A PEO-based all-solid-state polymer electrolyte, its preparation method and application

By synergistically designing basalt fiber and g-C3N4 composite functional filler, the problems of high crystallinity and low ionic conductivity of PEO-based solid electrolytes were solved, achieving efficient Li+ transport and mechanical reinforcement, and improving the overall performance of the electrolyte.

CN123120859APending Publication Date: 2026-11-17HENAN UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611392194.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

PEO-based solid electrolytes have high crystallinity at room temperature, low ionic conductivity, and insufficient mechanical properties, making them difficult to meet the needs of practical applications.

Method used

By employing basalt fiber and g-C3N4 composite functional filler, and through dimensional complementary design, PEO crystallization is synergistically suppressed, a highly efficient Li+ transport network is constructed, and the overall performance of the electrolyte is improved.

Benefits of technology

It significantly improves room temperature ionic conductivity, enhances mechanical properties, broadens the electrochemical stability window, and improves battery cycle life and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120859A_ABST
    Figure CN123120859A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of lithium battery solid electrolyte materials technology, and discloses a PEO-based all-solid polymer electrolyte, its preparation method, and its application, solving the technical problems of low room-temperature ionic conductivity, high crystallinity, and insufficient mechanical properties of PEO-based solid electrolytes. A PEO-based all-solid polymer electrolyte includes a PEO matrix, a lithium salt, and a composite functional filler; wherein the composite functional filler is basalt fiber with g-C3N4 loaded on its surface, and the mass ratio of basalt fiber to g-C3N4 is 1:0.05-0.8. This composite functional filler significantly reduces the crystallinity of PEO through the synergistic effect of the three-dimensional network skeleton effect of basalt fiber and the local crystallization inhibition effect of g-C3N4; simultaneously, the polar groups on the fiber surface and the layered structure of g-C3N4 synergistically construct a highly efficient lithium electrolyte. + The transmission channel significantly improves ionic conductivity. The electrolyte described in this invention achieves a room temperature ionic conductivity of up to 10. ‑4 With a strength above mS / cm, it also possesses excellent mechanical properties and electrochemical stability, effectively suppressing lithium dendrite growth, making it suitable for all-solid-state lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid electrolyte materials technology for new energy lithium-ion batteries, and particularly relates to a PEO-based all-solid polymer electrolyte. Background Technology

[0002] With the rapid development of portable electronic devices and electric vehicles, the demand for high-energy-density and high-safety energy storage systems is becoming increasingly urgent. Currently, traditional lithium-ion batteries generally use organic liquid electrolytes, which pose safety hazards such as leakage, combustion, and even explosion, making them unable to meet increasingly stringent safety requirements. All-solid-state lithium batteries, by replacing liquid organic electrolytes with solid electrolytes, fundamentally solve the safety problem and are expected to achieve higher energy densities, thus being considered an important development direction for next-generation lithium battery technology.

[0003] Among numerous solid-state electrolyte materials, polyethylene oxide (PEO)-based solid polymer electrolytes have attracted considerable attention due to their unique advantages. PEO exhibits excellent solubility for lithium salts, effectively dissociating them and promoting Li⁺ transport. Simultaneously, PEO possesses superior flexibility and film-forming properties, is easy to process, and demonstrates good chemical / mechanical compatibility with lithium metal anodes, making it one of the most promising solid-state electrolyte matrix materials. However, the practical application of PEO-based solid-state electrolytes faces several key technical bottlenecks, the most critical of which is the high crystallinity of PEO at room temperature. The crystalline regions formed by the regular arrangement of PEO molecular chains severely restrict chain segment movement, resulting in extremely low ionic conductivity at room temperature, typically only 10⁻⁶. -8 ~10 -6 The S / cm ratio is far from meeting the needs of practical applications. In addition, the electrochemical stability window of PEO-based electrolytes is narrow (usually below 3.9 V), which limits their compatibility with high-voltage cathode materials; at the same time, insufficient mechanical strength leads to a high risk of lithium dendrite puncture, affecting the cycle life and safety of the battery.

[0004] To address the aforementioned issues, researchers have proposed various modification strategies, including: (1) adding inorganic fillers to form composite polymer electrolytes, which inhibit crystallization through interfacial interactions between the fillers and PEO segments; (2) introducing plasticizers or organic additives to reduce the crystallinity of PEO; and (3) designing block copolymers or cross-linked network structures to alter the movement characteristics of polymer segments. Among these, adding inorganic nanofillers to construct composite polymer electrolytes is considered one of the most effective and simplest strategies.

[0005] In recent years, graphitic carbon nitride (g-C3N4), as a novel two-dimensional inorganic material, has attracted attention due to its unique electronic structure and abundant surface functional groups. Previous studies have incorporated g-C3N4 as an inorganic filler into PEO-based solid electrolytes. For example, some studies have prepared g-C3N4 using thermal polymerization and blended it with polyethylene oxide / lithium perchlorate (PEO / LiClO4) to prepare composite polymer solid electrolytes. The results showed that the internal interactions within the composite electrolyte could suppress PEO crystallization to a certain extent. However, the existing technologies still have the following shortcomings: firstly, the dispersibility of g-C3N4 as an inorganic filler in the PEO matrix needs improvement, its inhibitory effect on PEO crystallization is not ideal, and the improvement in room temperature ionic conductivity is limited, making it difficult to meet practical application requirements.

[0006] Therefore, developing a novel PEO-based solid electrolyte and its preparation method that can effectively inhibit PEO crystallization, significantly improve room temperature ionic conductivity and enhance mechanical properties is of great research significance and application value. Summary of the Invention

[0007] To address the technical problems of existing PEO-based solid electrolytes, such as low room-temperature ionic conductivity, high crystallinity, and insufficient mechanical properties, this invention proposes a PEO-based all-solid-state polymer electrolyte, its preparation method, and its applications. Through the design of a composite functional filler of basalt fiber and g-C3N4, synergistic inhibition of PEO crystallization and the construction of a highly efficient Li-based electrolyte are achieved. + The goal is to improve the transmission network and enhance the overall performance of the electrolyte.

[0008] To achieve the above objectives, the technical solution of the present invention is implemented as follows:

[0009] A PEO-based all-solid polymer electrolyte includes a PEO matrix, a lithium salt, and a composite functional filler; wherein the composite functional filler is basalt fiber with g-C3N4 loaded on its surface (the loading method can be chemical bonding or physical adsorption, etc.), and the mass ratio of basalt fiber to g-C3N4 is 1:0.05-0.8.

[0010] By loading two-dimensional g-C3N4 nanosheets onto the surface of one-dimensional basalt fibers, a synergistic design with complementary dimensions is achieved. On one hand, the one-dimensional fibers spontaneously form a three-dimensional permeable network within the PEO matrix, while the g-C3N4 loaded on the fiber surface provides highly active interfaces at each "node" and "branch" of this network. Simultaneously, the three-dimensional network of basalt fibers divides the PEO matrix into micron-scale confined regions, while the two-dimensional sheets of g-C3N4 further divide the space into nanoscale regions. This dual-scale spatial confinement significantly affects the conformational entropy of PEO segments, causing them to tend to adopt a more extended conformation rather than folding into a crystalline state, thus effectively inhibiting crystallization. On the other hand, this invention combines basalt fibers (possessing both inert and active characteristics) with g-C3N4 (a typical active filler), achieving functional division: the basalt fibers provide a three-dimensional physical barrier to disrupt the regular arrangement of chain segments, and the surface hydroxyl groups and TFSI... - Hydrogen bonding promotes lithium salt dissociation, the fiber surface serves as a fast transport channel, and mechanical reinforcement inhibits dendrite penetration; g-C3N4 induces amorphous conformation through coordination of PEO with surface Lewis base sites, and N atoms provide Lewis acid sites to promote Li... + -Anion dissociation and interlayer channels provide Li + Jumping sites lower the migration energy barrier and induce the formation of a stable LiF-rich SEI film. The synergy between these two factors achieves macro- and micro-scale dual-scale crystallization inhibition, anion fixation and cation activation, surface conduction and interlayer conduction synergy, and a combination of physical barriers and chemical passivation.

[0011] The "dual-mode" crystallization inhibition mechanism overcomes the limitations of a single filler system through the structural design of the composite filler. Mode 1 is "short-range amorphization" induced by the fiber surface: hydroxyl groups on the surface of basalt fibers combine with the ether oxygen atoms of PEO through hydrogen bonds, inducing PEO segments to adopt an amorphous conformation in the near-surface region of the fiber. The large aspect ratio of the basalt fibers allows the "amorphous shell" to form a continuous "amorphous skeleton" in the matrix. Mode 2 is "long-range chemical inhibition" by g-C3N4: nitrogen-containing functional groups and Lewis base sites on the surface of g-C3N4 disrupt the local conformational order of PEO segments through weak Lewis acid-base interactions. This interaction is of moderate strength and can still affect the conformational entropy of the segments at a relatively long distance. The "amorphous region connectivity effect" generated by the synergy of the two modes enables the short-range amorphization of fibers to construct an amorphous phase network framework on a macroscopic scale, while the long-range chemical inhibition of g-C3N4 further expands the thickness of the "amorphous shell" of each fiber on a microscopic scale, and makes the amorphous regions between different fibers overlap and connect with each other.

[0012] In terms of ion transport mechanism: when g-C3N4 is loaded onto the surface of basalt fibers, Li +The transport path becomes: PEO segment transport → g-C3N4 interlayer hopping → fiber surface migration → next g-C3N4 sheet. This multi-step relay mechanism will transfer Li + The migration mechanism shifted from a "pure segment motion-dependent" mode to a hybrid conduction mode involving "segment motion + interface hopping + intralayer migration," significantly broadening the types and number of ion transport pathways. Simultaneously, hydroxyl groups on the basalt fiber surface and nitrogen-containing groups on the g-C3N4 surface interact with TFSI through hydrogen bonds or weak electrostatic interactions. - Anion binding occurs, producing an "anion anchoring" effect; the Lewis base site of g-C3N4 binds to Li. + The weak coordination effect reduced the Li + The effective coordination number between Li and the oxygen atom of PEO ether makes Li + "Dissociation" from PEO segments is more likely to occur. Anions are fixed on the filler surface, and cations are "activated" by g-C3N4. The synergistic effect of the two increases the lithium-ion transference number from that of the pure PEO system.

[0013] The "mechanical-electrochemical" coupling enhancement mechanism: The composite filler of this invention achieves decoupling of mechanical properties and ionic conductivity through the functional division of "rigid skeleton bearing the load and active interface undertaking the transport." The three-dimensional network of basalt fibers (Young's modulus ~90 GPa) acts as a mechanical "load-bearing skeleton" in the PEO matrix, preferentially bearing stress under tension or compression, protecting the PEO matrix from large deformation; while ion conduction mainly occurs in the interlayer of g-C3N4 and on the fiber surface, and these conduction paths do not depend on the large movement of PEO chain segments. Therefore, the electrolyte of this invention possesses both high conductivity and high mechanical strength.

[0014] The aforementioned basalt fibers are surface-activated chopped basalt fibers or ground basalt fibers; the diameter of the chopped basalt fibers or ground basalt fibers is 5-20 μm, and the length is 10-2000 μm. Further, the diameter of the aforementioned chopped basalt fibers or ground basalt fibers is 5-15 μm, the length is 50-2000 μm, and the aspect ratio is 3-400.

[0015] Furthermore, the aforementioned surface activation treatment refers to treating chopped basalt fibers or ground basalt fibers with at least one of hydroxyl, carboxyl, and amino groups.

[0016] The above-mentioned g-C3N4 has a layered structure with a sheet diameter of 100-5000 nm and a thickness of 2-100 nm.

[0017] The amount of the above-mentioned composite functional filler added is 1%-20% of the mass of the PEO matrix; the mass ratio of lithium salt to PEO matrix is ​​1:2-6. Among them, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or lithium bis(fluorosulfonyl)imide (LiFSI).

[0018] The preparation method of the above-mentioned PEO-based all-solid-state polymer electrolyte comprises the following steps:

[0019] (1) Continuous basalt fibers are chopped or ground to obtain chopped basalt fibers or ground basalt fibers. The basalt fibers can be obtained commercially or by self-production. The specific preparation steps for self-production are as follows: natural basalt ore is crushed into particles with a particle size of 1-10 mm, washed and dried, and then put into an electric arc furnace or resistance furnace. It is melted at 1500-1700℃ for 2-4 hours. The melt is drawn into fibers through a platinum-rhodium alloy spinneret, and the drawing speed is controlled at 500-2000 m / min to obtain continuous basalt fibers.

[0020] (2) The chopped basalt fibers or ground basalt fibers obtained in step (1) are subjected to at least one surface activation treatment of hydroxyl, carboxyl, and amino groups to obtain activated basalt fibers. For example, the surface activation treatment is at least one of hydrogen peroxide solution oxidation treatment, low-temperature plasma treatment, and a combined process of first performing hydrogen peroxide solution oxidation treatment and then performing low-temperature plasma treatment. The process conditions for hydrogen peroxide treatment are: hydrogen peroxide volume fraction 5%-30%, treatment temperature 50-90℃, and treatment time 1-6 hours. The process conditions for low-temperature plasma treatment are: oxygen or air atmosphere, treatment power 30-200 W, treatment time 5-30 minutes, and air pressure 10-100 Pa. Through hydrogen peroxide oxidation and / or plasma treatment, hydroxyl and a small amount of carboxyl groups are introduced into the surface of the basalt fibers. These functional groups serve as chemical anchoring points for g-C3N4 and achieve a firm loading of g-C3N4 through hydrogen bonding or esterification reactions. On the other hand, as adsorption sites for PEO segments, an amorphous PEO layer is induced to form on the fiber surface through hydrogen bonding between PEO ether oxygen atoms and surface hydroxyl groups. The "amorphous PEO layer" on the fiber surface and the "Lewis acid-ether oxygen coordination layer" on the g-C3N4 surface work together to form a double-layer amorphous region around the filler, significantly increasing the volume fraction of the PEO amorphous phase.

[0021] (3) Activated basalt fibers are composited with g-C3N4 in situ or out-of-situ to obtain basalt fibers with g-C3N4 loaded on the surface. The specific process steps of in situ composite are as follows: the activated basalt fibers are uniformly mixed with melamine or urea and placed in a covered crucible. The temperature is raised to 400-600℃ in a tube furnace at a heating rate of 2-10℃ / min and held for 2-4 hours for thermal polycondensation reaction. After natural cooling, the mixture is ground to obtain g-C3N4 powder with a sheet diameter of 200-400 nm. Out-of-situ composite refers to solvent dispersion or grinding of the activated basalt fibers with the pre-prepared g-C3N4 powder. Optionally, a silane coupling agent or a titanate coupling agent is added during this composite process. The amount of coupling agent is 1%-5% of the mass of the basalt fibers.

[0022] (4) Dissolve the PEO matrix and lithium salt in an organic solvent (such as anhydrous acetonitrile or tetrahydrofuran), stir at 40-60℃ until completely dissolved, add the basalt fiber with surface-loaded g-C3N4 obtained in step (3), stir for 4-12 hours until uniform, pour into a mold (such as polytetrafluoroethylene or glass), let stand at room temperature for 12-24 hours to allow the solvent to evaporate, and then vacuum dry at 40-80℃ for 12-36 hours to obtain the PEO-based all-solid polymer electrolyte. The basalt fiber with surface-loaded g-C3N4 (i.e., composite functional filler) can also be added by ultrasonic-assisted dispersion, with an ultrasonic time of 30-60 minutes and an ultrasonic power of 100-300 W.

[0023] An all-solid-state lithium battery includes a positive electrode, a negative electrode, and the aforementioned PEO-based all-solid-state polymer electrolyte.

[0024] The beneficial effects of this invention are:

[0025] (1) In this invention, the basalt fiber / g-C3N4 composite functional filler synergistically inhibits PEO crystallization through multiple pathways. First, basalt fiber, as a one-dimensional inorganic filler, has a large aspect ratio and specific surface area, enabling it to form a three-dimensional network structure in the PEO matrix. This network structure can effectively disrupt the regular arrangement of PEO molecular chains, acting as physical crosslinking points and nucleation inhibitors during crystallization, thereby reducing the crystallization temperature and crystallinity of PEO. Second, g-C3N4, as a two-dimensional layered material, has abundant nitrogen-containing functional groups (such as -NH2, =NH, etc.) on its surface, which can form hydrogen bonds with ether oxygen atoms in PEO segments, further disrupting the orderly arrangement of PEO molecular chains and inhibiting the formation and growth of crystalline regions. At the same time, the layered structure of g-C3N4 can form a "physical barrier" in the matrix, hindering the regular stacking of PEO segments. More importantly, the composite structure of basalt fiber and g-C3N4 produces a "synergistic crystallization inhibition effect": the three-dimensional network of basalt fiber divides the PEO matrix into micro-regions, while g-C3N4 loaded on the fiber surface plays a local role in inhibiting crystallization in each micro-region. The combination of the two achieves comprehensive crystallization inhibition from the macro to the micro scale.

[0026] (2) In this invention, the composite functional filler not only inhibits crystallization, but also actively constructs a highly efficient Li + Transport channels. The large number of hydroxyl groups (-OH) introduced into the surface of basalt fibers after activation treatment can react with lithium salt anions (such as TFSI). - Hydrogen bonds are formed, promoting the dissociation of lithium salts and increasing the number of free Li. + Concentration. Simultaneously, the polar groups on the fiber surface can adsorb Li. + This forms an "ion migration highway" on its surface. The layered structure of g-C3N4 contains regular channels, and the nitrogen vacancies and edge functional groups formed in-plane can act as Li... + The skipping site reduces Li + The migration energy barrier. When g-C3N4 is loaded on the surface of basalt fibers, the multi-level interface structure of "fiber-g-C3N4-PEO" formed at the interface between the two is Li + It provides a continuous, low-barrier transmission path. This structure effectively shortens the Li... + The migration distance in the PEO amorphous region enables a shift from a "chain segment motion-dependent" to an "interface transport-dominated" ion conduction mechanism.

[0027] (3) The basalt fiber used in this invention has high strength and high modulus. Its three-dimensional network structure plays a "skeleton reinforcement" role in the PEO matrix, significantly improving the tensile strength and puncture resistance of the electrolyte membrane and effectively inhibiting the growth and penetration of lithium dendrites. In addition, basalt fiber has excellent heat resistance (the operating temperature can reach above 600℃), and its introduction can significantly improve the thermal decomposition temperature and thermal dimensional stability of the composite electrolyte. Finally, the semiconductor properties of g-C3N4 can induce the formation of a stable electrode / electrolyte interface layer (SEI), suppress interfacial side reactions, broaden the electrochemical stability window of the electrolyte, and improve electrochemical stability. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0029] Figure 1 These are scanning electron microscope (SEM) images of the basalt fiber material of the present invention at low magnification (a) and high magnification (b).

[0030] Figure 2 Low-magnification (a) and high-magnification (b) scanning electron microscope (SEM) images of the individual g-C3N4 material prepared in Example 1 of this invention.

[0031] Figure 3 Low-magnification (a) and high-magnification (b) scanning electron microscope (SEM) images of the composite functional filler (i.e., basalt fiber / g-C3N4 composite material) prepared for this invention.

[0032] Figure 4 Low-magnification (a) and high-magnification (b) scanning electron microscope (SEM) images of the PEO-based all-solid-state polymer electrolyte prepared for this invention.

[0033] Figure 5 X-ray diffraction (XRD) patterns of different materials. Detailed Implementation

[0034] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0035] Example 1

[0036] The preparation method of the PEO-based all-solid-state polymer electrolyte in this embodiment includes the following steps:

[0037] (1) Basalt short-cut fibers (10 μm in diameter and 100 μm in length) were placed in a 20% hydrogen peroxide solution and refluxed at 80°C for 4 hours. After washing and drying, hydroxylated basalt fibers were obtained. Figure 1 These are scanning electron microscope (SEM) images of the basalt fiber material of the present invention at low magnification (a) and high magnification (b). The basalt fiber has a smooth surface and a diameter of about 10 μm.

[0038] (2) Melamine was placed in a covered crucible and heated to 550°C in a tube furnace at a heating rate of 5°C / min. The temperature was maintained for 3 hours to carry out a thermal polycondensation reaction. After natural cooling, the mixture was ground to obtain g-C3N4 powder with a sheet diameter of 100-500 nm and a thickness of 2-10 nm (e.g., Figure 2 (As shown).

[0039] (3) Disperse 1.0 g of hydroxylated basalt fiber obtained in step (1) in 100 mL of deionized water, add 0.3 g of g-C3N4 and 0.03 g of KH-550 silane coupling agent, sonicate for 45 minutes, stir at 80°C for 8 hours, filter after the reaction, wash with deionized water and anhydrous ethanol alternately 4 times, and vacuum dry at 90°C for 16 hours to obtain composite functional filler, named basalt@C3N4. Figure 3 Low-magnification (a) and high-magnification (b) scanning electron microscope (SEM) images of the basalt fiber / g-C3N4 composite material (basalt@C3N4) prepared in this embodiment show that g-C3N4 nanosheets are uniformly loaded on the surface of basalt fiber.

[0040] (4) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 3:1. After stirring and dissolving at 50°C, the composite functional filler (8% of the mass of PEO) prepared in step (3) was added and stirred for 8 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 50°C for 24 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte. Figure 4 The low-magnification (a) and high-magnification (b) scanning electron microscope (SEM) images of the PEO-based composite electrolyte material prepared in this embodiment show that the functional filler still maintains the basalt fiber / g-C3N4 morphology.

[0041] Example 2

[0042] The preparation method of the PEO-based all-solid-state polymer electrolyte in this embodiment includes the following steps:

[0043] (1) Basalt short-cut fibers (9 μm in diameter and 2000 μm in length) were placed in a 5% hydrogen peroxide solution and refluxed at 90°C for 1 hour. After washing and drying, hydroxylated basalt fibers were obtained.

[0044] (2) Hydroxylated basalt fiber and melamine (mass ratio of 1:0.05) were placed in a covered crucible and heated to 600℃ in a tube furnace at a heating rate of 10℃ / min. The temperature was maintained for 2 hours to carry out a thermal polycondensation reaction. After natural cooling, the mixture was ground to obtain a composite functional filler, named basalt@C3N4. The particle size of the g-C3N4 powder was 200-5000 nm, and the thickness was 30-100 nm.

[0045] (3) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 6:1. After dissolving by stirring at 40°C, the composite functional filler (1% of the mass of PEO) prepared in step (2) was added and stirred for 4 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 40°C for 24 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte.

[0046] Example 3

[0047] The preparation method of the PEO-based all-solid-state polymer electrolyte in this embodiment includes the following steps:

[0048] (1) Basalt short-cut fibers (diameter 20 μm, length 2000 μm) were placed in 30% hydrogen peroxide solution and refluxed at 50°C for 6 hours. After washing and drying, hydroxylated basalt fibers were obtained.

[0049] (2) Hydroxylated basalt fiber and melamine (mass ratio of 1:0.8) were placed in a covered crucible and heated to 500°C in a tube furnace at a heating rate of 10°C / min. The temperature was maintained for 2 hours to carry out a thermal polycondensation reaction. After natural cooling, the mixture was ground to obtain a composite functional filler, named basalt@C3N4. The particle size of the g-C3N4 powder was 300-5000 nm, and the thickness was 20-100 nm.

[0050] (3) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 2:1. After dissolving by stirring at 60°C, the composite functional filler (20% of the mass of PEO) prepared in step (2) was added and stirred for 12 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 80°C for 12 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte.

[0051] Example 4

[0052] The preparation method of the PEO-based all-solid-state polymer electrolyte in this embodiment includes the following steps:

[0053] (1) Basalt short-cut fibers (10 μm in diameter and 500 μm in length) were placed in a plasma treatment device and subjected to low-temperature plasma treatment in an oxygen atmosphere. The treatment power was 100 W and the treatment time was 20 minutes to obtain hydroxylated basalt fibers.

[0054] (2) Hydroxylated basalt fiber and melamine (mass ratio of 1:0.6) were placed in a covered crucible and heated to 400℃ in a tube furnace at a heating rate of 10℃ / min. The temperature was maintained for 2 hours to carry out a thermal polycondensation reaction. After natural cooling, the mixture was ground to obtain a composite functional filler, named basalt@C3N4. The particle size of the g-C3N4 powder was 300-5000 nm, and the thickness was 20-100 nm.

[0055] (3) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 3:1. After dissolving by stirring at 50°C, the composite functional filler (10% of the mass of PEO) prepared in step (2) was added and stirred for 8 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 40°C for 36 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte.

[0056] Example 5

[0057] The preparation method of the PEO-based all-solid-state polymer electrolyte in this embodiment includes the following steps:

[0058] (1) Basalt short-cut fibers (5 μm in diameter and 2000 μm in length) were first placed in 20% hydrogen peroxide solution and refluxed at 70°C for 5 hours, then washed and dried; then placed in a plasma treatment device and subjected to low-temperature plasma treatment in an oxygen atmosphere. The treatment power was 100 W and the treatment time was 20 minutes to obtain hydroxylated basalt fibers.

[0059] (2) Hydroxylated basalt fiber and melamine (mass ratio of 1:0.5) were placed in a covered crucible and heated to 600℃ in a tube furnace at a heating rate of 10℃ / min. The temperature was maintained for 2 hours to carry out a thermal polycondensation reaction. After natural cooling, the mixture was ground to obtain a composite functional filler, named basalt@C3N4. The particle size of the g-C3N4 powder was 300-5000 nm, and the thickness was 20-100 nm.

[0060] (3) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 3:1. After dissolving by stirring at 50°C, the composite functional filler (8% of the mass of PEO) prepared in step (2) was added and stirred for 8 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 50°C for 24 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte.

[0061] Comparative Example 1

[0062] The preparation method of the PEO-based all-solid polymer electrolyte in this comparative example differs from that in Example 1 in that no composite functional filler is added in step (4). The steps are as follows:

[0063] PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 3:1 and stirred at 50°C to obtain a homogeneous electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 50°C for 24 hours to obtain a composite solid electrolyte membrane, namely a PEO-based all-solid polymer electrolyte.

[0064] Comparative Example 2

[0065] The preparation method of the PEO-based all-solid-state polymer electrolyte in this comparative example differs from that in Example 1 in that only basalt fibers are added. The steps are as follows:

[0066] (1) Basalt short-cut fibers (10 μm in diameter and 100 μm in length) were placed in a 20% hydrogen peroxide solution and refluxed at 80°C for 4 hours. After washing and drying, hydroxylated basalt fibers were obtained.

[0067] (2) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 3:1. After dissolving by stirring at 50°C, the hydroxylated basalt fiber (8% of the mass of PEO) obtained in step (1) was added and stirred for 8 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 50°C for 24 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte.

[0068] Comparative Example 3

[0069] The preparation method of the PEO-based all-solid-state polymer electrolyte in this comparative example differs from that in Example 1 in that only g-C3N4 powder is added. The steps are as follows:

[0070] (1) Melamine was placed in a covered crucible and heated to 550°C in a tube furnace at a heating rate of 5°C / min. The temperature was maintained for 3 hours to carry out the thermal polycondensation reaction. After natural cooling, the mixture was ground to obtain g-C3N4 powder with a sheet diameter of 100-500 nm and a thickness of 2-10 nm.

[0071] (2) PEO and LiTFSI were dissolved in anhydrous acetonitrile at a mass ratio of 3:1. After stirring and dissolving at 50°C, g-C3N4 powder (8% of the mass of PEO) obtained in step (1) was added and stirred for 8 hours to obtain a uniform electrolyte slurry. The electrolyte slurry was cast into a PTFE mold and allowed to stand at room temperature for 24 hours to allow the solvent to evaporate. Then, it was vacuum dried at 50°C for 24 hours to obtain a composite solid electrolyte membrane, namely, a PEO-based all-solid polymer electrolyte.

[0072] Figure 5 The XRD patterns of basalt fibers, g-C3N4, and the basalt fiber / g-C3N4 composite functional filler prepared in Example 1 are shown in comparison. The results show that pure basalt fibers exhibit a broad, diffuse diffraction peak in the range of 2θ = 20°-30°, belonging to their amorphous silicate glass phase. Pure g-C3N4 exhibits two sharp characteristic diffraction peaks at 2θ = 13.1° and 27.4°, corresponding to the (100) in-plane packing peak and the (002) interlayer packing peak of g-C3N4, respectively. The XRD patterns of the composite functional filler retain both the amorphous diffuse characteristics of basalt fibers and clearly show the (002) crystal plane diffraction peak of g-C3N4, with no significant shift in peak position. This indicates that g-C3N4 has successfully adhered to the surface of the basalt fibers, and that the phase structures of both remain intact during the composite process, without any phase transition caused by chemical reaction.

[0073] The room temperature ionic conductivity of the PEO-based all-solid polymer electrolytes prepared in Example 1 and Comparative Examples 1-3 was tested, and the results are shown in Table 1.

[0074] Table 1

[0075]

[0076] As shown in Table 1, the room-temperature ionic conductivity of the PEO-based all-solid-state polymer electrolyte prepared in Example 1 of this invention is nearly an order of magnitude higher than that of pure PEO electrolyte, and also significantly improved compared to single-filler modification, indicating a significant synergistic effect between the basalt fiber and the g-C3N4 composite functional filler. Simultaneously, the crystallinity is significantly reduced, and both mechanical properties and electrochemical stability are significantly improved.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A PEO-based all-solid-state polymer electrolyte, characterized in that, It includes a PEO matrix, lithium salt, and composite functional filler; wherein the composite functional filler is basalt fiber with g-C3N4 surface loaded, and the mass ratio of basalt fiber to g-C3N4 is 1:0.05-0.

8.

2. The PEO-based all-solid-state polymer electrolyte according to claim 1, characterized in that, The basalt fiber is a surface-activated chopped basalt fiber or a ground basalt fiber; the diameter of the chopped basalt fiber or the ground basalt fiber is 5-20 μm, the length is 50-2000 μm, and the aspect ratio is 3-400.

3. The PEO-based all-solid-state polymer electrolyte according to claim 2, characterized in that, The surface activation treatment refers to treating short-cut basalt fibers or ground basalt fibers with at least one of hydroxyl, carboxyl, and amino groups.

4. The PEO-based all-solid-state polymer electrolyte according to claim 1, characterized in that, The g-C3N4 has a layered structure with a sheet diameter of 100-5000 nm and a thickness of 2-100 nm.

5. The PEO-based all-solid-state polymer electrolyte according to claim 1, characterized in that, The amount of the composite functional filler added is 1%-20% of the mass of the PEO matrix; the mass ratio of lithium salt to PEO matrix is ​​1:2-6.

6. The method for preparing the PEO-based all-solid-state polymer electrolyte according to any one of claims 1-5, characterized in that, The steps are as follows: (1) Basalt fibers are chopped or ground to obtain chopped basalt fibers or ground basalt fibers; (2) The short-cut basalt fibers or ground basalt fibers obtained in step (1) are subjected to at least one of the following surface activation treatments: hydroxyl, carboxyl and amino groups, to obtain activated basalt fibers; (3) The activated basalt fiber is subjected to thermal polycondensation reaction with melamine or urea, and then ground after natural cooling to obtain a basalt fiber composite material with g-C3N4 loaded on the surface; or the activated basalt fiber is mixed with g-C3N4 powder by solvent dispersion or grinding to obtain a basalt fiber composite material with g-C3N4 loaded on the surface. (4) Dissolve the PEO matrix and lithium salt in an organic solvent, add the basalt fiber with surface-loaded g-C3N4 obtained in step (3), stir evenly, pour into a mold, let stand at room temperature to allow the solvent to evaporate, and after drying, obtain the PEO-based all-solid polymer electrolyte.

7. The method for preparing the PEO-based all-solid-state polymer electrolyte according to claim 6, characterized in that, In step (2), the surface activation treatment is at least one of the following: hydrogen peroxide solution oxidation treatment, low-temperature plasma treatment, and a combined process of first performing hydrogen peroxide solution oxidation treatment and then performing low-temperature plasma treatment.

8. The method for preparing the PEO-based all-solid-state polymer electrolyte according to claim 7, characterized in that, The conditions for hydrogen peroxide solution oxidation treatment are: hydrogen peroxide volume fraction 5%-30%, treatment temperature 50-90℃, and treatment time 1-6 hours; the process conditions for low-temperature plasma treatment are: oxygen or air atmosphere, treatment power 30-200 W, and treatment time 5-30 minutes.

9. The method for preparing the PEO-based all-solid-state polymer electrolyte according to claim 6, characterized in that, In step (3), the thermal polycondensation reaction refers to heating to 400-600℃ at a heating rate of 2-10℃ / min and holding at that temperature for 2-4 hours; silane coupling agent or titanate coupling agent needs to be added during the dispersion mixing or grinding mixing process; in step (4), the organic solvent is anhydrous acetonitrile or tetrahydrofuran, and the drying is vacuum drying at 40-80℃ for 12-36 hours.

10. An all-solid-state lithium battery, comprising a positive electrode, a negative electrode, and an electrolyte, characterized in that, The electrolyte is the PEO-based all-solid-state polymer electrolyte according to any one of claims 1-5.