A PPS-based solid electrolyte containing 1,3-PS plasticizer and its preparation method
By introducing 1,3-propane sulfonyl lactone plasticizer into a polymer-based solid electrolyte through covalent grafting and cross-linking network structure with polyphenylene sulfide resin, combined with lithium fluoride montmorillonite nanosheet modification, the problems of low ionic conductivity and insufficient structural stability of polymer-based solid electrolytes are solved, enabling the application of lithium-ion batteries with high safety and long life.
Patent Information
- Application Number
- CN202611334664.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polymer-based solid electrolytes in lithium-ion batteries suffer from low ionic conductivity, high interfacial contact resistance, and insufficient structural stability, making it difficult to meet the requirements for high safety and long lifespan.
A covalent graft structure was formed by using 1,3-propane sulfonyl lactone plasticizer and polyphenylene sulfide resin. A cross-linking network was constructed by combining allyl functionalized ionic liquid monomers and mercaptosilane coupling agents. Lithium fluoride montmorillonite nanosheets were used for modification to form a multi-level ion transport pathway, thereby improving the flexibility and structural stability of the material.
It significantly improves lithium-ion conductivity and long-term electrolyte stability, enhances battery cycle life and rate performance, and ensures the stability of electrode-electrolyte interface adhesion.
Smart Images

Figure CN123120857A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer-based solid electrolyte materials technology, and in particular to a PPS-based solid electrolyte containing 1,3-PS plasticizer and its preparation method. Background Technology
[0002] Lithium-ion batteries are the core energy storage devices in the current energy storage field. Traditional liquid lithium-ion batteries have safety hazards such as electrolyte leakage, flammability and explosion, and poor cycle stability, making them unsuitable for the high safety and long lifespan requirements of high-end energy storage and new energy vehicles. Solid electrolytes, with their advantages of no leakage, high safety, and excellent thermal stability, are gradually becoming the core material to replace liquid electrolytes.
[0003] Polymer-based solid electrolytes (SEEs) possess excellent flexibility, ease of processing into films, and good interfacial compatibility, making them a mainstream research direction in solid electrolytes. Among them, polyphenylene sulfide (PPS) resin exhibits excellent heat resistance, mechanical strength, chemical corrosion resistance, and dimensional stability, making it an ideal matrix material for preparing high-performance SEEs. However, pure PPS resin molecules are rigid and highly regular, with weak molecular chain mobility, resulting in a lack of lithium-ion conduction channels and extremely low ionic conductivity. Furthermore, its poor compatibility with lithium salts and high interfacial contact resistance significantly limit its practical application in the field of solid electrolytes.
[0004] Currently, the industry typically modifies polymer matrices by adding plasticizers, inorganic nanofillers, and ionic liquids to improve electrolyte ion conductivity. However, conventional small-molecule plasticizers suffer from easy migration and poor thermal stability, leading to precipitation and failure with long-term use, resulting in decreased mechanical and electrical properties of the electrolyte membrane. Ordinary inorganic fillers exhibit weak interfacial bonding with the polymer matrix, easily leading to aggregation and hindering the uniform construction of a continuous ion transport network. Furthermore, traditional modification systems lack effective cross-linking structures, resulting in insufficient overall electrolyte structural stability and susceptibility to volume deformation during cycling, further impacting battery cycle life and rate performance. Existing modification technologies cannot simultaneously achieve the mechanical stability, thermal stability, and high ion conductivity of polyphenylene sulfide (PPS)-based electrolytes, making it difficult to meet the demands of industrial applications. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides a PPS-based solid electrolyte containing 1,3-PS plasticizer and its preparation method. The technical solution is as follows:
[0006] A PPS-based solid electrolyte containing 1,3-PS plasticizer, based on 100 parts of polyphenylene sulfide resin, comprises the following components:
[0007] 100 parts of polyphenylene sulfide resin;
[0008] 8-18 parts of 1,3-propanesulfonyl lactone plasticizer;
[0009] 15-30 parts of alkali metal lithium salt;
[0010] 5-15 parts of lithium fluoride montmorillonite nanosheets;
[0011] Contains 0.8–3 parts of mercaptosilane coupling agent;
[0012] 2-8 parts of allyl-functionalized ionic liquid monomer;
[0013] Antioxidant 0.1 to 1 part;
[0014] In this process, the sulfonyl ring of the 1,3-propane sulfonyl lactone plasticizer undergoes ring-opening and electrophilic substitution with the benzene ring of the polyphenylene sulfide resin to form covalently grafted lithium propanesulfonate groups; the allyl functionalized ionic liquid monomer and the mercapto group in the mercaptosilane coupling agent undergo a thiol-ene click reaction at the melt blending temperature to form a crosslinked network; the lithium fluoride montmorillonite nanosheets are layered silicate nanosheets that have undergone hydrothermal treatment with ammonium fluoride and alkali metal lithium salt ion exchange treatment.
[0015] Optionally, based on 100 parts of polyphenylene sulfide resin, 10-14 parts of 1,3-propane sulfonyl lactone plasticizer, 18-25 parts of alkali metal lithium salt, 8-12 parts of lithium fluoride montmorillonite nanosheets, 1.0-2.0 parts of mercaptosilane coupling agent, and 3-5 parts of allyl functionalized ionic liquid monomer;
[0016] The polyphenylene sulfide resin has a weight-average molecular weight of 40,000 to 70,000, a melt index of 80 g / 10 min to 150 g / 10 min measured at 315°C and 5 kg load, and a moisture content of less than or equal to 0.05 wt%.
[0017] Optionally, the grafting rate of the 1,3-propane sulfonyl plasticizer to the polyphenylene sulfide resin in the polyphenylene sulfide-based solid electrolyte is 30% to 70%; the alkali metal lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate borate.
[0018] Optionally, the lithium fluoride montmorillonite nanosheets have a sheet thickness of 1 nm to 5 nm, a sheet diameter of 100 nm to 500 nm, a fluorine content of 1 wt% to 5 wt%, and an interlayer lithium-ion exchange capacity of 0.8 mmol / g to 1.2 mmol / g; the mercaptosilane coupling agent is at least one of γ-mercaptopropyltriethoxysilane and γ-mercaptopropyltrimethoxysilane.
[0019] Optionally, the allyl-functionalized ionic liquid monomer is at least one of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 1-allyl-3-vinylimidazolium bis(fluorosulfonyl)imide salt; the antioxidant is at least one of hindered phenolic antioxidant 1010 and phosphite antioxidant 168.
[0020] A method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer, comprising the following steps:
[0021] Step 1: Sodium-based montmorillonite is added to an aqueous solution of ammonium fluoride and hydrothermally reacted at 80℃~120℃ for 6h~24h. After centrifugation and washing until neutral, it is dispersed in an aqueous solution of alkali metal lithium salt and ion exchanged at 50℃~80℃ for 4h~12h. After drying and grinding, lithium-fluoride montmorillonite nanosheets are obtained.
[0022] Step 2: Under an inert atmosphere, 1,3-propane sulfonyl lactone plasticizer, alkali metal lithium salt and allyl functionalized ionic liquid monomer are mixed to obtain plasticizer, lithium salt and ionic liquid premix.
[0023] Step 3: The lithium fluoride montmorillonite nanosheets and the mercapto-containing silane coupling agent are subjected to a pre-condensation reaction at 60℃~90℃ for 0.5h~2h under an inert atmosphere to obtain organo-fluoride lithium montmorillonite nanosheets with mercapto groups on the surface.
[0024] Step 4: Under an inert atmosphere, add polyphenylene sulfide resin and antioxidant to the main feed port of the twin-screw extruder; inject the premix obtained in S2 into the twin-screw extruder through the liquid injection port; add the organic fluorinated lithium montmorillonite nanosheets obtained in S3 through the side feed port; and carry out reactive melt blending at 270℃~300℃ and screw speed 100rpm~300rpm to obtain a blend.
[0025] Step 5: After crushing the blend, hot press it into a film. The hot pressing temperature is 260℃~280℃, the pressure is 10MPa~20MPa, and the pressure is held for 10min~30min to obtain a polyphenylene sulfide-based solid electrolyte membrane containing 1,3-propane sulfonyl lactone plasticizer.
[0026] Optionally, in step 1, the concentration of the ammonium fluoride aqueous solution is 0.5 mol / L to 2.0 mol / L, the solid-liquid ratio of sodium montmorillonite to the ammonium fluoride aqueous solution is 1:50 to 1:100; centrifugation and washing are performed until the pH of the washing solution is 6 to 7; the concentration of the alkali metal lithium salt aqueous solution is 0.5 mol / L to 1.5 mol / L; the drying temperature is 60 to 90℃; and the material is ground until D50 is less than or equal to 10 μm.
[0027] Optionally, the inert atmosphere in step 2 is argon or nitrogen; the mixing temperature is 40℃~70℃, the mixing time is 0.5h~2h; and the molar ratio of 1,3-propane sulfonyl lactone plasticizer, alkali metal lithium salt and allyl functionalized ionic liquid monomer is 1:0.5~1:2:0.1~0.5.
[0028] Optionally, the inert atmosphere in step 3 is argon or nitrogen; the pre-condensation reaction temperature is 60℃~90℃, and the reaction time is 0.5h~2h; the mass ratio of lithium fluoride montmorillonite nanosheets to mercaptosilane coupling agent is 1:0.05~1:0.3.
[0029] Optionally, in step 4, the twin-screw extruder is a co-rotating twin-screw extruder with a length-to-diameter ratio of 36:1 to 48:1, and has eight temperature zones: the first to third temperature zones are 270℃ to 280℃, the fourth to sixth temperature zones are 285℃ to 300℃, and the seventh to eighth temperature zones are 275℃ to 285℃; the liquid injection port is located in the third temperature zone, and the side feed port is located in the fourth temperature zone; the reactive melt blending time is 2 min to 6 min; the particle size of the blend after crushing in step 5 is less than or equal to 500 μm; the hot pressing is carried out in stages: first, pre-pressing at 260℃ to 265℃ and 5 MPa for 5 min, then holding at 270℃ to 280℃ and 15 MPa for 10 min to 30 min; then cooling to room temperature at 0.5℃ / min to 2℃ / min and demolding to obtain a polyphenylene sulfide-based solid electrolyte membrane with a thickness of 50 μm to 200 μm.
[0030] In summary, the present invention has at least one of the following beneficial technical effects:
[0031] This invention provides a PPS-based solid electrolyte containing 1,3-PS plasticizer and its preparation method. Through component optimization and reactive melt blending modification processes, the structure and function of the polyphenylene sulfide matrix are modified and enhanced. The 1,3-propane sulpholactone plasticizer forms a covalent graft structure with the benzene ring of the polyphenylene sulfide resin through a ring-opening reaction, stably introducing lithium propanesulfonate functional groups. This effectively improves the flexibility of the resin molecular chain, enhances the mobility of molecular chain segments, and constructs a stable lithium-ion transport channel. It also eliminates the problem of migration and precipitation of traditional small molecule plasticizers, significantly improving the long-term stability of the electrolyte.
[0032] Allyl-functionalized ionic liquid monomers undergo a thiol-ene click reaction with a mercaptosilane coupling agent to construct a dense and uniform cross-linked network structure in situ. This effectively improves the overall mechanical strength and dimensional stability of the electrolyte membrane, suppresses electrolyte deformation and damage during battery charging and discharging, and enhances the interfacial adhesion stability between the electrode and the electrolyte.
[0033] Fluorinated and lithium-ion exchange-modified montmorillonite nanosheets can be uniformly dispersed in a polymer matrix. Their layered nanostructure creates multi-level continuous ion transport pathways, enhancing lithium-ion migration efficiency. Simultaneously, the introduction of fluorine optimizes interfacial properties, reduces interfacial impedance, and further improves electrolyte ionic conductivity. After organic modification with a silane coupling agent, the modified montmorillonite exhibits significantly improved compatibility with the polyphenylene sulfide matrix, eliminating agglomeration defects and ensuring material structural uniformity. Attached Figure Description
[0034] Figure 1 This is a schematic flowchart of a method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer according to the present invention. Detailed Implementation
[0035] The present invention will be further described in detail below with reference to the accompanying drawings.
[0036] This invention discloses a PPS-based solid electrolyte containing 1,3-PS plasticizer and its preparation method.
[0037] Reference Figure 1 Example 1, a PPS-based solid electrolyte containing 1,3-PS plasticizer, based on 100 parts of polyphenylene sulfide resin, includes the following components:
[0038] 100 parts of polyphenylene sulfide resin;
[0039] 8-18 parts of 1,3-propanesulfonyl lactone plasticizer;
[0040] 15-30 parts of alkali metal lithium salt;
[0041] 5-15 parts of lithium fluoride montmorillonite nanosheets;
[0042] Contains 0.8–3 parts of mercaptosilane coupling agent;
[0043] 2-8 parts of allyl-functionalized ionic liquid monomer;
[0044] Antioxidant 0.1 to 1 part;
[0045] In this process, the sulfonyl ring of the 1,3-propane sulfonyl lactone plasticizer undergoes ring-opening and electrophilic substitution with the benzene ring of the polyphenylene sulfide resin to form covalently grafted lithium propanesulfonate groups; the allyl functionalized ionic liquid monomer and the mercapto group in the mercaptosilane coupling agent undergo a thiol-ene click reaction at the melt blending temperature to form a crosslinked network; the lithium fluoride montmorillonite nanosheets are layered silicate nanosheets that have undergone hydrothermal treatment with ammonium fluoride and alkali metal lithium salt ion exchange treatment.
[0046] By adopting the above technical solution, polyphenylene sulfide resin is used as the matrix, and its molecular chain is composed of alternating benzene rings and thioether bonds, which endows the material with intrinsic flame retardancy and high temperature resistance. Based on 100g of polyphenylene sulfide resin, the weight parts of other components are also referenced to this.
[0047] The dosage of 1,3-propanesulfonyl plasticizer is 8 to 18 g. This substance is liquid at room temperature, and its sulfonyl ring exhibits ring strain. At a melt blending temperature of 270°C to 300°C, the ring undergoes thermal ring-opening, generating a propanesulfonic acid-based active intermediate. This intermediate is a strong electrophile, undergoing an electrophilic substitution reaction with electron-rich sites on the benzene ring of the polyphenylene sulfide resin to form carbon-sulfur covalent bonds, thereby grafting the propanesulfonic acid group onto the polyphenylene sulfide backbone. After grafting, the propanesulfonic acid group undergoes ion exchange with lithium ions in the system, forming lithium propanesulfonate groups. This grafting process, on the one hand, disrupts the regular arrangement of the polyphenylene sulfide molecular chain, reduces crystallinity, and increases chain segment mobility; on the other hand, it introduces lithium ion coordination sites onto the polyphenylene sulfide backbone, forming a cooperative transport pathway between grafted lithium sulfonate and free anions with the free alkali metal lithium salt. If the amount used is less than 8g, the grafting density is insufficient, the crystallinity decreases only slightly, and there are too few lithium-ion coordination sites; if it is more than 18g, excessive grafting leads to excessive loss of rigidity of the polyphenylene sulfide main chain and a significant decrease in mechanical strength.
[0048] The amount of alkali metal lithium salt used is 15 to 30 g. Its function is to provide free lithium ions. In the polyphenylene sulfide matrix, the anion of alkali metal lithium salt interacts electrostatically with the cations of the grafted lithium propanesulfonate group and the allyl-functionalized ionic liquid monomer, promoting the dissociation of lithium salt. When the amount is less than 15 g, the free carrier concentration is insufficient and the ionic conductivity is low; when the amount is more than 30 g, the undissociated lithium salt forms ion pairs or ion clusters, which reduces the effective carrier concentration and increases the viscosity of the system.
[0049] The dosage of lithium fluoride montmorillonite nanosheets ranges from 5 to 15 g. These nanosheets are two-dimensional layered silicates. After hydrothermal treatment with ammonium fluoride, some hydroxyl groups on the surface are covalently replaced by fluorine atoms. The interlayer cations are lithium ions after alkali metal lithium salt ion exchange. The surface and interlayer spaces provide rapid lithium ion transport channels. When the dosage is below 5 g, the proportion of inorganic fast ion channels is too low, resulting in limited improvement in ionic conductivity. When the dosage is above 15 g, the nanosheets tend to aggregate, forming ion transport dead zones, and the system viscosity increases sharply, making processing difficult.
[0050] The amount of mercaptosilane coupling agent used is 0.8 to 3 g. One end of the coupling agent is a siloxane group, and the other end is a mercapto group. The siloxane group condenses with the residual silanol groups on the surface of the lithium fluoride montmorillonite nanosheets to form siloxane-silicon covalent bonds, achieving organic coating of the nanosheets. The mercapto group serves as the reaction site for the subsequent thiol-ene click reaction. When the amount is less than 0.8 g, the mercapto group density on the nanosheet surface is insufficient, resulting in too few crosslinking points; when the amount is greater than 3 g, excess silane coupling agent remains free in the matrix, self-condensing at high temperatures to form oligomeric siloxanes, reducing the uniformity of the electrolyte membrane.
[0051] The allyl-functionalized ionic liquid monomer is used in amounts ranging from 2 to 8 g. This monomer contains both allyl and imidazolium cations. The allyl group reacts with the thiol group in the mercaptosilane coupling agent via a thermally initiated thiol-ene click reaction at the melt blending temperature, forming thioether crosslinks and constructing an organic-inorganic interpenetrating crosslink network. The imidazolium cation electrostatically associates with the alkali metal lithium salt anion, weakening the coordination between lithium ions and anions and promoting lithium salt dissociation. When the dosage is below 2 g, the crosslink density is insufficient and the promoting effect on lithium salt dissociation is not significant; when the dosage is above 8 g, the crosslink network is too dense, restricting the movement of polyphenylene sulfide chain segments and hindering ion transport.
[0052] The antioxidant dosage is 0.1 to 1 g. Its function is to prevent thermo-oxidative degradation of polyphenylene sulfide resin and organic components during high-temperature processing. A dosage below 0.1 g results in insufficient antioxidant effect; a dosage above 1 g may cause the antioxidant itself to migrate to the interface, affecting ion conduction.
[0053] The ring-opening grafting reaction of the 1,3-propane sulfonyl lactone plasticizer and the thiol-ene click reaction of the allyl-functionalized ionic liquid monomer proceed synergistically. The former introduces flexible lithium sulfonate side groups onto the polyphenylene sulfide backbone, while the latter establishes a covalent crosslinking bridge between the inorganic nanosheets and the polyphenylene sulfide matrix. The combined effect enables the solid electrolyte to possess both high ionic conductivity and high mechanical strength.
[0054] Example 2: Based on 100 parts of polyphenylene sulfide resin, 10-14 parts of 1,3-propane sulfonyl lactone plasticizer, 18-25 parts of alkali metal lithium salt, 8-12 parts of lithium fluoride montmorillonite nanosheets, 1.0-2.0 parts of mercaptosilane coupling agent, and 3-5 parts of allyl functionalized ionic liquid monomer.
[0055] The polyphenylene sulfide resin has a weight-average molecular weight of 40,000 to 70,000, a melt index of 80 g / 10 min to 150 g / 10 min measured at 315°C and 5 kg load, and a moisture content of less than or equal to 0.05 wt%.
[0056] By adopting the above technical solution, the weight-average molecular weight of polyphenylene sulfide resin is controlled to be between 40,000 and 70,000. When the weight-average molecular weight is too low, there is insufficient entanglement between molecular chains, resulting in low melt strength and easy breakage during hot pressing. When the weight-average molecular weight is too high, the melt viscosity is too high, making it difficult to uniformly plasticize in a twin-screw extruder. Furthermore, although there are many grafting reaction sites, chain segment movement is restricted, which is not conducive to ion conduction. The melt index, measured at 315℃ and a 5kg load, ranges from 80g / 10min to 150g / 10min. The melt index reflects the melt flowability of the resin. Below 80g / 10min, the melt is too viscous, making it difficult to uniformly disperse inorganic nanosheets; above 150g / 10min, the melt strength is too low, making film formation difficult. A moisture content of less than or equal to 0.05wt% is used to avoid the hydrolysis and chain breakage of the thioether bonds in the polyphenylene sulfide main chain during high-temperature processing, thus maintaining the stability of the matrix molecular weight.
[0057] In Example 3, the grafting rate of the 1,3-propane sulfonyl plasticizer to the polyphenylene sulfide resin in the polyphenylene sulfide-based solid electrolyte is 30% to 70%; the alkali metal lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate borate.
[0058] By employing the above technical solution, the grafting rate of 1,3-propanesulfonyl plasticizer to polyphenylene sulfide resin in polyphenylene sulfide-based solid electrolytes ranges from 30% to 70%. The grafting rate is defined as the ratio of the actual mass of propanesulfonic acid groups covalently grafted onto a unit mass of polyphenylene sulfide resin to the theoretically fully grafted mass. When the grafting rate is below 30%, the decrease in polyphenylene sulfide crystallinity is insufficient, chain segment mobility is limited, and there are too few lithium propanesulfonate grafting sites, resulting in a lack of significant improvement in ionic conductivity. When the grafting rate is above 70%, the polyphenylene sulfide backbone is covered by a large number of lithium propanesulfonate side groups, increasing the interchain distance. Although chain segment mobility is enhanced, mechanical strength decreases sharply. A grafting rate range of 30% to 70% maximizes ionic conductivity while maintaining acceptable mechanical strength.
[0059] The alkali metal lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate borate. Lithium bis(trifluoromethanesulfonyl)imide exhibits high dissociation and good thermal stability; its anions are large in size, have a high degree of charge delocalization, and exhibit weak association with lithium ions. Lithium bis(fluorosulfonyl)imide has smaller anions, which is beneficial for improving ionic conductivity, but its thermal stability is slightly lower. Lithium difluorooxalate borate can participate in the formation of a stable solid electrolyte interface layer on the cathode surface, inhibiting electrolyte oxidative decomposition under high voltage. Using these three salts individually or in combination can balance ionic conductivity, thermal stability, and electrochemical window.
[0060] Example 4: The lithium fluoride montmorillonite nanosheets have a sheet thickness of 1 nm to 5 nm, a sheet diameter of 100 nm to 500 nm, a fluorine content of 1 wt% to 5 wt%, and an interlayer lithium-ion exchange capacity of 0.8 mmol / g to 1.2 mmol / g; the mercaptosilane coupling agent is at least one of γ-mercaptopropyltriethoxysilane and γ-mercaptopropyltrimethoxysilane.
[0061] By employing the above technical solution, the thickness of the lithium fluorinated montmorillonite nanosheets ranges from 1 nm to 5 nm, and the sheet diameter ranges from 100 nm to 500 nm. The sheet thickness, approaching a single layer to several layers, facilitates the two-dimensional conduction of lithium ions along the sheet surface. If the sheet diameter is too small, the specific surface area of the nanosheets becomes too large, increasing surface defects and edge effects, leading to discontinuous ion transport paths; if the sheet diameter is too large, the nanosheets are difficult to disperse uniformly in the melt and are prone to stacking. The fluorine content ranges from 1 wt% to 5 wt%. Fluorine atoms partially replace the silanol groups on the montmorillonite surface, reducing surface polarity, improving compatibility with the polyphenylene sulfide matrix, and preventing nanosheet aggregation. If the fluorine content is too low, surface modification will be insufficient; if the fluorine content is too high, the interlayer structure may collapse, resulting in the loss of two-dimensional channels. The interlayer lithium-ion exchange capacity ranges from 0.8 mmol / g to 1.2 mmol / g, ensuring sufficient lithium-ion concentration between layers to form a continuous conduction path for lithium ions.
[0062] The mercaptosilane coupling agent is at least one of γ-mercaptopropyltriethoxysilane or γ-mercaptopropyltrimethoxysilane. Both can condense with the siloxane terminus of lithium fluoride montmorillonite on its surface. During condensation, the ethoxy and methoxy groups respectively remove small molecules of ethanol and methanol. At high temperature, the mercapto terminus undergoes a thiol-alkene click reaction with the allyl group of the allyl-functionalized ionic liquid monomer, forming a thioether crosslinking bridge. These two silane coupling agents were chosen because of their high mercapto reactivity and stability at the processing temperature of polyphenylene sulfide, preventing premature uncontrolled oxidation or decomposition.
[0063] Example 5, wherein the allyl-functionalized ionic liquid monomer is at least one of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 1-allyl-3-vinylimidazolium bis(fluorosulfonyl)imide salt; and the antioxidant is at least one of hindered phenolic antioxidant 1010 and phosphite antioxidant 168.
[0064] By employing the above technical solution, the allyl-functionalized ionic liquid monomer is at least one of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt or 1-allyl-3-vinylimidazolium bis(fluorosulfonyl)imide salt. Both monomers contain an imidazolium cation and an allyl group. The positive charge of the imidazolium cation is delocalized on the five-membered ring, and its electrostatic interaction with the alkali metal lithium salt anion is weaker than the coordination between lithium ions and anions. Therefore, it can effectively weaken the association between lithium ions and anions and increase the concentration of free lithium ions. Under thermal conditions, the allyl group undergoes a thiol-ene click reaction with the mercapto group without the need for an additional initiator, and the reaction produces no small molecule byproducts. The 1-allyl-3-vinylimidazolium bis(fluorosulfonyl)imide salt also contains vinyl groups, which can provide additional unsaturated bonds to participate in crosslinking, further increasing the crosslinking density.
[0065] The antioxidant is at least one of hindered phenolic antioxidant 1010 or phosphite antioxidant 168. The hindered phenolic antioxidant terminates the free radical chain reaction by donating hydrogen atoms, while the phosphite antioxidant works by decomposing hydroperoxides. The combination of both can simultaneously inhibit thermal and oxidative degradation.
[0066] Based on 100g of polyphenylene sulfide resin, the preferred components are 10-14g of 1,3-propane sulfonyl lactone plasticizer, 18-25g of alkali metal lithium salt, 8-12g of lithium fluoride montmorillonite nanosheets, 1.0-2.0g of mercaptosilane coupling agent, and 3-5g of allyl-functionalized ionic liquid monomer. This preferred range achieves an optimal balance between the density of grafted lithium sulfonate groups, the concentration of free lithium salt, the content of inorganic fast ion channels, and the crosslinking density. The grafted lithium sulfonate groups and the free lithium salt form a continuous lithium-ion conduction network, the lithium fluoride montmorillonite nanosheets provide additional two-dimensional conduction pathways, and the crosslinking network maintains structural integrity. The synergistic effect among the components is most significant within this range.
[0067] Example 6: A method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer, comprising the following steps:
[0068] Step 1: Sodium-based montmorillonite is added to an aqueous solution of ammonium fluoride and hydrothermally reacted at 80℃~120℃ for 6h~24h. After centrifugation and washing until neutral, it is dispersed in an aqueous solution of alkali metal lithium salt and ion exchanged at 50℃~80℃ for 4h~12h. After drying and grinding, lithium-fluoride montmorillonite nanosheets are obtained.
[0069] Step 2: Under an inert atmosphere, 1,3-propane sulfonyl lactone plasticizer, alkali metal lithium salt and allyl functionalized ionic liquid monomer are mixed to obtain plasticizer, lithium salt and ionic liquid premix.
[0070] Step 3: The lithium fluoride montmorillonite nanosheets and the mercapto-containing silane coupling agent are subjected to a pre-condensation reaction at 60℃~90℃ for 0.5h~2h under an inert atmosphere to obtain organo-fluoride lithium montmorillonite nanosheets with mercapto groups on the surface.
[0071] Step 4: Under an inert atmosphere, add polyphenylene sulfide resin and antioxidant to the main feed port of the twin-screw extruder; inject the premix obtained in S2 into the twin-screw extruder through the liquid injection port; add the organic fluorinated lithium montmorillonite nanosheets obtained in S3 through the side feed port; and carry out reactive melt blending at 270℃~300℃ and screw speed 100rpm~300rpm to obtain a blend.
[0072] Step 5: After crushing the blend, hot press it into a film. The hot pressing temperature is 260℃~280℃, the pressure is 10MPa~20MPa, and the pressure is held for 10min~30min to obtain a polyphenylene sulfide-based solid electrolyte membrane containing 1,3-propane sulfonyl lactone plasticizer.
[0073] Using the above technical solution, step 1 involves the preparation of lithium-fluorinated montmorillonite nanosheets. Sodium-based montmorillonite is added to an aqueous ammonium fluoride solution for a hydrothermal reaction. Ammonium fluoride provides fluoride ions, which undergo a nucleophilic substitution reaction with the silanol groups on the surface of the montmorillonite sheets, with fluoride atoms covalently replacing some of the hydroxyl groups. The hydrothermal conditions provide a uniform temperature and pressure field, promoting the entry of fluoride ions into the interlayer and their reaction with the surface. After the reaction, the nanosheets are centrifuged and washed until neutral to remove unreacted ammonium fluoride and byproducts. Subsequently, the fluorinated modified montmorillonite is dispersed in an aqueous solution of alkali metal lithium salt. Lithium ions replace the original sodium ions in the interlayer through ion exchange, converting the interlayer cations into lithium ions. After drying and grinding, lithium-fluorinated montmorillonite nanosheets are obtained. This step involves fluorination before lithiation to prevent lithium ions from being eluted during the fluorination process.
[0074] Step 2 involves the preparation of the premix. 1,3-propane sulpholactone plasticizer, alkali metal lithium salt, and allyl-functionalized ionic liquid monomer are mixed under an inert atmosphere. The inert atmosphere prevents the decomposition of the alkali metal lithium salt and the oxidation of 1,3-propane sulpholactone by moisture and oxygen in the air. All three components are either liquid or soluble in liquid 1,3-propane sulpholactone, and the mixture forms a molecularly homogeneous premix. This premix ensures that the three functional components enter the melt in a uniform proportion during subsequent injection into the twin-screw extruder, avoiding incomplete reactions caused by uneven local concentrations.
[0075] Step 3 involves the preparation of organofluorinated lithium montmorillonite nanosheets. The lithium fluorinated montmorillonite nanosheets are pre-condensed with a mercaptosilane coupling agent under an inert atmosphere. The siloxane groups of the mercaptosilane coupling agent condense with the residual silanol groups on the surface of the lithium fluorinated montmorillonite, forming siloxane-silicon covalent bonds and removing small molecule alcohols. The pre-condensation is carried out at 60°C to 90°C, a temperature lower than the processing temperature of a twin-screw extruder, to prevent the silane coupling agent from undergoing self-condensation or mercapto oxidation before entering the high-temperature zone. After pre-condensation, a mercapto-containing organic coating layer is formed on the surface of the nanosheets, providing uniformly distributed reaction sites for the subsequent thiol-ene click reaction.
[0076] Step 4 is reactive melt blending. Polyphenylene sulfide resin and antioxidant are added through the main feed port, the premix is injected through the liquid injection port, and the organic fluorinated lithium-ion montmorillonite nanosheets are added through the side feed port. The main feed port is located in the first temperature zone of the extruder, where the resin begins to melt. The liquid injection port is located in the third temperature zone, where the resin is completely melted, allowing for rapid dispersion of the premix after injection. The side feed port is located in the fourth temperature zone, where the melt temperature has risen above 285°C, and the organic nanosheets immediately mix with the melt and undergo a thiol-ene click reaction upon addition. At 270°C to 300°C and a screw speed of 100 rpm to 300 rpm, the ring-opening grafting of 1,3-propanesulfonyl lactone and the thiol-ene click reaction occur simultaneously. The screw provides shear force, promoting nanosheet dispersion and reactant contact. The reactive melt blending is completed to obtain the blend.
[0077] Step 5 is hot pressing for film formation. The blend is crushed and placed in a mold for hot pressing. Crushing to an appropriate particle size facilitates uniform spreading within the mold. The hot pressing temperature is 260℃ to 280℃, slightly lower than the processing temperature of a twin-screw extruder. At this temperature, the cross-linked network has largely formed, and hot pressing primarily serves to densify and shape the material. A pressure of 10MPa to 20MPa allows the blend to flow fully and expel residual gas. Holding pressure for 10 to 30 minutes relaxes the internal stress of the film, forming a uniform and dense structure. After hot pressing, a polyphenylene sulfide-based solid electrolyte membrane containing 1,3-propane sulfonyl lactone plasticizer is obtained.
[0078] In Example 7, in step 1, the concentration of the ammonium fluoride aqueous solution was 0.5 mol / L to 2.0 mol / L, and the solid-liquid ratio of sodium montmorillonite to the ammonium fluoride aqueous solution was 1:50 to 1:100; centrifugation and washing were performed until the pH of the washing solution was 6 to 7; the concentration of the alkali metal lithium salt aqueous solution was 0.5 mol / L to 1.5 mol / L; the drying temperature was 60 to 90°C; and the material was ground until D50 was less than or equal to 10 μm.
[0079] By employing the above technical solution, the concentration of the ammonium fluoride aqueous solution is 0.5 mol / L to 2.0 mol / L. If the concentration is too low, the fluorination reaction rate is slow, and the degree of fluorine substitution is insufficient; if the concentration is too high, the ammonium fluoride itself decomposes rapidly, and excessive fluorination damages the layered structure of montmorillonite. The solid-liquid ratio of sodium-based montmorillonite to the ammonium fluoride aqueous solution is 1:50 g / mL to 1:100 g / mL. If the solid-liquid ratio is too high, the total amount of ammonium fluoride is insufficient, and fluorine substitution is uneven; if the solid-liquid ratio is too low, too much solution is used, increasing the burden on subsequent centrifugal washing. Centrifugation and washing are performed until the pH of the washing solution reaches 6 to 7 to remove residual ammonium fluoride and hydrogen fluoride, preventing acidic substances from affecting lithium-ion exchange in subsequent steps. The concentration of the alkali metal lithium salt aqueous solution is 0.5 mol / L to 1.5 mol / L. This concentration range provides sufficient lithium-ion concentration to fully replace interlayer sodium ions, while avoiding excessive concentration that would lead to lithium salt waste and washing difficulties. The drying temperature is 60℃ to 90℃, within which moisture can be completely removed and the interlayer structure of the lithium fluoride montmorillonite nanosheets will not collapse due to excessive temperature. Grinding to a D50 of less than or equal to 10μm ensures good dispersibility of the nanosheets in subsequent melt blending, avoiding localized agglomeration caused by excessively large particle size.
[0080] In Example 8, the inert atmosphere in step 2 is argon or nitrogen; the mixing temperature is 40℃~70℃, and the mixing time is 0.5h~2h; the molar ratio of 1,3-propane sulfonyl lactone plasticizer, alkali metal lithium salt and allyl functionalized ionic liquid monomer is 1:0.5~1:2:0.1~0.5.
[0081] By adopting the above technical solution, the inert atmosphere in step 2 is argon or nitrogen. Both are chemically inert gases, which can effectively isolate moisture and oxygen in the air. The mixing temperature is 40℃ to 70℃. At this temperature range, 1,3-propanesulfonyl lactone remains liquid and does not undergo thermal ring-opening, allowing the alkali metal lithium salt and allyl functionalized ionic liquid monomer to fully dissolve and form a uniform and transparent premix. If the mixing temperature is below 40℃, the alkali metal lithium salt dissolves slowly, resulting in uneven mixing; if it is above 70℃, 1,3-propanesulfonyl lactone may begin partial ring-opening, leading to premature uncontrollable reactions in the premix. The mixing time is 0.5h to 2h to ensure that all components achieve molecular-level uniform mixing. The molar ratio of 1,3-propanesulfonyl lactone plasticizer, alkali metal lithium salt, and allyl functionalized ionic liquid monomer is 1:0.5 to 1:2:0.1 to 0.5. This molar ratio determines the relative amounts of the lithium sulfonate precursor, free lithium salt, and crosslinked monomers in the system. If the lithium salt molar ratio is too low, the free carrier concentration is insufficient; if it is too high, undissociated lithium salts aggregate to form ion pairs or clusters. If the allyl-functionalized ionic liquid monomer molar ratio is too low, there are too few crosslinking points and the crosslinking network is incomplete; if the molar ratio is too high, the crosslinking density is too high, restricting chain segment movement.
[0082] In Example 9, the inert atmosphere in step 3 is argon or nitrogen; the pre-condensation reaction temperature is 60℃~90℃, and the reaction time is 0.5h~2h; the mass ratio of lithium fluoride montmorillonite nanosheets to mercaptosilane coupling agent is 1:0.05~1:0.3.
[0083] By adopting the above technical solution, the inert atmosphere in step 3 is argon or nitrogen to prevent the mercapto groups from being oxidized to disulfide bonds during the pre-condensation process. The pre-condensation reaction temperature is 60℃ to 90℃. Within this temperature range, the condensation reaction rate between the siloxane groups and the silanol groups on the surface of lithium fluoride montmorillonite is moderate, and the reaction can proceed fully within 0.5h to 2h. If the temperature is below 60℃, the condensation reaction rate is too slow, and the pre-condensation is insufficient; if the temperature is above 90℃, the self-condensation of the silane coupling agent intensifies, forming free oligomeric siloxanes. The reaction time is 0.5h to 2h, matched with the reaction temperature, to ensure that the siloxane groups and surface hydroxyl groups react fully. The mass ratio of lithium fluoride montmorillonite nanosheets to mercapto-containing silane coupling agent is 1:0.05 to 1:0.3. This mass ratio ensures that the silane coupling agent forms a uniform coating of monolayer to several molecular layers on the surface of the nanosheets. When the mass ratio is less than 1:0.05, the surface thiol density is insufficient, resulting in too few subsequent crosslinking points; when the mass ratio is greater than 1:0.3, the excess silane coupling agent exists in a free form and self-condenses during subsequent high-temperature extrusion, reducing the uniformity and density of the electrolyte membrane.
[0084] In Example 10, the twin-screw extruder in step 4 is a co-rotating twin-screw extruder with a length-to-diameter ratio of 36:1 to 48:1, and has eight temperature zones: the first to third temperature zones are 270℃ to 280℃, the fourth to sixth temperature zones are 285℃ to 300℃, and the seventh to eighth temperature zones are 275℃ to 285℃; the liquid injection port is located in the third temperature zone, and the side feed port is located in the fourth temperature zone; the reactive melt blending time is 2 min to 6 min; the particle size of the blend after crushing in step 5 is less than or equal to 500 μm; the hot pressing is carried out in stages: first, pre-pressing at 260℃ to 265℃ and 5 MPa for 5 min, then holding at 270℃ to 280℃ and 15 MPa for 10 min to 30 min; then cooling to room temperature at 0.5℃ / min to 2℃ / min and demolding to obtain a polyphenylene sulfide-based solid electrolyte membrane with a thickness of 50 μm to 200 μm.
[0085] By adopting the above technical solution, the twin-screw extruder in step 4 is a co-rotating twin-screw extruder with an aspect ratio of 36:1 to 48:1. The aspect ratio determines the residence time of the material in the extruder. If the aspect ratio is too small, the reaction time is insufficient, and the grafting and crosslinking reactions are incomplete; if the aspect ratio is too large, the material residence time is too long, and the polyphenylene sulfide resin may undergo thermal degradation. Eight temperature zones are set: zones one to three are 270℃ to 280℃, zones four to six are 285℃ to 300℃, and zones seven to eight are 275℃ to 285℃. Zones one to three allow the polyphenylene sulfide resin to completely melt but not yet reach the violent ring-opening temperature of 1,3-propanesulfonyl lactone, ensuring that the premix is fully mixed with the melt after injection before entering the high-temperature zone. Zones four to six are the main reaction zones, where the ring-opening grafting reaction of 1,3-propanesulfonyl lactone and the thiol-ene click reaction proceed simultaneously and rapidly within this temperature range. The temperature drops slightly in the seventh and eighth temperature zones, allowing the reaction to proceed more completely and reducing melt viscosity, which is beneficial for subsequent extrusion granulation. The liquid injection port is located in the third temperature zone, where the resin is completely melted, and the liquid premix can be rapidly dispersed under screw shear after injection. The side feed port is located in the fourth temperature zone, where the melt temperature has risen above 285℃, and the organic nanosheets immediately participate in the cross-linking reaction after addition. The reactive melt blending time is 2 to 6 minutes. This time range is matched with the aspect ratio and screw speed to ensure that the reaction is fully completed without causing thermal degradation.
[0086] In step 5, the particle size of the crushed blend is less than or equal to 500 μm. This particle size range ensures that the blend is evenly spread in the hot press mold, avoiding uneven thickness caused by large particles. Hot pressing is carried out in stages: first, pre-pressing at 260℃ to 265℃ and 5MPa for 5 min, then holding at 270℃ to 280℃ and 15MPa for 10 min to 30 min. The pre-pressing stage has a slightly lower temperature and pressure to remove residual air between the blend particles and to initially compact the material. In the holding stage, the temperature is increased to 270℃ to 280℃ and the pressure is increased to 15MPa, allowing the blend to flow fully in the mold and form a dense and uniform film structure. Subsequently, it is cooled to room temperature at a rate of 0.5℃ / min to 2℃ / min and then demolded. Slow cooling gradually releases the thermal stress within the film, reduces the generation of microcracks, and ensures the integrity and mechanical strength of the electrolyte membrane. The final result is a polyphenylene sulfide-based solid electrolyte membrane with a thickness of 50 μm to 200 μm, which is suitable for the electrolyte layer in solid-state batteries.
[0087] The following specific embodiments illustrate the implementation principle of the present invention:
[0088] A polyphenylene sulfide-based solid electrolyte containing 1,3-propane sulfonyl lactone plasticizer is used in lithium metal solid-state batteries. Based on 100g of polyphenylene sulfide resin, the composition includes 100g of polyphenylene sulfide resin, 12g of 1,3-propane sulfonyl lactone plasticizer, 20g of alkali metal lithium salt, 10g of lithium fluoride montmorillonite nanosheets, 1.5g of mercaptosilane coupling agent, 4g of allyl-functionalized ionic liquid monomer, and 0.5g of antioxidant. The alkali metal lithium salt is a mixture of 15g of lithium bis(trifluoromethanesulfonyl)imide and 5g of lithium difluorooxalate borate. The mercaptosilane coupling agent is γ-mercaptopropyltriethoxysilane. The allyl-functionalized ionic liquid monomer is 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide. The antioxidant is hindered phenolic antioxidant 1010. The selected polyphenylene sulfide resin had a weight-average molecular weight of 52,000, a melt index of 120 g / 10 min measured at 315℃ and 5 kg load, and a moisture content of 0.03 wt%. The lithium fluoride montmorillonite nanosheets had a layer thickness of 2 nm, a sheet diameter of 300 nm, a fluorine content of 3.2 wt%, and an interlayer lithium-ion exchange capacity of 1.0 mmol / g.
[0089] The preparation method is as follows. Step 1: 10g of sodium-based montmorillonite was added to 600mL of a 1.0mol / L ammonium fluoride aqueous solution, with a solid-liquid ratio of 1:60g / mL. The mixture was hydrothermally reacted at 90℃ for 12h, centrifuged at 10000rpm for 10min, and washed with deionized water until the pH of the washing solution reached 6.8. Then, it was dispersed in a 0.8mol / L lithium bis(trifluoromethanesulfonyl)imide aqueous solution and subjected to ion exchange at 60℃ for 8h. After centrifugation, washing with deionized water, and vacuum drying at 80℃ for 12h, the mixture was ground to a D50 of 8μm to obtain lithium fluoride montmorillonite nanosheets. Step 2: Under an argon atmosphere, 1,3-propanesulfonyl plasticizer, alkali metal lithium salt, and allyl-functionalized ionic liquid monomer were mixed at a molar ratio of 1:1:0.2 and stirred at 50℃ for 1h to obtain a transparent premix. Step 3: Under an argon atmosphere, lithium fluorinated montmorillonite nanosheets and γ-mercaptopropyltriethoxysilane are mixed at a mass ratio of 1:0.15 and pre-condensed at 80°C for 1 hour to obtain organic lithium fluorinated montmorillonite nanosheets. Step 4: Polyphenylene sulfide resin and antioxidant are added to the main feed port of a co-rotating twin-screw extruder. The premix is injected from the liquid injection port of the third temperature zone, and the organic lithium fluorinated montmorillonite nanosheets are added from the side feed port of the fourth temperature zone. The extruder's first to third temperature zones are set to 270°C, 275°C, and 280°C respectively; the fourth to sixth temperature zones are set to 290°C, 295°C, and 290°C respectively; and the seventh to eighth temperature zones are set to 285°C and 280°C respectively. The screw speed is 200 rpm, and reactive melt blending is performed for 4 minutes to obtain the blend. Step 5: The blend is crushed to a particle size of 200 μm, placed in a mold, pre-pressed at 265℃ and 5 MPa for 5 min, then held at 275℃ and 15 MPa for 15 min, cooled to room temperature at 1℃ / min, and demolded to obtain a 120 μm thick polyphenylene sulfide-based solid electrolyte membrane containing 1,3-propane sulfonyl lactone plasticizer, which is then vacuum dried at 80℃ for 12 h. This solid electrolyte membrane is used in lithium metal solid-state batteries, with lithium iron phosphate as the positive electrode and lithium metal as the negative electrode.
[0090] Comparative Example: A conventional polyphenylene sulfide (PPS)-based solid electrolyte, based on 100g of PPS resin, comprises 100g of PPS resin, 20g of alkali metal lithium salt, 10g of ordinary sodium montmorillonite, and 0.5g of antioxidant. The alkali metal lithium salt is lithium bis(trifluoromethanesulfonyl)imide. The antioxidant is hindered phenolic antioxidant 1010. The preparation method involves directly adding the PPS resin, alkali metal lithium salt, ordinary sodium montmorillonite, and antioxidant to the main feed inlet of a co-rotating twin-screw extruder, melting and blending at 280°C to 300°C and a screw speed of 200 rpm for 4 minutes, followed by crushing and hot pressing at 270°C and 15 MPa for 15 minutes to obtain a conventional PPS-based solid electrolyte membrane.
[0091] To objectively evaluate the differences in the overall performance of the two solid electrolytes, the polyphenylene sulfide-based solid electrolyte membrane containing 1,3-propane sulfonyl lactone plasticizer obtained from the complete specific implementation case and the traditional polyphenylene sulfide-based solid electrolyte membrane obtained from the comparative example were respectively assembled into lithium metal symmetric batteries and lithium iron phosphate full batteries. Under the same test conditions, the ionic conductivity, lithium-ion transport number, electrochemical window, tensile strength, thermal decomposition temperature, interfacial impedance, and full battery cycle performance were systematically tested. The test results are shown in Table 1.
[0092] Table 1
[0093]
[0094] This polyphenylene sulfide-based solid electrolyte, containing 1,3-propane sulfonate plasticizer, achieves ring-opening of 1,3-propane sulfonate at the melt blending temperature, followed by electrophilic substitution with the benzene ring of polyphenylene sulfide to form covalently grafted lithium propanesulfonate groups. This significantly reduces the crystallinity of polyphenylene sulfide and provides lithium ion coordination sites. Simultaneously, the allyl-functionalized ionic liquid monomer undergoes a thermally initiated thiol-ene click reaction with a mercaptosilane coupling agent to form an organic-inorganic interpenetrating crosslinked network, stably bridging lithium fluoride montmorillonite nanosheets to the polyphenylene sulfide matrix. The ionic liquid cation further promotes lithium salt dissociation. These synergistic effects enable this solid electrolyte to maintain high mechanical strength and high heat resistance while achieving... It exhibits high room temperature ionic conductivity, a lithium-ion transference number of 0.72, and an electrochemical window of 5.2V. Its interface impedance is as low as 50Ωcm², and its capacity retention reaches 95% after 100 full-cell cycles. Its overall performance is significantly better than that of traditional polyphenylene sulfide-based solid electrolytes.
[0095] This traditional polyphenylene sulfide (PPS)-based solid electrolyte is prepared solely through a simple physical melt blending of PPS resin with alkali metal lithium salts and ordinary montmorillonite. The PPS molecular chains maintain high crystallinity, hindering chain segment movement. The lithium salts exhibit low dissociation and lack continuous lithium-ion conduction channels. The ordinary montmorillonite, without fluorination or lithiation modification, has poor compatibility with the PPS matrix and high interfacial impedance. Therefore, its room-temperature ionic conductivity is only [insert value here]. The lithium-ion transference number is as low as 0.25, the electrochemical window is only 4.0V, the tensile strength and thermal decomposition temperature are also significantly lower, and the capacity retention rate after 100 full-cell cycles is only 68%, which cannot meet the practical application requirements of high-performance lithium metal solid-state batteries.
[0096] The above are all preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Therefore, all equivalent changes made in accordance with the structure, shape and principle of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A PPS-based solid electrolyte containing 1,3-PS plasticizer, characterized in that, Based on 100 parts of polyphenylene sulfide resin, the following components are included: 100 parts of polyphenylene sulfide resin; 8-18 parts of 1,3-propanesulfonyl lactone plasticizer; 15-30 parts of alkali metal lithium salt; 5-15 parts of lithium fluoride montmorillonite nanosheets; Contains 0.8–3 parts of a mercaptosilane coupling agent; 2-8 parts of allyl-functionalized ionic liquid monomer; Antioxidant 0.1 to 1 part; In this process, the sulfonyl ring of the 1,3-propane sulfonyl lactone plasticizer undergoes ring-opening and electrophilic substitution with the benzene ring of the polyphenylene sulfide resin to form covalently grafted lithium propanesulfonate groups; the allyl functionalized ionic liquid monomer and the mercapto group in the mercaptosilane coupling agent undergo a thiol-ene click reaction at the melt blending temperature to form a crosslinked network; the lithium fluoride montmorillonite nanosheets are layered silicate nanosheets that have undergone hydrothermal treatment with ammonium fluoride and alkali metal lithium salt ion exchange treatment.
2. The PPS-based solid-state electrolyte containing 1,3-PS plasticizer according to claim 1, characterized in that, Based on 100 parts of polyphenylene sulfide resin, 10-14 parts of 1,3-propane sulfonyl lactone plasticizer, 18-25 parts of alkali metal lithium salt, 8-12 parts of lithium fluoride montmorillonite nanosheets, 1.0-2.0 parts of mercaptosilane coupling agent, and 3-5 parts of allyl functionalized ionic liquid monomer. The polyphenylene sulfide resin has a weight-average molecular weight of 40,000 to 70,000, a melt index of 80 g / 10 min to 150 g / 10 min measured at 315°C and 5 kg load, and a moisture content of less than or equal to 0.05 wt%.
3. The PPS-based solid-state electrolyte containing 1,3-PS plasticizer according to claim 2, characterized in that, The grafting rate of the 1,3-propane sulfonyl plasticizer to the polyphenylene sulfide resin in the polyphenylene sulfide-based solid electrolyte is 30% to 70%; the alkali metal lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalate borate.
4. The PPS-based solid-state electrolyte containing 1,3-PS plasticizer according to claim 3, characterized in that, The lithium fluorinated montmorillonite nanosheets have a sheet thickness of 1 nm to 5 nm, a sheet diameter of 100 nm to 500 nm, a fluorine content of 1 wt% to 5 wt%, and an interlayer lithium-ion exchange capacity of 0.8 mmol / g to 1.2 mmol / g; the mercaptosilane coupling agent is at least one of γ-mercaptopropyltriethoxysilane and γ-mercaptopropyltrimethoxysilane.
5. The PPS-based solid-state electrolyte containing 1,3-PS plasticizer according to claim 4, characterized in that, The allyl-functionalized ionic liquid monomer is at least one of 1-allyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt and 1-allyl-3-vinylimidazolium bis(fluorosulfonyl)imide salt; the antioxidant is at least one of hindered phenolic antioxidant 1010 and phosphite antioxidant 168.
6. A method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer, characterized in that: The preparation of the PPS-based solid electrolyte containing 1,3-PS plasticizer as described in claim 5 comprises the following steps: Step 1: Sodium-based montmorillonite is added to an aqueous solution of ammonium fluoride and hydrothermally reacted at 80℃~120℃ for 6h~24h. After centrifugation and washing until neutral, it is dispersed in an aqueous solution of alkali metal lithium salt and ion exchanged at 50℃~80℃ for 4h~12h. After drying and grinding, lithium-fluoride montmorillonite nanosheets are obtained. Step 2: Under an inert atmosphere, 1,3-propane sulfonyl lactone plasticizer, alkali metal lithium salt and allyl functionalized ionic liquid monomer are mixed to obtain plasticizer, lithium salt and ionic liquid premix. Step 3: The lithium fluoride montmorillonite nanosheets and the mercapto-containing silane coupling agent are subjected to a pre-condensation reaction at 60℃~90℃ for 0.5h~2h under an inert atmosphere to obtain organofluoride lithium fluoride montmorillonite nanosheets with mercapto groups on the surface. Step 4: Under an inert atmosphere, add polyphenylene sulfide resin and antioxidant to the main feed port of the twin-screw extruder; inject the premix obtained in S2 into the twin-screw extruder through the liquid injection port; add the organic fluorinated lithium montmorillonite nanosheets obtained in S3 through the side feed port; and carry out reactive melt blending at 270℃~300℃ and screw speed 100rpm~300rpm to obtain a blend. Step 5: After crushing the blend, hot press it into a film. The hot pressing temperature is 260℃~280℃, the pressure is 10MPa~20MPa, and the pressure is held for 10min~30min to obtain a polyphenylene sulfide-based solid electrolyte membrane containing 1,3-propane sulfonyl lactone plasticizer.
7. The method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer according to claim 6, characterized in that: In step 1, the concentration of the ammonium fluoride aqueous solution is 0.5 mol / L to 2.0 mol / L, and the solid-liquid ratio of sodium montmorillonite to the ammonium fluoride aqueous solution is 1:50 to 1:100; centrifugation and washing are performed until the pH of the washing solution is 6 to 7; the concentration of the alkali metal lithium salt aqueous solution is 0.5 mol / L to 1.5 mol / L; the drying temperature is 60 to 90℃, and the material is ground until D50 is less than or equal to 10 μm.
8. The method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer according to claim 7, characterized in that: In step 2, the inert atmosphere is argon or nitrogen; the mixing temperature is 40℃~70℃, and the mixing time is 0.5h~2h; the molar ratio of 1,3-propane sulfonyl lactone plasticizer, alkali metal lithium salt and allyl functionalized ionic liquid monomer is 1:0.5~1:2:0.1~0.
5.
9. The method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer according to claim 8, characterized in that: In step 3, the inert atmosphere is argon or nitrogen; the pre-condensation reaction temperature is 60℃~90℃, and the reaction time is 0.5h~2h; the mass ratio of lithium fluoride montmorillonite nanosheets to mercaptosilane coupling agent is 1:0.05~1:0.
3.
10. The method for preparing a PPS-based solid electrolyte containing 1,3-PS plasticizer according to claim 9, characterized in that: In step 4, the twin-screw extruder is a co-rotating twin-screw extruder with a length-to-diameter ratio of 36:1 to 48:1, and has eight temperature zones: the first to third temperature zones are 270℃ to 280℃, the fourth to sixth temperature zones are 285℃ to 300℃, and the seventh to eighth temperature zones are 275℃ to 285℃; the liquid injection port is located in the third temperature zone, and the side feed port is located in the fourth temperature zone; the reactive melt blending time is 2 min to 6 min; in step 5, the particle size of the blend after crushing is less than or equal to 500 μm; the hot pressing is carried out in stages: first, pre-pressing at 260℃ to 265℃ and 5 MPa for 5 min, then holding at 270℃ to 280℃ and 15 MPa for 10 min to 30 min; then cooling to room temperature at 0.5℃ / min to 2℃ / min and demolding to obtain a polyphenylene sulfide-based solid electrolyte membrane with a thickness of 50 μm to 200 μm.