Mott-Schottky heterostructure modified battery separator, its preparation method and application
By preparing nitrogen-doped carbon-coated porous mottled-Schottky heterostructure molybdenum-based materials to modify battery separators, the problems of polysulfide dissolution and lithium dendrite growth in lithium-sulfur batteries were solved, achieving efficient polysulfide conversion and improved battery performance.
Patent Information
- Application Number
- CN202611060167.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-16
- Publication Date
- 2026-11-17
AI Technical Summary
The shuttle effect caused by polysulfide dissolution and the growth of lithium dendrites at the anode in existing lithium-sulfur batteries are difficult to solve effectively with traditional modified materials, and modification strategies are difficult to enhance the adsorption sites of polar materials and change the slow kinetics of polysulfide conversion.
A modified battery separator using a Motschottky heterostructure was developed by preparing a nitrogen-doped carbon-coated porous Motschottky heterostructure molybdenum-based material and coating it onto the surface of a commercial polypropylene separator to form a modified battery separator, which enhances the chemical adsorption performance and electrolytic activity of polysulfides.
It effectively suppresses the shuttle effect of polysulfides, improves the cycle life and discharge performance of lithium-sulfur batteries, and exhibits excellent electrochemical performance, such as a discharge specific capacity of 1221.9 mAh g-1 and 686.7 mAh g-1 at 0.2C and 5C rates, respectively, and a capacity decay rate of only 0.043% per cycle after 1000 cycles.
Smart Images

Figure CN123121065A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of membrane material preparation technology, and in particular to a Mott-Schottky heterostructure modified battery membrane, its preparation method, and its application. Background Technology
[0002] To achieve carbon neutrality, electric vehicles and large-scale energy storage systems have seen rapid development. For many years, lithium-ion batteries have been widely used in these fields as a green power source. They possess a high theoretical specific capacity (1675 mAh g⁻¹). -1 ) and energy density (2600 Wh kg) -1 Lithium-sulfur batteries have attracted widespread attention from researchers and are considered one of the most promising high-energy storage systems. The rechargeability of these batteries primarily relies on the presence of long or short sulfur chains (from S8...). 2- To S2 2- The redox conversion of polysulfides is a major challenge in their practical application. A key issue is the "shuttle effect" caused by polysulfides dissolving in the electrolyte. These soluble polysulfides migrate unimpeded through porous membranes to the lithium anode, leading to loss of active material and shortened battery cycle life. Over the past few decades, numerous immobilization strategies have been developed to address this problem, such as composite cathodes, polysulfide adsorption, solid electrolytes, and electrolyte additives. While these strategies have prevented soluble polysulfides from escaping from the cathode to some extent, increasing evidence suggests that uneven lithium-ion deposition on the anode side can lead to dendrite growth and battery short circuits. Furthermore, "dead sulfur" generated near commercially available polypropylene separators during charge-discharge cycles also poses a serious problem. Therefore, some researchers have proposed modifying conventional separators by coating them with functional materials. Common modification materials based on physical barriers and chemisorption include carbon nanotubes, graphene, nitrides, and sulfides, which are coated onto the surface of conventional separators to prevent soluble polysulfides from escaping from the cathode. However, modification strategies struggle to enhance the adsorption sites of polar materials and alter the slow kinetics of polysulfide conversion. Therefore, developing novel modified materials with excellent chemisorption properties and high electrolytic activity remains an important research topic. Summary of the Invention
[0003] The purpose of this invention is to provide a Mott-Schottky heterostructure modified battery separator, its preparation method and application, aiming to develop a novel modified battery separator to accelerate the redox reaction kinetics of sulfur and suppress the "shuttle effect" of polysulfides.
[0004] In a first aspect, the present invention provides a method for preparing a Mott-Schottky heterostructure modified battery separator, the method comprising: Step S1: Add ammonium molybdate tetrahydrate to a mixed solution of concentrated nitric acid and water, and stir thoroughly to obtain a mixed solution; Step S2: The mixed solution is transferred to a reaction vessel for hydrothermal reaction to obtain a first precipitate. The first precipitate is washed with ethanol and water to obtain the MoO3 precursor material. Step S3: Dissolve tris(hydroxymethyl)aminomethane in deionized water to obtain a buffer solution. Add the polymer monomer and the MoO3 precursor material to the buffer solution and stir thoroughly to obtain a second precipitate. Wash the second precipitate with ethanol and water to obtain polymer-coated MoO3 material. Step S4: Anneal the polymer-coated MoO3 material to obtain a nitrogen-doped carbon-coated porous mottled-Schottky heterostructure molybdenum-based material. Step S5: Mix the nitrogen-doped carbon-coated porous molybdenum-based heterostructure material with PVDF binder and add it to N-methylpyrrolidone solvent and stir evenly to form a slurry. Coat the slurry onto the surface of a commercial polypropylene separator to obtain a modified battery separator.
[0005] In some embodiments, in step S1, the volume ratio of concentrated nitric acid to water is 1:6 to 6:1; and the concentration of ammonium molybdate tetrahydrate is 0.01 to 0.1 mmol / mL.
[0006] In some embodiments, in step S2, the temperature of the hydrothermal reaction is 100~200°C. o C, the reaction time is 6~24 h.
[0007] In some embodiments, in step S3, the polymer monomer includes at least one of aniline and dopamine hydrochloride.
[0008] In some embodiments, in step S3, the concentration of tris(hydroxymethyl)aminomethane is 0.005~0.02 mmol / mL, the mass ratio of the polymer monomer to the MoO3 precursor material is 1:4~4:1, and the stirring time is 6~24 h.
[0009] In some embodiments, in step S4, the annealing atmosphere is at least one of N2 and Ar, and the annealing temperature is 600~1000℃. o C, heating rate is 1~5 o C / min, annealing time is 1~10 h.
[0010] In some embodiments, in step S5, the coating thickness is 10~100 μm.
[0011] In some embodiments, the mass ratio of the Mott-Schottky heterostructure molybdenum-based material to the PVDF binder is 180~220:21~25.
[0012] Secondly, the present invention provides a Mott-Schottky heterostructure modified battery separator, which is prepared according to the above-described method for preparing a Mott-Schottky heterostructure modified battery separator.
[0013] Thirdly, the present invention provides the application of the above-described Mott-Schottky heterostructure modified battery separator in lithium-sulfur batteries.
[0014] Compared with the prior art, the present invention has the following advantages: 1. The nitrogen-doped carbon-coated porous mottled-Schottky heterostructure molybdenum-based separator prepared in this invention exhibits uniform elemental doping. The synergistic effect among the multiple active components enables the electrocatalyst to effectively resist polysulfides, accelerate the redox reaction kinetics of sulfur, and suppress the "shuttle effect" of polysulfides. Furthermore, when the obtained mottled-Schottky heterostructure molybdenum-based modified battery separator is used to assemble lithium-sulfur batteries, the assembled lithium-sulfur batteries exhibit excellent performance, such as a discharge specific capacity of 1221.9 mAh g⁻¹ at 0.2C and 5C rates. -1 and 686.7mAh g -1 Furthermore, at a current multiplier of 1 C, the capacity decay rate per cycle after 1000 cycles is only 0.043%.
[0015] 2. This invention utilizes various strategies to adjust the electronic structure of the membrane material, such as heteroatom doping and defect engineering, which can effectively improve chemical interaction and catalytic activity. Specifically, molybdenum-based materials, due to their tunable crystal structure, adjustable composition, and variable valence of Mo, can interact strongly with soluble polysulfides through various mechanisms to suppress the "shuttle effect." Furthermore, molybdenum-based materials also exhibit lithiophilicity, which helps suppress the formation of lithium dendrites on the anode and extend the cycle life of lithium-sulfur batteries. Simultaneously, the formed Motter-Schottky heterostructure exposes more active sites, effectively improving the redox kinetics of sulfur and lowering the polysulfide conversion energy barrier, potentially further enhancing the material's catalytic conversion effect on polysulfides. Attached Figure Description
[0016] Figure 1 The X-ray diffraction pattern of the molybdenum-based modified membrane with a Mott-Schottky heterostructure prepared in Example 1; Figure 2 A scanning electron microscope image of the molybdenum-modified diaphragm with a Mott-Schottky heterostructure prepared in Example 1; Figure 3 This is a schematic diagram of the physical properties of the Mott-Schottky heterostructure modified battery separator prepared in Example 1; Figure 4 This is a schematic diagram of the long-cycle performance of a lithium-sulfur battery assembled with the Mott-Schottky heterostructure modified battery separator prepared in Example 1. Figure 5 This is a schematic diagram of the rate performance of a lithium-sulfur battery assembled with the Mott-Schottky heterostructure modified battery separator prepared in Example 1.
[0017] The following detailed description, in conjunction with the accompanying drawings, will further illustrate the present invention. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical or scientific terms used herein should have the ordinary meaning understood by those skilled in the art. The terms "comprising" and similar expressions used herein mean that the element or object preceding the word covers the element or object listed after the word and its equivalents, but does not exclude other elements or objects.
[0019] Example 1 A method for preparing a molybdenum-modified battery separator with a Mott-Schottky heterostructure includes the following steps: Step S1: Add 1.1122 g of ammonium molybdate tetrahydrate to 30 mL of a mixed solution of concentrated nitric acid and water with a volume ratio of 1:5, and stir thoroughly for 30 min to obtain a mixed solution; Step S2: Transfer the mixed solution to a 50 mL reaction vessel at 200 rpm. o The first precipitate was obtained by hydrothermal reaction at C for 20 h. The first precipitate was washed three times with ethanol and water at 60 °C. o MoO3 precursor material was obtained after vacuum drying at C for 12 h.
[0020] Step S3: Dissolve 0.2432 g of tris(hydroxymethyl)aminomethane (TRIS) buffer in 200 mL of deionized water. Add 0.25 g of dopamine hydrochloride and 0.5 g of MoO3 to the buffer solution and stir thoroughly for 12 h to obtain a second precipitate. Wash the second precipitate three times with ethanol and water. o After vacuum drying at C for 12 h, polydopamine-coated MoO3 material was obtained; Step S4: The polydopamine-coated MoO3 material is placed in an Ar / H2 (10%) mixed atmosphere at 3 oHeating rate increased to 800 °C / min o Nitrogen-doped carbon-coated porous molybdenum-based heterostructure material was obtained by C annealing for 5 h. Step S5: Mix 20 mg of nitrogen-doped carbon-coated porous molybdenum-based heterostructure material with 2.3 mg of PVDF binder and add it to 100 mg of N-methylpyrrolidone solvent. Stir until homogeneous to form a slurry. Coat the slurry onto the surface of a commercial polypropylene separator with a thickness of 20 μm. Dry at 60 °C for 12 h to obtain a modified battery separator.
[0021] Example 2 This embodiment is basically the same as Embodiment 1, except that the annealing temperature in step S4 is adjusted to 900°C. o C, to obtain a nitrogen-doped carbon-coated porous molybdenum-based heterostructure membrane.
[0022] Comparative Example 1 This comparative example is basically the same as Example 1, except that steps S1 to S4 are deleted, and in step S5, CNTs are used to replace nitrogen-doped carbon to coat the porous mottled Schottky heterostructure molybdenum-based material to form a separator, thus obtaining a CNT lithium-sulfur battery separator.
[0023] Comparative Example 2 This comparative example is basically the same as Example 1, except that steps S1 to S5 are deleted, that is, no active material is loaded on the polypropylene separator, and a blank polypropylene lithium-sulfur battery separator is obtained directly.
[0024] Comparative Example 3 This comparative example is basically the same as Example 1, except that steps S1 to S3 are deleted, and the polydopamine-coated MoO3 material in Example 1 is replaced with the MoO3@ZIF-8 precursor material prepared by existing patent CN119231090A. The specific steps are as follows: S1: Mix 200 mg MoO3, 1 g polyvinylpyrrolidone (PVP) and 5 mmol zinc nitrate hexahydrate (1487.45 mg) in 60 mL of anhydrous methanol and stir thoroughly to obtain a mixed solution. S2: Dissolve 40 mmol of 2-methylimidazole in 60 mL of anhydrous methanol and stir thoroughly to obtain a clear solution. S3: Mix the mixed solution and the clear solution, stir for 30 min to obtain a precipitate, collect the precipitate by centrifugation, wash three times with water and ethanol, and vacuum dry to obtain the MoO3@ZIF-8 precursor material.
[0025] The separators from Examples 1 to Comparative Examples 3 were assembled into lithium-sulfur batteries using the following method, and electrochemical tests were performed: The modified separator was used to assemble lithium-sulfur batteries and electrochemical tests were performed. (1) Mix sulfur powder and Super C at a mass ratio of 7:3 and grind for 30 min. Then place in an oven at 155 ℃ for 12 h and cool to obtain sulfur-carbon cathode material.
[0026] (2) After mixing and grinding the sulfur-carbon cathode material, conductive carbon, and PVDF binder in a mass ratio of 8:1:1, the slurry is coated onto the surface of the carbon-coated aluminum foil, dried under vacuum at 60 ℃, and then cut into round pieces with a diameter of 10 mm to obtain the sulfur-carbon electrode sheet.
[0027] (3) Assemble button batteries in a glove box filled with argon gas. The positive electrode is a sulfur-carbon electrode, the negative electrode is metallic lithium, the separator is the separator prepared in Examples 1 to Comparative Examples 3, and the electrolyte composition is: 1 mol / L lithium bis(trifluoromethanesulfonyl)imide and 2 wt% lithium nitrate; the solvent is a mixture of 1,3-dioxolane and ethylene glycol dimethyl ether in a volume ratio of 1:1.
[0028] Figure 1 The image shows the X-ray diffraction pattern of the nitrogen-doped carbon-coated porous mottle-Schottky heterostructure molybdenum-based electrocatalyst prepared in Example 1. The X-ray diffraction pattern of the product shows that the synthesized product is a heterostructure of Mo and Mo2C, which is consistent with the standard card PDF#35-0787 of Mo2C and the standard card PDF#42-1120 of Mo.
[0029] Figure 2 The image shown is a scanning electron microscope (SEM) image of a nitrogen-doped carbon-coated porous molybdenum-based heterostructure membrane prepared in Example 1. The SEM image shows that the membrane is in the form of nanorods, and a polydopamine coating layer can be clearly observed on the surface.
[0030] Figure 3 The image shows the physical properties of the molybdenum-based modified battery separator with a Mott-Schottky heterostructure prepared in Example 1. After the modified separator was folded and restored, the modified material did not fall off, which indicates that the modified separator has good physical properties.
[0031] Figure 4 The image shows the long-cycle performance of a lithium-sulfur battery assembled with the molybdenum-modified molybdenum-based heterostructure battery separator prepared in Example 1. The long-cycle performance of the lithium-sulfur battery assembled with the modified separator at 1 C shows an initial discharge specific capacity of 987.3 mAh g⁻¹. -1 It still maintains 561.6 mAh g after 1000 cycles. -1 The capacity decay rate per cycle is only 0.043%.
[0032] Figure 5The figure shows the rate performance of a lithium-sulfur battery assembled with the molybdenum-modified molybdenum-based heterostructure battery separator prepared in Example 1. The lithium-sulfur battery assembled with the modified separator exhibits excellent rate performance and reversibility. The discharge specific capacity reaches 1221.9 mAh g⁻¹ at 0.2, 0.5, 1, 2, 3, and 5 C, respectively. -1 993.0 mAh g -1 908.3 mAh g -1 815.7 mAh g -1 760.7 mAh g -1 686.7 mAh g -1 When the discharge temperature returns to 0.2 C, the specific capacity is still 985.8 mAh g. -1 It exhibits excellent redox reversibility.
[0033] Table 1 below shows the performance data of lithium-sulfur batteries assembled using the separators prepared in Comparative Examples 1 to 4: Table 1
[0034] Analysis of the results from Examples 1 and 2 shows that different annealing temperatures have a significant impact on the electrochemical performance of the prepared membrane materials. Furthermore, Example 1 exhibits an initial discharge specific capacity as high as 987.3 mAh g⁻¹ at a current density of 1C. -1 It still maintains a capacity of 561.6 mAh g after 1000 cycles. -1 The high discharge specific capacity, with a single-cycle capacity decay rate of only 0.043%, not only far exceeds all comparative examples but is also significantly better than Example 2 (0.054%), where the ratio of Mo and Mo2C components was adjusted by changing the annealing temperature to achieve the optimal ratio. This demonstrates that the coating source type and carbonization temperature provided by this invention jointly ensure the excellent structural integrity of the membrane material. Secondly, in terms of rate performance, Example 1 exhibits the highest or near-highest discharge specific capacity across the entire test current density range from 0.2C to 5C, especially maintaining 686.7 mAh g at 5C. -1 The discharge specific capacity of Example 1 (CNT membrane) is significantly lower than that of commercial CNT and PP membranes, which in stark contrast to Comparative Example 1 (CNT membrane) at 5C, exhibiting a lower discharge specific capacity (558.4 mAh g⁻¹). -1 Comparative Example 2 (polypropylene membrane) only showed 255.7 mAh g, while Comparative Example 2 (polypropylene membrane) only showed 255.7 mAh g. -1The extremely low discharge specific capacity reveals that the innovative nitrogen-doped carbon-coated heterojunction molybdenum-based separator of this invention has significant advantages over commercially available separators. As demonstrated in Example 1 and Comparative Examples 1 to 3, this application utilizes specific materials and specific steps to achieve the preparation of novel high-performance separator materials.
[0035] While embodiments of the present invention have been described in detail above, it will be apparent to those skilled in the art that various modifications and variations can be made to these embodiments. However, it should be understood that such modifications and variations fall within the scope and spirit of the invention as set forth in the claims. Furthermore, the invention described herein may have other embodiments and can be implemented or carried out in various ways.
Claims
1. A method for preparing a Mott-Schottky heterostructure modified battery separator, characterized in that, The preparation method includes: Step S1: Add ammonium molybdate tetrahydrate to a mixed solution of concentrated nitric acid and water, and stir thoroughly to obtain a mixed solution; Step S2: The mixed solution is transferred to a reaction vessel for hydrothermal reaction to obtain a first precipitate. The first precipitate is washed with ethanol and water to obtain the MoO3 precursor material. Step S3: Dissolve tris(hydroxymethyl)aminomethane in deionized water to obtain a buffer solution. Add the polymer monomer and the MoO3 precursor material to the buffer solution and stir thoroughly to obtain a second precipitate. Wash the second precipitate with ethanol and water to obtain polymer-coated MoO3 material. Step S4: Anneal the polymer-coated MoO3 material to obtain a nitrogen-doped carbon-coated porous mottled-Schottky heterostructure molybdenum-based material. Step S5: Mix the nitrogen-doped carbon-coated porous molybdenum-based heterostructure material with PVDF binder and add it to N-methylpyrrolidone solvent and stir evenly to form a slurry. Coat the slurry onto the surface of a commercial polypropylene separator to obtain a modified battery separator.
2. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, In step S1, the volume ratio of concentrated nitric acid to water is 1:6 to 6:1; the concentration of ammonium molybdate tetrahydrate is 0.01 to 0.1 mmol / mL.
3. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, In step S2, the temperature of the hydrothermal reaction is 100~200°C. o C, the reaction time is 6~24 h.
4. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, In step S3, the polymer monomer includes at least one of aniline and dopamine hydrochloride.
5. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, In step S3, the concentration of tris(hydroxymethyl)aminomethane is 0.005~0.02 mmol / mL, the mass ratio of the polymer monomer to the MoO3 precursor material is 1:4~4:1, and the stirring time is 6~24 h.
6. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, In step S4, the annealing atmosphere is at least one of N2 and Ar, and the annealing temperature is 600~1000℃. o C, heating rate is 1~5 o C / min, annealing time is 1~10 h.
7. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, In step S5, the coating thickness is 10~100 μm.
8. The method for preparing the Mott-Schottky heterostructure modified battery separator according to claim 1, characterized in that, The mass ratio of the motter-Schottky heterostructure molybdenum-based material to the PVDF binder is 180~220:21~25.
9. A Mott-Schottky heterostructure modified battery separator, characterized in that, It is prepared by the method of any one of claims 1-8 for the preparation of the Mott-Schottky heterostructure modified battery separator.
10. The application of the Mott-Schottky heterostructure modified battery separator as described in claim 9 in lithium-sulfur batteries.
Citation Information
Patent Citations
Preparation method and application of selenium-nitrogen co-doped carbon-loaded molybdenum-based lithium-sulfur battery diaphragm
CN119231090A