A nanocellulose / polyionic liquid dual-network solid electrolyte, its preparation method and application
By utilizing a nanocellulose/polyionic liquid dual-network structure, the problems of low conductivity and insufficient mechanical strength of solid polymer electrolytes are solved, resulting in a lithium metal battery electrolyte with high conductivity, mechanical strength, and a wide electrochemical stability window, suitable for lithium metal batteries.
Patent Information
- Application Number
- CN202611165632.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing solid polymer electrolytes suffer from low room temperature conductivity, insufficient mechanical strength, and poor high-voltage stability, which limits the improvement of the safety and energy density of lithium metal batteries.
A dual-network structure of nanocellulose/polyionic liquid is adopted. By constructing a dual-network structure in which the physical network of nanocellulose and the chemical cross-linking network of polyionic liquid interpenetrate each other, and utilizing functionalized polymerizable ionic liquid for in-situ cross-linking, a solid electrolyte with high conductivity and high mechanical strength is formed.
It achieves room temperature ionic conductivity on the order of 10⁻³ S/cm, excellent mechanical strength, and an electrochemical stability window widened to above 5.0 V. It suppresses lithium dendrite growth, balances high conductivity and high mechanical strength, and has a simple and environmentally friendly preparation process.
Smart Images

Figure CN123120852A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid electrolyte technology for lithium metal batteries, and specifically relates to a nanocellulose / polyionic liquid dual-network solid electrolyte, its preparation method, and its application. Background Technology
[0002] Lithium metal batteries are considered an important direction for the next generation of high-energy-density rechargeable batteries due to their high theoretical specific capacity and high energy density potential. However, traditional liquid electrolyte systems have safety hazards such as flammability, leakage, and instability at the lithium metal interface. Furthermore, they are prone to oxidation and decomposition under high-voltage positive electrode conditions, which limits further improvements in battery safety and energy density.
[0003] Polymer solid electrolytes have the advantages of being free of flowing liquids, suppressing lithium dendrite growth, and improving safety. However, most existing solid polymer electrolytes are based on polyethylene oxide (PEO) systems, which still have problems such as low room temperature ionic conductivity, insufficient mechanical strength, and poor high voltage stability.
[0004] Existing cellulose-based solid electrolytes often improve ion conduction and electrochemical stability by weakening hydrogen bonds and promoting lithium salt dissociation through surface functionalization, introduction of ionic groups, and coordination / crosslinking. However, their ion conduction is still often limited by a single framework network and lithium salt system, and their room temperature conductivity is often around 10. -5 It has a strength on the order of S / cm, and there is still room for further improvement in the electrochemical stability window under high-voltage cathode scenarios. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing solid polymer electrolytes, such as low room temperature conductivity, insufficient mechanical strength, and poor high voltage stability, and to provide a method for preparing a nanocellulose / polyionic liquid dual-network solid electrolyte.
[0006] Another object of the present invention is to provide a nanocellulose / polyionic liquid dual-network solid electrolyte prepared by the method described above.
[0007] Another object of the present invention is to provide the application of the aforementioned nanocellulose / polyionic liquid dual-network solid electrolyte.
[0008] The objective of this invention is achieved through the following technical solution:
[0009] A method for preparing a nanocellulose / polyionic liquid dual-network solid electrolyte includes the following steps:
[0010] (1) Weigh the following components by mass percentage: 15-35% functionalized polymerizable ionic liquid monomer, 15-35% free ionic liquid, 5-30% lithium salt, 1-10% crosslinking agent, 0.05-2% initiator, and 5-40% nanocellulose CNF;
[0011] (2) After the functionalized polymerizable ionic liquid monomer, free ionic liquid and lithium salt are stirred and dissolved, crosslinking agent and initiator are added and stirred and mixed evenly to obtain ionic liquid precursor solution;
[0012] (3) Disperse nanocellulose CNF in anhydrous acetonitrile to obtain CNF dispersion; then cast the CNF dispersion into a film, dry it to obtain CNF porous membrane; then add or coat the ionic liquid precursor liquid onto the surface of CNF porous membrane, let it stand, and then irradiate it with ultraviolet light or heat it to make it polymerize and crosslink in situ, and finally dry it under vacuum to obtain the nanocellulose / polyionic liquid dual network solid electrolyte.
[0013] Preferably, in step (1), the following components are weighed in terms of mass percentage: 15-35% functionalized polymerizable ionic liquid monomer, 25.5-35% free ionic liquid, 5-20% lithium salt, 4-9% crosslinking agent, 0.05-1% initiator, and 5-30% nanocellulose CNF.
[0014] Preferably, the initiator in step (1) is at least one of a photoinitiator and a thermal initiator; more preferably, it is at least one of 2-hydroxy-2-methyl-1-phenylpropanone (HMPP), azobisisobutyronitrile (AIBN), and dimethyl azobisisobutyrate.
[0015] Preferably, when the initiator is a photoinitiator, the amount used is 0.1-2% (preferably 1%) by mass percentage; when the initiator is a thermal initiator, the amount used is 0.05-1% (preferably 0.05-0.08%) by mass percentage.
[0016] Preferably, the cation of the functionalized polymerizable ionic liquid monomer in step (1) is a vinyl-containing imidazolium-type or pyrrolidine-type ionic liquid, and the anion is bis(trifluoromethanesulfonyl)imide (TFSI). - ) or bis(fluorosulfonyl)imide (FSI) - ).
[0017] More preferably, the functionalized polymerizable ionic liquid monomer in step (1) is 1-vinyl-3-butylimidazolium trifluoromethanesulfonylimide salt (VBIM-TFSI).
[0018] Preferably, the free ionic liquid in step (1) is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt (EMIM-TFSI).
[0019] Preferably, the lithium salt in step (1) is at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI).
[0020] Preferably, the Li in the lithium salt described in step (1) + The molar ratio of the anion to the functionalized polymerizable ionic liquid monomer (Li + The ratio of ionic liquid anions to lithium salts is (0.2–3.0):1; more preferably (0.2–2.0):1. This range ensures that the lithium salt is fully dissociated and provides sufficient charge carriers, while avoiding excessive lithium salts that could lead to increased system viscosity or phase separation.
[0021] Preferably, the crosslinking agent in step (1) is at least one of pentaerythritol tetraacrylate (PET4A), polyethylene glycol diacrylate (PEGDA), and trimethylolpropane triacrylate (TMPTA); more preferably, pentaerythritol tetraacrylate.
[0022] Preferably, the nanocellulose CNF described in step (1) can be treated by TEMPO oxidation, carboxylation, sulfonation, or grafting lithium salt affinity groups to improve compatibility and interfacial bonding strength with the ionic liquid monomer / lithium salt system; preferably, TEMPO-oxidized nanocellulose (TEMPO-CNF) is prepared by the following method:
[0023] Nanocellulose (CNF) was dispersed in water to prepare a suspension. TEMPO (2,2,6,6-tetramethylpiperidine oxide) and NaBr were added sequentially, followed by the addition of NaClO solution to carry out the oxidation reaction. During the reaction, the pH was maintained at 10–10.5, and the reaction was carried out at 20–25°C for 2–4 hours. After the reaction, ethanol was added to terminate the reaction. The TEMPO-CNF was obtained by centrifugation, washing, or dialysis purification.
[0024] Preferably, the diameter of the nanocellulose CNF is ≤10nm and the fiber length is ≤100m; more preferably, the diameter is 3-10nm and the length is 10-100nm.
[0025] Preferably, the concentration of the suspension is 1 to 2 wt%.
[0026] Preferably, the mass ratio of the nanocellulose (CNF), TEMPO and NaBr is 1:0.016:0.1.
[0027] Preferably, the pH is adjusted using NaOH solution; more preferably, the pH is adjusted to 10-10.5.
[0028] Preferably, the amount of NaClO used is calculated as 5-10 mmol of NaClO per gram of nanocellulose (CNF).
[0029] Preferably, the dialysis is performed for more than 48 hours using a dialysis bag with a molecular weight cutoff of 10,000 Da.
[0030] Preferably, the conditions for stirring and dissolving in step (2) are: temperature 30-60℃, stirring for 0.5-3h; more preferably 45℃, stirring for 1.5h.
[0031] Preferably, the conditions for uniform mixing in step (2) are: temperature 30-60℃, stirring for 5-30 min; more preferably 45℃, stirring for 20 min.
[0032] Preferably, the solid content in the CNF dispersion (i.e., the acetonitrile dispersion of nanocellulose CNF) in step (3) is 0.5-5 wt%, more preferably 1-3 wt%; it can be obtained by dispersing nanocellulose into anhydrous acetonitrile, or by replacing the solvent water in the nanocellulose CNF aqueous dispersion with anhydrous acetonitrile; more preferably, it is prepared by the following method:
[0033] The aqueous dispersion of nanocellulose (CNF) was centrifuged to remove the supernatant, and then anhydrous acetonitrile was added and ultrasonically dispersed under ice-water bath conditions to complete the first displacement, thus obtaining an acetonitrile dispersion of CNF. The steps of centrifugation to remove the supernatant, adding anhydrous acetonitrile, and ultrasonic dispersion were repeated 2 to 3 times to obtain a uniform and stable CNF dispersion.
[0034] Preferably, the water content of the anhydrous acetonitrile is ≤50ppm to ensure that the resulting dispersion system meets the low moisture requirements of lithium metal batteries.
[0035] Preferably, the conditions for ultrasonic dispersion are: ultrasonic power 200-600W, working frequency 20-25kHz, working / interruption time ratio of (1-5)s / (2-10)s, and total ultrasonic time of 5-20min; more preferably, the conditions are: ultrasonic power 400W, working frequency 20kHz, working / interruption time ratio of 2s / 3s, and total ultrasonic time of 10min.
[0036] Preferably, the casting process described in step (3) is carried out on a polytetrafluoroethylene (PTFE) pad.
[0037] Preferably, the thickness of the CNF porous membrane in step (3) is 100-150 μm; more preferably, it is 120 μm.
[0038] Preferably, the drying conditions for the CNF porous membrane in step (3) are: temperature 40-80℃, vacuum drying for 6-24h; more preferably: 60℃, vacuum drying for 12h.
[0039] Preferably, the settling time in step (3) is 30 to 60 minutes, so that the ionic liquid precursor solution can fully penetrate into the pore structure of the CNF membrane.
[0040] Preferably, the ultraviolet irradiation conditions in step (3) are: wavelength 365nm and light intensity 10mW / cm². 2 The temperature is 25–40℃, and the irradiation time is 15–60 min; more preferably, the wavelength is 365 nm and the light intensity is 10 mW / cm². 2 Temperature 25℃, irradiation time 15-20 min.
[0041] Preferably, the heating conditions in step (3) are: temperature 60-100℃, heating for 1-4 hours; more preferably: heating in an 80℃ oven for 2 hours.
[0042] Preferably, the vacuum drying conditions in step (3) are: drying at 40-80℃ and vacuum degree ≤-0.095MPa for 12-48h; more preferably, drying at 50-60℃ and vacuum degree ≤-0.095MPa for 24h, and the electrolyte membrane obtained after drying is sealed and stored in an inert atmosphere.
[0043] Preferably, the thickness of the nanocellulose / polyionic liquid dual-network solid electrolyte in step (3) is about 50-80 μm; wherein, the thickness of the CNF porous membrane is 100-150 μm, which is the thickness of the porous membrane obtained after casting and drying, and it has a rich pore structure inside; after subsequent infiltration and filling by ionic liquid precursor liquid and in-situ polymerization, due to the filling of pores and the volume shrinkage during the formation of polymer network, the final thickness of the solid electrolyte membrane will be reduced to about 50-80 μm.
[0044] A nanocellulose / polyionic liquid dual-network solid electrolyte is prepared by any of the methods described above.
[0045] The application of the nanocellulose / polyionic liquid dual-network solid electrolyte in the preparation of lithium metal batteries.
[0046] The present invention has the following advantages and effects compared with the prior art:
[0047] (1) This invention achieves a synergistic improvement in ion conductivity and mechanical properties by constructing a dual-network structure in which a physical network of nanocellulose and a chemically cross-linked network of polyionic liquid interpenetrate each other. The electrolyte membrane exhibits a room temperature ion conductivity of 10. -3It has a strength on the order of S / cm and excellent mechanical strength, effectively balancing high electrical conductivity and high mechanical strength, which is beneficial for suppressing lithium dendrite growth.
[0048] (2) The functionalized polymerizable ionic liquid in this invention, after in-situ polymerization and cross-linking, effectively inhibits polymer crystallization, broadens the electrochemical stability window to above 5.0V, and can be well matched with high voltage cathode materials.
[0049] (3) The preparation process of this invention is simple and mild. The nanocellulose in the raw material is renewable and degradable. The system is green and environmentally friendly and compatible with existing battery manufacturing processes, making it easy to achieve large-scale production. Attached Figure Description
[0050] Figure 1 The image shows the AC impedance diagrams of the solid electrolytes prepared in Example 1 and Comparative Example 1 at 30°C.
[0051] Figure 2 The figure shows the current-voltage characteristic curves of lithium-ion / solid electrolyte / steel-sheet coin cells assembled using the solid electrolytes prepared in Example 1 and Comparative Example 1.
[0052] Figure 3 The graph shows the cyclic charge-discharge performance of the solid electrolytes prepared in Example 1 and Comparative Example 1 at 30°C and 0.5C rate.
[0053] Figure 4 The graph shows the cyclic charge-discharge performance of the solid electrolytes prepared in Examples 5 and 1 at 30°C and 0.5C rate.
[0054] Figure 5 This is a comparison graph of the AC impedance of the solid electrolytes prepared in Example 5 and Example 1 at 30°C.
[0055] Figure 6 The figure shows the current-voltage characteristic curves of lithium-ion / solid electrolyte / steel-sheet coin cells assembled using the solid electrolytes prepared in Examples 1 and 5. Detailed Implementation
[0056] The present invention will be further described in detail below with reference to embodiments, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field. Test methods in the following embodiments that do not specify specific experimental conditions are generally performed according to conventional experimental conditions.
[0057] The materials used in the embodiments of this invention can be commercially available or synthesized using conventional methods in the art, wherein:
[0058] ①TEMPO oxidation of cellulose nanoparticles (TEMPO-CNF): Disperse 1g of cellulose nanoparticles (CNF) in deionized water to prepare a 1-2wt% suspension. Add 0.016g of TEMPO (approximately 0.1mmol) and 0.1g of NaBr (approximately 1mmol) sequentially. After stirring and dissolving, adjust the pH to 10-10.5 with NaOH. Slowly add NaClO solution (effective chlorine content 5-10mmol / g cellulose, i.e., 5-10mmol NaClO per gram of cellulose) under stirring to initiate the oxidation reaction. During the reaction, continuously add NaOH to maintain the pH at 10-10.5, and react at 20-25℃ for 2-4 hours. The reaction was terminated by adding excess ethanol. Residual reagents were removed by centrifugation and washing (3-5 times) or dialysis purification (molecular weight cutoff 10000 Da, 48 hours or more). Finally, the TEMPO-CNF aqueous dispersion was obtained by ultrasonication (20 kHz, 10-15 min) or high-pressure homogenization (600-1000 bar treatment for dissociation). The nanocellulose (CNF) was purchased from Zhejiang Jinjiahao Green Nanomaterials Co., Ltd., model CNF-H1, with a fiber diameter of 3-10 nm, a length of 10-100 nm, and a solid content of 2.5%. TEMPO was purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0059] ② 1-Vinyl-3-butylimidazolium trifluoromethanesulfonylimide salt (VBIM-TFSI), also known as 1-butyl-3-vinylimidazolium bis(trifluoromethanesulfonyl)imide salt or 1-vinyl-3-butylimidazolium bis(trifluoromethanesulfonyl)imide salt, CAS No. 1007390-44-4, purity 99%, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0060] ③ 1-Ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt (EMIM-TFSI), also known as 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, CAS No. 174899-82-2, purity 99%, purchased from Shanghai Maclean Biochemical Technology Co., Ltd., item number E808653.
[0061] ④ Lithium salt LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), 99% purity, battery grade, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0062] ⑤ Pentaerythritol tetraacrylate (PET4A), 97% purity, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0063] ⑥ 2-Hydroxy-2-methyl-1-phenylpropanone, 99% pure, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0064] ⑦ The solvent is anhydrous acetonitrile, with a purity of ≥99.9% and a water content of ≤50ppm, purchased from Shanghai Maclean Biochemical Technology Co., Ltd.
[0065] ⑧ Polyethylene oxide (PEO), molecular weight Mw=600000, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0066] ⑨ Polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), also known as poly(vinylidene fluoride-co-hexafluoropropylene), CAS No. 9011-17-0, purity 99%, purchased from Shanghai Maclean Biochemical Technology Co., Ltd., item number MFCD00212573.
[0067] ⑩ Polymethyl methacrylate (PMMA), 99% purity, Mw=350000, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0068] Furthermore, the lithium salt, functionalized polymerizable ionic liquid monomer, and the resulting solid electrolyte membrane are pre-dried under an inert atmosphere or vacuum before use to control the moisture content to ≤100ppm.
[0069] Example 1
[0070] (1) At room temperature of 25℃, an aqueous dispersion containing 2.0 g of TEMPO-CNF (dry weight) was taken, and after centrifugation to remove the supernatant, 98.0 g of anhydrous acetonitrile was added and redispersed to prepare a suspension with a solid content of 2.0 wt%. The above suspension was placed in an ultrasonic cell disruptor and ultrasonically dispersed for 10 min under ice-water bath conditions (ultrasonic power 400 W, working frequency 20 kHz, working / intermittent time ratio of 2 s / 3 s) to complete the first displacement. Then, the above operation of "centrifugation to remove supernatant - adding an equal amount of anhydrous acetonitrile - ultrasonic dispersion for 10 min" was repeated twice to finally obtain a uniform and stable nanocellulose-acetonitrile dispersion.
[0071] (2) Preparation of ionic liquid precursor solution: Taking the preparation of a solid electrolyte membrane (dry basis) with a total mass of 10.0 g (8 g of ionic liquid precursor solution + 2 g of TEMPO-CNF) as an example, in a glove box filled with argon (O2 < 0.1 ppm, H2O < 0.1 ppm), the following components were weighed according to the formula: VBIM-TFSI 2.55 g (25.5 wt%), EMIM-TFSI 2.55 g (25.5 wt%), LiTFSI 2.0 g (20 wt%), PET4A 0.8 g (8 wt%), and HMPP 0.1 g (1 wt%). First, VBIM-TFSI, EMIM-TFSI and LiTFSI were mixed and stirred at 45 °C for 1.5 h until completely dissolved. Then, PET4A and HMPP were added and stirred at 45 °C for 20 min to obtain a homogeneous ionic liquid precursor solution.
[0072] (3) The nanocellulose-acetonitrile dispersion obtained in step (1) is placed on a polytetrafluoroethylene (PTFE) pad and cast into a film using a doctor blade. The thickness of the cast wet film is about 120 μm. The film is then dried in a vacuum drying oven at 60 °C for 12 h to obtain a CNF porous membrane (the thickness after drying is about 120 μm). The ionic liquid precursor solution obtained in step (2) is slowly added / coated onto the surface of the CNF membrane and allowed to stand for 30–60 min to allow the ionic liquid precursor solution to fully penetrate into the pore structure of the CNF membrane.
[0073] (4) Place the wet film prepared in step (3) in an ultraviolet curing chamber and cure it at a wavelength of 365 nm and an irradiation intensity of 10 mW / cm. 2 Under these conditions, the VBIM-TFSI monomers were irradiated at 25°C for 15 min to induce in-situ polymerization and crosslinking. They were then transferred to a vacuum drying oven and dried at 60°C and a vacuum of ≤-0.095 MPa for 24 h. The electrolyte membrane, approximately 50–80 μm thick, was then peeled off in a glove box.
[0074] Example 2
[0075] Adjust the proportions of each component in the ionic liquid precursor solution in the formulation, and follow the same steps as in Example 1: (1) TEMPO-CNF 2.0g (octane-dry weight, 20wt%); (2) Ionic liquid precursor solution components: VBIM-TFSI 1.5g (15wt%), EMIM-TFSI 3.5g (35wt%), LiTFSI 2.0g (20wt%), PET4A 0.9g (9wt%), HMPP 0.1g (1wt%). The resulting electrolyte membrane thickness is approximately 50–80 μm.
[0076] Example 3
[0077] Adjust the lithium salt ratio and nanocellulose content in the formulation, and follow the same steps as in Example 1: (1) TEMPO-CNF 3.0g (30wt%); (2) Ionic liquid precursor components: VBIM-TFSI 3.0g (30wt%), EMIM-TFSI 3.0g (30wt%), LiTFSI 0.5g (5wt%), PET4A 0.4g (4wt%), HMPP 0.1g (1wt%). The resulting electrolyte membrane thickness is approximately 50–80 μm.
[0078] Example 4
[0079] The nanocellulose content in the formulation was adjusted, and other steps were the same as in Example 1: (1) TEMPO-CNF 0.5g (5wt%); (2) Ionic liquid precursor components: VBIM-TFSI 3.5g (35wt%), EMIM-TFSI 3.0g (30wt%), LiTFSI 2.0g (20wt%), PET4A 0.9g (9wt%), HMPP 0.1g (1wt%). The resulting electrolyte membrane thickness was approximately 50–80 μm.
[0080] Example 5
[0081] Thermally initiated polymerization was used, with other steps the same as in Example 1: the formulation was the same as in Example 1, except that the photoinitiator HMPP was replaced with an equal amount of thermal initiator azobisisobutyronitrile (AIBN, 0.1 g, 1 wt%). Polymerization method: The cast film prepared in step (3) was placed in an 80°C oven and heated for 2 h for thermally initiated polymerization. Drying conditions: Vacuum drying at 60°C and a vacuum degree ≤ -0.095 MPa for 24 h. The resulting electrolyte film thickness was approximately 50–80 μm.
[0082] Comparative Example 1 (Pure PEO System)
[0083] Polyethylene oxide (PEO) (Mv=600000) and lithium salt LiTFSI were weighed and prepared at an EO:Li molar ratio of 16:1, where EO represents the ethylene oxide group in the repeating unit of PEO and Li represents the lithium element in LiTFSI. PEO and LiTFSI were added to an appropriate amount of anhydrous acetonitrile (preferably until completely dissolved, approximately 10 mL / g polymer) and stirred at 40 °C for 12 h until completely dissolved. The solution was poured into a polytetrafluoroethylene mold and cast into a film, which was then vacuum dried at 50–60 °C and a vacuum degree ≤-0.095 MPa for 24 h to obtain the solid electrolyte membrane of Comparative Example 1, with a thickness of approximately 60–80 μm.
[0084] Comparative Example 2 (Pure PVDF-HFP System)
[0085] Weigh 1.0 g of PVDF-HFP and 0.5 g of LiTFSI, add them to 10 mL of anhydrous acetonitrile, and stir at 50 °C for 6 h until completely dissolved. Pour the solution into a polytetrafluoroethylene mold and cast it into a film. Dry it under vacuum at 60 °C and a vacuum degree ≤ -0.095 MPa for 24 h to obtain the solid electrolyte membrane of Comparative Example 2, with a thickness of about 50–80 μm.
[0086] Comparative Example 3 (only nanocellulose physical network, no polyionic liquid network)
[0087] (1) At room temperature of 25℃, an aqueous dispersion containing 2.0 g of TEMPO-CNF (octane-dry weight) was taken, and after centrifugation to remove the supernatant, 98.0 g of anhydrous acetonitrile was added and redispersed to prepare a suspension with a solid content of 2.0 wt%. The above suspension was placed in an ultrasonic cell disruptor and ultrasonically dispersed for 10 min under ice-water bath conditions (ultrasonic power 400 W, working frequency 20 kHz, working / interval time ratio of 2 s / 3 s) to complete the first displacement. Then, the above operation of "centrifugation to remove supernatant - adding an equal amount of anhydrous acetonitrile - ultrasonic dispersion for 10 min" was repeated twice to finally obtain a uniform and stable nanocellulose-acetonitrile dispersion with a solid content of 2%.
[0088] (2) Add 2.0g LiTFSI to the nanocellulose-acetonitrile dispersion obtained in step (1) above, stir to dissolve and then cast into a film.
[0089] (3) The wet membrane obtained in step (2) is dried at 60°C and vacuum degree ≤ -0.095 MPa for 24 h to obtain a single-network nanocellulose solid electrolyte membrane with a thickness of about 120 μm.
[0090] Comparative Example 4 (polyionic liquid chemical network only, without nanocellulose)
[0091] (1) The ionic liquid precursor solution formulation of Example 1 (excluding nanocellulose, total mass of precursor solution 8.0 g): VBIM-TFSI 2.55g (31.875wt%), EMIM-TFSI 2.55g (31.875wt%), LiTFSI 2.0g (25wt%), PET4A 0.8g (10wt%), HMPP 0.1g (1.25wt%), were mixed evenly and stirred at 45°C until completely dissolved to obtain the ionic liquid precursor solution.
[0092] (2) The above ionic liquid precursor solution was directly cast into a film, and then polymerized under ultraviolet irradiation at 25°C for 15 min at a wavelength of 365 nm and an irradiation intensity of 10 mW / cm². Then it was dried at 60°C and a vacuum degree ≤ -0.095 MPa for 24 h to obtain the solid electrolyte membrane of Comparative Example 4 with a thickness of about 50 μm.
[0093] Comparative Example 5 (Traditional nonionic liquid polymer electrolyte)
[0094] Weigh 1.0 g of polymethyl methacrylate (PMMA, Mw=350000) and 0.5 g of LiTFSI, add them to 10 mL of anhydrous acetonitrile, and stir at 40 °C for 8 h until completely dissolved. Pour the solution into a polytetrafluoroethylene mold and cast it into a film. Vacuum dry at 60 °C and a vacuum degree ≤-0.095 MPa for 24 h to obtain the solid electrolyte membrane of Comparative Example 5, with a thickness of approximately 50–80 μm.
[0095] Comparative Example 6 (physical blending, non-in-situ interpenetration)
[0096] (1) Preparation of CNF membrane alone: Take an aqueous dispersion containing 2.0 g of TEMPO-CNF at oven-dry weight, remove the supernatant by centrifugation, add anhydrous acetonitrile and redisperse, and disperse by ultrasonication (ultrasonic power 400W, working frequency 20kHz, working / intermittent time ratio of 2 s / 3 s) for 10 min to obtain CNF-acetonitrile dispersion. Cast into a film and vacuum dry at 60℃ for 24 h to obtain TEMPO-CNF membrane.
[0097] (2) Preparation of polyionic liquid membrane alone: According to the formulation of Example 1 (excluding TEMPO-CNF): VBIM-TFSI 2.55g, EMIM-TFSI 2.55g, LiTFSI 2.0g, PET4A 0.8g, HMPP 0.1g, after being mixed evenly, the mixture was cast into a film and tested at a wavelength of 365nm and an irradiation intensity of 10mW / cm. 2 Under the conditions of UV irradiation at 25℃ for 15 min, VBIM-TFSI was polymerized and crosslinked, and then vacuum dried at 60℃ and vacuum degree ≤ -0.095MPa for 24 h to obtain a polyionic liquid membrane.
[0098] (3) Physical blending for film formation: The TEMPO-CNF membrane obtained in step (1) and the polyionic liquid membrane obtained in step (2) are pulverized into powder or fragments respectively, and mixed at a mass ratio of TEMPO-CNF:polyionic liquid = 2.0:8.0 (consistent with the dry basis ratio in Example 1). An appropriate amount of anhydrous acetonitrile is added as a dispersion medium, and the mixture is stirred vigorously for 4 hours to ensure that the two are physically mixed uniformly. The mixed slurry is cast into a film and dried at 60°C and a vacuum degree ≤ -0.095MPa for 24 hours to obtain a physically blended solid electrolyte composite membrane with a thickness of about 60-80 μm.
[0099] Effect Example
[0100] 1. Performance Testing
[0101] 1.1 The solid electrolyte membranes prepared in Examples 1-5 and Comparative Examples 1-6 were stamped into 16mm diameter discs and assembled into steel sheet / solid electrolyte / steel sheet coin cells in a glove box (the coin cell casing model was CR2032, and the steel sheets used had a diameter of 16mm and a thickness of 0.5mm and 1mm). Their ionic conductivity was tested (test temperatures were 30℃ and 60℃). The test frequency was 0.1MHz to 0.1Hz. The experiment was repeated three times.
[0102] 1.2 The solid electrolyte membranes prepared in Examples 1-5 and Comparative Examples 1-6 were stamped into 16mm diameter discs and assembled into lithium-ion / solid electrolyte / steel-coated coin cells in a glove box (the coin cell casing model was CR2032; the lithium-ion sheet diameter was 16mm and the thickness was 0.5mm; the steel sheet diameter was 16mm and the thickness was 1mm). Their electrochemical stability window was then tested. The test potential voltage ranged from 2.0V to 5.5V, and the scan rate was set to 10mV / s. The experiment was repeated three times.
[0103] 1.3 The solid electrolyte membranes prepared in Examples 1-5 and Comparative Examples 1-6 were stamped into 16mm diameter discs and assembled into lithium-ion / solid electrolyte / lithium iron phosphate cathode / steel-coated coin cells (button cell casing model CR2032, lithium-ion cell diameter 16mm, thickness 0.5mm; cathode diameter 12mm) in a glove box. Cyclic performance was then tested using a battery cycling system. The test voltage range was 2.0V to 4.2V, and the charge / discharge rate was 0.5C. The experiment was repeated three times.
[0104] 1.4 The solid electrolyte membranes prepared in Examples 1-5 and Comparative Examples 1-6 were cut into ISO37 Type 4 dumbbell-shaped standard strips and subjected to tensile testing using a universal testing machine at a tensile rate of 10 mm / min, with at least 5 parallel samples per group.
[0105] 2. Experimental Results
[0106] Figure 1 These are the AC impedance diagrams of the solid electrolytes prepared in Example 1 and Comparative Example 1 at 30°C. Figure 1 As can be seen, the impedance arc radius of Example 1 is much smaller than that of Comparative Example 1, indicating that the dual-network structure of the present invention significantly reduces the interfacial impedance and bulk impedance of the electrolyte and improves the ion conduction capability.
[0107] Figure 2 This is a graph showing the current-voltage characteristic of lithium-ion / solid electrolyte / steel-sheet coin cells assembled using the solid electrolytes prepared in Example 1 and Comparative Example 1. Figure 2 As can be seen, the electrochemical stability window of Example 1 can reach 5.0V (vs. Li). +The voltage of / Li is significantly better than that of Comparative Example 1 (4.4V), indicating that the present invention can be well matched with high-voltage cathode materials.
[0108] Figure 3 This is a graph showing the cyclic charge-discharge (charge-discharge rate 0.5C) conditions of the solid electrolytes prepared in Example 1 and Comparative Example 1 at 30°C. Figure 3 As can be seen, after 100 cycles, the capacity retention rate of Example 1 is significantly higher than that of Comparative Example 1, and the coulombic efficiency is more stable, indicating that the dual-network structure of the present invention effectively suppresses lithium dendrite growth and improves cycle stability.
[0109] Figure 4 This is a comparison chart of the cycle charge-discharge performance of the solid electrolytes prepared in Examples 1 and 5 at 30°C and 0.5C rate. Figure 4 As can be seen, the initial discharge capacity of Example 5 (using thermally initiated polymerization, AIBN, heated at 80°C for 2 hours) is approximately 148 mAh / g, and the capacity retention rate after 100 cycles is approximately 89%. Compared with Example 1 (using photoinitiated polymerization, HMPP, 365nm UV irradiation for 15 minutes), which has an initial capacity of approximately 152 mAh / g and a retention rate of approximately 91%, the performance of the two examples is highly similar. This result indicates that the polymerization initiation method (photoinitiation or thermal initiation) has a relatively small impact on the final performance of the electrolyte. Both methods can achieve sufficient cross-linking polymerization of functionalized polymerizable ionic liquid monomers, forming a complete dual-network structure. This conclusion provides a basis for flexibly selecting the polymerization process based on existing equipment conditions in industrial production—when the production line does not have UV curing equipment, thermal initiation can be used as an alternative without affecting product performance.
[0110] Figure 5 This is a comparison of the AC impedance of the solid electrolytes prepared in Examples 1 and 5 at 30°C. Figure 5 As can be seen, the impedance arc radius of Example 5 is basically the same as that of Example 1, and the two are at the same level. According to fitting calculations, the room temperature ionic conductivity of Example 5 is 1.6 × 10⁻⁶. -4 S / cm, compared to 1.8 × 10 in Example 1 -4 The very close S / cm ratio further confirms the equivalence of thermally initiated polymerization and photoinitiated polymerization in constructing ion-conducting networks. Both initiation methods enable the polymerization of VBIM-TFSI monomers to form a continuous polyionic liquid conductive phase, which in turn forms a fully interpenetrating structure with the nanocellulose physical network, thereby achieving efficient ion transport.
[0111] Figure 6 This is a comparison of the volt-ampere characteristic curves of lithium-ion / solid-state electrolyte / steel-sheet coin cells assembled using the solid-state electrolytes prepared in Examples 1 and 5. Figure 6As can be seen, the electrochemical stability window of Example 5 reaches 4.5V (vs. Li). + The voltage ( / Li) is slightly lower than 5.0V in Example 1. This difference is mainly attributed to the possibility that trace byproducts (such as isobutyronitrile radicals) generated during the thermally initiated polymerization process may form minor defects in the electrolyte, slightly affecting the stability of the electrode / electrolyte interface and resulting in a slight narrowing of the electrochemical window. To further broaden the electrochemical window of the thermally initiated system, the amount of AIBN can be optimized (further reduced to 0.05–0.08 wt%) or a higher purity thermal initiator (such as dimethyl azobisisobutyrate) can be used to reduce the impact of byproducts.
[0112] The electrochemical and mechanical performance data of each embodiment (Examples 1-5) and each comparative example (Comparative Examples 1-6) are summarized in Table 1. The data in Table 1 show that the performance of this invention can be flexibly adjusted over a wide range by adjusting the component ratios: Example 3 has the highest tensile strength (9.2 MPa), suitable for applications with high mechanical requirements; Example 4 has the highest elongation at break (65%), suitable for applications with high flexibility requirements; Example 2 has the highest room temperature ionic conductivity (2.5 × 10⁻⁶ MPa). -4 (S / cm), suitable for scenarios with high magnification performance requirements. The overall performance of each embodiment is significantly better than that of the comparative examples, proving the universality and superiority of the technical solution of the present invention.
[0113] Table 1. Performance test results of the examples and comparative examples.
[0114]
[0115] Experimental comparisons demonstrate that the dual-network structure of the nanocellulose physical network and the polyionic liquid chemical cross-linking network constructed in this invention achieves a synergistic improvement in ion conduction and mechanical properties. Nanocellulose provides a rigid framework and ion migration channels, while the polyionic liquid imparts high conductivity and a wide electrochemical window. This interlocking structure resolves the contradiction between high conductivity, high strength, and a wide electrochemical window inherent in traditional solid electrolytes. Compared to Comparative Example 1 (pure PEO), this invention significantly improves room-temperature conductivity and electrochemical stability window, and greatly enhances mechanical strength. Comparative Example 2 (pure PVDF-HFP) and Comparative Example 5 (pure PMMA) exhibit inferior overall performance compared to this invention. Comparative Example 3 (nanocellulose only) has high strength but is brittle and has extremely low conductivity; Comparative Example 4 (polyionic liquid only) has conductivity close to that of this invention but insufficient strength for practical applications.
[0116] Furthermore, in Example 5, thermally initiated polymerization (AIBN, heating at 80°C for 2 hours) was used instead of photoinitiated polymerization (HMPP, 365nm UV irradiation for 15 minutes) in Example 1. The ionic conductivity of both methods was 1.6 × 10⁻⁶. -4S / cm vs 1.8×10 -4 The S / cm and tensile strength (8.2 MPa vs 8.5 MPa) are very close, indicating that both thermally initiated and photo-initiated polymerization methods can achieve full cross-linking polymerization of functionalized polymerizable ionic liquid monomers. The resulting dual-network structure has similar ionic conductivity, high voltage withstand capability, and mechanical properties. This result provides a flexible process option for industrial production—thermal initiation can be used as an alternative when the production line lacks UV curing equipment or needs to process opaque thick films.
[0117] Furthermore, in Comparative Example 6, CNF membrane and polyionic liquid membrane were separately pulverized and then mixed to form a film using a physical blending method. The resulting film had a tensile strength of only 2.5 MPa and a room temperature conductivity of only 0.9 × 10⁻⁶. -4 S / cm, both key performance indicators are significantly lower than those of Example 1 (8.5 MPa and 1.8 × 10⁻⁶). -4 (S / cm). This indicates that simple physical mixing cannot achieve synergistic enhancement of CNF and polyionic liquid—CNF fragments not only lose the mechanical transport capability of the continuous network but also block the long-range ion conduction pathways of the polyionic liquid, leading to a dual degradation of mechanical and electrochemical properties. Only through the process of "CNF film formation first—ionic liquid precursor liquid infiltration—in-situ polymerization" of this invention, which enables the chemical cross-linked network of the polyionic liquid to be generated in-situ within the CNF physical network and form interpenetration, can a continuous ion conduction channel be constructed while maintaining the integrity of the CNF network, thereby achieving a synergistic improvement in mechanical properties and ionic conductivity.
[0118] This invention allows for flexible performance adjustment over a wide range by modifying the component ratios to meet diverse needs. The data above demonstrates that the method of this invention can yield solid-state electrolyte membranes with significantly superior overall performance compared to existing typical polymer systems, providing crucial material support for high-safety, high-energy-density lithium metal batteries.
[0119] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A method for preparing a nanocellulose / poly ionic liquid double network solid-state electrolyte, characterized by, Includes the following steps: (1) Weigh the following components by mass percentage: 15-35% functionalized polymerizable ionic liquid monomer, 15-35% free ionic liquid, 5-30% lithium salt, 1-10% crosslinking agent, 0.05-2% initiator, and 5-40% nanocellulose CNF; (2) After the functionalized polymerizable ionic liquid monomer, free ionic liquid and lithium salt are stirred and dissolved, crosslinking agent and initiator are added and stirred and mixed evenly to obtain ionic liquid precursor solution; (3) Disperse nanocellulose CNF in anhydrous acetonitrile to obtain CNF dispersion; then cast the CNF dispersion into a film, dry it to obtain CNF porous membrane; then add or coat the ionic liquid precursor liquid onto the surface of CNF porous membrane, let it stand, and then irradiate it with ultraviolet light or heat it to make it polymerize and crosslink in situ, and finally dry it under vacuum to obtain the nanocellulose / polyionic liquid dual network solid electrolyte.
2. The preparation method according to claim 1, characterized in that: In step (1), weigh the following components by mass percentage: 15-35% functionalized polymerizable ionic liquid monomer, 25.5-35% free ionic liquid, 5-20% lithium salt, 4-9% crosslinking agent, 0.05-1% initiator, and 5-30% nanocellulose CNF; The cation of the functionalized polymerizable ionic liquid monomer in step (1) is an imidazolium-type or pyrrolidine-type ionic liquid containing vinyl groups, and the anion is bis(trifluoromethanesulfonyl)imide or bis(fluorosulfonyl)imide. Li in the lithium salt in step (1) + molar ratio of the functionalized polymerizable ionic liquid monomer to the anion is 0.2-3.0:
1.
3. The preparation method according to claim 1 or 2, characterized in that: The functionalized polymerizable ionic liquid monomer mentioned in step (1) is 1-vinyl-3-butylimidazolium trifluoromethanesulfonylimide salt; The free ionic liquid mentioned in step (1) is 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; The lithium salt mentioned in step (1) is at least one of lithium bis(trifluoromethanesulfonyl)imide and lithium bis(fluorosulfonyl)imide; The crosslinking agent mentioned in step (1) is at least one of pentaerythritol tetraacrylate, polyethylene glycol diacrylate, and trimethylolpropane triacrylate; The initiator mentioned in step (1) is at least one of a photoinitiator and a thermal initiator; The nanocellulose CNF mentioned in step (1) is nanocellulose CNF that has been treated by TEMPO oxidation, carboxylation, sulfonation or grafting lithium salt affinity groups.
4. The preparation method according to claim 3, characterized in that: The crosslinking agent mentioned in step (1) is pentaerythritol tetraacrylate; The initiator mentioned in step (1) is at least one of 2-hydroxy-2-methyl-1-phenylpropanone, azobisisobutyronitrile, and dimethyl azobisisobutyrate; The nanocellulose CNF mentioned in step (1) is TEMPO oxidized nanocellulose; wherein the diameter of the nanocellulose CNF is ≤10nm and the fiber length is ≤100m.
5. The preparation method according to claim 1, characterized in that: The solid content in the acetonitrile dispersion of nanocellulose (CNF) mentioned in step (3) is 0.5–5 wt%. The thickness of the CNF porous membrane mentioned in step (3) is 100-150 μm; The thickness of the nanocellulose / polyionic liquid dual-network solid electrolyte described in step (3) is 50-80 μm.
6. The preparation method according to claim 1, characterized in that: The CNF dispersion mentioned in step (3) is prepared by the following method: after centrifuging to remove the supernatant from the aqueous dispersion of nanocellulose CNF, anhydrous acetonitrile is added and ultrasonic dispersion is performed under ice-water bath conditions to complete the first displacement, thereby obtaining an acetonitrile dispersion of CNF; then the steps of centrifuging to remove the supernatant, adding anhydrous acetonitrile and ultrasonic dispersion are repeated 2 to 3 times to obtain a uniform and stable CNF dispersion. The conditions for ultrasonic dispersion are: ultrasonic power 200-600W, working frequency 20-25kHz, working / intermittent time ratio 1-5s / 2-10s, and total ultrasonic time 5-20min.
7. The preparation method according to claim 1, characterized in that: The drying conditions for the CNF porous membrane mentioned in step (3) are: temperature 40-80℃, vacuum drying for 6-24h; The settling time mentioned in step (3) is 30 to 60 minutes; The conditions of the UV irradiation in step (3) are: wavelength 365 nm, light intensity 10 mW / cm 2 , temperature 25-40 °C, irradiation time 15-60 min. The conditions for the heat treatment described in step (3) are: temperature 60-100℃, heating for 1-4 hours; The vacuum drying conditions described in step (3) are: drying at 40-80℃ and vacuum degree ≤-0.095MPa for 12-48h.
8. The preparation method according to claim 1, characterized in that: The conditions for stirring and dissolving in step (2) are: temperature 30-60℃, stirring for 0.5-3 hours; The conditions for uniform mixing in step (2) are: temperature 30-60℃, stirring for 5-30 minutes.
9. A nanocellulose / polyionic liquid double network solid-state electrolyte, characterized by: It is prepared by the method described in any one of claims 1 to 8.
10. The application of the nanocellulose / polyionic liquid dual-network solid electrolyte of claim 9 in the preparation of lithium metal batteries.