A single cell, a battery pack, and a method for manufacturing a single cell.

By incorporating a temperature- or pressure-triggered electrolyte reservoir within a single cell, the problem of electrolyte replenishment after lithium-ion battery formation is solved, enabling efficient production without secondary electrolyte injection and improving battery production efficiency and quality.

CN123120993APending Publication Date: 2026-11-17SUNWODA MOBILITY ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611496045.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing lithium-ion battery manufacturing processes, a second electrolyte injection is required after formation, resulting in low production efficiency and quality risks.

Method used

An electrolyte reservoir is installed inside the casing of a single battery cell. The reservoir is ruptured by temperature or pressure to replenish the electrolyte, thus avoiding secondary electrolyte injection.

Benefits of technology

Simplify processes, improve production efficiency, reduce quality risks, and increase the production efficiency of individual cells and battery packs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120993A_ABST
    Figure CN123120993A_ABST
Patent Text Reader

Abstract

This invention relates to the field of battery technology and discloses a single-cell battery, a battery pack, and a method for manufacturing a single-cell battery. The single-cell battery of this invention includes a casing, an electrode core, and a reservoir. The casing has a receiving cavity. The electrode core is disposed within the receiving cavity. The reservoir is disposed within the receiving cavity and has a storage space for storing a first electrolyte. The reservoir is configured such that it ruptures when the temperature inside the receiving cavity rises to a preset temperature, allowing the first electrolyte to flow from the storage space into the receiving cavity. By providing a reservoir containing the first electrolyte within the casing, the temperature inside the receiving cavity rises during the formation process of the single-cell battery. When the temperature reaches the preset temperature, the reservoir ruptures, allowing the first electrolyte to flow into the receiving cavity, replenishing the consumed electrolyte. Therefore, secondary electrolyte replenishment is unnecessary after formation, simplifying the process and improving the production efficiency of the single-cell battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and specifically to a single cell, a battery pack, and a method for manufacturing a single cell. Background Technology

[0002] The manufacturing process of lithium-ion batteries typically involves multiple steps, including initial electrolyte filling, formation, and secondary electrolyte filling. During the initial charge and discharge of a lithium-ion battery, the electrolyte undergoes a reduction decomposition reaction on the surface of the negative electrode, forming a layer of SEI film (solid electrolyte interface film) covering the electrode surface. The formation of this SEI film consumes a certain amount of electrolyte components. Therefore, to ensure sufficient electrolyte inside the battery and guarantee its electrochemical performance and cycle life, current technologies require secondary electrolyte filling after formation to replenish the consumed electrolyte, resulting in low production efficiency. Summary of the Invention

[0003] This application aims to address at least one of the technical problems existing in the prior art. To this end, this application proposes a single-cell battery that can improve production efficiency.

[0004] This application also proposes a battery pack having the above-mentioned single cell and a method for manufacturing the single cell.

[0005] A single-cell battery according to a first aspect embodiment of this application includes a casing, an electrode core, and a reservoir. The casing has a receiving cavity. The electrode core is disposed within the receiving cavity. The reservoir is disposed within the receiving cavity and has a reservoir space for storing a first electrolyte. The reservoir is configured such that when the temperature inside the receiving cavity rises to a preset temperature, the reservoir ruptures, allowing the first electrolyte to flow from the reservoir space into the receiving cavity.

[0006] The single cell according to the embodiments of this application has at least the following beneficial effects: a reservoir containing a first electrolyte is provided in the casing. During the formation process of the single cell, the temperature inside the reservoir will rise. When the temperature rises to a preset temperature, the reservoir will rupture, allowing the first electrolyte to flow into the reservoir and replenish the consumed electrolyte. Therefore, there is no need to replenish the electrolyte after formation, which simplifies the process and improves the production efficiency of the single cell.

[0007] According to some embodiments of this application, the single battery cell further includes a separator membrane disposed within the receiving cavity, the separator membrane being located between the electrode core and the inner wall of the housing, the liquid storage bladder being connected to the side of the separator membrane facing the electrode core, and / or, the liquid storage bladder being connected to the side of the separator membrane facing the inner wall of the housing.

[0008] According to some embodiments of this application, the single cell includes a plurality of said liquid storage bladders, at least some of said liquid storage bladders having a preset pressure, and when said liquid storage bladders are subjected to pressure that rises to said preset pressure, said liquid storage bladders rupture to allow the first electrolyte to flow from said liquid storage space to said receiving cavity.

[0009] According to some embodiments of this application, when the reservoir is connected to the side of the separator facing the electrode core, and when the reservoir is connected to the side of the separator facing the inner wall of the housing; the reservoir includes a first reservoir and a second reservoir, the first reservoir is connected to the side of the separator facing the inner wall of the housing, the second reservoir is connected to the side of the separator facing the electrode core, the first reservoir has a first preset pressure, the second reservoir has a second preset pressure, and the first preset pressure is greater than the second preset pressure.

[0010] According to some embodiments of this application, the single battery cell includes a plurality of liquid storage bladders, the separator has a connecting surface facing the electrode core or the inner wall of the housing, the plurality of liquid storage bladders are connected to the connecting surface, the liquid storage bladders located on the connecting surface include a third liquid storage bladder and a fourth liquid storage bladder, the third liquid storage bladder and the fourth liquid storage bladder are spaced apart along the extension direction of the connecting surface, the minimum dimension of the third liquid storage bladder along the extension direction of the connecting surface is greater than the maximum dimension of the fourth liquid storage bladder along the extension direction of the connecting surface, and / or, the wall thickness of the third liquid storage bladder is less than the wall thickness of the fourth liquid storage bladder.

[0011] According to some embodiments of this application, the connecting surface includes a central region and an edge region. Along the normal of the connecting surface on a plane parallel to the connecting surface, the orthographic projection of the central region covers the center point of the orthographic projection of the electrode core. The third liquid reservoir is connected to the edge region, and the fourth liquid reservoir is connected to the central region.

[0012] According to some embodiments of this application, the connecting surface is the side surface of the separator facing the electrode core.

[0013] According to some embodiments of this application, the single battery cell includes a plurality of liquid storage bladders, the separator has a connecting surface facing the electrode core or the inner wall of the casing, the connecting surface includes a central region and an edge region, the liquid storage bladder includes a fifth liquid storage bladder and a sixth liquid storage bladder, the fifth liquid storage bladder is connected to the central region, the sixth liquid storage bladder is connected to the edge region, along the normal of the connecting surface on a plane parallel to the connecting surface, the orthographic projection of the central region covers the center point of the orthographic projection of the electrode core, and the arrangement density of the fifth liquid storage bladder is greater than the arrangement density of the sixth liquid storage bladder.

[0014] According to some embodiments of this application, the maximum dimension of the fifth reservoir along the connecting surface is smaller than the minimum dimension of the sixth reservoir along the connecting surface.

[0015] According to some embodiments of this application, the single cell includes a second electrolyte disposed in the receiving cavity, and the content of film-forming additives in the first electrolyte is greater than the content of film-forming additives in the second electrolyte.

[0016] According to some embodiments of this application, the material of the reservoir includes at least one of ethylene-vinyl acetate copolymer and polyvinylidene fluoride-hexafluoropropylene copolymer.

[0017] The battery pack according to the second aspect of this application includes any one of the individual cells in the first aspect of the embodiment.

[0018] The battery pack according to the embodiments of this application has at least the following beneficial effects: the individual battery has a reservoir containing a first electrolyte inside the casing. During the formation process, the temperature inside the reservoir will rise. When the temperature rises to a preset temperature, the reservoir will rupture, allowing the first electrolyte to flow into the reservoir and replenish the consumed electrolyte. Therefore, there is no need for secondary electrolyte replenishment after formation, which simplifies the process, improves the production efficiency of the individual battery, and thus improves the production efficiency of the battery pack.

[0019] A method for manufacturing a single-cell battery according to a third aspect of this application is used to manufacture a single-cell battery as described in any one of the first aspect embodiments. The manufacturing method includes: mixing a first electrolyte with an oil phase solution to form an emulsion droplet; solidifying the emulsion droplet to solidify the oil phase solution to form the reservoir, and the reservoir storing the first electrolyte.

[0020] The method for manufacturing a single-cell battery according to the embodiments of this application has at least the following beneficial effects: The first electrolyte is an aqueous phase. After mixing the first electrolyte and an oil phase to form a water-in-oil emulsion droplet, the oil phase solution is solidified to form a reservoir with a storage space, and the first electrolyte is stored within the storage space of the reservoir. This allows for continuous production of the reservoir using microfluidic chips or similar methods, improving the production efficiency of the reservoir and thus increasing the production efficiency of the single-cell battery.

[0021] According to some embodiments of this application, the manufacturing method includes: obtaining a separator membrane, dispersing the reservoir in an adhesive, coating the mixture of the reservoir and the adhesive onto the surface of the separator membrane and drying it, wrapping the separator membrane around the outer peripheral surface of the electrode core, and inserting them together into the receiving cavity.

[0022] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description

[0023] The present application will be further described below with reference to the accompanying drawings and embodiments, wherein: Figure 1 This is an exploded view of a single cell in one embodiment of this application; Figure 2 This is a top view of a single battery cell in one embodiment of this application; Figure 3 for Figure 2 First-state sectional view of the AA section line; Figure 4 for Figure 2 Second-state sectional view of section line AA in the middle; Figure 5 This is a schematic diagram of the distribution of the reservoir in the first embodiment of this application; Figure 6 This is a schematic diagram of the distribution of the reservoir in the second embodiment of this application; Figure 7 This is a schematic diagram showing the distribution of the reservoir in the third embodiment of this application; Figure 8 This is a schematic diagram of the distribution of the reservoir in the fourth embodiment of this application.

[0024] Reference numerals: Single cell 100; Casing 101; Receiving cavity 102; Electrode core 103; Liquid reservoir 104; Separator 105; Liquid storage space 301; First liquid reservoir 501; Second liquid reservoir 502; Connecting surface 801; Third liquid reservoir 802; Fourth liquid reservoir 803; Central region 804; Edge region 805; Fifth liquid reservoir 806; Sixth liquid reservoir 807. Detailed Implementation

[0025] The embodiments of this application are described in detail below. Examples of these embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application.

[0026] In the description of this application, it should be understood that the orientation descriptions, such as up, down, front, back, left, right, etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.

[0027] In the description of this application, "several" means one or more, "multiple" means two or more, "greater than," "less than," and "exceeding" are understood to exclude the stated number, while "above," "below," and "within" are understood to include the stated number. The use of "first" and "second" in the description is merely for distinguishing technical features and should not be construed as indicating or implying relative importance, or implicitly indicating the number of indicated technical features, or implicitly indicating the order of the indicated technical features.

[0028] In the description of this application, unless otherwise expressly defined, terms such as "setup," "installation," and "connection" should be interpreted broadly, and those skilled in the art can reasonably determine the specific meaning of the above terms in this application in conjunction with the specific content of the technical solution.

[0029] In the description of this application, the terms "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0030] refer to Figures 1 to 4 According to a first aspect embodiment of the present application, a single-cell battery 100 includes a housing 101, an electrode core 103, and a reservoir 104. The housing 101 has a receiving cavity 102. The electrode core 103 is disposed within the receiving cavity 102. The reservoir 104 is disposed within the receiving cavity 102 and has a reservoir space 301 for storing a first electrolyte. The reservoir 104 is configured such that when the temperature inside the receiving cavity 102 rises to a preset temperature, the reservoir 104 ruptures, allowing the first electrolyte to flow from the reservoir space 301 into the receiving cavity 102. A reservoir 104 containing a first electrolyte is provided inside the housing 101. During the formation process of the single cell 100, the temperature inside the containment cavity 102 will rise. When the temperature rises to a preset temperature, the reservoir 104 will rupture, allowing the first electrolyte to flow into the containment cavity 102 to replenish the consumed electrolyte. Therefore, there is no need for secondary electrolyte replenishment after formation, which simplifies the process and improves the production efficiency of the single cell 100.

[0031] It should be noted that the rupture of the reservoir 104 refers to the rise in internal temperature of the single cell 100 during the formation process. The wall material of the reservoir 104 is a thermosensitive polymer, and its glass transition temperature or melting point is set within the formation temperature range. When the temperature reaches the preset temperature, the bladder wall softens or undergoes a phase transition, significantly reducing its mechanical strength. Under the action of internal gas pressure or external mechanical stress, it ruptures, releasing the first electrolyte. This thermosensitive triggering mechanism is perfectly synchronized with the formation process, requiring no additional heating equipment.

[0032] Existing technologies pose significant quality control risks for individual battery cells 100 because secondary electrolyte filling requires reopening the sealed battery. This process carries risks such as moisture intrusion, electrolyte leakage, and contamination. Particularly in high-humidity environments, even brief opening of the battery seal can allow moisture to enter, affecting battery performance. Furthermore, the quality of resealing after secondary electrolyte filling is difficult to guarantee, posing a risk of electrolyte leakage after long-term use. This application addresses this issue by incorporating a electrolyte reservoir 104 that ruptures automatically at a preset temperature to replenish the electrolyte, eliminating the need for a secondary electrolyte replenishment process. This reduces quality issues associated with secondary replenishment and improves the yield rate of individual battery cells 100.

[0033] refer to Figure 1 , Figures 5 to 7In some embodiments of this application, the single cell 100 further includes a separator 105 disposed in the receiving cavity 102, the separator 105 being located between the electrode core 103 and the inner wall of the housing 101, and a liquid storage bladder 104 being connected to the side of the separator 105 facing the electrode core 103, and / or, the liquid storage bladder 104 being connected to the side of the separator 105 facing the inner wall of the housing 101. The separator 105 can wrap the electrode core 103 during the assembly of the single cell 100, preventing the electrode core 103 from being scratched by the housing 101 during installation. Therefore, the separator 105 is positioned between the electrode core 103 and the inner wall of the housing 101. The liquid storage bladder 104 is connected to the separator 105. This facilitates the positioning of the liquid storage bladder 104. For example, the liquid storage bladder 104 can be positioned on the side of the separator 105 facing the electrode core 103 to replenish the space between the electrode core 103 and the separator 105. Alternatively, the liquid storage bladder 104 can be connected to the side of the separator 105 facing the inner wall of the housing 101 to replenish the space between the housing 101 and the separator 105. The space between the 5 cells is used for liquid replenishment, which also enhances the functionality of the separator 105. It serves not only as a protective membrane to prevent the electrode core 103 from being scratched when it enters the casing, but also as a functional membrane that houses the liquid reservoir 104 with liquid replenishment function. This fully utilizes the positional advantage of the separator 105 in the structure of the single cell 100, upgrading the traditional protective component into a functional component. Furthermore, unlike the existing technology that sets up an independent liquid reservoir or adds microcapsules to the electrolyte, the liquid reservoir 104 in this application is integrated and connected to the separator 105, making full use of the space of the existing components, without occupying additional internal space of the single cell 100, and without reducing the energy density of the battery.

[0034] refer to Figures 2 to 4 In some embodiments of this application, the single-cell battery 100 includes multiple reservoirs 104, at least some of which have a preset pressure. When the pressure of a reservoir 104 rises to the preset pressure, the reservoir 104 ruptures, allowing the first electrolyte to flow from the reservoir space 301 to the receiving cavity 102. During the formation process, the electrode materials undergo volume expansion due to the insertion and extraction of lithium ions in the positive and negative electrode materials, generating mechanical stress. This mechanical stress acts on the reservoirs 104 on the separator 105. When the stress exceeds the rupture threshold of the reservoir 104, i.e., the preset stress, the reservoir 104 ruptures and releases the first electrolyte. This mechanical triggering mechanism utilizes the natural physical changes during the formation process without external intervention.

[0035] It should be noted that in some embodiments, there are various types of reservoir 104. Some of them soften or undergo a phase change when the temperature reaches a preset temperature, resulting in a significant decrease in mechanical strength and rupture under internal gas pressure or external mechanical stress. Other reservoir 104 has better heat resistance and will not rupture in this case, but will rupture when the pressure rises to a preset pressure. The mechanical stress is caused by the expansion of the electrode core 103, resulting in the joint compression of the electrode core 103 and the shell 101 (see reference). Figure 4 The expansion of the electrode core 103 occurs during the formation process and multiple cycles of use. This part of the reservoir 104 can be used for electrolyte replenishment in the above-mentioned scenarios. This application can adjust the different conditions for triggering the rupture mechanism by using reservoirs 104 with different compositions, sizes or wall thicknesses, so that different types of reservoirs 104 can meet the electrolyte replenishment requirements in different scenarios.

[0036] It should be noted that, in some embodiments, a trigger control layer can be provided on the reservoir 104 to more precisely control the timing of electrolyte replenishment. The trigger control layer can be a thin film with specific mechanical properties. Its function is to disperse and buffer the pressure generated by the expansion of the electrode core 103 during the initial cycling of the single-cell battery 100, protecting the reservoir 104 from premature rupture. When the electrode core 103 expands to a certain extent, the trigger control layer yields or ruptures, allowing the pressure to act directly on the reservoir 104, thereby triggering rupture. For example, in some embodiments, polypropylene (PP), polyethylene (PE), or homopolymer polyvinylidene fluoride (PVDF) can be used as the trigger control layer, covering part of the surface of the reservoir 104 to improve its mechanical properties. This prevents this part of the reservoir 104 from rupturing due to excessive decrease in mechanical strength caused by temperature rise during formation, allowing it to withstand greater mechanical stress from the expansion of the electrode core 103 during later cycling processes before rupture, thus enhancing the functional versatility of the reservoir 104.

[0037] refer to Figures 3 to 7In some embodiments of this application, the reservoir 104 is connected to the side of the isolation membrane 105 facing the electrode core 103, and when the reservoir 104 is connected to the side of the isolation membrane 105 facing the inner wall of the housing 101; the reservoir 104 includes a first reservoir 501 and a second reservoir 502, the first reservoir 501 is connected to the side of the isolation membrane 105 facing the inner wall of the housing 101, the second reservoir 502 is connected to the side of the isolation membrane 105 facing the electrode core 103, the first reservoir 501 has a first preset pressure, the second reservoir 502 has a second preset pressure, and the first preset pressure is greater than the second preset pressure. The first reservoir 501 faces the housing 101, and its first preset pressure is set higher to make it less likely to rupture. This is suitable for electrolyte replenishment of the electrode core 103 in the later stages of cycle use (e.g., after completing 1000-2000 charge-discharge cycles). At this time, the electrode core 103 expands to a larger volume, resulting in higher pressure on the reservoir 104, which triggers the rupture of the first reservoir 501. The second reservoir 502 faces the electrode core 103 and can directly sense the pressure from the expansion of the electrode core 103. Its second preset pressure is set lower to make it suitable for electrolyte replenishment during the mid-cycle expansion of the electrode core 103 (e.g., after completing 500-1000 charge-discharge cycles). The design facing the electrode core 103 also allows for rapid electrolyte replenishment to the area around the electrode core 103. When the second reservoir 502 ruptures, the released first electrolyte will diffuse into the pores of the electrode core 103 under the drive of concentration gradient and capillary action, replenishing the consumed electrolyte. Because the electrolyte reservoir 104 adheres tightly to the electrode core 103 after expansion, the released electrolyte can quickly diffuse into the electrodes and diaphragm of the electrode core 103, ensuring uniform electrolyte distribution. A first electrolyte reservoir 501 and a second electrolyte reservoir 502 are configured to implement a staged replenishment strategy. The second electrolyte reservoir 502 ruptures first to replenish the electrolyte during the middle stage of the cycle, and the first electrolyte reservoir 501 ruptures later to replenish the electrolyte during the later stage of the cycle.

[0038] refer to Figure 3 , Figure 4 and Figure 8In some embodiments of this application, the single battery cell 100 includes a plurality of liquid storage sacs 104, the separator 105 has a connection surface 801 facing the electrode core 103 or the inner wall of the housing 101, the plurality of liquid storage sacs 104 are connected to the connection surface 801, the liquid storage sacs 104 located on the connection surface 801 include a third liquid storage sac 802 and a fourth liquid storage sac 803, the third liquid storage sac 802 and the fourth liquid storage sac 803 are spaced apart along the extension direction of the connection surface 801, the minimum dimension of the third liquid storage sac 802 along the extension direction of the connection surface 801 is greater than the maximum dimension of the fourth liquid storage sac 803 along the extension direction of the connection surface 801, and / or, the wall thickness of the third liquid storage sac 802 is less than the wall thickness of the fourth liquid storage sac 803. It should be noted that the extension direction of the connecting surface 801 refers to any direction parallel to the connecting surface 801. The third liquid reservoir 802 and the fourth liquid reservoir 803 are designed with different dimensions and wall thicknesses to achieve different rupture thresholds. For example, along the extension direction of the connecting surface 801, the size of the third liquid reservoir 802 is larger than that of the fourth liquid reservoir 803, making its internal pressure more unstable, its deformation resistance lower, and its susceptibility to rupture caused by external pressure fluctuations or disturbances. Similarly, the wall thickness of the third liquid reservoir 802 is smaller than that of the fourth liquid reservoir 803, resulting in lower structural strength, lower deformation resistance, and susceptibility to rupture caused by external pressure fluctuations or disturbances. Therefore, the third liquid reservoir 802 is more prone to rupture than the fourth liquid reservoir 803, realizing a graded rupture strategy for the liquid reservoir 104, enabling the third liquid reservoir 802 and the fourth liquid reservoir 803 to achieve electrolyte replenishment at different stages of the single cell 100. For example, in some embodiments, the third reservoir 802 and the second reservoir 502 are the same reservoir 104, which is located on the side of the separator 105 facing the electrode core 103. The characteristic of being easier to break can be used to replenish the electrolyte in the middle of the cycle; the fourth reservoir 803 and the first reservoir 501 are the same reservoir 104, which is located on the side of the separator 105 facing the shell 101. It has a higher rupture threshold and the characteristic of not being easy to break can be used to replenish the electrolyte in the later stage of the cycle.

[0039] It should be noted that the ability of the reservoir 104 to resist deformation and rupture can be achieved by changing the wall thickness of the reservoir 104 (increasing the wall thickness increases the rupture threshold, decreasing the wall thickness decreases the rupture threshold), changing the size of the reservoir 104 (increasing the size decreases the rupture threshold, decreasing the size increases the rupture threshold), and changing the material of the reservoir 104 (adding polymers such as polypropylene and polyethylene can increase structural strength and heat resistance).

[0040] It should be noted that the reference Figure 8 In some embodiments, the reservoir 104 may be spherical, elliptical, or other irregular shapes.

[0041] refer to Figure 8In some embodiments of this application, the connecting surface 801 includes a central region 804 and an edge region 805. Along the normal to the connecting surface 801 on a plane parallel to the connecting surface 801, the orthographic projection of the central region 804 covers the center point of the orthographic projection of the pole core 103. The third liquid reservoir 802 is connected to the edge region 805, and the fourth liquid reservoir 803 is connected to the central region 804. (See reference...) Figure 4 During the cycling process, the expansion of the electrode core 103 is most significant in the central region and relatively smaller in the edge region. Therefore, a fourth liquid reservoir 803 is set in the central region 804 of the connection surface 801. The fourth liquid reservoir 803 has a higher rupture threshold. A third liquid reservoir 802 is set in the edge region 805 of the connection surface 801. The third liquid reservoir 802 has a lower rupture threshold. When the electrode core 103 expands, the expansion of the central region first compresses the fourth liquid reservoir 803, and the expansion of the edge region then compresses the third liquid reservoir 802. This achieves synchronous rupture of the third liquid reservoir 802 and the fourth liquid reservoir 803, avoiding premature rupture of the edge region or delayed rupture of the central region, and achieving uniform and timely replenishment of electrolyte.

[0042] It should be noted that the center point of the orthographic projection of the pole core 103 refers to the geometric center of the orthographic projection of the pole core 103, or it can refer to the projection point of the centroid of the pole core 103 onto a plane parallel to the connecting surface 801 along the normal of the connecting surface 801. The fact that the central area 804 covers the center point means that the central area 804 can cover more of the middle area of ​​the pole core 103 during expansion, and that the edge area 805 can cover the edge area of ​​the pole core 103.

[0043] In some embodiments of this application, the connection surface 801 is the surface of the separator 105 facing the electrode core 103. This design facing the electrode core 103 allows for rapid replenishment of electrolyte to the area surrounding the electrode core 103. When the third reservoir 802 ruptures, the released first electrolyte diffuses into the pores of the electrode core 103 under the influence of concentration gradient and capillary action, replenishing the consumed electrolyte. Because the reservoir 104 adheres tightly to the electrode core 103 after expansion, the released electrolyte can diffuse more quickly into the electrodes and separator of the electrode core 103.

[0044] refer to Figure 8In some embodiments of this application, the single cell 100 includes multiple liquid storage bladders 104, and the separator 105 has a connection surface 801 facing the electrode core 103 or the inner wall of the housing 101. The connection surface 801 includes a central region 804 and an edge region 805. The liquid storage bladders 104 include a fifth liquid storage bladder 806 and a sixth liquid storage bladder 807. The fifth liquid storage bladder 806 is connected to the central region 804, and the sixth liquid storage bladder 807 is connected to the edge region 805. Along the normal of the connection surface 801 on a plane parallel to the connection surface 801, the orthographic projection of the central region 804 covers the center point of the orthographic projection of the electrode core 103. The arrangement density of the fifth liquid storage bladder 806 is greater than the arrangement density of the sixth liquid storage bladder 807. The density setting refers to the number of electrolyte reservoirs 104 per unit area in the central region 804 or the edge region 805. Setting a denser fifth electrolyte reservoir 806 in the central region 804 can improve the overall deformation resistance, disperse the mechanical stress, reduce stress concentration in local electrolyte reservoirs 104, and increase the rupture threshold. Setting a relatively sparse sixth electrolyte reservoir 807 in the edge region 805 can lower the rupture threshold. Since the expansion of the electrode core 103 is most significant in the central region and relatively smaller in the edge region during the cycle, the fifth electrolyte reservoir 806 and the sixth electrolyte reservoir 807 can be ruptured simultaneously, avoiding premature rupture in the edge region or delayed rupture in the central region, and achieving uniform and timely replenishment of electrolyte.

[0045] refer to Figure 8 In some embodiments of this application, the maximum dimension of the fifth liquid reservoir 806 extending along the connecting surface 801 is smaller than the minimum dimension of the sixth liquid reservoir 807 extending along the connecting surface 801. The size of the sixth liquid reservoir 807 is smaller than that of the fourth liquid reservoir 803 along the connecting surface 801, making its internal pressure more unstable, its deformation resistance lower, and making it more susceptible to rupture due to external pressure fluctuations or disturbances. When the electrode core 103 expands, the expansion of the central region first compresses the fifth liquid reservoir 806, and the expansion of the edge region then compresses the sixth liquid reservoir 807, achieving synchronous rupture of the fifth liquid reservoir 806 and the sixth liquid reservoir 807, avoiding premature rupture of the edge region or delayed rupture of the central region, and achieving uniform and timely replenishment of the electrolyte.

[0046] It should be noted that in some embodiments, the first reservoir 501, the fourth reservoir 803, and the fifth reservoir 806 refer to the same reservoir 104, and the second reservoir 502, the third reservoir 802, and the sixth reservoir 807 refer to the same reservoir 104. That is, a portion of the reservoir 104 is disposed in the central region 804, and this portion of the reservoir 104 has a larger thickness, a smaller size, and a larger placement density, resulting in a higher rupture threshold; another portion of the reservoir 104 is disposed in the edge region 805, and this portion of the reservoir 104 has a smaller thickness, a larger size, and a smaller placement density, resulting in a lower rupture threshold.

[0047] In some embodiments of this application, the single-cell battery 100 includes a second electrolyte disposed in the receiving cavity 102, and the content of film-forming additives in the first electrolyte is greater than that in the second electrolyte. Film-forming additives are trace chemical components in the electrolyte specifically designed to preferentially decompose on the negative electrode surface to form a stable solid electrolyte interphase (SEI) film, such as vinylene carbonate. By disposing of the first electrolyte containing film-forming additives in the reservoir 104, the reservoir 104 can better repair and optimize the SEI film after rupture during the formation process. This not only replenishes the consumed electrolyte components but also improves the SEI film quality by adding film-forming additives, thereby enhancing the performance and cycle life of the single-cell battery 100. In some embodiments, the first electrolyte may also contain functional additives such as flame retardants and overcharge protectants, depending on specific needs, to improve the performance of the replenished electrolyte.

[0048] In some embodiments, the separator 105 is connected to the electrolyte reservoir 104 on both the side facing the electrode core 103 (inner layer) and the side facing the housing 101 (outer layer). The electrolyte compositions encapsulated in the inner and outer electrolyte reservoirs 104 are also different. The electrolyte encapsulated in the inner electrolyte reservoir 104 uses a high concentration of LiFSI salt (lithium bisfluorosulfonyl imide) and FEC (fluoroethylene carbonate) solvent, which is more suitable for silicon-carbon anode systems and can form a more stable SEI film. The electrolyte encapsulated in the outer electrolyte reservoir 104 uses conventional LiPF6 (lithium hexafluorophosphate) salt and VC (ethylene carbonate) additive, mainly used to replenish the consumed electrolyte and maintain the basic performance of the single cell 100.

[0049] In some embodiments of this application, the reservoir 104 is made of at least one of ethylene-vinyl acetate copolymer (EVA) and polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP). By controlling the content of the comonomer (such as the VA (vinyl acetate) content in EVA, or the HFP (hexafluoropropylene) content in PVDF-HFP), it can be made to soften significantly at the formation temperature. Combined with the extrusion pressure inside the shell 101, this causes the reservoir 104 to rupture, allowing it to rupture at a preset temperature to replenish the electrolyte.

[0050] Here is a specific example: EVA (VA content 26.7 wt%) was selected as the vesicle wall material for the reservoir 104, with a Vicat softening point of 45°C. The Vicat softening point is an indicator of when a thermoplastic begins to soften and lose its rigidity under heating conditions. A Vicat softening point of 45°C means that EVA with a VA content of 26.7 wt% will begin to soften significantly at 45°C. It should be noted that the Vicat softening point of the material in this embodiment is a material characteristic, and the Vicat softening point of many materials can be found in corresponding material data sheets or measured using a Vicat softening point measuring instrument. This temperature was set in the mid-stage of the formation process, when the SEI film formation reaction reaches its peak, providing a good opportunity for the film-forming additives to take effect. During the formation of the single cell 100, the internal temperature of the single cell 100 gradually increases with the Joule heating effect of the formation charge and discharge current. When the temperature reaches 45°C, EVA begins to soften significantly; when the temperature continues to rise to 48°C, the material strength drops below the critical value, and the reservoir 104 vesicles rupture under the drive of the internal base pressure to release the electrolyte. The released first electrolyte replenishes the electrolyte of the single cell 100, and the film-forming additives in the first electrolyte directly participate in the initial construction and optimization of the SEI film.

[0051] EVA is semi-crystalline at room temperature (25℃) with a tensile strength of approximately 1.8 MPa. As the internal temperature of the battery gradually increases during the formation process: Below 40℃: EVA maintains high crystallinity and mechanical strength, and the vesicle structure remains intact. 45℃ (Vicat softening point): The material begins to transform from a glassy state to a highly elastic state, and the tensile strength decreases significantly, but structural integrity can still be maintained. 48℃: The material softens further, and the tensile strength drops to approximately 0.1~0.8 MPa, which is no longer sufficient to effectively resist the basic pressure inside the vesicles.

[0052] During the early formation phase (temperature rises from 25℃ to 40℃): EVA vesicle walls exhibit high crystallinity and a tensile strength of approximately 0.1-1.8 MPa, exceeding the baseline internal pressure (approximately 0.005-0.3 MPa) caused by residual gas during encapsulation. The vesicle structure remains intact, ensuring reliable sealing and withstanding mechanical stress and pressure fluctuations from processes such as liquid injection, vacuum baking, and the initial temperature rise during formation. During this stage, the vesicles do not rupture, and the pre-encapsulated electrolyte is completely preserved.

[0053] During the mid-stage of formation (temperature rises from 40℃ to 45℃): As the temperature approaches and reaches the Vicat softening point of EVA, the material gradually softens, and its tensile strength begins to decrease. However, the strength of the vesicle walls is still sufficient to maintain structural integrity, preventing premature leakage. At this stage, the vesicles do not rupture, ensuring that they are released only at the moment when SEI film formation is most intense.

[0054] In the late-mid stage of formation (temperature reaches 48℃): the tensile strength of the wall material decreases to approximately 0.2~0.8 MPa, which is no longer sufficient to restrain the original internal pressure of approximately 0.005~0.3 MPa within the vesicles. Under the influence of internal pressure, the wall surface undergoes slow creep expansion, and the wall thickness continues to decrease, eventually resulting in viscoelastic tearing at the weakest point. The vesicles rupture, releasing the encapsulated electrolyte. At this point, formation enters the late-mid stage, and the SEI film formation reaction is at its peak. The released functionalized electrolyte contains a high concentration of film-forming additives, which directly participate in the initial construction and optimization of the SEI film—providing sufficient film-forming material during the most intense window of SEI film formation, contributing to the formation of a more uniform, dense, and low-resistivity SEI film.

[0055] Here are some specific examples:

[0056] The diameter of the reservoir 104 refers to the inner wall diameter when the reservoir 104 is spherical, and the rupture temperature threshold refers to the temperature at which the reservoir 104 ruptures. As can be seen from the comparison of Examples 1, 2 and 3, reducing the VA content can increase the Vicat softening point temperature, causing the reservoir 104 of Example 2 to rupture again in the later stage of the formation process, and the reservoir 104 of Example 3 to rupture again at the end of the formation process.

[0057] The detection of the rupture trigger stage of the reservoir 104 can be achieved by real-time monitoring of the voltage, capacity, or impedance spectrum of the region where the reservoir 104 is located within the single cell 100. A sudden change that deviates from normal electrochemical behavior indicates that the corresponding reservoir 104 has ruptured. Alternatively, during the research and development phase, a transparent or semi-transparent shell model 101 can be used to directly observe the rupture process of the reservoir 104 using a high-speed microscope. The rupture temperature threshold of the reservoir 104 is the temperature of the containing cavity 102 detected at the time of rupture.

[0058] The wall thickness of the reservoir 104 can be measured by cutting it open after fabrication to form a cross-section and then measuring it using an electron microscope, or by connecting the reservoir 104 to the isolation membrane 105 and then cutting both together to form a cross-section for measurement. The diameter of the reservoir 104 can be measured by connecting the reservoir 104 to the isolation membrane 105 and using an industrial camera to photograph and measure the maximum dimension of the reservoir 104 along the extension direction of the connection surface 804.

[0059] The following are some specific examples:

[0060] The rupture pressure threshold refers to the pressure experienced when the reservoir 104 ruptures. As shown in Examples 4 and 5, increasing the wall thickness of the reservoir 104 can increase the rupture pressure threshold. As shown in Examples 5 and 6, decreasing the diameter of the reservoir 104 can increase the rupture pressure threshold. The rupture pressure threshold can be determined by applying pressure to the reservoir 104 in real time after its preparation and detecting the current pressure value and the state of the reservoir 104. The current pressure threshold is recorded when the reservoir 104 ruptures.

[0061] Therefore, by adjusting parameters such as the material, wall thickness, and size of the reservoir 104, the rupture pressure threshold or rupture temperature threshold of the reservoir 104 can be controlled, so that it matches the temperature rise generated during the formation process or cycling stage of the single cell 100 and the pressure caused by the expansion of the electrode core 103, thereby achieving multi-stage replenishment of electrolyte for the single cell 100 at different stages.

[0062] The battery pack according to the second aspect of the present application includes a single cell 100 of any one of the first aspect embodiments. The single cell 100 has a reservoir 104 containing a first electrolyte within a housing 101. During the formation process, the temperature inside the reservoir 102 rises. When the temperature reaches a preset temperature, the reservoir 104 ruptures, allowing the first electrolyte to flow into the reservoir 102, replenishing the consumed electrolyte. Therefore, no secondary electrolyte replenishment is required after formation, simplifying the process and improving the production efficiency of the single cell 100, thereby improving the production efficiency of the battery pack.

[0063] A method for manufacturing a single-cell battery 100 according to a third aspect embodiment of this application is used to manufacture the single-cell battery 100 of any one of the first aspect embodiments. The manufacturing method includes: mixing a first electrolyte with an oil phase solution to form an emulsion droplet; solidifying the emulsion droplet to solidify the oil phase solution to form a reservoir 104, and storing the first electrolyte in a reservoir space 301. The first electrolyte is an aqueous phase. After mixing the first electrolyte and the oil phase to form a water-in-oil emulsion droplet, solidifying the oil phase solution forms the reservoir 104 with the reservoir space 301, and the first electrolyte is stored within the reservoir space 301 of the reservoir 104. This allows for continuous production of the reservoir 104 using microfluidic chips or similar methods, improving the production efficiency of the reservoir 104 and thus improving the production efficiency of the single-cell battery 100.

[0064] It should be noted that in some embodiments, the emulsion droplets are WO-type emulsions (water-in-oil emulsions), which are emulsion systems formed by dispersing the aqueous phase in the form of tiny droplets in a continuous oil phase. The first electrolyte serves as the internal dispersed phase, and the oil phase solution serves as the external continuous phase. By solidifying the oil phase solution, a reservoir 104 with a reservoir space 301 can be formed, and the first electrolyte is stored in the reservoir space 301 of the reservoir 104.

[0065] In some embodiments of this application, the manufacturing method includes: obtaining a separator 105, dispersing a liquid reservoir 104 in an adhesive, coating a mixture of the liquid reservoir 104 and the adhesive onto the surface of the separator 105 and drying it, wrapping the separator 105 around the outer peripheral surface of the electrode core 103, and fitting them together into the receiving cavity 102. By coating, a large number of liquid reservoirs 104 can be efficiently connected to the separator 105, improving the processing efficiency of the separator 105 with the liquid reservoirs 104 connected, thereby improving the processing efficiency of the single-cell battery 100.

[0066] The following are specific manufacturing examples: This embodiment applies to a square aluminum-cased lithium iron phosphate (LFP) single-cell battery system 100, which features high safety and long cycle life, but still consumes a certain amount of electrolyte during formation. The single-cell battery 100 adopts a square aluminum-cased structure with a capacity of 52 Ah and is used in an energy storage system. The separator 105 uses Mylar sheets with a 30 μm thick polyester film (PET) as the substrate. An array of reservoir bladders 104 is arranged in the inner layer of the separator 105 (on the side facing the electrode core 103). The reservoir bladders 104 have a spherical structure with a diameter of 100-300 μm and an average diameter of 200 μm. The wall material of the reservoir bladders 104 is polypropylene (PP) with a wall thickness of 8-15 μm and an average wall thickness of 10 μm. The distribution density of the reservoir bladders 104 on the separator 105 is 5 × 10⁻⁶. 5 The electrolyte reservoirs 104 are evenly distributed across the entire surface of the separator 105. Each reservoir 104 contains approximately 60 pL (picoliter) of a first electrolyte, comprising 5% VC (ethylene carbonate) and 2% LiDFOB (lithium difluorooxalate borate). The total electrolyte capacity of the reservoirs 104 is 180 μL / cm², and the total electrolyte capacity of the entire separator 105 (taking a 200 cm² area as an example) is 36 mL, approximately 10% of the total electrolyte volume of the single cell 100.

[0067] Manufacturing steps Step 1: Preparation of the reservoir 104. The reservoir 104 was prepared using microfluidic technology. A 5% polymer solution was dissolved in xylene to form the oil phase, and the electrolyte was used as the aqueous phase. The flow rates of both phases were controlled using a microfluidic chip: the oil phase flow rate was 10 mL / h, and the aqueous phase flow rate was 2 mL / h, to prepare a W / O emulsion. The emulsion droplets served as the precursor for the reservoir 104. By adjusting the flow rate ratio and channel size, the size of the reservoir 104 was controlled within the range of 100-300 μm.

[0068] Step 2: Curing of the reservoir 104. The prepared emulsion droplets are collected in a curing bath (cold ethanol, 5°C). The xylene solvent in the polymer solution evaporates, and the PP polymer cures to form the wall of the reservoir 104, encapsulating the electrolyte inside. The cured reservoir 104 is then centrifuged (3000 rpm, 5 minutes) and washed to remove unreacted monomers and solvent.

[0069] Step 3: Fixing the reservoir 104. The prepared reservoir 104 is uniformly dispersed in an adhesive, which is a 5% solution of PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene copolymer) dissolved in NMP (N-methylpyrrolidone). The reservoir 104-adhesive mixture is then coated onto the inner surface of the separator 105 to a thickness of 15 μm. Vacuum drying at 80°C for 2 hours removes the solvent, firmly fixing the reservoir 104 to the separator 105.

[0070] Step 4: Assembly of single cell 100. A separator 105 with an array of reservoir 104 is wrapped around the electrode core 103, with the reservoir 104 facing the electrode core 103. The square aluminum-cased cells are assembled according to conventional processes, and the electrode core 103 is installed into the single cell 100 casing 101.

[0071] Step 5: Initial electrolyte injection. Inject electrolyte through the injection port. The amount of electrolyte injected is 90% of the total required amount for 100 cells (108 mL, total required amount is 120 mL). After injection, let the cells stand under vacuum for 2 hours to allow the electrolyte to soak in.

[0072] Step 6: Formation process. Place the single cell 100 in the formation cabinet and perform formation according to the following temperature curve: (1) Charge to 3.0V at room temperature with a current of 0.05C; (2) Charge to 3.2V with a current of 0.1C, while raising the temperature to 50℃ and holding for 4 hours; (3) Charge to 3.4V at 50℃ with a current of 0.2C; (4) Cool to room temperature to complete the formation.

[0073] During the formation process, when the temperature reaches 50℃, the PP wall material of the reservoir 104 softens, and its mechanical strength decreases significantly. Simultaneously, the gas pressure generated during formation (approximately 0.2 MPa) acts on the wall of the reservoir 104, causing it to rupture and release the pre-stored 3 mL of the first electrolyte. The released electrolyte rapidly replenishes the electrodes and diaphragm through diffusion and capillary action, compensating for the electrolyte consumed during the formation process.

[0074] Step 7: Seal the single cell 100. After formation, the electrolyte injection hole is sealed by laser welding to complete the manufacturing of the single cell 100.

[0075] To verify the technical advantages of this application, a comparative experiment was conducted. Three groups of individual cells 100 were set up in the experiment: the first group consisted of individual cells 100 using the conventional secondary electrolyte injection process; the second group consisted of individual cells 100 with only an increased initial electrolyte injection volume (100% electrolyte injection volume) but without secondary electrolyte injection; and the third group consisted of individual cells 100 using the technology of this application. The experimental conditions were: charge / discharge rate 1C, temperature 25℃, and cutoff voltage 2.0-3.65V.

[0076] Experimental results show that after 2000 cycles, the capacity retention rate of the first group of conventional single-cell batteries 100 is 82%, the capacity retention rate of the second group of single-cell batteries 100 is 78% (due to insufficient electrolyte after formation), while the capacity retention rate of the third group of single-cell batteries 100 using the technology of this application reaches 85%. This indicates that the electrolyte replenishment effect of this application is superior to the secondary electrolyte injection process. Regarding the process cycle, the manufacturing cycle of the first group of conventional single-cell batteries 100 is 36 hours (including initial electrolyte injection, formation, secondary electrolyte injection, and settling), the manufacturing cycle of the second group of single-cell batteries 100 is 32 hours (without secondary electrolyte injection), and the manufacturing cycle of the third group of single-cell batteries 100 using the technology of this application is 32 hours (without secondary electrolyte injection). This indicates that this application shortens the manufacturing cycle by 4 hours and increases production capacity by approximately 12% while maintaining the performance of the single-cell batteries 100. In terms of cost, the first group of conventional processes requires secondary electrolyte injection equipment and secondary sealing equipment, with an equipment investment of approximately 5 million yuan; the third group using the technology of this application does not require these equipment, reducing equipment investment by approximately 2 million yuan, a reduction of 20%. In addition, the technology of this application reduces the labor cost and quality control cost of the secondary injection process, resulting in an overall cost reduction of approximately 8%.

[0077] The embodiments of this application have been described in detail above with reference to the accompanying drawings. However, this application is not limited to the above embodiments. Within the scope of knowledge possessed by those skilled in the art, various changes can be made without departing from the spirit of this application. Furthermore, unless otherwise specified, the embodiments and features described in the embodiments of this application can be combined with each other.

Claims

1. A single cell, characterized by, include: The housing (101) has a receiving cavity (102). The electrode core (103) is disposed within the receiving cavity (102); A reservoir (104) is disposed in the receiving cavity (102). The reservoir (104) has a reservoir space (301) for storing a first electrolyte. The reservoir (104) is configured such that when the temperature inside the receiving cavity (102) rises to a preset temperature, the reservoir (104) ruptures, so that the first electrolyte flows from the reservoir space (301) to the receiving cavity (102).

2. The cell according to claim 1, wherein The single cell (100) also includes a separator (105), which is disposed in the receiving cavity (102) and located between the electrode core (103) and the inner wall of the housing (101). The liquid storage bladder (104) is connected to the side of the separator (105) facing the electrode core (103), and / or the liquid storage bladder (104) is connected to the side of the separator (105) facing the inner wall of the housing (101).

3. The cell according to claim 2, wherein The single cell includes a plurality of the liquid storage sacs (104), at least a portion of the liquid storage sacs (104) having a preset pressure. When the pressure of the liquid storage sacs (104) rises to the preset pressure, the liquid storage sacs (104) rupture to allow the first electrolyte to flow from the liquid storage space (301) to the receiving cavity (102).

4. The cell according to claim 3, wherein The reservoir (104) is connected to the side of the isolation membrane (105) facing the electrode core (103), and when the reservoir (104) is connected to the side of the isolation membrane (105) facing the inner wall of the housing (101); the reservoir (104) includes a first reservoir (501) and a second reservoir (502), the first reservoir (501) is connected to the side of the isolation membrane (105) facing the inner wall of the housing (101), the second reservoir (502) is connected to the side of the isolation membrane (105) facing the electrode core (103), the first reservoir (501) has a first preset pressure, the second reservoir (502) has a second preset pressure, and the first preset pressure is greater than the second preset pressure.

5. The cell according to claim 2, wherein The single battery cell includes multiple liquid storage bladders (104), the separator (105) has a connection surface (801) facing the electrode core (103) or the inner wall of the housing (101), the multiple liquid storage bladders (104) are connected to the connection surface (801), the liquid storage bladders (104) located on the connection surface (801) include a third liquid storage bladder (802) and a fourth liquid storage bladder (803), the third liquid storage bladder (802) and the fourth liquid storage bladder (803) are distributed at intervals along the extension direction of the connection surface (801), the minimum size of the third liquid storage bladder (802) along the extension direction of the connection surface (801) is greater than the maximum size of the fourth liquid storage bladder (803) along the extension direction of the connection surface (801), and / or, the wall thickness of the third liquid storage bladder (802) is less than the wall thickness of the fourth liquid storage bladder (803).

6. The cell according to claim 5, wherein The connecting surface (801) includes a central region (804) and an edge region (805). The normal of the connecting surface (801) lies on a plane parallel to the connecting surface (801). The orthographic projection of the central region (804) covers the center point of the orthographic projection of the pole core (103). The third liquid reservoir (802) is connected to the edge region (805), and the fourth liquid reservoir (803) is connected to the central region (804).

7. The cell according to claim 5, wherein The connecting surface (801) is the side surface of the separator (105) facing the pole core (103).

8. The cell according to claim 2, wherein The single cell (100) includes a plurality of liquid storage bladders (104), the separator (105) has a connection surface (801), the connection surface (801) faces the electrode core (103) or the inner wall of the housing (101), the connection surface (801) includes a central area (804) and an edge area (805), the liquid storage bladder (104) includes a fifth liquid storage bladder (806) and a sixth liquid storage bladder (807), the fifth liquid storage bladder (806) is connected to the central area (804), the sixth liquid storage bladder (807) is connected to the edge area (805), along the normal of the connection surface (801) on a plane parallel to the connection surface (801), the orthographic projection of the central area (804) covers the center point of the orthographic projection of the electrode core (103), the arrangement density of the fifth liquid storage bladder (806) is greater than the arrangement density of the sixth liquid storage bladder (807).

9. The cell according to claim 8, wherein The maximum dimension of the fifth reservoir (806) extending along the connecting surface (801) is smaller than the minimum dimension of the sixth reservoir (807) extending along the connecting surface (801).

10. The cell of claim 1 wherein, The single cell (100) includes a second electrolyte, which is disposed in the receiving cavity (102), and the content of film-forming additives in the first electrolyte is greater than the content of film-forming additives in the second electrolyte.

11. The single-cell battery according to claim 1, characterized in that, The reservoir (104) is made of at least one of ethylene-vinyl acetate copolymer and polyvinylidene fluoride-hexafluoropropylene copolymer.

12. A battery pack, characterized in that, Includes the single cell (100) according to any one of claims 1 to 11.

13. A method for manufacturing a single-cell battery, used to manufacture the single-cell battery (100) according to any one of claims 1 to 11, characterized in that, The manufacturing method includes: The first electrolyte is mixed with the oil phase solution to form emulsion droplets; The emulsion droplets are solidified to solidify the oil phase solution to form the reservoir (104), and the reservoir space (301) stores the first electrolyte.

14. The method for manufacturing a single-cell battery according to claim 13, characterized in that, The manufacturing method includes: Obtain the separator membrane (105), disperse the reservoir (104) in the adhesive, coat the mixture of the reservoir (104) and the adhesive on the surface of the separator membrane (105) and dry it, wrap the separator membrane (105) around the outer peripheral surface of the electrode core (103) and put them together into the receiving cavity (102).