Methods for densifying the solid-solid interface in all-solid-state batteries, all-solid-state batteries and their fabrication methods and electrical devices
The densification of bare cell stacks in all-solid-state batteries by using a multi-stage gradient hot-pressing method solves the problem of poor solid-solid interface contact, achieves efficient and safe solid-solid interface bonding, and improves battery production efficiency and battery performance.
Patent Information
- Application Number
- CN202611560355.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
The solid-solid interface of existing all-solid batteries has nanoscale unevenness and interparticle gaps, resulting in high interface impedance, slow lithium-ion migration, severe polarization, and easy induction of electrolyte decomposition and lithium dendrite growth. In addition, the isostatic pressing process has safety hazards and low production efficiency.
A multi-stage gradient hot pressing method is used to densify the bare cell stack, including three stages: pre-pressing, densification, and shaping. By independently controlling the rolling parameters and gap of each set of pressure rollers, a tight bond between solid and solid interfaces is achieved, eliminating interlayer gaps and preventing high-pressure puncture of the electrolyte membrane and electrode powder shedding.
It significantly increases the solid-solid interface contact area, reduces production safety risks, lowers production costs and equipment investment, improves production efficiency and product yield, and ensures long cycle life and high interface bonding strength of the battery.
Smart Images

Figure CN123120902A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of all-solid-state lithium-ion battery manufacturing technology, and more specifically, to a method for densifying the solid-solid interface of an all-solid-state battery, an all-solid-state battery and its preparation method, and an electrical device thereof. Background Technology
[0002] Sulfide solid-state batteries have high theoretical energy density, good thermal stability, and a wide temperature range, making them an important development direction for next-generation power batteries. However, all components of solid-state batteries are in rigid contact, resulting in nanoscale unevenness and interparticle gaps at the solid-solid interface. This leads to high interfacial impedance, slow lithium-ion migration, severe polarization, and is prone to inducing electrolyte decomposition, lithium dendrite growth, and rapid capacity decay.
[0003] The current mainstream isostatic pressing process involves immersing the entire battery cell in oil and pressurizing it, forcing the electrodes and electrolyte layer to undergo plastic deformation and eliminating interparticle gaps. However, because the encapsulation material hardly deforms under high pressure, the internal battery cell shrinks in volume, resulting in irreversible wavy wrinkles in the encapsulation material. This necessitates unpacking and repackaging, which not only increases waste of encapsulation materials and adds to the process and equipment investment, but also because isostatic pressing equipment is a high-pressure vessel that is prone to fatigue failure after long-term service, posing a risk of cell explosion. Furthermore, the simple isostatic pressing high-pressure mode can easily cause electrolyte layer brittleness, severely restricting the improvement of battery yield.
[0004] In view of this, the present invention is proposed. Summary of the Invention
[0005] The purpose of this invention is to provide a method for densifying the solid-solid interface of an all-solid battery, an all-solid battery and its preparation method, and an electrical device thereof.
[0006] This invention is implemented as follows: In a first aspect, the present invention provides a method for densifying the solid-solid interface of an all-solid-state battery, comprising stacking and assembling a positive electrode, a solid electrolyte layer and a negative electrode to obtain a bare cell stack; and performing densification treatment on the bare cell stack.
[0007] The densification process includes multi-stage gradient hot pressing of bare cell stacks using hot pressing rollers; the multi-stage gradient hot pressing process includes a pre-pressing stage, a densification stage, and a shaping stage; the roller pressing pressure and roller pressing temperature in the densification stage are higher than those in the pre-pressing stage and the shaping stage; the roller pressing temperature in the pre-pressing stage is higher than that in the shaping stage.
[0008] In an optional implementation, each stage of the multi-stage gradient hot pressing is provided with at least one set of pressure roller mechanisms, and each set of pressure roller mechanisms independently controls the roller pressing parameters; the roller pressing parameters include at least one of roller pressing temperature, roller pressing pressure, roller gap and roller pressing speed; each set of pressure roller mechanisms has multiple roller pressing zones, and the roller gap of each roller pressing zone is independently controlled.
[0009] In an optional implementation, the method for independently controlling the roll gap of each rolling zone includes: setting a thickness tester in the discharge area of at least one set of pressure roller mechanisms at each stage; each thickness tester collects the actual thickness of at least one region of the bare cell stack; the target thickness difference between different regions of the bare cell stack is obtained by subtracting the actual thickness from the target thickness; when the absolute value of the target thickness difference is ≥0.1mm, the thickness data of the region of the bare cell stack corresponding to the target thickness difference is abnormal thickness data; and adjusting the roll gap of the rolling zone corresponding to the region of abnormal thickness data: when the target thickness difference is positive, increasing the roll gap; when the target thickness difference is negative, decreasing the roll gap.
[0010] In an optional embodiment, the rolling temperature during the pre-compression stage is 45~95℃, the rolling pressure is 5~25MPa, and the rolling speed is 1~5m / min; the compression rate during the pre-compression stage is 5~10%.
[0011] Preferably, the rolling temperature during the densification stage is 65~205℃, the rolling pressure is 15~50MPa, and the rolling speed is 1~5m / min; the compression rate during the densification stage is 10~15%.
[0012] Preferably, the rolling temperature during the shaping stage is 19~145℃, the rolling pressure is 10~30MPa, and the rolling speed is 1~5m / min; the compression rate during the shaping stage is 5~10%.
[0013] Preferably, the roll gap of at least one pressing roller mechanism in the densification stage satisfies the following condition: in the direction of movement of the bare cell stack, the roll gap at both ends of the pressing roller mechanism is greater than the roll gap in the middle region.
[0014] In an optional embodiment, the material of the transport structure of the bare cell stack during the densification process is a high-temperature resistant material, including glass fiber PTFE or aramid-based PTFE composite material.
[0015] In an optional implementation, the process also includes shaping the densified bare cell stack.
[0016] The shaping parameters include: shaping temperature of 15~80℃, shaping pressure of 1~5MPa, and shaping time of 10~30s.
[0017] Preferably, the flatness of the shaped bare cell stack is ≤0.1mm / m, and the deviation between the actual thickness and the target thickness of the shaped bare cell stack is ≤±0.1mm.
[0018] Secondly, the present invention provides a method for preparing an all-solid-state battery, comprising preparing a positive electrode sheet, a solid electrolyte layer and a negative electrode sheet, and then performing a densification treatment using any of the methods described in the foregoing embodiments to obtain a densified bare cell stack, and encapsulating the densified bare cell stack.
[0019] In an optional implementation, prior to encapsulation, tabs are welded onto the densified bare cell stack, the welding method including either ultrasonic welding or laser welding.
[0020] Thirdly, the present invention provides an all-solid-state battery, which is prepared by the method described in the foregoing embodiments.
[0021] Fourthly, the present invention provides an electrical device comprising an all-solid-state battery as described in the foregoing embodiments.
[0022] The present invention has the following beneficial effects: This invention provides a method for densifying the solid-solid interface of an all-solid-state battery, an all-solid-state battery and its preparation method, and an electrical device. The method employs a multi-stage gradient hot pressing process to densify a stack of bare cells. In the pre-pressing stage, a lower pressure is used to pre-expel air between the electrodes and the electrolyte. In the densification stage, high pressure is used to achieve a tight bond between the solid and solid interfaces, eliminating interlayer gaps. Then, the pressure and temperature are reduced to shape the cells. These three stages are rolled sequentially. Under conditions without isostatic pressing, the contact area of the solid-solid interface is significantly increased. This method also suppresses cell thickness rebound and avoids defects such as instantaneous high-pressure puncture of the electrolyte membrane and electrode powder shedding. Because the method provided by this invention eliminates the isostatic pressing process, safety risks are significantly reduced. Furthermore, there is no need to encapsulate the bare cell stack before densification, nor is there a need for removing encapsulation materials and re-encapsulating after densification. Production costs and equipment investment are significantly reduced, production efficiency is improved, and the risk of electrode scratching and damage during aluminum-plastic film unpacking is effectively avoided, resulting in improved product yield. This method can be applied to the manufacturing of lithium batteries such as power batteries and energy storage batteries. Attached Figure Description
[0023] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0024] Figure 1 This is a schematic diagram of the multi-segment gradient hot pressing process for bare cell stacks provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the structure of a single pressure roller mechanism provided in an embodiment of the present invention; Figure 3 A flowchart illustrating the preparation method of an all-solid-state battery provided in an embodiment of the present invention; Figure 4 This is a schematic diagram of the structure of an all-solid-state battery provided in an embodiment of the present invention; Figure 5 This is a schematic diagram of the structure of an electrical device provided in an embodiment of the present invention.
[0025] Explanation of key component symbols: 110-pressure roller mechanism; 111-upper roller; 112-lower roller; 120-belt; 130-thickness tester. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The components of the embodiments of the present invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations.
[0027] Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. All other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the invention.
[0028] It should be noted that similar labels and letters in the following figures indicate similar items. Therefore, once an item is defined in one figure, it does not need to be further defined and explained in subsequent figures.
[0029] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, or the orientation or positional relationship commonly used when the product of this invention is in use. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this invention. In addition, the terms "first," "second," "third," etc., are only used to distinguish descriptions and should not be construed as indicating or implying relative importance.
[0030] Furthermore, terms such as "horizontal" and "vertical" do not imply that components must be absolutely horizontal or suspended, but rather that they can be slightly tilted. For example, "horizontal" simply means that its direction is more horizontal than "vertical," and does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0031] In the description of this invention, it should also be noted that, unless otherwise explicitly specified and limited, the terms "set," "install," "connect," and "link" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.
[0032] In the manufacturing process of sulfide solid-state batteries, the interface treatment between the electrode and electrolyte layers is a core technical challenge. Unlike liquid batteries, all components in solid-state batteries are in rigid contact, which easily leads to increased porosity between the active material particles in the electrodes and nanoscale surface unevenness between the electrolyte and electrode layers. These microscopic gaps result in a significantly higher interfacial contact resistance in solid-state batteries compared to liquid lithium batteries. This interfacial impedance not only drastically reduces the lithium-ion migration rate and induces significant polarization, but also leads to uneven distribution of lithium ions at the interface during charging and discharging, accelerating lithium dendrite growth and interfacial side reactions, ultimately manifesting as rapid capacity decay and shortened cycle life.
[0033] To address the issue of poor solid-solid interface contact, the industry currently commonly uses isostatic pressing (HSP) to densify the interface between the electrode and electrolyte layers. The specific method involves stacking the electrode and electrolyte layers, encapsulating them, and then placing them in a hot isostatic pressing (HIP) machine. Using hydraulic oil within the machine's chamber as a carrier, the battery cell is completely immersed in the oil. A hydraulic cylinder pressurizes the oil within the chamber to 300-500 MPa and then holds the pressure. This hydraulic pressure causes plastic deformation of the electrode sheets and electrolyte layer. The high hydraulic pressure compresses the gaps between the particles in the electrode sheets and electrolyte layer, resulting in a tight solid-solid interface. The core advantages of this technology are uniform pressure, excellent solid-solid interface contact, long battery cell cycle life, and low internal resistance.
[0034] However, during isostatic pressing, the encapsulation material hardly deforms under high pressure, while the internal cell structure shrinks in volume under high pressure. This difference in deformation causes irreversible wavy wrinkles in the encapsulation material. Therefore, after isostatic pressing, an additional process of disassembling and resealing the encapsulation material is required. This not only wastes the encapsulation material but also increases the investment in unnecessary equipment and processes, leading to increased production costs and reduced production efficiency. Furthermore, isostatic pressing equipment is a high-pressure vessel. Long-term operation under high pressure can easily cause fatigue failure of the hydraulic cavity, leading to high-pressure failure of the cylinder and the risk of cylinder explosion, seriously threatening the personal safety of workers. Therefore, the inventors propose the following solution.
[0035] In a first aspect, the present invention provides a method for densifying the solid-solid interface of an all-solid-state battery, comprising stacking and assembling a positive electrode, a solid electrolyte layer and a negative electrode to obtain a bare cell stack; and performing densification treatment on the bare cell stack.
[0036] It should be noted that the number of positive electrode plates, solid electrolyte layers, and negative electrode plates in the bare cell stack of the present invention can be set according to actual production needs. For example, each of the positive electrode plate, solid electrolyte layer, and negative electrode plate can be a single piece, and they can be stacked sequentially to obtain a single-layer stacked bare cell stack; or multiple pieces of positive electrode plates, solid electrolyte layers, and negative electrode plates can be stacked sequentially to form a positive electrode plate group, all solid electrolyte layers can be stacked sequentially to form a solid electrolyte group, and all negative electrode plates can be stacked sequentially to form a negative electrode plate group. Then, the positive electrode plate group, solid electrolyte group, and negative electrode plate group can be stacked sequentially to obtain a multi-layer stacked bare cell stack.
[0037] like Figure 1 As shown, the densification process includes multi-stage gradient hot pressing of the bare cell stack using hot pressing rollers; the multi-stage gradient hot pressing stages include a pre-pressing stage, a densification stage, and a shaping stage; the roller pressing pressure and roller pressing temperature in the densification stage are higher than those in the pre-pressing stage and the shaping stage; the roller pressing temperature in the pre-pressing stage is higher than that in the shaping stage.
[0038] By employing a multi-stage gradient hot pressing process to densify the stacked bare cells, a smaller pressure is used in the pre-pressing stage to remove air between the electrodes and the electrolyte. In the densification stage, a high pressure is used to achieve a tight bond between the solid and solid interfaces and eliminate interlayer gaps. Then, the pressure and temperature are reduced to shape the cells. The three stages are rolled sequentially. Under the condition of no isostatic pressure, the contact area of the solid and solid interfaces is significantly improved. At the same time, this method can also suppress the cell thickness rebound and avoid defects such as instantaneous high pressure piercing the electrolyte membrane and electrode powder shedding.
[0039] Furthermore, since the multi-stage gradient hot pressing method provided by this invention eliminates the isostatic pressing process, the safety risks in the production process are significantly reduced. At the same time, there is no need to encapsulate the bare cell stack before densification treatment, nor is there a need to remove the encapsulation material and re-encapsulate after densification treatment. Production costs and equipment investment are significantly reduced, production efficiency is improved, and the risk of electrode scratching and damage during aluminum-plastic film unsealing is effectively avoided, resulting in improved product yield. It can be applied to the manufacturing fields of lithium batteries such as power batteries and energy storage batteries.
[0040] In alternative implementations, such as Figure 2 As shown, each stage of the multi-stage gradient hot pressing is equipped with at least one set of pressure roller mechanisms 110, and each set of pressure roller mechanisms 110 independently controls the rolling parameters; the rolling parameters include at least one of rolling temperature, rolling pressure, roller gap, and rolling speed. By independently controlling the rolling parameters of each set of pressure roller mechanisms 110, the densification rolling requirements of the bare cell stack at different stages can be achieved.
[0041] It should be noted that each stage corresponds to at least one set of rolling mechanisms. Each set of rolling mechanisms has two pressure rollers: an upper roller 111 and a lower roller 112. The gap between the upper roller 111 and the lower roller 112 is the roller gap. The bare cell stack passes through the roller gap and achieves interlayer densification through the compression of the upper roller 111 and the lower roller 112. Therefore, by adjusting the rolling parameters of the rolling mechanisms corresponding to each stage in the densification process, the staged densification treatment of the bare cell stack can be achieved.
[0042] Furthermore, each pressure roller of the pressure roller mechanism 110 is equipped with multiple pressure roller zones, and the gap between the rollers of each pressure roller zone is controlled independently.
[0043] Because the thickness of the bare cell stack is uneven, there may be areas that are thinner or thicker. However, the purpose of densification is to ensure that the layers are dense and that the thickness of the cells is within the allowable error range. To ensure that the thickness of different cells is uniform after densification, it is necessary to perform zoned control on each area of each pressure roller.
[0044] For example, such as Figure 2 As shown, each pressure roller is divided into 10 regions. The 10 regions of the upper roller 111 are labeled A1, B1, C1, D1, E1, F1, G1, H1, I1, and J1, respectively; the 10 regions of the lower roller 112 are labeled A2, B2, C2, D2, E2, F2, G2, H2, I2, and J2, respectively. The moving direction of the bare cell stack is... Figure 2The cross-sectional direction of the pressure roller shown is perpendicular (i.e., the direction of the upper roller 111 from A1 to J1). Therefore, when the bare cell stack passes through the roll gap between the upper roller 111 and the lower roller 112, the surface of the bare cell stack is in contact with the A~J regions of the pressure roller at the same time. According to the thickness difference of the bare cell stack at different positions, the roll gap of each region A~J of the upper roller 111 and the lower roller 112 can be controlled individually to ensure that the thickness of all regions of the cell is uniform after densification treatment.
[0045] Preferably, to avoid edge warping of the battery cell and to prevent bulging and springback in the middle of the battery cell, the gap between the rollers at both ends of the pressure roller mechanism 110 is larger than the gap in the middle, i.e. Figure 2 The structure shown is designed to accommodate situations where bare cell stacks are thin on both sides and thick in the middle, thereby achieving uniform thickness across the large surface area of the cells.
[0046] Furthermore, the structure of the pressure roller is not limited to, for example... Figure 2 The drum-shaped structure shown can also be adjusted according to the thickness of different bare cell stacks. In optional embodiments, the method for independently controlling the roll gap of each rolling section includes: Figure 1 As shown, a thickness tester 130 is set in the discharge area of at least one set of pressure roller mechanisms 110 in each stage. Each thickness tester 130 collects the actual thickness of at least one area of the bare cell stack. The target thickness difference between different areas of the bare cell stack is obtained by subtracting the actual thickness from the target thickness. When the absolute value of the target thickness difference is ≥0.1mm, the thickness data of the area of the bare cell stack corresponding to the target thickness difference is abnormal thickness data. The roller gap of the roller pressing zone corresponding to the area where the abnormal thickness data is located is adjusted: when the target thickness difference is positive, the roller gap is increased; when the target thickness difference is negative, the roller gap is decreased.
[0047] By dynamically adjusting the roller gap, closed-loop control of thickness uniformity in different areas of the bare cell stack is achieved, ensuring consistent compaction density in each zone and controllable and repeatable interface densification. This enables precise densification at the micro-level during continuous rolling, effectively suppressing electrolyte membrane rupture or electrode powder shedding caused by local overpressure, as well as interface voids caused by underpressure, ultimately ensuring spatial consistency of the solid-solid interface contact quality of the entire cell.
[0048] by Figure 2 Taking the partition shown as an example, assuming that the thickness tester 130 detects abnormal thickness data in region D of the pressure roller corresponding to the bare cell stack, and the target thickness difference in this region is negative, the gap between the rollers in region D can be further reduced, that is, the distance between D1 and D2 can be shortened.
[0049] If the thickness tester 130 detects abnormal thickness data in region D of the pressure roller corresponding to the bare cell stack, and the target thickness difference in this region is positive, then the gap between the rollers in region D can be increased, that is, the distance between D1 and D2 can be increased.
[0050] In addition, it should be noted that, Figure 2 The partition diagram shown is for illustrative purposes only and is not intended to limit the number of partitions on the pressure rollers in this invention. In other embodiments, the number of partitions on the pressure rollers can be [number missing]. Figure 2 The number of sections can be reduced from the base number, for example, to 2, 3, 5, or 8; or the number of sections for the pressure rollers can also be reduced. Figure 2 On the basis of this, for example, when used in industrial production or when producing solid-state batteries with stricter requirements for thickness uniformity, the number of sections of the pressure roller can be increased to 12, 15, 20 or even more.
[0051] In an optional embodiment, the rolling temperature during the pre-compression stage is 45~95℃, the rolling pressure is 15~25MPa, and the rolling speed is 1~5m / min; the compression rate during the pre-compression stage is 5~10%.
[0052] In an optional embodiment, the rolling temperature during the pre-pressing stage can be any value or a range of any two values from 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, and 95°C.
[0053] The roller pressure during the pre-compression stage can be any value or a range of any two values from 15MPa, 16MPa, 17MPa, 18MPa, 19MPa, 20MPa, 21MPa, 22MPa, 23MPa, 24MPa and 25MPa.
[0054] The roller speed during the pre-compression stage can be any value or a range of any two values from 1 m / min, 1.5 m / min, 2 m / min, 2.5 m / min, 3 m / min, 3.5 m / min, 4 m / min, 4.5 m / min, and 5 m / min.
[0055] The compression rate during the pre-compression stage can be any value or a range of any two values, such as 5%, 6%, 7%, 8%, 9%, or 10%.
[0056] Preferably, the rolling pressure during the pre-compression stage is evenly distributed within each zone of the pressure roller to ensure that the overall surface of the bare cell stack is subjected to balanced force, achieve initial wrinkle-free bonding between the solid electrolyte layer and the positive / negative electrode interface, and fully expel interlayer trapped air, avoiding local stress concentration that could lead to electrolyte microcracks or electrode edge warping, thus providing a flat, stable interface foundation with low initial impedance for the subsequent high-voltage densification stage.
[0057] It should be noted that in some implementations, if the initial thickness uniformity of the bare cell stack is significantly poor, a slightly higher rolling pressure can be applied to the thicker areas of the bare cell stack during the pre-pressing stage, which is beneficial for further compaction in the subsequent densification stage.
[0058] Furthermore, the pressure of the roller gap in different areas can be adjusted by changing the roller gap.
[0059] Preferably, the rolling temperature during the densification stage is 65~205℃, the rolling pressure is 15~50MPa, and the rolling speed is 1~5m / min; the compression rate during the densification stage is 10~15%.
[0060] In an optional embodiment, the rolling temperature during the densification stage can be any value or a range of any two values from 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C, 200°C, and 205°C.
[0061] The rolling pressure during the densification stage can be any value or a range of any two values from 15MPa, 18MPa, 20MPa, 22MPa, 25MPa, 28MPa, 30MPa, 32MPa, 35MPa, 38MPa, 40MPa, 42MPa, 45MPa, 48MPa and 50MPa.
[0062] The rolling speed during the densification stage can be any value or a range of any two values from 1 m / min, 1.5 m / min, 2 m / min, 2.5 m / min, 3 m / min, 3.5 m / min, 4 m / min, 4.5 m / min, and 5 m / min.
[0063] The compression rate during the densification stage can be any value or a range of any two values, such as 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5, or 15%.
[0064] Controlling the rolling temperature between 65 and 205°C can moderately reduce the yield strength of the solid electrolyte layer and enhance its micro-plastic deformation capability, avoiding sudden fracture caused by high pressure at room temperature. A pressure range of 15–50 MPa is sufficient to overcome the Coulomb forces and van der Waals barriers between electrode particles, promoting controllable dense rearrangement in the three-phase contact area of the positive / electrolyte / negative electrode, significantly reducing nanoscale pores and voids. A rolling speed of 1–5 m / min ensures sufficient relaxation time for the material in the stress field, preventing stress accumulation and interlayer slip instability caused by excessively high strain rates. By controlling the parameters of the densification stage within the above range, a unified approach of high interfacial bonding strength, low contact resistance, and high structural integrity is achieved within the solid-state battery cell, providing a reliable physical interface foundation for obtaining all-solid-state batteries with long cycle life and high rate stability.
[0065] Preferably, the rolling pressure during the densification stage is unevenly distributed within the various sections of the pressure roller, and exhibits a trend of first increasing and then decreasing according to the travel direction of the bare cell stack; that is, the rolling pressure at both ends of the pressure roller is less than the rolling pressure in the middle, for example... Figure 2 The distribution of each area of the pressure roller shown can be achieved.
[0066] By controlling the roller pressure distribution during the densification stage, it is possible to achieve progressively stronger plastic deformation in the cell thickness direction from the edge to the center, while ensuring that the solid electrolyte layer does not fracture brittlely and the active material of the electrode sheets does not detach. The middle region bears higher pressure to fully compact the interlayer gaps, increase the interface contact area and ion pathway connectivity; the pressure at both ends is moderately reduced to effectively suppress defects such as edge wrinkling of the electrode sheets, edge curling of the electrolyte membrane, or stress concentration in the aluminum-plastic film sealing area caused by rigid constraints. This balances the overall densification effect and structural integrity of the cell, laying a reliable foundation for uniform stress release and thickness stability in the subsequent medium-pressure shaping stage.
[0067] Preferably, the rolling temperature during the shaping stage is 19~145℃, the rolling pressure is 10~30MPa, and the rolling speed is 1~5m / min; the compression rate during the shaping stage is 5~10%.
[0068] In an optional embodiment, the rolling temperature during the shaping stage can be any value or a range of any two values from 19°C, 22°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, and 145°C.
[0069] The rolling pressure during the shaping stage can be any value or a range of any two values from 10MPa, 12MPa, 15MPa, 18MPa, 20MPa, 22MPa, 25MPa, 28MPa and 30MPa.
[0070] The rolling speed during the shaping stage can be any value or a range of any two values from 1 m / min, 1.5 m / min, 2 m / min, 2.5 m / min, 3 m / min, 3.5 m / min, 4 m / min, 4.5 m / min, and 5 m / min.
[0071] The compression rate during the finalization stage can be any value or a range of any two values, such as 5%, 6%, 7%, 8%, 9%, or 10%.
[0072] The purpose of the shaping stage is not to further compress the material significantly, but to suppress thickness rebound through stress relaxation under moderate pressure, and to synergistically correct local thickness unevenness caused by the rolling process or initial deviations in the stacking. Therefore, the rolling pressure in the shaping stage can be uniformly or unevenly distributed within the various zones of the pressure rollers, and can be dynamically determined based on the actual thickness distribution of the bare cell stack after the previous densification stage.
[0073] In an optional embodiment, the material of the transport structure in the densification process of the bare cell stack is a high-temperature resistant material, including glass fiber PTFE or aramid-based PTFE composite material. The glass fiber PTFE has a high-temperature resistance of ≥260℃, and the aramid-based PTFE composite material has a high-temperature resistance of 220~230℃, neither of which will cause impurities to adhere to the surface of the bare cell stack.
[0074] Preferably, the conveyor structure is a common structure such as a belt or conveyor belt.
[0075] Preferably, in order to avoid slippage or displacement of the bare cell stack, the conveying structure is also equipped with a limiting fixture to limit the bare cell stack, realize tension-free flat plate conveying, and avoid misalignment of each layer during subsequent rolling.
[0076] In an optional implementation, the process also includes shaping the densified bare cell stack.
[0077] The shaping parameters include: shaping temperature of 15~80℃, shaping pressure of 1~5MPa, and shaping time of 10~30s.
[0078] In an optional implementation, the shaping temperature can be any value or a range of any two values from 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, and 80°C. By covering the room temperature correction to the thermal stress relaxation range, thermally induced electrolyte decomposition is avoided in the bare cell stack while maintaining dimensional stability.
[0079] The shaping pressure can be any value or a range of any two values from 1MPa, 1.5MPa, 2MPa, 2.5MPa, 3MPa, 3.5MPa, 4MPa, 4.5MPa and 5MPa.
[0080] The shaping time can be any value or a range of any two values from 10s, 12s, 15s, 18s, 20s, 22s, 25s, 28s, and 30s.
[0081] Preferably, the flatness of the shaped bare cell stack is ≤0.1mm / m, and the deviation between the actual thickness and the target thickness of the shaped bare cell stack is ≤±0.1mm.
[0082] Secondly, the present invention provides a method for preparing an all-solid-state battery, such as... Figure 3 As shown, the process includes preparing a positive electrode sheet, a solid electrolyte layer, and a negative electrode sheet, and then performing a densification process using any of the methods described in the preceding embodiments to obtain a densified bare cell stack, and then encapsulating the densified bare cell stack.
[0083] In an optional embodiment, prior to encapsulation, tabs are welded onto the densified bare cell stack, the welding method of which includes either ultrasonic welding or laser welding.
[0084] Thirdly, the present invention provides an all-solid-state battery, which is prepared by the method described in the foregoing embodiments.
[0085] This invention does not impose any particular limitation on the shape of the battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 4 This is a square-structured battery as an example. It is understood that the arrangement of the tabs is not limited to being arranged at two opposite ends of the battery as shown in the figure; they can also be arranged on the same side for both positive and negative electrodes. This invention does not limit this arrangement.
[0086] In some embodiments, the battery includes a casing, and the electrode assemblies are encapsulated within the casing. The battery may contain one or more electrode assemblies, which can be selected by those skilled in the art according to specific practical needs.
[0087] Fourthly, the present invention provides an electrical device comprising an all-solid-state battery as described in the foregoing embodiments.
[0088] Solid-state batteries can be used as a power source for electrical devices or as an energy storage unit for electrical devices. Electrical devices can include mobile devices (typically mobile phones, laptops, etc.), electric vehicles (typically pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships, satellites, or energy storage systems.
[0089] Figure 5 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0090] The features and performance of the present invention will be further described in detail below with reference to embodiments.
[0091] Example 1 This embodiment provides a method for densifying the solid-solid interface of an all-solid-state battery, including the following steps: S01. The NCM811 positive electrode, solid electrolyte layer and graphite negative electrode are stacked and assembled in sequence to obtain a bare cell stack.
[0092] S02. Densification treatment is carried out on the bare cell stack.
[0093] Specifically, the bare battery cell stack is placed on the transfer belt 120, which is made of high-temperature resistant material. The bare battery cell stack is positioned by the limiting fixture on the transfer belt 120 to prevent misalignment during the subsequent rolling process.
[0094] The bare cell stack passes through three sets of pressure roller mechanisms 110 via a transfer belt 120. Each set of pressure roller mechanisms corresponds to a multi-stage gradient hot pressing stage. The bare cell stack undergoes a pre-pressing stage, a densification stage, and a shaping stage for densification treatment.
[0095] like Figure 2 As shown, each pressure roller mechanism 110 has 10 pressure zones, and the gap between the rollers in each pressure zone is controlled independently. The 10 zones of the upper roller 111 are labeled A1, B1, C1, D1, E1, F1, G1, H1, I1, and J1, respectively; the 10 zones of the lower roller 112 are labeled A2, B2, C2, D2, E2, F2, G2, H2, I2, and J2, respectively.
[0096] The pre-compression stage has a roller temperature of 50℃, a roller pressure of 20MPa, and a roller speed of 2m / min. The roller pressure in the pre-compression stage is evenly distributed in each section of the pressure roller to ensure that the compression rate in the pre-compression stage is 6~8%.
[0097] The rolling temperature during the densification stage is 70℃, the rolling pressure is 45MPa, and the rolling speed is 2m / min. The rolling pressure at both ends of the roller during the densification stage is less than that in the middle, so that the roller presents a drum-shaped structure. The compression rate during the densification stage is 12~15%.
[0098] The rolling temperature during the shaping stage is 22℃, the rolling pressure is 25MPa, and the rolling speed is 2m / min. The rolling pressure during the shaping stage is dynamically adjusted according to the thickness of the product, and the compression rate during the shaping stage is 5~6%.
[0099] In this embodiment, the roller pressure in each region of each pressure roller can be adjusted by the roller gap. The specific adjustment method is as follows: A thickness tester 130 is installed in the discharge area of each pressure roller mechanism 110. Each thickness tester 130 collects the actual thickness of at least one area of the bare cell stack. The target thickness difference between different areas of the bare cell stack is obtained by subtracting the actual thickness from the target thickness. When the absolute value of the target thickness difference is ≥0.1mm, the thickness data of the area of the bare cell stack corresponding to the target thickness difference is abnormal thickness data. The roller gap of the roller pressing zone corresponding to the area where the abnormal thickness data is located is adjusted: when the target thickness difference is positive, the roller gap is increased; when the target thickness difference is negative, the roller gap is decreased.
[0100] S03. Shape the bare cell stack after densification treatment.
[0101] The shaping parameters include: shaping temperature of 15~80℃, shaping pressure of 1~5MPa, and shaping time of 10~30s.
[0102] The flatness of the shaped bare cell stack is ≤0.1mm / m, and the deviation between the actual thickness and the target thickness of the shaped bare cell stack is ≤±0.1mm.
[0103] This embodiment also provides an all-solid-state battery, the preparation method of which is as follows: A positive electrode sheet, a solid electrolyte layer, and a negative electrode sheet are prepared. Then, the bare cell stack is densified using the method described in this embodiment to obtain a densified bare cell stack. Electrode tabs are ultrasonically welded onto the densified bare cell stack, and then it is packaged.
[0104] Example 2 This embodiment provides a method for densifying the solid-solid interface of an all-solid-state battery, including the following steps: S01. The NCM811 positive electrode, solid electrolyte layer and silicon-carbon negative electrode are stacked and assembled in sequence to obtain a bare cell stack.
[0105] S02. Densification treatment is carried out on the bare cell stack.
[0106] Specifically, the bare battery cell stack is placed on the transfer belt 120, which is made of high-temperature resistant material. The bare battery cell stack is positioned by the limiting fixture on the transfer belt 120 to prevent misalignment during the subsequent rolling process.
[0107] The bare cell stack passes through three sets of pressure roller mechanisms 110 via a transfer belt 120. Each set of pressure roller mechanisms corresponds to a multi-stage gradient hot pressing stage. The bare cell stack undergoes a pre-pressing stage, a densification stage, and a shaping stage for densification treatment.
[0108] like Figure 2 As shown, each pressure roller mechanism 110 has 10 pressure zones, and the gap between the rollers in each pressure zone is controlled independently. The 10 zones of the upper roller 111 are labeled A1, B1, C1, D1, E1, F1, G1, H1, I1, and J1, respectively; the 10 zones of the lower roller 112 are labeled A2, B2, C2, D2, E2, F2, G2, H2, I2, and J2, respectively.
[0109] The pre-compression stage has a roller temperature of 90℃, a roller pressure of 6MPa, and a roller speed of 1.5m / min. The roller pressure in the pre-compression stage is evenly distributed in each section of the pressure roller to ensure that the compression rate in the pre-compression stage is 6~8%.
[0110] The rolling temperature during the densification stage is 200℃, the rolling pressure is 20MPa, and the rolling speed is 1.5m / min. During the densification stage, the rolling pressure at both ends of the roller is less than that in the middle, so that the roller has a drum-shaped structure. The compression rate during the densification stage is 12~15%.
[0111] The rolling temperature during the shaping stage is 140℃, the rolling pressure is 12MPa, and the rolling speed is 1.5m / min. The rolling pressure during the shaping stage is dynamically adjusted according to the thickness of the product, and the compression rate during the shaping stage is 5~6%.
[0112] In this embodiment, the roller pressure in each region of each pressure roller can be adjusted by the roller gap. The specific adjustment method is as follows: A thickness tester 130 is installed in the discharge area of each pressure roller mechanism 110. Each thickness tester 130 collects the actual thickness of at least one area of the bare cell stack. The target thickness difference between different areas of the bare cell stack is obtained by subtracting the actual thickness from the target thickness. When the absolute value of the target thickness difference is ≥0.01mm, the thickness data of the area of the bare cell stack corresponding to the target thickness difference is abnormal thickness data. The roller gap of the roller pressing zone corresponding to the area where the abnormal thickness data is located is adjusted: when the target thickness difference is positive, the roller gap is increased; when the target thickness difference is negative, the roller gap is decreased.
[0113] S03. Shape the bare cell stack after densification treatment.
[0114] The shaping parameters include: shaping temperature of 60~80℃, shaping pressure of 1~5MPa, and shaping time of 10~30s.
[0115] The flatness of the shaped bare cell stack is ≤0.1mm / m, and the deviation between the actual thickness and the target thickness of the shaped bare cell stack is ≤±0.1mm.
[0116] This embodiment also provides an all-solid-state battery, the preparation method of which is as follows: A positive electrode sheet, a solid electrolyte layer, and a negative electrode sheet are prepared. Then, the bare cell stack is densified using the method described in this embodiment to obtain a densified bare cell stack. Electrode tabs are ultrasonically welded onto the densified bare cell stack, and then it is packaged.
[0117] Comparative Example 1 This comparative example provides a traditional isostatic pressing method for preparing all-solid-state batteries, including the following steps: S01. The NCM811 positive electrode, solid electrolyte layer and silicon-carbon negative electrode are stacked and assembled in sequence to obtain a bare cell stack.
[0118] S02. Perform isostatic compaction treatment on the bare cell stack.
[0119] Specifically, after the bare battery cell stack is encapsulated with aluminum-plastic film, it is first pressed on both sides with a 40Cr steel plate with a flatness of ≤0.02mm and a thickness of 10mm after heat treatment; The battery cells, which are fixed with pressure plates, are placed in the hydraulic tank of an isostatic pressing equipment for densification treatment.
[0120] Its isostatic parameters are as follows: Boost phase: Initial pressure setting: 10MPa, first stage pressure holding setting: 100MPa, first stage pressure holding time setting: 10s, first stage pressure compensation setting: 90MPa.
[0121] Second-stage pressure holding setting: 200MPa, second-stage pressure holding time setting: 10s, second-stage pressure compensation setting: 190MPa.
[0122] Three-stage pressure holding setting: 300MPa, three-stage pressure holding time setting: 10s, three-stage pressure compensation setting: 290MPa.
[0123] Final pressure setting: 510MPa, pressure holding time setting: 1800s, final pressure compensation setting: 485MPa.
[0124] Decompression phase: Pneumatic pressure relief setting: 190MPa, first-stage pressure relief setting: 400MPa, first-stage pressure relief time setting: 10s.
[0125] Second-stage pressure relief setting: 300MPa, second-stage pressure relief time setting: 10s.
[0126] Three-stage pressure relief setting: 200MPa; three-stage pressure relief time setting: 10s.
[0127] Isostatic oil temperature: 30℃.
[0128] S03. After the isostatic pressing is completed, remove the battery cell from the isostatic pressing plate.
[0129] S04. Clean the hydraulic oil on the surface of the battery cell with non-woven cloth.
[0130] Comparative Example 2 This comparative example provides a method for densifying the solid-solid interface of an all-solid-state battery. The only difference from Example 1 is that it does not include a pre-pressing stage, but directly performs densification treatment, followed by shaping and reshaping.
[0131] This comparative example also provides an all-solid-state battery, which is prepared in the same way as in Example 1, except that the densification treatment is performed using the method provided in this comparative example.
[0132] Comparative Example 3 This comparative example provides a method for densifying the solid-solid interface of an all-solid battery. The only difference from Example 1 is that it does not include a shaping stage. After pre-pressing, densification is performed, and then shaping is performed directly.
[0133] This comparative example also provides an all-solid-state battery, which is prepared in the same way as in Example 1, except that the densification treatment is performed using the method provided in this comparative example.
[0134] Comparative Example 4 This comparative example provides a method for densifying the solid-solid interface of an all-solid-state battery. The only difference from Example 1 is that it does not include the pre-pressing stage and the shaping stage, but directly performs densification treatment and then shaping.
[0135] This comparative example also provides an all-solid-state battery, which is prepared in the same way as in Example 1, except that the densification treatment is performed using the method provided in this comparative example.
[0136] Comparative Example 5 This comparative example provides a method for densifying the solid-solid interface of an all-solid battery. The only difference from Example 1 is that it does not include a densification stage, and the pre-pressing is completed directly into shaping and molding.
[0137] This comparative example also provides an all-solid-state battery, which is prepared in the same way as in Example 1, except that the densification treatment is performed using the method provided in this comparative example.
[0138] Comparative Example 6 This comparative example provides a method for densifying the solid-solid interface of an all-solid-state battery. The only difference from Example 1 is that the pre-pressing stage, densification stage, and shaping stage all use a pressure of 6MPa for rolling.
[0139] This comparative example also provides an all-solid-state battery, which is prepared in the same way as in Example 1, except that the densification treatment is performed using the method provided in this comparative example.
[0140] Comparative Example 7 This comparative example provides a method for densifying the solid-solid interface of an all-solid-state battery. The only difference from Example 1 is that the roller heating function is turned off in the pre-pressing stage, densification stage and shaping stage, and the roller pressing is performed at room temperature of 25°C.
[0141] This comparative example also provides an all-solid-state battery, which is prepared in the same way as in Example 1, except that the densification treatment is performed using the method provided in this comparative example.
[0142] Experimental Example 1 The all-solid-state batteries provided in Examples 1-2 and Comparative Examples 1-7 were subjected to performance tests, and the results are shown in Table 1.
[0143] Table 1 Performance of all-solid-state batteries
[0144] As shown in Table 1, the method provided in this embodiment of the invention can significantly reduce the solid-solid interface impedance instead of isostatic pressing, thereby improving battery capacity, initial coulombic efficiency, and battery capacity cycle retention, effectively enhancing the electrochemical performance of the battery. Furthermore, this embodiment of the invention employs a multi-stage gradient hot pressing method, enabling continuous production of solid-state batteries, improving production efficiency, reducing equipment footprint, and eliminating the need for isostatic pressing equipment and additional unpacking and repackaging equipment, thus reducing production costs.
[0145] Comparative Example 1 uses a traditional isostatic pressing process to densify solid-state batteries. This isostatic pressing process is intermittent, increasing equipment investment, safety risks, and production efficiency. Furthermore, the solid-solid interface impedance obtained by the traditional isostatic pressing process is significantly higher than that of the embodiments of this invention, leading to a decline in battery performance.
[0146] Comparative Examples 2-5, by eliminating one or two of the pre-pressing, shaping, and densification stages respectively, resulted in varying degrees of deterioration in the first discharge specific capacity, first coulombic efficiency, 0.5C cycle retention rate, and 1C discharge capacity of the resulting all-solid-state batteries. A significant increase in solid-solid interface impedance was also observed. This indicates that the three-stage rolling mode provided in this embodiment of the invention is beneficial for achieving interlayer densification between the positive and negative electrode sheets and the electrolyte layer. Comparative Example 6 used a single pressure for all three stages, and Comparative Example 7 performed rolling at room temperature. Both resulted in varying degrees of deterioration in the first discharge specific capacity, first coulombic efficiency, 0.5C cycle retention rate, and 1C discharge capacity, and a significant increase in solid-solid interface impedance. This demonstrates that even with a three-stage rolling mode, rolling under a single pressure or at a single temperature cannot achieve maximum densification between the positive and negative electrode sheets and the electrolyte layer, leading to varying degrees of deterioration in the relevant electrical performance parameters.
[0147] This invention provides a method for densifying the solid-solid interface in an all-solid-state battery, an all-solid-state battery and its fabrication method, and an electrical device thereof, which have at least the following advantages: 1. Significantly improved production efficiency: The method provided in this embodiment of the invention can realize continuous operation of cutting, stacking, densification and packaging, and the production line utilization rate is increased from <30% to more than 85%; the isostatic pressing and subsequent aluminum-plastic film unpacking / repacking process is eliminated, the equipment purchase cost is reduced by more than 60% and the footprint is reduced by 45%.
[0148] 2. Solid-solid interface performance optimization: The embodiments of the present invention effectively remove interlayer bubbles at the solid-solid interface through multi-stage gradient hot pressing, increasing the solid-solid interface contact area by 12-18%, reducing the DC internal resistance of the cell by 8-15%, and significantly improving the rate discharge performance.
[0149] 3. Enhanced interface compaction stability: The embodiments of the present invention can suppress the rebound of the electrode after being compressed by multi-stage gradient hot pressing, and the compaction density retention rate is increased from <60% under normal temperature roller pressing to more than 92%, and the long-term interface stability is close to the level of hot isostatic pressing.
[0150] 4. Significantly improved product yield: The method provided in this embodiment of the invention eliminates the bare cell disassembly and assembly process, avoids the risk of scratches and damage, and increases the finished product yield from 82-88% to over 97%.
[0151] 5. Improved production safety level: Completely eliminates the risk of high-pressure cavities in 300~500 MPa isostatic pressure equipment, significantly reducing the difficulty of high-pressure safety management in the workshop and the threat to personal safety.
[0152] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for densifying the solid-solid interface of an all-solid-state battery, characterized in that, The process includes stacking and assembling a positive electrode, a solid electrolyte layer, and a negative electrode to obtain a bare cell stack; and then performing a densification process on the bare cell stack. The densification process includes performing multi-stage gradient hot pressing on the bare cell stack using hot pressing rollers; the multi-stage gradient hot pressing includes a pre-pressing stage, a densification stage, and a shaping stage; the roller pressing pressure and roller pressing temperature in the densification stage are both higher than those in the pre-pressing stage and the shaping stage; the roller pressing temperature in the pre-pressing stage is higher than that in the shaping stage.
2. The method according to claim 1, characterized in that, Each stage of the multi-stage gradient hot pressing is provided with at least one set of pressure roller mechanisms, and each set of pressure roller mechanisms independently controls the roller pressing parameters; the roller pressing parameters include at least one of roller pressing temperature, roller pressing pressure, roller gap and roller pressing speed; each set of pressure roller mechanisms is provided with multiple roller pressing zones, and the roller gap of each roller pressing zone is independently controlled.
3. The method according to claim 2, characterized in that, The method for independently controlling the roll gap of each of the rolling sections includes: setting a thickness tester in the discharge area of at least one set of pressure roller mechanisms at each stage; each thickness tester collecting the actual thickness of at least one region of the bare cell stack; obtaining the target thickness difference between different regions of the bare cell stack by subtracting the actual thickness from the target thickness; when the absolute value of the target thickness difference is ≥0.1mm, the thickness data of the region of the bare cell stack corresponding to the target thickness difference is abnormal thickness data; and adjusting the roll gap of the rolling section corresponding to the region where the abnormal thickness data is located.
4. The method according to claim 3, characterized in that, The method for adjusting the roll gap of the roll pressing zone corresponding to the area where the abnormal thickness data is located includes: increasing the roll gap when the target thickness difference is positive; and decreasing the roll gap when the target thickness difference is negative.
5. The method according to claim 1, characterized in that, The pre-compression stage has a roller temperature of 45~95℃, a roller pressure of 5~25MPa, and a roller speed of 1~5m / min; the compression rate of the pre-compression stage is 5~10%.
6. The method according to claim 1, characterized in that, The rolling temperature during the densification stage is 65~205℃, the rolling pressure is 15~50MPa, and the rolling speed is 1~5m / min; the compression rate during the densification stage is 10~15%.
7. The method according to claim 1, characterized in that, The rolling temperature during the shaping stage is 19~145℃, the rolling pressure is 10~30MPa, and the rolling speed is 1~5m / min; the compression rate during the shaping stage is 5~10%.
8. The method according to claim 1, characterized in that, The roll gap of at least one pressing roller mechanism in the densification stage satisfies the following condition: in the direction of movement of the bare cell stack, the roll gap at both ends of the pressing roller mechanism is greater than the roll gap in the middle region.
9. The method according to claim 1, characterized in that, The material of the transport structure in the densification process of the bare cell stack is a high-temperature resistant material, including glass fiber PTFE or aramid-based PTFE composite material.
10. The method according to claim 1, characterized in that, It also includes shaping the bare cell stack after densification treatment.
11. The method according to claim 10, characterized in that, The shaping parameters include: shaping temperature of 15~80℃, shaping pressure of 1~5MPa, and shaping time of 10~30s.
12. The method according to claim 10 or 11, characterized in that, The flatness of the bare cell stack after shaping is ≤0.1mm / m.
13. The method according to claim 10 or 11, characterized in that, The actual thickness of the shaped bare cell stack is ≤ ±0.1 mm from the target thickness.
14. A method for preparing an all-solid-state battery, characterized in that, The process includes preparing a positive electrode, a solid electrolyte layer, and a negative electrode, and then performing a densification process using the method described in any one of claims 1 to 13 to obtain a densified bare cell stack, and then encapsulating the densified bare cell stack.
15. The preparation method according to claim 14, characterized in that, Prior to encapsulation, tabs are welded onto the densified bare cell stack.
16. The preparation method according to claim 15, characterized in that, The welding methods for electrode tabs include either ultrasonic welding or laser welding.
17. An all-solid-state battery, characterized in that, It is prepared by the method described in any one of claims 14 to 16.
18. An electrical appliance, characterized in that, Including the all-solid-state battery as described in claim 17.