A method for in-situ polymerization modification of PP membrane

By modifying PP separators through in-situ polymerization, the problems of insufficient mechanical strength and conductivity of lithium-ion battery separators are solved, and lithium dendrites are effectively suppressed and battery performance is improved, making it suitable for mass production.

CN123121068APending Publication Date: 2026-11-17NINGBO UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510638471.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators suffer from low mechanical strength, weak electrical conductivity, and poor wettability, leading to uncontrolled lithium dendrite growth and posing safety hazards. Furthermore, traditional suppression measures are costly, complex, or ineffective.

Method used

An in-situ polymerization method for modifying PP separators involves mixing functional monomers, crosslinking agents, ionic liquids, and lithium salt solutions to form a precursor solution, which is then used to assemble batteries and react to form a modified PP separator, enhancing its mechanical properties and inhibiting lithium dendrite growth.

Benefits of technology

The modified PP separator can stably cycle 2000 times at 1C rate, with a discharge specific capacity of 109.8 mAh·g-1 and a capacity retention rate of 80.6%, while reducing costs and making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121068A_ABST
    Figure CN123121068A_ABST
Patent Text Reader

Abstract

This invention provides a method for in-situ polymerization modification of PP separators, comprising the following steps: a) mixing a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution to obtain a precursor solution; wherein the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; b) assembling a battery using the precursor solution obtained in step a), and after reaction, forming an in-situ polymerized modified PP separator, thereby obtaining a modified battery. Compared with the prior art, this invention selects specific raw materials and specific process steps to achieve better overall interaction. The modified PP separator has improved mechanical properties while inhibiting the growth of lithium dendrites. Furthermore, the method provided by this invention has low technical cost, simple process, and is suitable for large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium battery technology, and more specifically, to a method for in-situ polymerization modification of PP separators. Background Technology

[0002] The development of lithium-ion batteries (LIBs) stems from their outstanding performance in high energy density, long cycle life, and excellent storage characteristics, making them the primary conductive chemical energy storage technology for portable electronic devices and electric vehicles. However, their practical application faces significant challenges because the uneven deposition of lithium ions on the negative electrode surface, a phenomenon known as dendrite formation, raises safety concerns. These dendrites can breach the separator, causing direct contact between the negative and positive electrodes, leading to short circuits and posing a threat. Leakage of flammable liquid electrolytes under pressure, coupled with the inability of standard separators to resist dendrite penetration, often results in serious battery fires or explosions. Numerous measures have been proposed to suppress lithium dendrites. These include modifying the composition and properties of the electrolyte, such as using high-concentration lithium salts, adding specific additives, or employing solid-state electrolytes, which can inhibit dendrite growth and improve battery performance; or modifying the lithium battery separator to create a multifunctional separator that suppresses lithium dendrites, such as coating with alumina, silicon dioxide, or other metallic inorganic materials, or spraying the separator surface with poly(vinyl fluoride) or grafting organic polymers such as polybenzoyl diazole. However, traditional methods for suppressing lithium dendrites face several challenges, such as high raw material costs, uneven coating, excessive solvent consumption and waste, environmental pollution, and complex or ineffective polymer synthesis processes.

[0003] To suppress lithium dendrite formation and achieve long-life, high-safety lithium-ion batteries, in-situ polymerization technology for preparing polymer semi-solid lithium metal batteries has shown promising application prospects in recent years and may become the next generation of commercially viable lithium batteries. In-situ polymerization of lithium batteries refers to the process of directly polymerizing monomers into polymer electrolytes through chemical reactions inside the battery or on the electrode surface. This process typically utilizes external conditions such as light, heat, and electricity to initiate the polymerization reaction, allowing the monomers to form a uniform polymer electrolyte layer inside the battery. Precursors for in-situ polymerization usually include electrolytes, monomers, initiators, and crosslinking agents. However, traditional polymers suffer from problems such as increased interfacial impedance and low ionic conductivity. Therefore, in-situ polymerization usually places higher demands on lithium battery separators. Currently, commercially available polyolefin separators such as PP, PE, and PP / PE / PP suffer from low mechanical strength, weak conductivity, and poor wettability. Therefore, exploring precursors with high ionic conductivity and low impedance without altering the separator substrate is crucial for promoting the commercial application of in-situ polymerization technology. Summary of the Invention

[0004] In view of this, the purpose of the present invention is to provide a method for in-situ polymerization modification of PP separator, which has low technical cost, simple process and is suitable for large-scale production; and the modified PP separator has improved mechanical properties while inhibiting the growth of lithium dendrites.

[0005] This invention provides a method for in-situ polymerization modification of PP membranes, comprising the following steps:

[0006] a) A precursor solution is obtained by mixing a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution; wherein the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt.

[0007] b) The precursor solution obtained in step a) is used to assemble the battery. After reaction, an in-situ polymerized modified PP membrane is formed, and the modified battery is obtained.

[0008] Preferably, the functional monomer in step a) is selected from one or more of vinylene carbonate, methacrylic acid, ethylene glycol monomethacrylate, and N-(2-hydroxyethyl)acrylamide;

[0009] The crosslinking agent is selected from one or more of 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, and hexanediol dimethacrylate.

[0010] The initiator is selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide;

[0011] The lithium salt solution is a LiPF6 EC, EMC, and DMC solution.

[0012] Preferably, the volume ratio of EC, EMC, and DMC is 1:(0.5-1.5):(0.5-1.5).

[0013] Preferably, the concentration of the LiPF6 EC, EMC, and DMC solutions is 0.5M to 1.5M.

[0014] Preferably, the ratio of the amount of functional monomer, crosslinking agent, ionic liquid, initiator and lithium salt solution in step a) is (20-100 μL): (50-200 μL): (5-40 mg): (2-7 mg): (1500-2400 ml).

[0015] Preferably, the mixing method in step a) is stirring; the stirring time is 1h to 3h.

[0016] Preferably, the battery assembled in step b) is a lithium iron phosphate battery.

[0017] Preferably, after assembling the battery as described in step b), the method further includes:

[0018] Wipe the precursor solution off the surface of the assembled battery with alcohol.

[0019] Preferably, the reaction process described in step b) is carried out in an oven; the temperature of the oven is 50°C to 70°C.

[0020] Preferably, the reaction time in step b) is 4h to 6h.

[0021] This invention provides a method for in-situ polymerization modification of PP separators, comprising the following steps: a) mixing a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution to obtain a precursor solution; wherein the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; b) assembling a battery using the precursor solution obtained in step a), and after reaction, forming an in-situ polymerized modified PP separator, thereby obtaining a modified battery. Compared with the prior art, this invention selects specific raw materials and specific process steps to achieve better overall interaction. The modified PP separator has improved mechanical properties while inhibiting the growth of lithium dendrites. Furthermore, the method provided by this invention has low technical cost, simple process, and is suitable for large-scale production. Attached Figure Description

[0022] Figure 1 This is a SEM image of the PP membrane after impregnation with the precursor in Example 1 of the present invention.

[0023] Figure 2 This is a stress-strain diagram of the modified PP diaphragm in Example 1 of the present invention;

[0024] Figure 3 This is a cycle diagram of the lithium iron phosphate battery assembled in Example 1 of the present invention at a 1C rate.

[0025] Figure 4 The rate performance of the lithium iron phosphate battery assembled in Example 1 of this invention;

[0026] Figure 5 This is a SEM image of the PP membrane after impregnation with the precursor in Example 2 of the present invention.

[0027] Figure 6 This is a stress-strain diagram of the modified PP diaphragm in Example 2 of the present invention;

[0028] Figure 7 This is a cycle diagram of the lithium iron phosphate battery assembled in Example 2 of the present invention at a 1C rate.

[0029] Figure 8The rate performance of the lithium iron phosphate battery assembled in Example 2 of this invention;

[0030] Figure 9 This is a SEM image of the PP membrane after impregnation with the precursor in Example 3 of the present invention.

[0031] Figure 10 This is a stress-strain diagram of the modified PP diaphragm in Example 3 of the present invention;

[0032] Figure 11 This is a cycle diagram of the lithium iron phosphate battery assembled in Example 3 of the present invention at a 1C rate.

[0033] Figure 12 This refers to the rate performance of the lithium iron phosphate battery assembled in Example 3 of the present invention. Detailed Implementation

[0034] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0035] This invention provides a method for in-situ polymerization modification of PP membranes, comprising the following steps:

[0036] a) A precursor solution is obtained by mixing a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution; wherein the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt.

[0037] b) The precursor solution obtained in step a) is used to assemble the battery. After reaction, an in-situ polymerized modified PP membrane is formed, and the modified battery is obtained.

[0038] The present invention first mixes a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution to obtain a precursor solution. The present invention does not have any special restrictions on the source of the functional monomer, crosslinking agent, ionic liquid, initiator, and lithium salt solution, and commercially available products well known to those skilled in the art can be used.

[0039] In this invention, the functional monomer is preferably selected from one or more of vinylene carbonate, methacrylic acid, ethylene glycol monomethacrylate, and N-(2-hydroxyethyl)acrylamide, and more preferably vinylene carbonate; as a monomer containing unsaturated double bonds, it adapts to a specific ionic liquid in the presence of a specific crosslinking agent and initiator to realize the in-situ polymerization modified PP membrane of this invention.

[0040] In this invention, the crosslinking agent is preferably selected from one or more of 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, and hexanediol dimethacrylate, more preferably 1,4-butanediol diacrylate; the initiator is preferably selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide, more preferably azobisisobutyronitrile.

[0041] In this invention, the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, preferably 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; wherein, the functionalized ionic liquid 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide ionic liquid is shown in formula (I), and the 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide ionic liquid is shown in formula (II); specifically see the following structure:

[0042]

[0043] In this invention, the lithium salt solution is preferably a LiPF6 EC, EMC, and DMC solution; wherein the volume ratio of EC, EMC, and DMC is preferably 1:(0.5-1.5):(0.5-1.5), more preferably 1:1:1.

[0044] In this invention, the concentration of the LiPF6 EC, EMC, and DMC solutions is preferably 0.5M to 1.5M, more preferably 1M.

[0045] In this invention, the ratio of the amount of functional monomer, crosslinking agent, ionic liquid, initiator and lithium salt solution is (20-100 μL): (50-200 μL): (5-40 mg): (2-7 mg): (1500-2400 ml).

[0046] In this invention, the mixing method is preferably stirring; the stirring time is preferably 1 hour to 3 hours; and the mixing process is preferably as follows:

[0047] Weigh out a certain amount of functional monomer, crosslinking agent, initiator and ionic liquid, add them to an appropriate amount of lithium salt solution, and stir to form a homogeneous precursor solution.

[0048] After obtaining the precursor solution, the present invention uses the obtained precursor solution to assemble a battery, and after reaction, an in-situ polymerized modified PP membrane is formed, and the modified battery is obtained at the same time.

[0049] In this invention, the assembled battery is preferably a lithium iron phosphate battery; this invention does not impose any special restrictions on the assembled battery, and any technical solution of lithium iron phosphate battery well known to those skilled in the art can be used.

[0050] In this invention, after assembling the battery, it preferably further includes:

[0051] Wipe the precursor solution off the surface of the assembled battery with alcohol.

[0052] In this invention, the reaction process is preferably carried out in an oven, and a constant temperature oven well known to those skilled in the art can be used; the temperature of the oven is preferably 50℃~70℃, more preferably 60℃.

[0053] In this invention, the reaction time is preferably 4h to 6h, more preferably 5h.

[0054] This invention modifies the lithium iron phosphate battery separator through in-situ polymerization of PP membrane to prevent lithium dendrites from piercing the separator and affecting battery cycle life. Experimental results show that, under 1C rate conditions, the lithium iron phosphate battery can stably cycle for 2000 cycles with a discharge specific capacity of 109.8 mAh·g. -1 The capacity retention rate is 80.6%.

[0055] The present invention has the following beneficial effects:

[0056] In this invention, the carbon-carbon double bonds of the crosslinking agent effectively reduce the proportion of functional monomers (ethylene carbonate, methacrylic acid, etc.) in the precursor. In traditional in-situ polymerization, for example, VC can polymerize to form poly(ethylene carbonate) (PVCA) and be used as the main component of SEI. When the concentration of VC in the precursor is greater than 2 wt%, the battery internal resistance will increase significantly. However, the degree of polymerization of VC is low. During the charge-discharge cycle of the battery, the polymerization of the precursor will lead to an increase in the battery internal resistance, which will accelerate the consumption of VC. The performance degradation of the battery will accelerate with the extension of the cycle time, and lithium dendrites will grow uncontrollably, piercing the separator and causing battery failure. Ionic liquid (3-(3-aminopropyl)-1-vinyl) Imidazole bis(trifluoromethanesulfonyl)imide and 1-ethyl-3-methylimazole bis(trifluoromethanesulfonyl)imide contain abundant electronegative amino and fluorine bonds. As functionalized ionic liquids, they can increase the ionic conductivity of the polymerized system, thereby accelerating the migration of lithium ions between chain segments and reducing polarization. Furthermore, the linear monomers, acting as crosslinking agents, can effectively promote the compatibility between VC and lithium metal. The ester groups in the chain segments can make the crosslinked three-dimensional network more stable. The liquid precursor before polymerization can easily wet the PP separator and electrode, ensuring complete contact between the electrolyte, separator, and electrode after polymerization, forming a tight and stable interface, increasing the mechanical properties of the separator while inhibiting the growth of lithium dendrites. Experimental results show that after heating polymerization, the lithium iron phosphate battery can stably cycle 2000 times at 1C, with a discharge specific capacity of 109.8 mAh·g. -1 The capacity retention rate is 80.6%.

[0057] This invention provides a method for in-situ polymerization modification of PP separators, comprising the following steps: a) mixing a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution to obtain a precursor solution; wherein the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt; b) assembling a battery using the precursor solution obtained in step a), and after reaction, forming an in-situ polymerized modified PP separator, thereby obtaining a modified battery. Compared with the prior art, this invention selects specific raw materials and specific process steps to achieve better overall interaction. The modified PP separator has improved mechanical properties while inhibiting the growth of lithium dendrites. Furthermore, the method provided by this invention has low technical cost, simple process, and is suitable for large-scale production.

[0058] To further illustrate the present invention, the following embodiments are provided for detailed description. All raw materials used in the following embodiments of the present invention are commercially available.

[0059] Example 1

[0060] In a glove box, 2 mg of azobisisobutyronitrile (AIBN), 70 μL of 1,4-butanediol dipropylene glycol (BDDA), 6 mg of 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonate)imide ionic liquid (AVBI), and 20 μL of vinylene carbonate (VC) were added to 1500 ml (1 M LiPF6 dissolved in EC:EMC:DMC = 1:1:1 Vol%). After stirring for 2 h, an appropriate amount of the precursor solution prepared above was transferred to assemble a battery. After assembly, the precursor solution on the battery surface was wiped with alcohol. The battery was heated in a constant temperature oven at 60 °C for 5 hours to complete the in-situ polymerization modification of the PP separator, and the modified coin cell was obtained.

[0061] To observe the morphology of the polymer PP separator surface, the assembled battery was disassembled, the separator was removed, and the morphology of the separator surface was observed using a scanning electron microscope (SEM). Figure 1 The modified membrane was then subjected to stress-strain testing. Figure 2 The assembled lithium iron phosphate battery was subjected to charge-discharge cycle testing at a 1C rate. The lithium iron phosphate battery stably completed 2000 cycles, with a discharge specific capacity of 109.8 mAh·g. -1 The capacity retention rate is 80.6% ( Figure 3 Furthermore, its rate capability is significantly improved compared to the control group. Figure 4 ).

[0062] Example 2

[0063] In a glove box, 3 mg of azobisisobutyronitrile (AIBN), 100 μL of 1,4-butanediol dipropylene ester, 10 mg of 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonate) ionic liquid (AVBI), and 30 μL of vinylene carbonate were added to 1700 ml (1 M LiPF6 dissolved in EC:EMC:DMC = 1:1:1 Vol%). After stirring for 2 h, an appropriate amount of the precursor solution prepared above was transferred to assemble the battery. After assembly, the precursor solution on the battery surface was wiped with alcohol. The battery was heated in a constant temperature oven at 60 °C for 5 hours to complete the in-situ polymerization modification of the PP separator, and the modified coin cell was obtained.

[0064] The polymerized PP membrane was removed and subjected to SEM testing to observe the morphology of the membrane surface. Figure 5 And stress-strain tests were performed. Figure 6 Finally, the reassembled battery was subjected to charge-discharge cycle testing. Figures 7-8 ).

[0065] Example 3

[0066] In a glove box, 4 mg of azobisisobutyronitrile (AIBN), 150 μL of 1,4-butanediol dipropylene ester, 15 mg of 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonate)imide ionic liquid (AVBI), and 50 μL of vinylene carbonate were added to 2200 ml (1 M LiPF6 dissolved in EC:EMC:DMC = 1:1:1 Vol%). After stirring for 2 h, an appropriate amount of the precursor solution prepared above was transferred to assemble the battery. After assembly, the precursor solution on the battery surface was wiped with alcohol. The battery was heated in a constant temperature oven at 60 °C for 5 hours to complete the in-situ polymerization modification of the PP separator, and the modified coin cell was obtained.

[0067] The polymerized PP membrane was removed and subjected to SEM testing to observe the morphology of the membrane surface. Figure 9 And stress-strain tests were performed. Figure 10 Finally, the reassembled battery was subjected to charge-discharge cycle testing. Figures 11-12 ).

[0068] In summary, this invention provides a method for in-situ polymerization modification of PP separators, and discloses the modification process in detail. Specifically, it uses inexpensive vinylene carbonate, 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonate) ionic liquid, and 1,4-butanediol diacrylate as raw materials, combined with in-situ polymerization technology, to modify commercially available PP separators. The resulting lithium iron phosphate battery can stably cycle 2000 times, with a discharge specific capacity of 109.8 mAh·g. -1 The capacity retention rate is 80.6%; at the same time, the modification method provided by this invention is simple, low-cost, requires little equipment investment, and is suitable for mass production.

[0069] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for in-situ polymerization modification of PP membranes, characterized in that, Includes the following steps: a) A precursor solution is obtained by mixing a functional monomer, a crosslinking agent, an ionic liquid, an initiator, and a lithium salt solution; wherein the ionic liquid is 3-(3-aminopropyl)-1-vinylimidazolium bis(trifluoromethanesulfonyl)imide and / or 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt. b) The precursor solution obtained in step a) is used to assemble the battery. After reaction, an in-situ polymerized modified PP membrane is formed, and the modified battery is obtained.

2. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, The functional monomer mentioned in step a) is selected from one or more of vinylene carbonate, methacrylic acid, ethylene glycol monomethacrylate, and N-(2-hydroxyethyl)acrylamide; The crosslinking agent is selected from one or more of 1,4-butanediol diacrylate, ethylene glycol dimethacrylate, and hexanediol dimethacrylate. The initiator is selected from one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide; The lithium salt solution is a LiPF6 EC, EMC, and DMC solution.

3. The method for in-situ polymerization modification of PP separator according to claim 2, characterized in that, The volume ratio of EC, EMC, and DMC is 1:(0.5-1.5):(0.5-1.5).

4. The method for in-situ polymerization modification of PP separator according to claim 2, characterized in that, The concentrations of the LiPF6 EC, EMC, and DMC solutions are 0.5 M to 1.5 M.

5. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, In step a), the ratio of the amount of functional monomer, crosslinking agent, ionic liquid, initiator and lithium salt solution is (20-100 μL): (50-200 μL): (5-40 mg): (2-7 mg): (1500-2400 ml).

6. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, The mixing method described in step a) is stirring; the stirring time is 1h to 3h.

7. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, The battery assembled in step b) is a lithium iron phosphate battery.

8. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, After assembling the battery as described in step b), the process further includes: Wipe the precursor solution off the surface of the assembled battery with alcohol.

9. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, The reaction process described in step b) is carried out in an oven at a temperature of 50°C to 70°C.

10. The method for in-situ polymerization modification of PP separator according to claim 1, characterized in that, The reaction time described in step b) is 4 to 6 hours.