A separator for a rechargeable battery and a rechargeable battery including the separator.
By using a core-shell fiber separator, the problems of insufficient heat resistance and electrolyte wettability of rechargeable lithium battery separators have been solved, thereby improving battery safety and capacity.
Patent Information
- Application Number
- CN202610637997.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-16
- Filing Date
- 2026-05-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing rechargeable lithium-ion battery separators have shortcomings in heat resistance and electrolyte wettability, which limits the improvement of battery safety and capacity.
The membrane adopts a core-shell type fiber membrane, with the core made of polyimide-based materials and the shell made of polysilsesquioxane-based materials. It is manufactured by electrospinning technology, with an average diameter between 30nm and 200nm, ensuring that the membrane has excellent heat resistance and electrolyte wettability.
It improves battery safety and capacity by reducing dry heat shrinkage and heat shrinkage in the electrolyte, enhancing lithium-ion mobility and battery stability, while also improving the mechanical strength of the separator.
Smart Images

Figure CN123121064A_ABST
Abstract
Description
[0001] This application claims priority and benefit to Korean Patent Application No. 10-2025-0064095, filed on May 16, 2025, with the Korean Intellectual Property Office, the entire disclosure of which is incorporated herein by reference. Technical Field
[0002] This disclosure relates to a separator for a rechargeable battery and a rechargeable battery including the separator. Background Technology
[0003] With the increasing prevalence of battery-powered electronic devices such as mobile phones, laptops, and electric vehicles, the demand for rechargeable batteries with high energy density and high capacity is growing. Therefore, improving the performance of rechargeable lithium batteries can be beneficial.
[0004] Rechargeable lithium batteries typically include a positive electrode and a negative electrode containing active materials capable of inserting and deintercalating lithium ions, and generate electrical energy through oxidation and reduction reactions when lithium ions are inserted into the positive electrode and deintercalated from the negative electrode, and when they are inserted into the negative electrode and deintercalated from the positive electrode. Summary of the Invention
[0005] One example embodiment includes a separator for a rechargeable battery having desired or improved heat resistance and desired or improved electrolyte wettability.
[0006] Another example embodiment includes a separator for rechargeable batteries comprising core-shell type fibers that can be manufactured without using a core-shell nozzle.
[0007] Another example embodiment includes a separator for a rechargeable battery that does not include a porous substrate.
[0008] Another example embodiment includes a rechargeable battery comprising the separator described above for a rechargeable battery.
[0009] According to one aspect of this disclosure, a separator for a rechargeable battery is provided.
[0010] The separator for a rechargeable battery includes a first layer comprising core-shell fibers having a core and a shell surrounding the core, the core comprising a polyimide material and the shell comprising a polysilsesquioxane material, and the core-shell fibers having an average diameter of about 30 nm or larger and about 200 nm or smaller.
[0011] According to another aspect of this disclosure, a rechargeable battery is provided.
[0012] A rechargeable battery includes a positive electrode, a negative electrode, and a separator for the rechargeable battery located between the positive and negative electrodes. Attached Figure Description
[0013] The above and other objects, features, and advantages of this disclosure will become more apparent to those skilled in the art by referring to the accompanying drawings, which describe exemplary embodiments of the present disclosure in detail. Figure 1 A cross-section of a core-shell fiber according to an example embodiment is shown; Figure 2 A cross-section of a core-shell fiber according to another example embodiment is shown; Figures 3 to 7 A separator for a rechargeable battery according to an example embodiment is shown; Figures 8 to 11 A rechargeable battery according to an example embodiment is schematically shown; and Figure 12 An electrode for a rechargeable battery according to an example embodiment is shown. Detailed Implementation
[0014] Example embodiments of this disclosure are described in detail below. However, these are presented by way of example, and this disclosure is not limited thereto, and is limited only by the scope of the claims described below.
[0015] Unless otherwise stated herein, when a component such as a layer, film, region, or plate is described as being “on” another component, this includes not only the case where the component is “directly on” the other component, but also the case where another component is present in between.
[0016] Unless otherwise stated, a singular expression may also include a plural expression. Additionally, unless otherwise stated, “A or B” may mean “including A, including B, or including both A and B”.
[0017] In the specification, “the combination of them” can mean a mixture of components, a laminate, a complex, a copolymer, an alloy, a blend, and a reaction product.
[0018] In this specification, "particle size (D50)" refers to the average particle size representing the size of particles that constitute 50% of the cumulative volume in a particle size distribution. Particle size distribution can be measured using methods well-known to those skilled in the art. For example, it can be measured using a particle size analyzer or by transmission electron microscopy (TEM) or scanning electron microscopy (SEM). Alternatively, particle size can be measured using a measuring device that utilizes dynamic light scattering. The number of particles in each particle size range can be counted through data analysis, and the D50 value can be calculated using the methods described above. Optionally, the number of particles can be measured using laser diffraction. When measured by laser diffraction, for example, the particles to be measured can be dispersed in a dispersion medium. By introducing the dispersion medium into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), irradiating it with ultrasound at approximately 28 kHz at a power of 60 W, and using this measuring device, the D50 can be calculated based on 50% of the particle size distribution.
[0019] If the above particles are spherical, the above dimensions may refer to the diameter.
[0020] In this specification, "(meth)acryloyl" refers to acryloyl and / or methacryloyl.
[0021] In chemical formulas, the symbol " "" indicates a portion connected to the same or different atoms, groups, or structural units. Unless otherwise stated in the chemical formula shown herein, it may be assumed that hydrogen bonds are present in the structure of the chemical formula.
[0022] When a numerical range is specified in this specification, “X to Y” means “X or greater and Y or less (greater than or equal to X and less than or equal to Y)”.
[0023] When the terms “about” or “substantially” are used in conjunction with numerical values in this specification, it means that the relevant numerical value includes a tolerance of ±10% around the stated value. When a range is specified, the range includes all values in increments such as 0.1%.
[0024] The following describes in detail the separator for a rechargeable battery and the rechargeable battery including the separator.
[0025] In the following description, only rechargeable lithium batteries are described. However, in addition to rechargeable lithium batteries, this disclosure can also be applied to rechargeable batteries with different metal ions.
[0026] Separator for rechargeable batteries The separator for rechargeable batteries according to the example embodiments (hereinafter also referred to as "separator") has desired or improved heat resistance, thus reducing or preventing the occurrence of short circuits and thereby enhancing battery safety.
[0027] The separator may have a dry heat shrinkage rate of about 1% or less, for example, in the range of about 0% to about 1%, and the heat shrinkage rate in the electrolyte may be about 1% or less, for example, in the range of about 0% to about 1%. Within these ranges, the heat resistance of the separator is desirable or improved, thereby increasing battery safety.
[0028] The separator has desired or improved electrolyte wettability, which results in high lithium-ion mobility and fast electrolyte injection rate, thereby improving battery capacity. Here, "electrolyte wettability" refers to the degree to which the electrolyte is absorbed into the separator.
[0029] The diaphragm can have a diameter of approximately 3.0 cm. 2 Approximately 6.0cm 2 The electrolyte wettability is within a certain range. Within this range, the battery capacity can be improved.
[0030] The separator has improved permeability, thus increasing lithium-ion mobility, ensuring rapid electrolyte injection, and enhancing battery stability. Here, "permeability" refers to the time it takes for 100 cc of air to pass through the separator. The separator can have a permeability of approximately 350 seconds / 100 cc or less, for example, in the range of approximately 80 seconds / 100 cc to approximately 120 seconds / 100 cc.
[0031] The diaphragm can have a strength of approximately 500 kgf / cm². 2 Or even higher, for example, at approximately 500 kgf / cm². 2 Approximately 3000 kgf / cm 2 or 2800 kgf / cm 2 Up to 3000 kgf / cm 2 Within the specified range of strength, the battery's safety can be increased due to its resistance to impacts or foreign objects.
[0032] The diaphragm can have a thickness of about 10 μm or less, for example, in the range of about 6 μm to about 10 μm.
[0033] First layer The membrane includes a first layer, which is or includes a fiber layer. The fiber layer can help improve the electrolyte wettability of the membrane.
[0034] In this specification, "fiber layer" can mean a layer formed by fibers that form a network, such as a mesh. Here, fibers can include one or more of nanofibers and microfibers, and may, for example, be or include nanofibers.
[0035] Although there are no particular limitations, fibers can be manufactured by electrospinning. Electrospinning can be performed using conventional methods known to those skilled in the art. The electrospinning method is described in more detail below.
[0036] In one example embodiment, the fibers may have an aspect ratio of about 5 or greater, for example, in the range of about 5 to about 10,000. Within this range, fiber networks can be readily formed and thus can be used in diaphragms. Here, the “aspect ratio” of the fibers refers to the ratio of the average length of the fibers to their average diameter.
[0037] The first layer comprises core-shell type fibers having a core and a shell surrounding the core. In one example embodiment, the first layer may be or comprise a fiber layer made of or comprising core-shell type fibers.
[0038] Core-shell fibers can include different materials in each of the core and shell, and have high strength due to the core-shell structure, thereby increasing the mechanical strength of the first layer. In one example embodiment, core-shell fibers can be included in the first layer in an amount of about 95 wt% or greater, for example, in the range of about 95 wt% to about 100 wt%, or 100 wt%.
[0039] The cross-section of core-shell fibers can be circular, elliptical, or amorphous, but is not limited to these.
[0040] Figure 1 and Figure 2 Each shows a cross-section of a core-shell fiber.
[0041] Reference Figure 1 In core-shell fibers, the diameter of core B can be significantly larger than the thickness of shell A. Optionally, refer to... Figure 2 In core-shell fibers, the diameter of the core (B) can be significantly smaller than the thickness of the shell (A). For example, as... Figure 1 As shown, the diameter of core B is significantly larger than the thickness of shell A, which allows for the achievement of desired or improved heat resistance and better control of air permeability through compression.
[0042] The core comprises a polyimide resin (hereinafter also referred to as "polyimide material"), and the shell comprises a polysilsesquioxane resin (hereinafter also referred to as "polysilsesquioxane material").
[0043] Even without using a core-shell nozzle, a core-shell combination of polyimide and polysilsesquioxane resins can be manufactured by electrospinning fibers. For example, when electrospinning a mixture of polyimide and polysilsesquioxane resins, core-shell fibers can be formed independently due to the viscosity difference between the polyimide and polysilsesquioxane resins, but this disclosure is not limited thereto. Here, "core-shell nozzle" can mean having a core nozzle and a shell nozzle having a predetermined or desired thickness surrounding the core nozzle.
[0044] Core-shell fiber structures incorporate polyimide resins in the core and polysilsesquioxane resins in the shell to reduce the dry heat shrinkage of the separator and the thermal shrinkage in the electrolyte, thereby improving the separator's heat resistance and increasing electrolyte wettability, thus improving battery capacity. Polyimide resins are generally known to have desired or improved heat resistance. However, by incorporating polysilsesquioxane resins into the shell of the core-shell structure, heat resistance can be further increased, and electrolyte wettability can also be improved to enhance battery capacity.
[0045] In one example embodiment, a polyimide material may be included in the core at about 95 wt% or more, for example, in the range of about 95 wt% to about 100 wt%, or in an amount of 100 wt%. In one example embodiment, a polysilsesquioxane material may be included in the shell at about 95 wt% or more, for example, in the range of about 95 wt% to about 100 wt%, or in an amount of 100 wt%. Within these ranges, the aforementioned membrane effect can be readily achieved.
[0046] Core-shell fibers have an average diameter of approximately 30 nm or larger and approximately 200 nm or smaller. When the average fiber diameter is less than approximately 30 nm, the membrane strength may be low, and the effect on improving heat resistance and electrolyte wettability may be low or minimal. When the average fiber diameter exceeds approximately 200 nm, the fiber diameter may be too large, resulting in smaller pores between the fibers, which may weaken the physical properties of the membrane used in rechargeable lithium batteries. For example, core-shell fibers can have an average diameter of approximately 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 85 nm, 90 nm, 95 nm, 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 145 nm, 150 nm, 155 nm, 160 nm, 165 nm, 170 nm, 175 nm, 180 nm, 185 nm, 190 nm, 195 nm, and 200 nm.
[0047] For example, the average diameter of the fiber can be about 100 nm or larger and about 120 nm or smaller, 130 nm or larger and 150 nm or smaller, or 150 nm or larger and 200 nm or smaller. Within these ranges, heat resistance and electrolyte wettability are significantly improved, and the fiber can be manufactured under relatively easy conditions.
[0048] In this specification, the “average diameter” of a fiber can be the average of the diameters of the fibers. For example, the average diameter can be obtained by drawing approximately 10 to approximately 30 fibers from a layer, or by selecting approximately 10 to approximately 30 cross-sections from the fiber profile, measuring each diameter using a microscope or similar tool, and calculating the average of the resulting diameters. The “diameter” of a fiber can refer to the normal diameter when the fiber profile is circular, and the longest diameter, which is the maximum value among the diameters measured in the cross-section, when the fiber profile is not circular but elliptical or amorphous.
[0049] The average diameter of core-shell fibers can be controlled by controlling the ratio of polyimide resin to polysilsesquioxane resin in the electrospinning solution used to manufacture core-shell fibers, or by controlling the voltage and / or needle size during electrospinning.
[0050] In one example embodiment, the core in the core-shell fiber may have a diameter of about 120 nm or larger and about 140 nm or smaller, such as 125 nm or larger and 135 nm or smaller, and the shell may have a thickness of about 10 nm or larger and about 30 nm or smaller, such as 15 nm or larger and 25 nm or smaller, such as 10 nm, 15 nm, 20 nm, 25 nm, 30 nm.
[0051] In core-shell fibers, the core content can range from approximately 10 wt% to approximately 95 wt% (e.g., 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%, 50 wt%, 51 wt%, 52 wt%). %, 53wt%, 54wt%, 55wt%, 56wt%, 57wt%, 58wt%, 59wt%, 60wt%, 61wt%, 62wt%, 63wt%, 64wt%, 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt%, 71wt%, 72wt%, 73wt%, 74wt%, 75wt%, 76wt%, 77wt%, 78wt%, 79wt%, 80wt%, 81wt%, 82wt%, 83wt%, 84wt%, 85wt%, 86wt%, 87wt%, 88wt%, 89wt%, 90wt%, 91wt%, 92wt%, 93wt%, 94wt%, 95wt%), within the range of 10wt% to 90wt% or 60wt% to 90wt%,The shell content can range from approximately 5 wt% to approximately 90 wt% (e.g., 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt%, 15 wt%, 16 wt%, 17 wt%, 18 wt%, 19 wt%, 20 wt%, 21 wt%, 22 wt%, 23 wt%, 24 wt%, 25 wt%, 26 wt%, 27 wt%, 28 wt%, 29 wt%, 30 wt%, 31 wt%, 32 wt%, 33 wt%, 34 wt%, 35 wt%, 36 wt%, 37 wt%, 38 wt%, 39 wt%, 40 wt%, 41 wt%, 42 wt%, 43 wt%, 44 wt%, 45 wt%, 46 wt%, 47 wt%, 48 wt%, 49 wt%). The concentrations can range from 50 wt%, 51 wt%, 52 wt%, 53 wt%, 54 wt%, 55 wt%, 56 wt%, 57 wt%, 58 wt%, 59 wt%, 60 wt%, 61 wt%, 62 wt%, 63 wt%, 64 wt%, 65 wt%, 66 wt%, 67 wt%, 68 wt%, 69 wt%, 70 wt%, 71 wt%, 72 wt%, 73 wt%, 74 wt%, 75 wt%, 76 wt%, 77 wt%, 78 wt%, 79 wt%, 80 wt%, 81 wt%, 82 wt%, 83 wt%, 84 wt%, 85 wt%, 86 wt%, 87 wt%, 88 wt%, 89 wt%, to 90 wt%), for example, from 5 wt% to 50 wt%, from 10 wt% to 50 wt%, or from 10 wt% to 20 wt%. Within these ranges, a diaphragm effect can be easily achieved.
[0052] Polyimide materials may include oligomers, polymers, copolymers, or combinations thereof having polyimide units. Polysilsesquioxane materials may include oligomers, polymers, copolymers, or combinations thereof having polysilsesquioxane units. This is described in detail below.
[0053] Polyimide materials Polyimide materials can help increase the heat resistance of the diaphragm. Furthermore, polyimide materials, when used in conjunction with a shell including polysilsesquioxane materials, can help improve the electrolyte wettability of the diaphragm.
[0054] Polyimide materials may include repeating units represented by the following chemical formula 1: Chemical Formula 1: .
[0055] In chemical formula 1, Indicates the connection point of an element. R 1 It may include or contain tetravalent organic groups, and R 2 It is or includes a divalent aliphatic organic group, a divalent alicyclic organic group, a divalent aromatic organic group, or a combination thereof having a total of about 3 carbon atoms to about 30 carbon atoms.
[0056] In one example embodiment, R in Formula 1 1 It may be or include at least one of the following moiety (or “group”) represented by the following chemical formulas:
[0057]
[0058]
[0059]
[0060] .
[0061] here, Indicates the connection point of an element.
[0062] For example, R in chemical formula 1 1 It may be or include a portion represented by one or more of the following chemical formulas 1-1 and 1-2.
[0063] Chemical formula 1-1: ; Chemical formulas 1-2: .
[0064] In chemical formula 1, R 2 It may be or include alkylene groups having about 3 carbon atoms to about 30 carbon atoms, cycloalkylene groups having about 3 carbon atoms to about 30 carbon atoms, arylene groups having about 6 carbon atoms to about 30 carbon atoms, or combinations thereof.
[0065] Optionally, R in chemical formula 1 2 It may be or include alkylene groups having about 3 carbon atoms to about 30 carbon atoms, cycloalkylene groups having about 3 carbon atoms to about 30 carbon atoms, arylene groups having about 6 carbon atoms to about 30 carbon atoms, or combinations thereof, and may each have a linking group such as or include at least one of -O-, -SO2-, -CO-, -CH2-, -C(CH3)2-, -OSi(CH3)2-, -C2H4O-, and -S-.
[0066] For example, R in chemical formula 1 2 It may be or include an arylene having about 6 carbon atoms to about 10 carbon atoms, or a combination thereof having a linking group such as or including at least one of -O-, -SO2-, -CO-, -CH2-, -C(CH3)2-, -OSi(CH3)2-, -C2H4O-, and -S-.
[0067] In one example embodiment, the polyimide material may include one or more units represented by one or more of the following chemical formulas 1-3 (Chemical Formula 1-3-1) and 1-4 (Chemical Formula 1-4-1). These materials can significantly improve the performance of the aforementioned diaphragm.
[0068] Chemical formulas 1-3: ; Chemical formula 1-3-1: .
[0069] Chemical formulas 1-4: ; Chemical formula 1-4-1: .
[0070] In the above chemical formulas 1-3 and 1-4, This represents the bonding sites of an element, and n is the number of moles of the unit in the material.
[0071] n can be from 1 to 1,000,000.
[0072] In one example embodiment, polyimide materials can be prepared by heat treatment of polyamic acid, which is prepared by polymerizing one or more dianhydrides represented by chemical formulas 1-5 to 1-13 with one or more diamines represented by chemical formulas 1-14 to 1-26. Here, the heat treatment can be performed during the process of manufacturing fibers or membranes. The heat treatment can be or includes an imidization reaction.
[0073] Chemical formulas 1-5: .
[0074] Chemical formulas 1-6: .
[0075] Chemical formulas 1-7: .
[0076] Chemical formulas 1-8: .
[0077] Chemical formulas 1-9: .
[0078] Chemical formulas 1-10: .
[0079] Chemical formula 1-11: .
[0080] Chemical formulas 1-12: .
[0081] Chemical formula 1-13: .
[0082] Chemical formulas 1-14: .
[0083] Chemical formulas 1-15: .
[0084] Chemical formulas 1-16: .
[0085] Chemical formula 1-17: .
[0086] Chemical formulas 1-18: .
[0087] Chemical formula 1-19: .
[0088] Chemical formulas 1-20: .
[0089] Chemical formula 1-21: .
[0090] Chemical formula 1-22: .
[0091] Chemical formula 1-23: .
[0092] Chemical formula 1-24: .
[0093] Chemical formula 1-25: .
[0094] Chemical formula 1-26: .
[0095] In one example embodiment, the polyimide material may have a weight-average molecular weight in the range of about 100,000 g / mol to about 300,000 g / mol, for example, from 200,000 g / mol to 250,000 g / mol. Within this range, the viscosity of the polyimide material can be easily controlled. In this specification, "weight-average molecular weight" can be obtained, for example, as a polystyrene equivalent using gel permeation chromatography.
[0096] In one example embodiment, the polyimide material may further include functional groups capable of thermal and / or photocrosslinking. Crosslinkable functional groups may include those described in the polysilsesquioxane materials described below. These crosslinkable functional groups can further improve the heat resistance, strength, and electrolyte wettability of the separator by enabling the polyimide material to crosslink with the polysilsesquioxane materials described below during the separator manufacturing process.
[0097] Polyimide materials can be prepared using conventional methods known to those skilled in the art.
[0098] Polysilsesquioxane materials Polysilsesquioxane materials can be used in conjunction with polyimide materials to facilitate the fabrication of core-shell fibers without the need for core-shell nozzles. Furthermore, polysilsesquioxane materials, together with a core comprising polyimide materials, can help improve the electrolyte wettability of the membrane.
[0099] Polysilsesquioxane materials can be random, trapezoidal, cage-like, or partially cage-like.
[0100] In one example embodiment, the polysilsesquioxane material may be or includes a non-crosslinkable material that is not cured by heat and / or light.
[0101] In another example embodiment, the polysilsesquioxane material may be or includes a crosslinkable material that is cured by heat and / or light. The crosslinkable material can be cured by heat and / or light crosslinking during the membrane manufacturing process without requiring a separate crosslinking process. Furthermore, the crosslinkable material can be crosslinked with a polyimide material during the membrane manufacturing process to further increase the membrane's strength.
[0102] Polysilsesquioxane materials can have units represented by the following chemical formula 2: Chemical formula 2: [RSiO 2 / 3 ] n .
[0103] In chemical formula 2, R is hydrogen, hydroxyl, an alkyl group having about 1 carbon atom to about 20 carbon atoms, an alkenyl group having about 2 carbon atoms to about 20 carbon atoms, an alkynyl group having about 2 carbon atoms to about 20 carbon atoms, a cycloalkyl group having about 3 carbon atoms to about 20 carbon atoms, an aryl group having about 6 carbon atoms to about 20 carbon atoms, an aralkyl group having about 7 carbon atoms to about 20 carbon atoms, a crosslinkable functional group, or a combination thereof. n is the number of moles in the unit.
[0104] n can be from 1 to 1,000,000.
[0105] In polysilsesquioxane materials, the R values in the units represented by chemical formula 2 can be the same or different.
[0106] In Formula 2, the crosslinkable functional group is or includes a functional group that can be crosslinked by heat and / or light, and may be or include at least one of (meth)acryloyl, (meth)acryloyloxyalkyl, epoxypropoxy, epoxypropoxyalkyl or combinations thereof.
[0107] In one example embodiment, the crosslinkable functional group may be or include one or more portions represented by one or more of the following chemical formulas 2-1 and 2-2: Chemical formula 2-1: .
[0108] Chemical formula 2-2: .
[0109] In chemical formulas 2-1 and 2-2, R 8 It is hydrogen or methyl, and R 7 R 9 and R 10 Each is independently an alkylene group having about 1 carbon atom to about 20 carbon atoms.
[0110] In one example embodiment, the polysilsesquioxane material may include units represented by the following chemical formulas 2-3: Chemical formula 2-3: .
[0111] In chemical formula 2-3, R 3R 4 R 5 and R 6 Each of the following is independently hydrogen, hydroxyl, alkyl having about 1 carbon atom to about 20 carbon atoms, alkenyl having about 2 carbon atoms to about 20 carbon atoms, alkynyl having about 2 carbon atoms to about 20 carbon atoms, cycloalkyl having about 3 carbon atoms to about 20 carbon atoms, aryl having about 6 carbon atoms to about 20 carbon atoms, aralkyl having about 7 carbon atoms to about 20 carbon atoms, crosslinkable functional groups, or combinations thereof. n is the number of moles in the unit.
[0112] n can be from 1 to 1,000,000.
[0113] In chemical formulas 2-3, the crosslinkable functional groups are the same as those defined in chemical formula 2.
[0114] For example, in chemical formula 2-3, R 3 R 4 R 5 and R 6 Each may be, independently or include at least one of hydroxyl, aryl having 6 to 20 carbon atoms, aralkyl having about 7 to about 20 carbon atoms, crosslinkable functional groups, or combinations thereof.
[0115] For example, polysilsesquioxane materials may include units represented by the following chemical formulas 2-4.
[0116] Chemical formula 2-4: .
[0117] In chemical formula 2-4, R 31 R 41 R 51 and R 61 Each of the following is independently at least one of hydrogen, hydroxyl, alkyl having about 1 carbon atom to about 20 carbon atoms, alkenyl having about 2 carbon atoms to about 20 carbon atoms, alkynyl having about 2 carbon atoms to about 20 carbon atoms, cycloalkyl having about 3 carbon atoms to about 20 carbon atoms, aryl having about 6 carbon atoms to about 20 carbon atoms, aralkyl having about 7 carbon atoms to about 20 carbon atoms, crosslinkable functional group, or combination thereof. R 31 R 41 R 51 and R 61 At least one of them is a crosslinkable functional group, and n is the number of moles in the unit.
[0118] n can be from 1 to 1,000,000.
[0119] In Formula 2-4, the crosslinkable functional groups may be the same as those defined in Formula 2. In one example embodiment, the crosslinkable functional groups in Formula 2-4 may be one or more portions represented by one or more of Formula 2-1 and Formula 2-2.
[0120] In polysilsesquioxane materials, in chemical formula 2-4, R 31 R 41 R 51 and R 61 Each is independently an aryl (e.g., phenyl) group having about 6 to about 20 carbon atoms, a crosslinkable functional group, or a combination thereof, and R 31 R 41 R 51 and R 61 At least one of them may be or includes a crosslinkable functional group.
[0121] For example, the crosslinkable functional group can be a part represented by one or more of chemical formulas 2-5 and 2-6: Chemical formula 2-5: .
[0122] Chemical formula 2-6: .
[0123] In the above chemical formulas 2-5 and 2-6, Indicates the connection point of an element.
[0124] Polysilsesquioxane materials can have a weight-average molecular weight in the range of about 10,000 g / mol to about 30,000 g / mol, for example, 15,000 g / mol to 20,000 g / mol. Within this range, the viscosity of polysilsesquioxane materials can be easily controlled.
[0125] The first layer may have a thickness of about 5 μm or greater, for example, in the range of about 6 μm to about 10 μm. Within this range, the first layer may enhance strength by being included in the diaphragm.
[0126] The first layer can be manufactured by electrospinning an electrospinning solution containing polyimide and polysilsesquioxane materials onto a substrate or release film. The electrospinning method is described in more detail below. After electrospinning, solvent drying and removal of the substrate or release film can be performed.
[0127] In addition to polyimide and polysilsesquioxane materials, the fiber may also include one or more of polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyamide-imide (PAI), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), polyvinyl alcohol (PVA), aromatic polyamide polymers, and polyurethane resins. This material may be incorporated into one or more of the fiber's core and shell.
[0128] In one example embodiment, the fiber may also comprise a resin having a low melting point relative to the imidization reaction temperature. The resin has a melting point of about 250°C or lower and may be, for example, polyvinylidene fluoride.
[0129] In one example embodiment, the fibers may also include polyurethane resin in one or more of the core and shell.
[0130] In one example embodiment, the fiber may also include an aromatic polyamide resin in one or more of the core and shell.
[0131] The fiber may also include additives such as phosphorus-based flame retardants. This can further enhance the flame retardancy of the fiber and the diaphragm that includes the fiber. Phosphorus-based flame retardants may include one or more of ammonium dihydrogen phosphate and ammonium polyphosphate.
[0132] Diversity of membrane structures The diaphragm can be a single layer or multiple layers.
[0133] In one example embodiment, the diaphragm may consist of only the first layer. For example, the diaphragm may be a single-layer diaphragm consisting of only the first layer, or it may be a multilayer diaphragm in which the first layer is laminated multiple times.
[0134] Figure 3 The laminate is shown to have a first layer of 200 membrane.
[0135] Figure 4 This illustrates a membrane laminated with three first layers of 200. (Example) Figure 4 As shown, the diaphragm comprises three first layers 200. Although Figure 4 Not shown in the diagram, but the electrospinning direction of each first layer 200 can be the same or different. Although Figure 4 Not shown, but each first layer 200 can be laminated so that each first layer 200 does not separate due to compression, etc.
[0136] In another example embodiment, the membrane may also include a heterogeneous layer in addition to the first layer. For convenience, the heterogeneous layer is referred to as the second layer.
[0137] The second layer may be or include fibrous layers, non-fibrous layers, or combinations thereof as defined above.
[0138] When the second layer is a fibrous layer: The diaphragm may include one or more first layers and one or more second layers.
[0139] The second layer can also be a fiber layer as defined above.
[0140] The second layer may include one or more types of core-shell fibers and non-core-shell fibers.
[0141] The fibers in the second layer can be manufactured by electrospinning, and there are no particular restrictions, as long as the fibers do not affect the performance of the membrane.
[0142] The fibers in the second layer may include one or more of the following: polyacrylonitrile, polyaniline, polypyrrole, polyrhodanine, melamine, polyurea, polyvinyl chloride, polyvinyl alcohol, polyethylene oxide, polymethyl methacrylate, polyacrylic acid, polylactic acid, polyimide, polyamide-imide, polyarylamide, polybenzylimidazole, polypropylene, resorcinol-formaldehyde resin, melamine-formaldehyde resin, asphalt, sucrose, glucose, cellulose, and polyvinylidene fluoride. For example, the fibers in the second layer may be polyimide. For example, the fibers in the second layer may be the same as or different from the polyimide material in the first layer.
[0143] In one example embodiment, the fibers of the second layer may be polyimide or a mixture comprising about 50 wt% or more of polyimide. This second layer can increase the heat resistance of the separator and, when combined with the first layer, can help reduce battery resistance, enhance adhesion, lower turn-off temperature, and increase processability.
[0144] In another example embodiment, the fibers of the second layer may be polyvinylidene fluoride (PVDF) or a mixture comprising about 50 wt% or more PVDF. This second layer can enhance the flexibility of the membrane and further enhance its adhesiveness.
[0145] In another example embodiment, the fibers of the second layer may be or include a mixture comprising about 50 wt% polyimide and polyvinylidene fluoride. This second layer can enhance the flexibility of the diaphragm, further enhance the adhesion of the diaphragm, and improve the processability of the diaphragm by counteracting the brittleness of the polyimide.
[0146] The fibers in the second layer can have an average diameter of about 30 nm or larger and about 200 nm or smaller. Within this range, the diaphragm can have desired or improved permeability without affecting electrolyte wettability. For example, the average diameter of the fibers can be about 100 nm or larger and about 120 nm or smaller, 130 nm or larger and 150 nm or smaller, or 150 nm or larger and 200 nm or smaller. Within this range, heat resistance and electrolyte wettability are significantly improved, and the fibers can be manufactured under relatively easy conditions.
[0147] In one example embodiment, the separator may not include a porous substrate. Porous substrates are manufactured by stretching or similar processes, and when the battery is exposed to heat, the porous substrate may undergo thermal shrinkage and melting at high temperatures. This could cause the overhangs in the separator to shrink, leading to a short circuit. Therefore, the separator has a thin thickness and is not susceptible to short circuit problems caused by thermal shrinkage and melting at high temperatures due to the porous substrate, thus ensuring high battery safety.
[0148] Here, "porous substrate" can refer to the substrate used in the manufacture of the diaphragm, such as a porous polyolefin substrate including a polyethylene substrate or a polypropylene substrate.
[0149] When the second layer is a non-fibrous layer: The diaphragm may include one or more first layers and one or more second layers.
[0150] As is known in the art, the second layer may be or include a coating, which includes a combination of an adhesive (containing a heat-resistant adhesive or a sticky adhesive) and / or a filler.
[0151] Figures 5 to 7 A diaphragm according to an example embodiment of the present disclosure is shown.
[0152] Reference Figure 5 The diaphragm may be or include two diaphragms comprising a first layer 200 and a second layer 300. (Refer to...) Figure 6 The diaphragm can be or includes a three-layer diaphragm comprising a first layer 200, a second layer 300, and a third layer 200. (Refer to...) Figure 7 The diaphragm can be or include a three-layer diaphragm comprising a second layer 300, a first layer 200, and a second layer 300.
[0153] electrospinning Both the first and second layers, which are fiber layers, can be manufactured, for example, by electrospinning. Electrospinning can be performed using conventional methods known to those skilled in the art.
[0154] Manufacturing of the first layer: The electrospinning solution used to manufacture the first layer may include a mixture of polyimide materials and polysilsesquioxane materials. Here, the polyimide material may be a separately synthesized polyimide material or a polyamic acid material.
[0155] In the above mixture, by controlling the weight-average molecular weight of the polyimide and polysilsesquioxane materials, as well as the weight ratio between these materials in the mixture, core-shell fibers can be manufactured without a core-shell nozzle. The weight ratio can be adjusted according to the diameter of the core and the thickness of the shell in the core-shell fiber.
[0156] The electrospinning solution may also include a solvent to promote the dispersion and dissolution of polyimide and polysilsesquioxane materials. The solvent may include, but is not limited to, at least one of methylformamide, dimethylacetamide, dimethyl sulfoxide, and methylpyrrolidone. To further enhance dispersion and dissolution, stirring and / or heating may be applied.
[0157] Electrospinning can be carried out, for example, in a space with an internal temperature range of about 25°C or higher, such as from about 25°C to about 60°C. Within this range, the solvent in the electrospinning solution evaporates to a high degree, resulting in no residual solvent and thus reducing the impact of the solvent on the battery.
[0158] Electrospinning can be performed by the following steps: positioning a nozzle assembly consisting of tips with needle sizes ranging from about 23G (gauge) to about 30G and a collecting roller at a predetermined or desired interval; adding an electrospinning solution to the tips; positioning the substrate on the collecting roller; and then applying a voltage ranging from about 35kV to about 90kV to the tips. The gap between the nozzle assembly and the collecting roller can be in the range of about 10cm to about 20cm. When the needle size of the tips is in the range of about 25G to about 30G, the needle size of the tips can be suitable because the first fiber layer can be formed into the desired shape.
[0159] According to the electrospinning process, an electrospinning solution is spun and stretched into a fiber shape, allowing a layer comprising nanofibers to be formed on a substrate. For example, the electrospinning solution is suspended as droplets at a tip due to surface tension, and when a voltage is applied, charges accumulate on the surface of the solution, generating repulsive forces between the charges. When the repulsive forces between the charges exceed a critical voltage that controls the surface tension of the solution, a conical Taylor cone is formed, and a jet of the electrospinning solution is ejected from the cone tip. This jet is highly stretched to form nanofibers, which then collect on the substrate to form a fiber layer.
[0160] The air pressure at the nozzle can be approximately 1 MPa or higher. Within this range, the solvent evaporates to a high degree, thus reducing the impact of residual solvent on the battery.
[0161] Proper control of the tip air can reduce or minimize interference between tips and allow electrospinning to occur uniformly. The tip air can be regulated by flowing compressed air at a pressure ranging from about 0.1 MPa to about 0.3 MPa.
[0162] The speed of the collecting roller can be adjusted so that the fiber layer can be formed to an appropriate thickness, and the speed of the collecting roller can be, for example, in the range of about 1 m / min to about 3 m / min. Furthermore, the flow rate of the electrospinning solution discharged from the tip can be adjusted to be discharged at a rate in the range of about 20 μL / min to about 200 μL / min. In one example embodiment, after the electrospinning process, a drying process (heat treatment) can be performed at a temperature in the range of about 50°C to about 120°C.
[0163] Manufacturing of the second layer: When the second layer is a fiber layer, the second layer can be manufactured by electrospinning an electrospinning solution containing fibers contained in the second layer.
[0164] Electrospinning can be carried out using the methods described above.
[0165] Diaphragm manufacturing: The diaphragm can be manufactured by making a fiber layer and then pressing the fiber layer together.
[0166] According to one example embodiment, the diaphragm can be manufactured by separately fabricating multiple fiber layers, sequentially laminating the fabricated multiple fiber layers, and then compressing the layers.
[0167] According to another example embodiment, the diaphragm can be manufactured by injecting an electrospinning solution containing a copolymer into sequentially positioned nozzles, and then sequentially spinning and simultaneously or concurrently compressing the copolymer.
[0168] There are no particular restrictions on compression, but it can be achieved by using rollers or similar devices.
[0169] rechargeable batteries According to one example embodiment, a rechargeable battery includes a separator, a positive electrode, and a negative electrode for the rechargeable battery.
[0170] The separator used in rechargeable batteries is described above. The separator for rechargeable batteries can be located between the positive and negative electrodes.
[0171] positive electrode The positive electrode for a rechargeable battery may include a current collector and a layer of positive electrode active material on the current collector. The positive electrode active material layer may include positive electrode active material, and may also include a binder and / or a conductive material.
[0172] For example, the positive electrode may also include additives that can form a sacrificial positive electrode.
[0173] Positive electrode active material The positive electrode active material may include compounds capable of intercalating and deintercalating lithium (lithium intercalation compounds). For example, at least one of the composite oxides of lithium and metals such as or including at least one of cobalt, manganese, nickel and combinations thereof may be used.
[0174] The composite oxide can be or includes lithium transition metal composite oxides. Examples of composite oxides may include at least one of lithium nickel oxides, lithium cobalt oxides, lithium manganese oxides, lithium iron phosphate compounds, cobalt-free lithium nickel manganese oxides, or combinations thereof.
[0175] As an example, a compound represented by any of the following chemical formulas can be used. Li a A 1-b X b O 2-c D c (0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); Li a Mn 2-b X b O 4-c D c (0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, and 0<α<2); Li a Ni 1-b- c Mn b X c O 2-α D α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, and 0<α<2); Li a Ni b Co c L 1 d G eO2 (0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0≤e≤0.1); Li a NiG b O2 (0.90≤a≤1.8, and 0.001≤b≤0.1); Li a CoG b O2 (0.90≤a≤1.8, and 0.001≤b≤0.1); Li a Mn 1-b G b O2 (0.90≤a≤1.8, and 0.001≤b≤0.1); Li a Mn2G b O4 (0.90≤a≤1.8, and 0.001≤b≤0.1); Li a Mn 1-g G g PO4 (0.90≤a≤1.8, and 0≤g≤0.5); Li (3-f) Fe2(PO4)3 (0≤f≤2); Li a FePO4 (0.90≤a≤1.8).
[0176] In the above chemical formulas, A is or includes at least one of Ni, Co, Mn, or combinations thereof; X is or includes at least one of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements, or combinations thereof; D is or includes at least one of O, F, S, P, or combinations thereof; G is or includes at least one of Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or combinations thereof; and L 1 It is or includes at least one of Mn, Al, or combinations thereof.
[0177] The positive electrode active material can be, or includes, for example, a high-nickel positive electrode active material, based on 100 mol% of metals other than lithium in a lithium transition metal complex oxide. The high-nickel positive electrode active material has a nickel content greater than or equal to about 80 mol%, greater than or equal to about 85 mol%, greater than or equal to about 90 mol%, greater than or equal to about 91 mol%, or greater than or equal to about 94 mol% and less than or equal to about 99 mol%. High-nickel positive electrode active materials can achieve high capacity and can be used in high-capacity, high-density rechargeable lithium batteries.
[0178] Based on a 100 wt% positive electrode active material layer, the amount of positive electrode active material can range from about 90 wt% to about 99.5 wt%. Based on a 100 wt% positive electrode active material layer, the amounts of binder and conductive material can range from about 0 wt% to about 5 wt% and about 0.5 wt% to about 5 wt%, respectively.
[0179] The binder causes the positive electrode active material particles to adhere to each other and also causes the positive electrode active material to adhere to the current collector. As a non-limiting example, examples of binders may include at least one of the following: polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylate resin, polyester resin, nylon, etc.
[0180] Conductive materials can impart conductivity (e.g., electrical conductivity) to electrodes. Any material that does not cause chemical changes (e.g., does not cause undesirable chemical changes in rechargeable lithium batteries) and conducts electrons can be used in batteries. Examples of conductive materials can include: carbon-based materials, such as at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials in the form of metal powder or metal fibers, including at least one of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.
[0181] Al can be used as a current collector, but current collectors are not limited to this.
[0182] negative electrode The negative electrode for a rechargeable battery may include a current collector and a layer of negative electrode active material on the current collector. The negative electrode active material layer may include a negative electrode active material and may further include a binder and / or a conductive material (e.g., an electrically conductive material).
[0183] For example, the negative electrode active material layer may include about 90 wt% to about 99 wt% of negative electrode active material, about 0.5 wt% to about 5 wt% of binder, and about 0 wt% to about 5 wt% of conductive material.
[0184] Negative electrode active material The negative electrode active material may include at least one of the following: materials that can reversibly insert / deintercalate lithium ions, lithium metal, lithium metal alloys, materials capable of doping / dedoping lithium, or transition metal oxides.
[0185] Materials capable of reversibly intercalating / deintercalating lithium ions may include carbon-based negative electrode active materials, such as crystalline carbon, amorphous carbon, or combinations thereof as examples. The crystalline carbon may be graphite, such as amorphous, flake-like, platelet-like, spherical or fibrous natural graphite or artificial graphite. The amorphous carbon may be or include at least one of soft carbon, hard carbon, mesophase pitch carbonized products, calcined coke, and the like.
[0186] Lithium metal alloys include alloys of lithium with at least one metal such as or including Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn.
[0187] Materials capable of doping / dedoping lithium may be or include Si-based negative electrode active materials or Sn-based negative electrode active materials. The Si-based negative electrode active material may include silicon, silicon-carbon composite, SiO x at least one of (0<x≤2), Si-Q alloy (wherein Q is or includes at least one of an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element (excluding Si), a Group 15 element, a Group 16 element, a transition metal, a rare earth element, and combinations thereof). The Sn-based negative electrode active material may include at least one of Sn, SnO₂, a Sn-based alloy, or a combination thereof.
[0188] The silicon-carbon composite may be or include a composite of silicon and amorphous carbon. According to an exemplary embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coated on surfaces of the silicon particles. For example, the silicon-carbon composite may include secondary particles (core) assembled from primary silicon particles and an amorphous carbon coating (shell) on surfaces of the secondary particles. Amorphous carbon may also be present between the primary silicon particles, and for example, the primary silicon particles may be coated with amorphous carbon. The secondary particles may be dispersed in an amorphous carbon matrix.
[0189] The silicon-carbon composite may further include crystalline carbon. For example, the silicon-carbon composite may include a core comprising crystalline carbon and silicon particles, and an amorphous carbon coating on a surface of the core.
[0190] The Si-based negative electrode active material or the Sn-based negative electrode active material may be used in combination with the carbon-based negative electrode active material.
[0191] The binder may cause the negative electrode active material particles to adhere to each other, and may cause the negative electrode active material to adhere to the current collector. The binder may include a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.
[0192] Non-aqueous adhesives may include at least one of the following: polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene-propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamide-imide, polyimide, or combinations thereof.
[0193] The waterborne adhesive may be or include at least one of styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepoxychloropropane, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0194] When an aqueous binder is used as the negative electrode binder, it may further include a cellulose compound capable of imparting viscosity. The cellulose compound may include at least one of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may include at least one of Na, K, or Li.
[0195] Dry adhesives can be or include fibrous polymeric materials. For example, dry adhesives can be or include at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or combinations thereof.
[0196] Conductive materials can impart electrical conductivity (e.g., electroconductivity) to electrodes. Any material that does not cause chemical changes (e.g., does not cause undesirable chemical changes in rechargeable lithium batteries) and conducts electrons can be used in the battery. Non-limiting examples of conductive materials may include: carbon-based materials, such as at least one of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials in the form of metal powders or metal fibers, including at least one of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof.
[0197] The negative electrode current collector may include at least one of copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, or a combination thereof.
[0198] Rechargeable batteries may also include an electrolyte solution.
[0199] Electrolyte solution Electrolyte solutions used in rechargeable batteries may include non-aqueous organic solvents and lithium salts.
[0200] Non-aqueous organic solvents can serve as media for transporting ions that participate in the electrochemical reactions of a battery.
[0201] Non-aqueous organic solvents may be or include at least one of carbonate solvents, ester solvents, ether solvents, ketone solvents, alcohol solvents, aprotic solvents, or combinations thereof.
[0202] Carbonate solvents may include at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC).
[0203] Ester solvents may include at least one of the following: methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, decanoic acid lactone, mevalonate lactone, caprolactone, etc.
[0204] Ether solvents may include at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, tetrahydrofuran, etc. Additionally, ketone solvents may include cyclohexanone, etc. Alcohol solvents may include ethanol, isopropanol, etc. Aprotic solvents may include at least one of the following: nitriles, such as R-CN (wherein R is a C2 to C20 straight-chain, branched, or cyclic hydrocarbon group, and may include double bonds, aromatic rings, or ether bonds, etc.); amides, such as dimethylformamide; dioxolane, such as 1,3-dioxolane, 1,4-dioxolane, etc.; sulfolane, etc.
[0205] Non-aqueous organic solvents can be used alone or in combination of two or more solvents.
[0206] Furthermore, when using carbonate solvents, cyclic carbonates and chain carbonates can be mixed together, and the cyclic carbonates and chain carbonates can be mixed in a volume ratio ranging from about 1:1 to about 1:9.
[0207] Lithium salts dissolved in organic solvents supply lithium ions in batteries, enabling basic operation of rechargeable lithium batteries and improving lithium ion transport between the positive and negative electrodes. Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F2y+1 At least one of the following: (SO2) (where x and y are integers in the range of 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFBOP), and lithium bis(oxalate)borate (LiBOB).
[0208] Based on their shape, rechargeable lithium batteries can be classified into cylindrical batteries, prismatic batteries, pouch batteries, or coin-shaped batteries, etc.
[0209] Figures 8 to 11 This is a schematic diagram illustrating a rechargeable lithium battery according to an example embodiment. Figure 8 A cylindrical battery is shown. Figure 9 A prismatic battery is shown. Figure 10 and Figure 11 A pouch-type battery is shown. (See reference) Figures 8 to 11 The rechargeable lithium battery 100 may include an electrode assembly 40 comprising a separator 30 between a positive electrode 10 and a negative electrode 20, and a housing 50 therein housing the electrode assembly 40. The positive electrode 10, negative electrode 20, and separator 30 may be impregnated with an electrolyte solution (not shown). Figure 8 As shown, the rechargeable lithium battery 100 may include a sealing member 60 of the sealed housing 50. Figure 9 In this context, the rechargeable lithium battery 100 may include a positive electrode lead connector 11, a positive electrode terminal 12 connected to the positive electrode lead connector 11, a negative electrode lead connector 21, and a negative electrode terminal 22 connected to the negative electrode lead connector 21. For example... Figure 10 and Figure 11 As shown, the rechargeable lithium battery 100 may include Figure 11 The electrode terminal 70 shown, or for example Figure 10 The positive electrode terminal 71 and negative electrode terminal 72 shown in the figure form an electrical path for guiding the current formed in the electrode assembly 40 to the outside of the rechargeable lithium battery 100.
[0210] As a non-limiting example, the rechargeable battery according to the example embodiment can be applied to, for example, automobiles, mobile phones and / or various types of electronic devices.
[0211] The above description only depicts the case where the separator of a rechargeable battery is included in the battery separately from the electrodes (e.g., the positive or negative electrode). However, the separator for a rechargeable battery can be integrated with the electrodes and included in the battery.
[0212] in this regard, Figure 12 A cross-sectional view of electrodes for a rechargeable battery according to an example embodiment is shown. (Refer to...) Figure 12The electrode 1 for a rechargeable battery may include an active material layer 2 for a rechargeable battery and a separator 3 integrated with one surface of the active material layer 2.
[0213] exist Figure 12 In the diagram, the active material layer 2 and the separator 3 for the rechargeable lithium battery are shown as being formed as separate layers, but the dashed lines indicate that the active material layer 2 and the separator 3 for the rechargeable lithium battery can be integrated with each other.
[0214] In one example embodiment, in addition to polyimide and polysilsesquioxane materials, the fiber may also include one or more of polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyamide-imide (PAI), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), polyvinyl alcohol (PVA), and aromatic polyamide polymers. The polyimide and polysilsesquioxane materials may be included in one or more of the core and shell of the fiber.
[0215] exist Figure 12 In this context, the diaphragm 3 is depicted as a single layer. However, the diaphragm 3 may comprise multiple laminated layers.
[0216] A rechargeable battery according to an example embodiment of this disclosure can be used in automobiles, mobile phones and / or various types of electronic devices, but this disclosure is not limited thereto.
[0217] This disclosure can be applied to various types of electrical devices that use batteries.
[0218] An electrical device according to an example embodiment of this disclosure may include an electric vehicle, a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), an electric bicycle, an electric scooter, an electric golf cart, and other vehicles that may utilize a battery pack as a power source.
[0219] An electrical apparatus according to an example embodiment of the present disclosure may include an electrical device comprising an energy storage system using batteries, and equipment and apparatus associated with the energy storage system.
[0220] An electrical device according to an example embodiment of this disclosure may include power tools, which may include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, and may include any device powered by a battery-based motor, such as an electric drill, electric grinder, electric wrench, electric screwdriver, electric hammer, impact drill, concrete vibrator, and electric planer.
[0221] An electrical device according to an example embodiment of this disclosure may include battery-powered applications such as mobile phones, tablet computers, laptop computers, wearable devices, electric toys, portable electric toys, game consoles, ships, aircraft, spacecraft, drones, and robots.
[0222] Examples and comparative examples of this disclosure are described below. However, the following examples are merely exemplary embodiments of this disclosure, and this disclosure is not limited to these examples.
[0223] Example 1 Preparation of electrospinning solutions for core-shell fibers 4,4'-Biphenyltetracarboxylic dianhydride (BPDA) and p-phenylenediamine (pPDA) are polymerized to prepare polyamic acid, and dimethylacetamide is mixed as a solvent to prepare an electrospinning solution for the core. The polyamic acid can provide polyimide units represented by the following chemical formula 1-3-1 during heat treatment during electrospinning as described below.
[0224] Chemical formula 1-3-1: .
[0225] Dimethylacetamide is reacted with R in the following chemical formulas 2-4. 31 R 41 R 51 and R 61 An electrospinning solution for the shell was prepared by mixing polysilsesquioxanes having structures represented by the following chemical formulas 2-5.
[0226] Chemical formula 2-4: .
[0227] Chemical formula 2-5: .
[0228] Electrospinning and diaphragm manufacturing An electrospinning apparatus equipped with a first nozzle positioned along the moving direction of a substrate (polyethylene film) is prepared. The first nozzle has a spinning orifice that is not divided into a core and a shell. Electrospinning solutions prepared for the core and for the shell are injected together into the first nozzle. While the substrate is moving, the electrospinning solution for the first layer is electrospinned from the first nozzle, the solvent is dried, and the first layer is heat-treated at 50°C for 1 hour and compressed. The substrate is then peeled off to produce a diaphragm.
[0229] The diaphragm consists of a first layer comprising core-shell type fibers, wherein, based on a total of 100 parts by weight of core and shell in the core-shell type fibers, the content of the core is 90 parts by weight and the content of the shell is 10 parts by weight. The core comprises a polyimide resin having units represented by chemical formula 1-3-1, and the shell comprises a polysilsesquioxane resin having units represented by chemical formula 2-4. The average diameter of the core-shell type fibers is 150 nm.
[0230] The electrospinning process is as follows: The internal temperature of the electrospinning space is 22°C. A nozzle assembly with a needle size of 25G is positioned 16cm apart from the collecting roller. The electrospinning solution is added to the tip, a voltage of 40kV to 75kV is applied, and electrospinning is performed. The collecting roller speed is set to 1m / min to 3m / min. Air pressure is applied by flowing air at a pressure of 0.275MPa. After electrospinning, the fibers are dried with hot air at 90°C.
[0231] Example 2 Preparation of electrospinning solutions for core-shell fibers Pyromellitic dianhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA) are polymerized to prepare polyamic acid, and dimethylacetamide is mixed as a solvent to prepare an electrospinning solution for the core. The polyamic acid can provide polyimide units represented by the following chemical formula 1-4-1 during heat treatment during electrospinning as described below.
[0232] Chemical formula 1-4-1: .
[0233] Dimethylacetamide, used as a solvent, reacts with R from the following chemical formulas 2-4. 31 R 41 R 51 and R 61 An electrospinning solution for the shell was prepared by mixing polysilsesquioxanes that are all phenyl.
[0234] Chemical formula 2-4: .
[0235] Electrospinning and diaphragm manufacturing An electrospinning apparatus is prepared, equipped with a first nozzle, a second nozzle, and a third nozzle sequentially positioned along the direction of movement of the substrate. Each of the first, second, and third nozzles has a spinning orifice that is not divided into a core and a shell. An electrospinning solution prepared for the core and an electrospinning solution prepared for the shell are injected together into each of the first, second, and third nozzles.
[0236] While moving the substrate, electrospinning solutions for the core and for the shell are sequentially electrospinned from the first nozzle, the second nozzle, and the third nozzle. The solvent is dried, and the layers are heat-treated at 50°C for 1 hour and compressed. The substrate is then peeled off to produce a diaphragm.
[0237] The diaphragm comprises a first layer, a second layer, and a third layer, each consisting of core-shell type fibers laminated sequentially. The core-shell type fibers contain 90 parts by weight of core and 10 parts by weight of shell, based on a total of 100 parts by weight of core and shell. The core comprises a polyimide resin with units represented by chemical formula 1-4-1, and the shell comprises a polysilsesquioxane resin with units represented by chemical formula 2-4. The average diameter of the core-shell type fibers is 150 nm.
[0238] Perform the electrospinning process according to the process described in Example 1 above.
[0239] Example 3 Preparation of electrospinning solutions for the first and third layers Referring to Example 2, an electrospinning solution capable of providing units represented by the following chemical formula 1-4-1 is prepared.
[0240] Chemical formula 1-4-1: .
[0241] Preparation of electrospinning solution for the second layer Referring to Example 2, an electrospinning solution for the nucleus is prepared, capable of providing units represented by the following chemical formula 1-4-1.
[0242] Chemical formula 1-4-1: .
[0243] Dimethylacetamide, used as a solvent, reacts with R from the following chemical formulas 2-4. 31 R 41 R 51 and R 61 An electrospinning solution for the shell was prepared by mixing polysilsesquioxanes having structures represented by the following chemical formulas 2-6.
[0244] Chemical formula 2-4: .
[0245] Chemical formula 2-6: .
[0246] Electrospinning and diaphragm manufacturing An electrospinning apparatus is prepared, equipped with a first nozzle, a second nozzle, and a third nozzle sequentially positioned along the direction of movement of the substrate. An electrospinning solution prepared above is injected into each of the first and third nozzles, and an electrospinning solution for the core and an electrospinning solution for the shell are injected into the second nozzle. The second nozzle has a spinning orifice that is not divided into a core and a shell.
[0247] While moving the substrate, the electrospinning solutions for the first layer, the second layer, and the third layer are electrospinned sequentially from the first nozzle, the second nozzle, and the third nozzle, respectively. The solvent is dried, and these layers are heat-treated at 50°C for 1 hour and compressed. Then, the substrate is peeled off to produce a diaphragm (thickness: 10 μm).
[0248] The membrane comprises a first layer made of polyimide resin fibers having units represented by chemical formula 1-4-1, a second layer comprising core-shell type fibers, and a third layer made of polyimide resin fibers having units represented by chemical formula 1-4-1, wherein, based on a total of 100 parts by weight of core and shell, the content of core is 90 parts by weight and the content of shell is 10 parts by weight, the core comprising polyimide resin having units represented by chemical formula 1-4-1, and the shell comprising polysilsesquioxane resin having units represented by chemical formula 2-4, wherein the average diameter of the core-shell type fibers is 150 nm.
[0249] Perform the electrospinning process according to the process described in Example 1 above.
[0250] Example 4 Preparation of electrospinning solutions for the first and third layers Refer to Example 1 to prepare an electrospinning solution for the core and an electrospinning solution for the shell.
[0251] Preparation of electrospinning solution for the second layer 4,4'-Biphenyltetracarboxylic dianhydride (BPDA) and p-phenylenediamine (pPDA) were polymerized to prepare polyamic acid, and dimethylacetamide was mixed to prepare an electrospinning solution.
[0252] Electrospinning and diaphragm manufacturing An electrospinning apparatus is prepared, equipped with a first nozzle, a second nozzle, and a third nozzle sequentially positioned along the direction of movement of the substrate. Both the first and third nozzles have a single spinning orifice that is not divided into a core and a shell. An electrospinning solution prepared for the core and an electrospinning solution prepared for the shell are injected together into each of the first and third nozzles, and an electrospinning solution for the second layer is injected into the second nozzle.
[0253] While moving the substrate, the electrospinning solutions for the first layer, the second layer, and the third layer are electrospinned sequentially from the first nozzle, the second nozzle, and the third nozzle, respectively. The solvent is dried, and these layers are heat-treated at 50°C for 1 hour and compressed. Then, the substrate is peeled off to manufacture the diaphragm.
[0254] The membrane comprises a first layer consisting of core-shell type fibers, a second layer made of polyimide resin fibers having units represented by chemical formula 1-3-1, and a third layer consisting of core-shell type fibers, sequentially laminated together. In the first layer, based on a total of 100 parts by weight of core and shell, the content of core is 90 parts by weight and the content of shell is 10 parts by weight. The core comprises a polyimide resin having units represented by chemical formula 1-3-1, and the shell comprises a polysilsesquioxane resin having units represented by chemical formula 2-4. In the third layer, based on a total of 100 parts by weight of core and shell, the content of core is 90 parts by weight and the content of shell is 10 parts by weight. The core comprises a polyimide resin having units represented by chemical formula 1-3-1, and the shell comprises a polysilsesquioxane resin having units represented by chemical formula 2-4. The average diameter of the core-shell type fibers is 150 nm.
[0255] Perform the electrospinning process according to the process described in Example 1 above.
[0256] Example 5 and Example 6 The diaphragm was manufactured in the same manner as in Example 4, except that the voltage was changed during electrospinning in Example 4. In Example 5, the average diameter of the core-shell fibers was 100 nm, and in Example 6, the average diameter of the core-shell fibers was 200 nm.
[0257] Compare Example 1 and Compare Example 2 The diaphragm (thickness: 10 μm) was manufactured in the same manner as in Example 4, except that the voltage was changed during electrospinning in Example 4. In Comparative Example 1, the average diameter of the core-shell fibers was 20 nm, and in Comparative Example 2, the average diameter of the core-shell fibers was 300 nm.
[0258] Comparison Example 3 4,4'-Biphenyltetracarboxylic dianhydride (BPDA) and p-phenylenediamine (pPDA) were polymerized to prepare polyamic acid, and dimethylacetamide was mixed to prepare an electrospinning solution. The diaphragm was manufactured in the same manner as in Example 4, except that the electrospinning solution prepared above was injected into each of the first, second, and third nozzles. The polyimide resin fibers had an average diameter of 150 nm. The diaphragm of Comparative Example 3 did not include core-shell fibers.
[0259] Battery manufacturing Manufacturing of the negative electrode: 97 wt% of graphite particles with an average particle size of 25 μm, 1.5 wt% of styrene-butadiene rubber (SBR) binder, and 1.5 wt% of carboxymethyl cellulose (CMC) were mixed, and then the mixture was placed in distilled water and stirred with a mechanical stirrer for 60 minutes to prepare a slurry for the negative electrode active material. The slurry was coated onto a 10 μm thick copper current collector using a doctor blade, dried in a hot air dryer at 100 °C for 0.5 hours, and then dried again under vacuum at 120 °C for 4 hours. Finally, it was rolled to fabricate the negative electrode.
[0260] Manufacturing of the positive electrode: A mixture of 97 wt% LiCoO2, 1.5 wt% carbon black powder as a conductive material, and 1.5 wt% polyvinylidene fluoride (PVdF) was placed in an N-methyl-2-pyrrolidone solvent and stirred for 30 minutes using a mechanical stirrer to prepare a slurry for the positive electrode active material. The slurry was then coated onto a 20 μm thick aluminum current collector using a doctor blade, dried in a hot air dryer at 100°C for 0.5 hours, and then dried again under vacuum at 120°C for 4 hours. Finally, the mixture was rolled to fabricate the positive electrode.
[0261] Electrode assembly core: Each diaphragm obtained according to the examples and comparative examples was placed between the positive and negative electrodes manufactured above, and then wound to manufacture the electrode assembly core. The core was inserted into a bag, electrolyte was injected, and the bag was vacuum sealed. As the electrolyte, 1.3 M LiPF6 was used dissolved in a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 30:50:20. The core inserted into the bag was pressed at 80°C for 3 minutes while applying 11.7 kgf / cm². 2 The pressure is used to manufacture rechargeable lithium batteries.
[0262] The following physical properties are evaluated for the diaphragms manufactured in the example and comparative examples.
[0263] Identification and average diameter of core-shell fibers The cross-section of the fibers included in the first layer of the membrane manufactured in the example was confirmed using SEM. The SEM results confirmed that the fibers were core-shell type fibers.
[0264] The average diameter is calculated by selecting 10 to 30 sections from the layer's cross-section, measuring each diameter using a microscope, and then calculating the average of the obtained diameters. When the fiber cross-section is circular, the normal diameter is used, while when the fiber cross-section is not circular but elliptical or amorphous, the longest diameter, which is the maximum value among the diameters measured in the cross-section, is used.
[0265] Dry heat shrinkage rate (unit: %) Each separator for rechargeable lithium batteries in the example and comparative examples was cut into 8cm × 8cm dimensions to create a sample. After drawing a 5cm × 5cm square on the surface of the sample, the sample was placed between paper or alumina powder and placed in an oven at 150°C for 1 hour. It was then removed, and the dimensions of the drawn square's sides were measured. The longitudinal (MD) and transverse (TD) thermal shrinkage rates were calculated. The thermal shrinkage rates were calculated according to the following mathematical formula 1. The MD and TD thermal shrinkage rates were calculated separately, and then the average value was obtained.
[0266] Mathematical formula 1: Thermal shrinkage rate = (L0-L1) / L0×100.
[0267] L0 is the initial length of the diaphragm, and L1 is the length of the diaphragm after being placed at 150°C for 1 hour.
[0268] Thermal shrinkage rate in electrolyte (unit: %) Each separator used in the example and comparative examples for rechargeable lithium batteries was cut into 8cm × 8cm dimensions to prepare samples. A 5cm × 5cm square was drawn on the surface of the sample. One sample was placed between the positive and negative electrodes to create three sets of positive electrode-sample-negative electrode laminates, which were then placed in a bag. 2g of electrolyte (1.5M LiPF6 dissolved in ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate (volume ratio 30:50:20)) was injected to completely saturate the laminate with the electrolyte, sealed, and placed at 25°C for 12 hours. Then, the sample was placed in an oven at 150°C for 1 hour, then removed, and the dimensions of the drawn square were measured to calculate the respective longitudinal (MD) and transverse (TD) thermal shrinkage rates. The thermal shrinkage rate was calculated according to Formula 1. The thermal shrinkage rates of MD and TD were calculated separately, and then the average value was obtained.
[0269] Electrolyte wettability (unit: cm) 2 ) The fabricated diaphragm was dried in an oven at 120°C for 12 hours and cut into 8cm × 8cm pieces to prepare samples. 15 μL of electrolyte (1.5 M LiPF6 dissolved in ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate (volume ratio 30:50:20)) was dropped onto the sample from a height of 1 cm, and the electrolyte wetting area of the sample was calculated after 30 seconds. The electrolyte wetting area was calculated using the ImageJ program.
[0270] Strength (unit: kgf / cm) 2 ) By cutting the manufactured diaphragm into 1cm × 12cm dimensions and using a measuring device (Instron 5965, Instron), the maximum force required to break the diaphragm is divided by (thickness × width) (unit: kgf / cm). 2 (This is used to measure the strength of the manufactured diaphragm.)
[0271] Breathability (unit: sec / 100cc) The permeability of the manufactured diaphragm was measured by measuring the time (in seconds) it takes for 100cc of air to pass through the diaphragm using a measuring device (EG01-55-1MR, Asahi Seiko).
[0272] Air permeability measuring device setting conditions: Measured pressure: 0.5 kg / cm 2 Cylinder pressure: 2.5 kg / cm² 2 Set time: 10 seconds Table 1:
[0273] As shown in Table 1 above, the example separator not only exhibits high heat resistance but also demonstrates high strength and desired or improved permeability, thereby improving battery safety. As shown in Table 1 above, the effect of the example separator cannot be achieved when comparing it to the example separator.
[0274] According to one example embodiment, the separator for a rechargeable battery has desired or improved heat resistance, resulting in low dry shrinkage and low shrinkage in the electrolyte, thereby reducing or preventing short circuits and improving battery safety.
[0275] According to one example embodiment, the separator for a rechargeable battery has desired or improved electrolyte wettability, which increases lithium-ion mobility and accelerates electrolyte injection rate, thereby improving battery capacity.
[0276] Since the separator for a rechargeable battery according to an example embodiment does not include a porous substrate, the separator has a thin thickness and does not have short-circuit problems caused by thermal shrinkage and melting at high temperatures due to the porous substrate, thus the battery safety can be high.
[0277] According to one example embodiment, the separator for a rechargeable battery can have desired or improved manufacturability by including core-shell fibers that can be manufactured without using a core-shell nozzle.
[0278] Although exemplary embodiments of the present disclosure have been described above, the present disclosure is not limited thereto, and various modifications can be made within the scope of the claims, the detailed description of the disclosure, and the drawings, and these modifications also fall within the scope of the present disclosure.
Claims
1. A separator for a rechargeable battery, the separator comprising: The first layer comprises core-shell fibers having a core and a shell surrounding the core. The core comprises a polyimide material, and the shell comprises a polysilsesquioxane material. The core-shell fiber has an average diameter of 30 nm or larger and 200 nm or smaller.
2. The diaphragm as claimed in claim 1, wherein, The diameter of the core is greater than the thickness of the shell.
3. The diaphragm as described in claim 1, wherein, The core has a diameter of 120 nm or greater and 140 nm or less, and the shell has a thickness of 10 nm or greater and 30 nm or less.
4. The diaphragm as claimed in claim 1, wherein, The polyimide material comprises repeating units represented by chemical formula 1: Chemical Formula 1: ; In chemical formula 1, Indicates the connection point of an element. R 1 Including tetravalent organic groups, and R 2 It includes at least one of the following: a divalent aliphatic organic group, a divalent alicyclic organic group, a divalent aromatic organic group, and combinations thereof, having a total of 3 to 30 carbon atoms.
5. The diaphragm as claimed in claim 1, wherein, The polyimide material has a weight-average molecular weight in the range of 100,000 g / mol to 300,000 g / mol.
6. The diaphragm as claimed in claim 1, wherein, The polyimide material includes crosslinkable functional groups.
7. The diaphragm as claimed in claim 1, wherein, The polysilsesquioxane material has a weight-average molecular weight in the range of 10,000 g / mol to 30,000 g / mol.
8. The diaphragm as claimed in claim 1, wherein, The polysilsesquioxane materials include one or more of crosslinkable functional groups and aryl groups having 6 to 20 carbon atoms.
9. The diaphragm as claimed in claim 1, wherein, The polysilsesquioxane-based material comprises units represented by chemical formulas 2-3: Chemical formula 2-3: ; In chemical formula 2-3, R 3 R 4 R 5 and R 6 Each of the following is independently hydrogen, hydroxyl, alkyl having 1 to 20 carbon atoms, alkenyl having 2 to 20 carbon atoms, alkynyl having 2 to 20 carbon atoms, cycloalkyl having 3 to 20 carbon atoms, aryl having 6 to 20 carbon atoms, aralkyl having 7 to 20 carbon atoms, crosslinkable functional groups, or combinations thereof. n is the number of moles in the unit.
10. The diaphragm as claimed in claim 9, wherein, The crosslinkable functional group includes one or more parts represented by one or more of chemical formulas 2-1 and 2-2: Chemical formula 2-1: ; Chemical formula 2-2: ; In chemical formulas 2-1 and 2-2, R 8 It is hydrogen or methyl, and R 7 R 9 and R 10 Each independently includes alkylene groups having a range of 1 to 20 carbon atoms.
11. The diaphragm as claimed in claim 1, wherein, The core-shell fiber has a core content ranging from 10 wt% to 95 wt% and a shell content ranging from 5 wt% to 90 wt%.
12. The diaphragm as claimed in claim 1, wherein, The diaphragm includes either a single layer or multiple layers containing the first layer.
13. The diaphragm as claimed in claim 12, wherein, The diaphragm comprises multiple layers including the first layer and the second layer.
14. The diaphragm as claimed in claim 13, wherein, The second layer includes a fibrous layer, a non-fibrous layer, or a combination thereof.
15. The diaphragm as claimed in claim 13, wherein, The fibers of the second layer include one or more of the following: polyacrylonitrile, polyaniline, polypyrrole, polyrhodanine, melamine, polyurea, polyvinyl chloride, polyvinyl alcohol, polyethylene oxide, polymethyl methacrylate, polyacrylic acid, polylactic acid, polyimide, polyamide-imide, polyarylamide, polybenzylimidazole, polypropylene, resorcinol-formaldehyde resin, melamine-formaldehyde resin, asphalt, sucrose, glucose, cellulose, and polyvinylidene fluoride.
16. The diaphragm as claimed in claim 13, wherein, The diaphragm is formed by sequentially laminating the first layer, the second layer, and the first layer, or by sequentially laminating the second layer, the first layer, and the second layer.
17. The diaphragm as claimed in claim 1, wherein, The diaphragm does not have a porous substrate.
18. The diaphragm as claimed in claim 1, wherein, The polyimide material comprises units represented by one or more of chemical formulas 1-3 and 1-4: Chemical formulas 1-3: ;as well as Chemical formulas 1-4: ,and The polysilsesquioxane-based material comprises units represented by chemical formulas 2-4: Chemical formula 2-4: ; In chemical formula 2-4, R 31 R 41 R 51 and R 61 Each independently includes the portion represented by chemical formulas 2-5, the portion represented by chemical formulas 2-6, or the phenyl group: Chemical formula 2-5: ;as well as Chemical formula 2-6: 。 19. The diaphragm as claimed in claim 1, wherein, The diaphragm has a thickness of 10 μm or less.
20. A rechargeable battery, said rechargeable battery comprising: Positive electrode; negative electrode; as well as The diaphragm as described in any one of claims 1-19 is located between the positive electrode and the negative electrode.
Citation Information
Patent Citations
Positive electrode active material for sodium secondary battery, method for preparing the same and sodium secondary battery including the same
KR1020250064095A