling easily occurs due to differences in elastic modulus and mismatch in volume changes, causing the impedance to rise rapidly. The total impedance increase after cycling is close to 96.7%, much higher than the 15.6% of Example 1.
[0097] 2. As shown in Table 1, the critical current densities of Examples 1, 2, and 3 reached 3.8 mA / cm², 3.4 mA / cm², and 3.1 mA / cm², respectively, which are significantly higher than 2.2 mA / cm² of Comparative Example 5 and 0.8–1.5 mA / cm² of Comparative Examples 1–4. This indicates that the introduction of lithium-affinity precursors such as Ag or Mg on the negative electrode side can form an interface layer in situ that is conducive to uniform lithium nucleation and deposition in the early stage of lithium metal contact, reducing local current concentration and the probability of dendrite initiation.
[0098] 3. Comparing Example 1 and Comparative Example 5, it can be seen that both adopt a continuous gradient structure, but Comparative Example 5 does not have a three-dimensional self-healing skeleton. As a result, its interface impedance increased from the initial 39Ω·cm² to 74Ω·cm², an increase of 84.6%, which is significantly higher than that of Example 1.
[0099] 4. Comparative Example 2 uses a single Li6PS5Cl sulfide system, and its room temperature ionic conductivity reaches 6.0 × 10⁻⁶. -3 The S / cm ratio was similar to or even slightly higher than that of the example, but the capacity retention of the full cell dropped below 50% after 50 cycles. This indicates that although a single sulfide has high ionic conductivity, it is prone to oxidative decomposition on the high-voltage positive electrode side and reduction side reactions on the lithium metal negative electrode side, making it difficult to support stable operation over long cycles. Comparative Example 3 used a single halide system, which improved the stability on the positive electrode side, but due to its low bulk ionic conductivity and insufficient reduction stability on the lithium negative electrode, its interfacial impedance reached 35 Ω·cm. 2 The CCD has a capacity of only 0.8 mA / cm². 2 The cycle performance was also unsatisfactory. Although Comparative Example 4 exhibited good chemical stability for the lithium anode, its overall ionic conductivity was only 4.5 × 10⁻⁶. -4 The current S / cm ratio is insufficient to meet the ion transport requirements under medium to high rate conditions. Therefore, a single system cannot simultaneously solve the problems of multi-interface compatibility and efficient lithium conduction. This invention achieves a better performance balance by organically integrating different functional components in the same film in a gradient manner.
[0100] 5. Examples 1 and 3 represent thicker film and thinner film designs, respectively. Example 1 has a total thickness of 55 μm and exhibits excellent cycle stability, maintaining a capacity retention of 86.5% after 1000 cycles. Example 3, with a total thickness reduced to 30 μm, achieves a capacity retention of 88.0% despite a shorter cycle count of 500 cycles, and further reduces the interface impedance to 7 Ω·cm². This demonstrates that the technical solution of this invention is applicable not only to thicker protective electrolyte membranes with long lifespans but also to thinner films with high energy density requirements. By adjusting the thickness ratio of the three zones, the gradient curve form, and the hot-pressing densification conditions, a balance can be achieved between cycle life, rate performance, and volumetric energy density.
[0101] 6. In Example 2, Ag was replaced with Mg, and Li2ZrCl6 / Li6PS5Cl was replaced with Li3InCl6 / Li 10 GeP2S 12 After that, it still achieved 7.2 × 10 -3 High room temperature ionic conductivity of S / cm, 3.4 mA / cm 2The high CCD and 84.0% capacity retention after 800 cycles demonstrate that the core of this invention is not limited to a specific inorganic electrolyte or a specific metal precursor, but rather lies in: (i) the continuous gradient composite of antioxidant components on the positive electrode side, intermediate high-conductivity components, and anti-reduction components on the negative electrode side; (ii) the in-situ lithium affinity interface construction on the negative electrode side; and (iii) the toughening and interface-stabilizing effect of the three-dimensional framework on the membrane. Therefore, this invention has strong platform adaptability and scalability.
[0102] Although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
[0103] Therefore, the above description is only a preferred embodiment of this application and is not intended to limit the scope of this application; that is, all equivalent modifications made in accordance with the scope of the claims of this application shall be within the protection scope of the claims of this application.
Claims
1. A composite solid electrolyte membrane, comprising, along its thickness direction, a positive electrode facing region, an ion-conducting main region, and a negative electrode facing region with continuous component transition, characterized in that: The electrolyte membrane is composed of a halide solid electrolyte component, a sulfide solid electrolyte component, and an anti-reduction component. The electrolyte membrane is permeated with a three-dimensional continuous porous polymer nanofiber framework, and the halide solid electrolyte component, sulfide solid electrolyte component and anti-reduction component fill the pores of the nanofiber framework.
2. The composite solid electrolyte membrane according to claim 1, characterized in that: The mass fraction of the halide component decreases monotonically from the positive electrode region to the negative electrode region along the thickness direction of the composite solid electrolyte membrane, the mass fraction of the sulfide component reaches its maximum value in the ion conduction host region, and the mass fraction of the anti-reduction component increases monotonically from the positive electrode region to the negative electrode region along the thickness direction of the composite solid electrolyte membrane.
3. The composite solid electrolyte membrane according to claim 1, characterized in that: The anti-reduction component is at least one of a nitrogen-containing component and a fluorine-containing component.
4. The composite solid electrolyte membrane according to claim 1, characterized in that: The negative electrode facing region contains a nanoparticle precursor of a lithium affinity metal or its compound, wherein the lithium affinity metal is selected from at least one of Mg, Ag, Zn, Au, Sn, Al, and Bi.
5. The composite solid electrolyte membrane according to claim 1, characterized in that: The three-dimensional porous polymer nanofiber framework comprises at least one self-healing polymer with dynamic reversible bonds; the self-healing polymer contains at least one of borate ester dynamic bonds, imine bonds, or a reversible hydrogen bond network.
6. The composite solid electrolyte membrane according to claim 1, characterized in that: The halide solid electrolyte component is selected from at least one of Li3InCl6, Li2ZrCl6, Li3YCl6, Li3YBr6, and Li3ScCl6; and / or, The sulfide solid electrolyte component is selected from at least one of Li6PS5Cl, Li6PS5Br, Li 10 GeP2S 12 , Li7P3S 11 , Li3PS4; and / or, The anti-reduction component is selected from at least one of Li3N, Li3N-doped silver-germanium sulfide, LiF, and Li2O-modified sulfides.
7. The composite solid electrolyte membrane according to claim 1, characterized in that, The anti-reducing component in the negative electrode facing region is a composite of Li3N and an electron insulating component selected from at least one of LiF, Li2O modified sulfide, and the overall electronic conductivity of the negative electrode facing region is less than 10 -8 S / cm.
8. The composite solid electrolyte membrane according to claim 1, characterized in that: The negative electrode facing region has a reduction potential to lithium metal lower than 0.1 V vs. Li / Li + .
9. The composite solid electrolyte membrane according to claim 1, characterized in that: The three-dimensional porous polymer nanofiber framework is prepared by electrospinning, with a fiber diameter of 50–800 nm and a porosity of 60%–90%.
10. The composite solid electrolyte membrane according to claim 1, characterized in that: The total thickness of the composite solid electrolyte membrane is 15–80 μm, of which the thickness of the positive electrode facing region is 5–30 μm, the thickness of the ion conduction host region is 5–40 μm, and the thickness of the negative electrode facing region is 3–20 μm.
11. The composite solid electrolyte membrane according to claim 1, characterized in that: The composite solid electrolyte film has an ion conductivity of 1x10 -3 ~1x10 -2 S / cm at 25℃, an interface impedance between the lithium metal negative electrode is lower than 15Ω·cm 2 , and a critical current density is not lower than 3 mA / cm 2 .
12. A method for preparing a composite solid electrolyte membrane as described in any one of claims 1-11, characterized in that, Includes the following steps: S1: Prepare halide electrolyte slurry, sulfide electrolyte slurry and anti-reduction component slurry respectively, and add lithium affinity metal nanoparticle precursor to the anti-reduction component slurry; S2: Provides a three-dimensional porous polymer nanofiber framework and places it on a cast substrate; S3: The halide electrolyte slurry, sulfide electrolyte slurry and anti-reduction component slurry are mixed in real time according to a continuously varying ratio along the film thickness direction, and then co-cast and impregnated into the pores of the nanofiber skeleton to form a continuous component gradient skeleton composite filled with the mixed slurry. S4: The skeleton composite filled with the mixed slurry is subjected to solvent evaporation treatment to obtain a dry gradient composite membrane; S5: The gradient composite membrane is subjected to thermal and pressure densification treatment under an inert atmosphere to obtain the integrated composite solid electrolyte membrane.
13. The preparation method according to claim 11, characterized in that, In step S3, a multi-channel gradient proportioning pump is used to achieve co-cast slurry. By controlling the instantaneous flow ratio of each channel pump, the mass fraction of each component is made to have a linear or S-shaped continuous transition curve along the thickness direction, and the mass fraction change rate of adjacent micro-areas is not greater than 5% / μm.
14. The preparation method according to claim 11 or 12, characterized in that, The co-casting process has a casting speed of 0.3–0.8 m / min, a doctor blade gap of 30–120 μm, and a substrate temperature of 20–40 ℃.