A fiber-ceramic composite lithium-ion battery separator, its preparation method, and the battery thereof.

By modifying the surface of organic fibers with amino-containing dendritic macromolecules in lithium-ion battery separators to form a bridging structure that combines with inorganic ceramic particles, the problems of coating peeling and low ion transport efficiency are solved, and the high-temperature stability and fast-charging performance are improved.

CN123121074APending Publication Date: 2026-11-17HEBEI GELLEC NEW ENERGY MATERIAL SCI&TECHNOLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611362010.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-03
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The coating of existing lithium-ion battery separators is prone to peeling and powdering at high temperatures, and the ion transport efficiency is low, making it difficult to meet the requirements of fast charging. The modification process is complex and costly.

Method used

The surface of organic fibers is modified with amino-containing dendritic macromolecules to form a bridging structure. Combined with inorganic ceramic particles and binders, a three-dimensional mesh support network is constructed to enhance the coating adhesion and construct lithium-ion transport pathways.

Benefits of technology

It improves the adhesion and ion transport efficiency of the coating, extends the cycle life of the separator, enhances battery safety and fast charging performance, and reduces battery impedance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123121074A_ABST
    Figure CN123121074A_ABST
Patent Text Reader

Abstract

This invention relates to the field of battery technology, and proposes a fiber-ceramic composite lithium-ion battery separator, its preparation method, and the battery thereof. The lithium-ion battery separator includes a base film and a coating disposed on at least one surface of the base film. The coating comprises organic fibers, inorganic ceramic particles, and a binder in a mass ratio of 3~25:20~70:3~20. The organic fibers are loaded with amino-containing dendritic macromolecules, which form an interface modification layer on the surface of the organic fibers. The organic fibers are distributed in a three-dimensional network within the coating, and the amino-containing dendritic macromolecules form a bridging structure between the organic fibers and the inorganic ceramic particles. The mass ratio of organic fibers to amino-containing dendritic macromolecules is 100:0.5~15, and the algebraic number of the amino-containing dendritic macromolecules ranges from 1 to 3. Through this technical solution, the internal bonding strength and electrochemical performance of the lithium-ion battery separator coating are simultaneously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, specifically to a fiber ceramic composite lithium-ion battery separator, its preparation method, and the battery thereof. Background Technology

[0002] With the rapid development of new energy vehicles and energy storage systems, the market has placed higher demands on the energy density, safety, and fast-charging performance of lithium-ion batteries. As a key component of the battery, the separator's thermal stability and ion conductivity directly affect the overall battery performance. To improve the heat resistance of the separator, the industry commonly employs a technique of coating the surface of a polyolefin-based membrane with a mixture of inorganic particles and heat-resistant fibers. However, this technique still has its shortcomings.

[0003] First, heat-resistant fibers (such as aramid fibers and polyimide fibers) have strong surface chemical inertness and poor interfacial compatibility with inorganic particles and binders. This leads to insufficient internal adhesion of the coating. Under long-term cyclic use or high-temperature operating conditions, the coating is prone to peeling and powdering, which not only weakens the mechanical integrity of the separator but may also cause internal short circuits.

[0004] Secondly, in traditional coating structures, there is a lack of effective ion transport synergy between inorganic particles and heat-resistant fibers, and the coating often becomes an obstacle layer for lithium-ion migration. Especially during high-rate charge and discharge processes, ion transport efficiency is limited, leading to increased battery polarization and accelerated capacity decay, making it difficult to meet the requirements of fast charging applications.

[0005] Third, existing modification methods are difficult to simultaneously achieve synergistic optimization of interface strengthening and ion conduction functions, and the modification process is complex and has high manufacturing costs, which is not conducive to large-scale promotion.

[0006] Therefore, there is an urgent need to develop a membrane coating technology that can simultaneously enhance the internal bonding of the coating, construct efficient lithium-ion transport channels, and improve electrochemical performance, so as to break through the current technical bottlenecks in the development of high-performance lithium-ion batteries. Summary of the Invention

[0007] This invention proposes a fiber-ceramic composite lithium-ion battery separator, its preparation method, and the battery thereof. This lithium-ion battery separator can simultaneously improve the internal adhesion of the coating and its electrochemical performance.

[0008] The technical solution of the present invention is as follows: This invention proposes a fiber-ceramic composite lithium-ion battery separator, comprising a base film and a coating disposed on at least one surface of the base film, wherein the coating comprises organic fibers, inorganic ceramic particles and a binder in a mass ratio of 3~25:20~70:3~20; The surface of the organic fiber is loaded with amino-containing dendritic macromolecules, which form an interface modification layer on the surface of the organic fiber. The amino-containing dendritic macromolecules include a first terminal amino group, which serves as a lithium ion coordination site. The organic fiber is distributed in a three-dimensional network in the coating, and the amino-containing dendritic macromolecules form a bridging structure between the organic fiber and the inorganic ceramic particles. The mass ratio of the organic fiber to the amino-containing dendritic macromolecules is 100:0.5~15, and the algebraic range of the amino-containing dendritic macromolecules is 1~3.

[0009] Preferably, the length L and diameter D1 of the organic fiber and the median particle size D50 of the inorganic ceramic particles satisfy the following condition: 0.05 nm. -1 ≤L / (D1×D50)≤0.1nm -1 ; Where L is 30~50μm, D1 is 300~500nm, and D50 is 1~2μm.

[0010] Preferably, the amino-containing dendritic macromolecule further includes a second terminal amino group, which is cross-linked by a cross-linking agent to form a three-dimensional cross-linked network; The mass ratio of the amino-containing dendritic macromolecule to the crosslinking agent is 100:0.05~2.

[0011] Preferably, the crosslinking agent includes at least one of glutaraldehyde, epichlorohydrin, genipin, and polyisocyanate.

[0012] Preferably, the organic fiber includes at least one of polyimide fiber, aramid fiber, polyphenylene sulfide fiber, and polytetrafluoroethylene fiber.

[0013] Preferably, the amino-containing dendritic macromolecule includes at least one of polyamide-amine dendritic macromolecule, polypropylene imine dendritic macromolecule, and lysine dendritic macromolecule.

[0014] Preferably, the inorganic ceramic particles include at least one of alumina, silicon dioxide, boehmite, titanium dioxide, and barium sulfate.

[0015] Preferably, the adhesive comprises at least one of acrylate copolymers, vinylidene fluoride copolymers, aramid nanofibers, polyvinyl alcohol, and waterborne polyurethane.

[0016] This invention also proposes a method for preparing a fiber-ceramic composite lithium-ion battery separator, comprising: The organic fibers are immersed in a solution containing amino dendritic macromolecules, mixed evenly, and dried to obtain modified organic fibers. The modified organic fibers, inorganic ceramic particles, binder, and dispersion medium are mixed evenly to obtain a slurry; The slurry is coated onto at least one surface of the base film and dried to obtain the lithium-ion battery separator.

[0017] The present invention also proposes a battery comprising the lithium-ion battery separator described above or the lithium-ion battery separator prepared by the preparation method described above.

[0018] The beneficial effects of this invention are as follows: This invention utilizes amino-containing dendritic macromolecules to functionalize the interface of organic fibers, forming a bridging structure between the organic fibers and inorganic ceramic particles. This improves the affinity between the organic fibers, inorganic ceramic particles, and binders, and inhibits coating powdering and flaking. Furthermore, some terminal amino groups of the amino-containing dendritic macromolecules act as lithium-ion coordination sites, constructing additional ion transport pathways within the coating and reducing ion migration impedance. The three-dimensional network distribution of organic fibers in the coating forms a continuous and interconnected supporting framework, ensuring electrolyte wetting and mass transfer while maintaining porosity and permeability. Crucially, this invention limits the generation range of the amino-containing dendritic macromolecules to 1-3. This range balances steric hindrance and active site density: too low a generation results in insufficient terminal amino group density and limited bridging and coordination effects; too high a generation leads to thicker branched layers and increased steric hindrance, hindering the diffusion and spread of amino-containing dendritic macromolecules to the organic fiber surface and pores, thus weakening interfacial bonding and ion transport. In addition, the mass ratio of organic fibers to amino-containing dendritic macromolecules is limited to 100:0.5~15, so that the loading of the interface modification layer is appropriate. On the one hand, it ensures sufficient bridging and coordination sites to guarantee the interface modification effect; on the other hand, it avoids excessive loading that would cause the slurry flow deformation to deteriorate and easily stack and block the pores, thereby achieving a simultaneous improvement in the internal bonding force and electrochemical performance of the coating. Attached Figure Description

[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0020] Figure 1 Here is a SEM image of the nanofiber membrane in Example 1; Figure 2 Here is an SEM image of the polyimide short-cut fibers in Example 1; Figure 3 This is a SEM image of the coating of the lithium-ion battery separator in Example 1. Detailed Implementation

[0021] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments. Various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0022] To make the objectives, technical solutions, and advantages of this invention clearer, specific implementation schemes will be described below.

[0023] A specific embodiment of the first aspect of the present invention provides a fiber-ceramic composite lithium-ion battery separator, the lithium-ion battery separator comprising a base membrane and a coating disposed on at least one surface of the base membrane. The base membrane may be selected from commonly used base membranes in the art, such as, but not limited to, polyethylene microporous membranes, polypropylene microporous membranes, and nonwoven fabrics. The coating has a thickness of 1~10 μm and comprises organic fibers, inorganic ceramic particles, and a binder in a mass ratio of 3~25:20~70:3~20.

[0024] Organic fibers form a uniformly distributed, continuous, three-dimensional support network within the coating, providing full-dimensional structural support for the lithium-ion battery separator. This three-dimensional support network enhances the electrolyte adsorption and retention capacity of the lithium-ion battery separator, prolongs electrolyte retention time, and improves interfacial stability during cycling. Simultaneously, it effectively disperses external stress, improves the coating's resistance to bending and impact, and reduces the risk of structural damage to the lithium-ion battery separator during cell assembly and charge-discharge cycles. The organic fibers can be selected from commonly used organic fibers in the field, such as, but not limited to, at least one of polyimide fibers, aramid fibers, polyphenylene sulfide fibers, and polytetrafluoroethylene fibers. Preferably, it is polyimide fiber, which combines excellent heat resistance and mechanical strength. Polyimide fibers themselves possess excellent intrinsic heat resistance due to their aromatic backbone, high glass transition temperature, and no melting deformation at high temperatures. The continuous three-dimensional rigid skeleton constructed by these fibers can form a full-range heat-resistant constraint network within the coating, effectively suppressing the high-temperature thermal shrinkage behavior of the polymer base film and the coating, and improving the thermal dimensional stability of the lithium-ion battery separator. Even at temperatures above 180°C, the three-dimensional skeleton of polyimide fibers maintains its intact structural morphology, preventing short circuits caused by direct contact between the positive and negative electrodes due to thermal shrinkage of the lithium-ion battery separator, thus providing reliable heat-resistant safety protection for the battery. Polyimide fibers can be produced by using aromatic dianhydrides and diamines as monomers, preparing polyamic acid precursors through polycondensation reactions, and then processing them through electrospinning, high-temperature sintering, and imidization.

[0025] The surface of organic fibers is loaded with amino-containing dendritic macromolecules, which can be fixed to the surface of organic fibers through physical adsorption and / or chemical bonding. Firstly, the amino-containing dendritic macromolecules form an interface modification layer on the surface of the organic fibers. The active amino groups enriched on the surface of the amino-containing dendritic macromolecules can form a systematic molecular bonding network at the three-phase interface of organic fibers, inorganic ceramic particles, and binders. Specifically, they form strong hydrogen bonds and chemical bonds with the hydroxyl sites on the surface of inorganic ceramic particles, generate intermolecular entanglement and dipole interactions with the polar groups in the binder molecular chains, and simultaneously form an anchoring effect with the functional groups on the surface of organic fibers, completely breaking the weak interface limitation of traditional coatings that rely solely on van der Waals forces. The bridging structure formed by the amino-containing dendritic macromolecules between the organic fibers and inorganic ceramic particles can improve the peel strength and structural integrity of the coating, effectively resisting interface damage caused by electrode volume deformation and electrolyte swelling and erosion during battery cycling. This fundamentally inhibits coating powdering, cracking, and peeling failure behaviors, significantly extending the cycle life of the separator. Secondly, the specific coordination of the terminal amino groups of amino-containing dendritic macromolecules with lithium ions can construct a skip-type ion transport pathway within the pores of the lithium-ion battery separator, distinct from traditional liquid-phase diffusion. The lone pair electrons of the nitrogen atoms in the amino groups can form a dynamic and reversible coordination-decoupling interaction with lithium ions, providing continuous low-barrier transport sites for lithium ions. Simultaneously, it can anchor free anions in the electrolyte, reducing concentration polarization caused by anion migration, effectively increasing the lithium-ion transport number, and significantly reducing the bulk and interfacial impedance of the lithium-ion battery separator. Thirdly, the highly branched structure of the dendritic macromolecules avoids the defect of linear polymers easily entangled and clogging the separator pores. While achieving functional modification, it can fully preserve the porosity and permeability of the lithium-ion battery separator, ensuring rapid electrolyte wetting and mass transfer efficiency. The mass ratio of organic fibers to amino-containing dendritic macromolecules is 100:0.5~15, including but not limited to any ratio or a range between two ratios of 100:0.5, 100:1, 100:5, 100:10, and 100:15. Within this range, the loading of amino-containing dendritic macromolecules is moderate, ensuring sufficient bridging and coordination sites to guarantee the interface modification effect, while avoiding excessive loading that could lead to deterioration of slurry flow deformation and easy stacking and pore blockage. The algebraic number of the amino-containing dendritic macromolecules is in the range of 1~3, including but not limited to any value of 1, 2, or 3. This algebraic number range can balance steric hindrance and active site density, avoiding both excessively low algebraic number leading to limited bridging and coordination effects, and excessively high algebraic number leading to thickened branched layers and increased steric hindrance, which would hinder the diffusion and spread of amino-containing dendritic macromolecules to the surface and pores of organic fibers, thereby weakening interfacial bonding and ion transport. The amino-containing dendritic macromolecules include at least one of polyamide-amine dendritic macromolecules, polypropyleneimine dendritic macromolecules, and lysine dendritic macromolecules, preferably polyamide-amine dendritic macromolecules.

[0026] Inorganic ceramic particles can synergistically construct coating reinforcement systems with organic fibers: organic fibers form a mesh-like framework, while inorganic ceramic particles are uniformly embedded and bridged at the interface by amino-containing dendritic macromolecules. The two form a rigid network, synergistically enhancing the internal adhesion of the coating. Furthermore, the high heat resistance of inorganic ceramic particles inhibits high-temperature thermal shrinkage, complementing the flexible framework of organic fibers and ensuring structural integrity and thermal safety under extreme temperatures. In addition, the synergy between inorganic ceramic particles and organic fibers can also improve porosity and electrolyte wettability, achieving gains in heat resistance, mechanical properties, and ion mass transfer. The inorganic ceramic particles can be selected from commonly used inorganic ceramic particles in the field, such as, but not limited to, at least one of alumina, silica, boehmite, titanium dioxide, and barium sulfate.

[0027] The binder bonds inorganic ceramic particles and organic fibers to the base film, enhancing the coating's cohesive strength and adhesion, inhibiting powdering and detachment, and complementing the three-dimensional skeleton of the organic fibers and the rigid network of the inorganic ceramic particles to maintain the stability of the wetting interface, achieving a simultaneous improvement in the coating's internal bonding strength and electrochemical performance. The binder can be selected from commonly used binders in the art, including but not limited to at least one of acrylate copolymers, vinylidene fluoride copolymers, aramid nanofibers, polyvinyl alcohol, and waterborne polyurethane.

[0028] In one embodiment of the present invention, the length L and diameter D1 of the organic fiber and the median particle size D50 of the inorganic ceramic particles satisfy 0.05 nm. -1 ≤L / (D1×D50)≤0.1nm -1 Wherein, L is 30~50μm, for example, including but not limited to any one value among 30μm, 35μm, 40μm, 45μm, 50μm and the range between two values; D1 is 300~500nm, for example, including but not limited to any one value among 300nm, 350nm, 400nm, 450nm, 500nm and the range between two values; D50 is 1~2μm, for example, including but not limited to any one value among 1μm, 1.2μm, 1.5μm, 1.8μm, 2μm and the range between two values.

[0029] In this invention, when the length L and diameter D1 of the organic fiber and the median particle size D50 of the inorganic ceramic particles satisfy the above-mentioned relationship, the internal bonding force and electrochemical performance of the coating can be further improved. If the ratio is greater than this range (the inorganic ceramic particles are too small or the organic fibers are too long), the inorganic ceramic particles are difficult to fill the bridging gaps, resulting in insufficient support and heat resistance, and the organic fibers are prone to agglomeration; if it is less than this range (the inorganic ceramic particles are too large), the inorganic ceramic particles are difficult to embed into the network, resulting in insufficient bridging and uncontrolled porosity, and the continuity and uniformity of the organic fiber-inorganic ceramic particle reinforced system decrease. Moreover, when the organic fiber meets the above-mentioned length and diameter range, the nanometer diameter gives the organic fiber a high specific surface area, and the micrometer length ensures that the organic fibers overlap and interpenetrate, which avoids the lack of a continuous skeleton in short fibers and solves the problems of agglomeration and uneven dispersion of long fibers.

[0030] In one embodiment of the present invention, some terminal amino groups of the amino-containing dendritic macromolecules are cross-linked by a cross-linking agent to form a three-dimensional cross-linked network. This can further ensure the stability of the interface modification layer and further improve the internal adhesion and electrochemical performance of the coating. The mass ratio of the amino-containing dendritic macromolecules to the cross-linking agent is 100:0.05~2, for example, including but not limited to any ratio or a range between two ratios of 100:0.05, 100:1, 100:1.2, 100:1.5, 100:1.8, and 100:2. Within this range, the stability of the three-dimensional cross-linked network can be guaranteed, while avoiding excessive cross-linking that would lead to a decrease in flexibility. The cross-linking agent can be selected from commonly used cross-linking agents in the art, for example, including but not limited to at least one of glutaraldehyde, epichlorohydrin, genipin, and polyisocyanates.

[0031] A second aspect of the present invention provides a method for preparing a fiber-ceramic composite lithium-ion battery separator, used to prepare the lithium-ion battery separator provided in the first aspect of the present invention, comprising the following steps: S1. Organic fibers are immersed in a solution containing amino dendritic macromolecules, mixed evenly, and dried to obtain modified organic fibers; S2. Mix the modified organic fibers, inorganic ceramic particles, binder, and dispersion medium evenly to obtain a slurry; S3. Coat the slurry onto at least one surface of the base film and dry it to obtain a lithium-ion battery separator.

[0032] In step S1 of this invention, the organic fibers can be subjected to surface activation treatments such as plasma treatment, alkaline etching, acid oxidation, or ultraviolet ozone treatment. The concentration of the amino-containing dendritic macromolecule solution is controlled at 1wt%~15wt%. During mixing, ultrasonic dispersion, mechanical stirring, or ball milling can be used, and the mixing time is preferably 10~120 min. The obtained modified organic fibers can be crosslinked. The crosslinking treatment can be carried out by steam fumigation, impregnation, or spraying. When steam fumigation is used, the fumigation time is 10~90 min, and the fumigation temperature is room temperature to 80℃.

[0033] In step S2 of this invention, the dispersion medium can be selected from commonly used dispersion media in the art, such as, but not limited to, at least one of water, N-methylpyrrolidone, ethanol, and isopropanol. A thickener can be added during the preparation of the slurry to adjust the viscosity. The thickener can be selected from commonly used thickeners in the art, such as, but not limited to, at least one of sodium carboxymethyl cellulose, xanthan gum, or sodium alginate. The solid content of the obtained slurry is controlled between 20 wt% and 60 wt%.

[0034] A specific embodiment of the third aspect of the present invention provides a battery, including a lithium-ion battery separator provided by the specific embodiment of the first aspect of the present invention or a lithium-ion battery separator prepared by the preparation method provided by the specific embodiment of the second aspect of the present invention.

[0035] In this invention, the battery can be a pouch battery, a square aluminum-cased battery, or a cylindrical battery. During battery operation, the terminal amino groups of the amino-containing dendritic macromolecules form a reversible coordination-dissociation dynamic equilibrium with lithium ions in the electrolyte, thereby improving the battery's rate performance and cycle life while ensuring high safety.

[0036] The present invention will now be described in detail with reference to preferred embodiments and comparative examples. The preferred embodiments of the invention described below can be modified in various ways, and therefore the scope of the invention should not be construed as limited to the preferred embodiments described in detail below. Preferred embodiments are provided to help those skilled in the art to more readily understand the invention.

[0037] In the following examples and comparative examples, the polyamide-amine dendrimer has ethylenediamine as its core, the polypropyleneimine dendrimer has 1,4-diaminobutane as its core, and the lysine dendrimer has lysine as its core.

[0038] Example 1 A method for preparing a fiber-ceramic composite lithium-ion battery separator includes the following steps: S1. Polyimide chopped fibers are immersed in a methanol solution of polyamide-amine dendritic macromolecules (the solute polyamide-amine dendritic macromolecules have an algebraic number of 1) and ultrasonically dispersed at room temperature (ultrasonic frequency of 40kHz, power of 200W, time of 30min). The ultrasonic cavitation effect allows the polyamide-amine dendritic macromolecules to overcome steric hindrance and penetrate into the microporous structure on the surface of the polyimide chopped fibers. They are then tightly adsorbed through electrostatic interaction and hydrogen bonding. The fibers are then dried in a vacuum drying oven at 80℃ for 2h to obtain modified polyimide chopped fibers. The mass ratio of polyimide chopped fibers to polyamide-amine dendritic macromolecules in the modified polyimide chopped fibers is 100:0.5. The preparation method of polyimide chopped fibers is as follows: using pyromellitic dianhydride (PMDA) and 4,4'-diaminodiphenyl ether (ODA) in a molar ratio of 1:1 as monomers, a polyimide acid (PAA) solution with a solid content of 15 wt% is synthesized by polycondensation reaction in N,N-dimethylacetamide (DMAc) solvent. The polyimide acid solution is then used to prepare nanofiber membranes by electrospinning, and its SEM image is shown below. Figure 1 As shown, the spinning voltage was set to 18kV, the receiving distance to 15cm, and the injection rate to 0.8mL / h. Subsequently, the obtained polyimide nanofiber membrane was placed in a high-temperature oven for gradient thermal imidization treatment under the following conditions: 80℃ for 1h, 150℃ for 1h, 250℃ for 1h, and 300℃ for 0.5h, thus obtaining a fully imidized polyimide (PI) nanofiber membrane. The polyimide nanofiber membrane was then chopped using a high-speed pulverizer, and after sieving, chopped polyimide fibers with a length of 30μm and a diameter of 500nm (weight-average molecular weight of 100,000) were obtained. Their SEM images are shown below. Figure 2 As shown; S2. Add the modified polyimide chopped fibers to water and disperse them at 2000 rpm for 30 min using a high-speed disperser. Then add alumina (median particle size of 0.7 μm) and premix by stirring at 1500 rpm for 30 min. Then transfer the mixture to a sand mill for wet grinding. Use 0.3 mm zirconia beads as the grinding media, with a linear velocity of 10 m / s and a grinding time of 45 min. Then add an acrylate water-based binder (model HSA-6280) and stir at 800 rpm for 30 min. Adjust the slurry viscosity to 2500 mPa·s (measured with a Brookfield viscometer, rotor No. 6, 20 rpm). Finally, filter the mixture through a 200-mesh filter to obtain a slurry with a solid content of 45 wt%. The mass ratio of polyimide chopped fibers, alumina, and acrylate water-based binder in the modified polyimide chopped fibers is 3:20:3. S3. A 9μm thick polyethylene microporous membrane (air permeability 85s / 100mL, porosity 55%) was selected as the base membrane. A microgravure coating process was used to coat the above slurry onto both sides of the base membrane at a coating speed of 30m / min. After coating, the membrane was sequentially dried at 60℃ for 1min, 70℃ for 1min, and 80℃ for 1min. The resulting lithium-ion battery separator had a single-sided coating thickness of 2μm. The SEM image of the coating is shown below. Figure 3 As shown.

[0039] Example 2 The only difference between this embodiment and Embodiment 1 is that in this embodiment, the algebra number of the polyamide-amine dendritic macromolecule is 2.

[0040] Example 3 The only difference between this embodiment and Embodiment 1 is that in this embodiment, the generation number of the polyamide-amine dendritic macromolecule is 3.

[0041] Example 4 The only difference between this embodiment and Example 1 is that in this embodiment, the mass ratio of polyimide chopped fibers to polyamide-amine dendritic macromolecules in the modified polyimide chopped fibers is 100:10.

[0042] Example 5 The only difference between this embodiment and Example 1 is that in this embodiment, the mass ratio of polyimide chopped fibers to polyamide-amine dendritic macromolecules in the modified polyimide chopped fibers is 100:15.

[0043] Example 6 The only difference between this embodiment and Embodiment 1 is that, in this embodiment, the mass ratio of polyimide chopped fibers, alumina, and acrylate waterborne binder in the modified polyimide chopped fibers is 25:70:20.

[0044] Example 7 The only difference between this embodiment and Embodiment 1 is that in this embodiment, the length of the polyimide chopped fibers is 30 μm and the diameter is 300 nm; the median particle size of the alumina is 1 μm.

[0045] Example 8 The only difference between this embodiment and Embodiment 1 is that in this embodiment, the length of the polyimide chopped fiber is 50 μm and the diameter is 500 nm; the median particle size of the alumina is 2 μm.

[0046] Example 9 The only difference between this embodiment and Embodiment 7 is that, in this embodiment, the median particle size of alumina is 0.5 μm.

[0047] Example 10 The only difference between this embodiment and Embodiment 7 is that, in this embodiment, the median particle size of alumina is 2.5 μm.

[0048] Example 11 The only difference between this embodiment and Embodiment 7 is that in this embodiment, the length of the polyimide chopped fibers is 15 μm and the diameter is 300 nm; the median particle size of the alumina is 0.5 μm.

[0049] Example 12 The only difference between this embodiment and Embodiment 7 is that in this embodiment, the length of the polyimide chopped fibers is 90 μm and the diameter is 300 nm; the median particle size of the alumina is 3 μm.

[0050] Example 13 The only difference between this embodiment and Example 1 is that in this embodiment, the modified polyimide chopped fibers are cross-linked. Specifically, the modified polyimide chopped fibers are placed in a sealed container, and an open vessel containing an aqueous solution of glutaraldehyde is placed at the bottom of the container. The mixture is then fumigated at a constant temperature of 60°C, so that the mass ratio of polyamide-amine dendritic macromolecules to glutaraldehyde in the modified polyimide chopped fibers is 100:0.5.

[0051] Example 14 The only difference between this embodiment and Example 13 is that, in this embodiment, the crosslinking method is as follows: the modified polyimide chopped fibers are impregnated in an epichlorohydrin solution at 50°C, so that the mass ratio of the polyamide-amine dendritic macromolecules in the modified polyimide chopped fibers to epichlorohydrin is 100:0.2.

[0052] Example 15 The only difference between this embodiment and Example 13 is that, in this embodiment, the mass ratio of polyamide-amine dendritic macromolecules to glutaraldehyde in the modified polyimide chopped fibers is 100:0.05.

[0053] Example 16 The only difference between this embodiment and Embodiment 13 is that, in this embodiment, the mass ratio of polyamide-amine dendritic macromolecules to glutaraldehyde in the modified polyimide chopped fibers is 100:2.

[0054] Example 17 The only difference between this embodiment and Example 13 is that, in this embodiment, the mass ratio of polyamide-amine dendritic macromolecules to glutaraldehyde in the modified polyimide chopped fibers is 100:0.01.

[0055] Example 18 The only difference between this embodiment and Example 13 is that, in this embodiment, the mass ratio of polyamide-amine dendritic macromolecules to glutaraldehyde in the modified polyimide chopped fibers is 100:0.25.

[0056] Example 19 The only difference between this embodiment and embodiment 13 is that, in this embodiment, after the polyimide nanofiber membrane is cut short to obtain polyimide short fibers, the polyimide short fibers are subjected to plasma surface activation treatment. Specifically, the polyimide short fibers are placed in an oxygen plasma cleaner with a power set to 100W and a treatment time of 5 minutes.

[0057] Example 20 The difference between this embodiment and Embodiment 19 is only that in this embodiment, step S2 is as follows: sodium carboxymethyl cellulose is added to water to obtain a thickener solution. Modified polyimide chopped fibers are added to the thickener solution and dispersed using a high-speed disperser at 2000 rpm for 30 minutes. Then, alumina (median particle size of 0.7 μm) is added and premixed by stirring at 1500 rpm for 30 minutes. The mixture is then transferred to a sand mill for wet grinding. The grinding media is 0.3 mm zirconia beads, and the linear velocity is 10 m / s. After 45 minutes, add the acrylate water-based binder (model HSA-6280) and stir at 800 rpm for 30 minutes. Adjust the slurry viscosity to 2500 mPa·s (measured with a Brookfield viscometer, rotor No. 6, 20 rpm). Finally, filter through a 200-mesh filter to obtain a slurry with a solid content of 45 wt%. The mass ratio of polyimide chopped fibers, alumina, acrylate water-based binder and sodium carboxymethyl cellulose in the modified polyimide chopped fibers is 3:20:3:0.75.

[0058] Example 21 The only difference between this embodiment and Embodiment 1 is that, in this embodiment, the polyimide chopped fibers are replaced with an equal amount of aramid fibers (model aramid 1313 fiber) of equal length and diameter, the polyamide-amine dendritic macromolecules are replaced with an equal amount of polypropyleneimide dendritic macromolecules (generation 2), the alumina is replaced with an equal amount of silica with equal median particle size, and the acrylate waterborne adhesive (model HSA-6280) is replaced with an equal amount of polyvinyl alcohol (model PVA-1788).

[0059] Example 22 The only difference between this embodiment and Embodiment 1 is that, in this embodiment, the polyimide chopped fibers are replaced with an equal amount of polyphenylene sulfide fibers (weight-average molecular weight of 50,000) of the same length and diameter; the polyamide-amine dendritic macromolecules are replaced with an equal amount of lysine dendritic macromolecules (generation number 2); the alumina is replaced with an equal amount of boehmite of the same median particle size; and the acrylate waterborne adhesive (model HSA-6280) is replaced with an equal amount of waterborne polyurethane (model R-5670 waterborne polyurethane, Ruijie Automotive Materials (Guangzhou) Co., Ltd.).

[0060] Comparative Example 1 The only difference between this comparative example and Example 1 is that the generation number of the polyamide-amine dendritic macromolecule in this comparative example is 0.

[0061] Comparative Example 2 The only difference between this comparative example and Example 1 is that the polyamide-amine dendritic macromolecule in this comparative example has an algebra number of 4.

[0062] Comparative Example 3 The only difference between this comparative example and Example 1 is that, in this comparative example, the mass ratio of polyimide chopped fibers to polyamide-amine dendritic macromolecules in the modified polyimide chopped fibers is 100:0.1.

[0063] Comparative Example 4 The only difference between this comparative example and Example 1 is that in this comparative example, the mass ratio of polyimide chopped fibers to polyamide-amine dendritic macromolecules in the modified polyimide chopped fibers is 100:20.

[0064] Comparative Example 5 The only difference between this comparative example and Example 1 is that in this comparative example, the polyimide chopped fibers were not modified with polyamide-amine dendritic macromolecules, and in step S2, the modified polyimide chopped fibers were replaced with an equal amount of polyimide chopped fibers.

[0065] Comparative Example 6 A method for preparing a fiber-ceramic composite lithium-ion battery separator includes the following steps: S1. Add polyimide chopped fibers (30μm in length and 500nm in diameter) to water and disperse them at 2000rpm for 30min using a high-speed disperser. Then add alumina (median particle size 0.7μm) and premix at 1500rpm for 30min. Then transfer to a sand mill for wet grinding. Use 0.3mm zirconia beads as the grinding media, with a linear velocity of 10m / s and a grinding time of 45min. Then add acrylate water-based binder (model HSA-6280) and polyamide-amine dendritic macromolecules and stir at 800rpm for 30min. Adjust the slurry viscosity to 2500mPa·s (Brookfield viscometer, rotor No. 6, 20rpm). Finally, filter through a 200-mesh filter to obtain a slurry with a solid content of 45wt%. The mass ratio of polyimide chopped fibers, alumina, acrylate water-based binder and polyamide-amine dendritic macromolecules is 3:20:3:0.15. S3. A polyethylene microporous membrane with a thickness of 9 μm (air permeability of 85 s / 100 mL and porosity of 55%) was selected as the base membrane. The above slurry was coated on both sides of the base membrane using a microgravure coating process at a coating speed of 30 m / min. After coating, the membrane was dried at 60℃ for 1 min, 70℃ for 1 min, and 80℃ for 1 min, respectively. After drying, a lithium-ion battery separator was obtained with a single-sided coating thickness of 2 μm.

[0066] Comparative Example 7 A method for preparing a fiber-ceramic composite lithium-ion battery separator includes the following steps: S1. Alumina (median particle size of 0.7 μm) was immersed in a methanol solution of polyamide-amine dendritic macromolecules (the solute polyamide-amine dendritic macromolecules had an algebraic number of 1), and ultrasonically dispersed at room temperature (ultrasonic frequency of 40 kHz, power of 200 W, time of 30 min). Then it was placed in a vacuum drying oven at 80 ℃ and dried for 2 h to obtain modified alumina. In the modified alumina, the mass ratio of alumina to polyamide-amine dendritic macromolecules was 20:0.15. S2. Add the modified alumina to water and disperse it at 2000 rpm for 30 min using a high-speed disperser. Then add polyimide short-cut fibers (30 μm in length and 500 nm in diameter) and premix at 1500 rpm for 30 min. Then transfer it to a sand mill for wet grinding. Use 0.3 mm zirconia beads as the grinding media, with a linear velocity of 10 m / s and a grinding time of 45 min. Then add an acrylic water-based binder (model HSA-6280) and stir at 800 rpm for 30 min. Adjust the slurry viscosity to 2500 mPa·s (measured with a Brookfield viscometer, rotor No. 6, 20 rpm). Finally, filter through a 200-mesh filter to obtain a slurry with a solid content of 45 wt%. The mass ratio of alumina, polyimide short-cut fibers and acrylic water-based binder in the modified alumina is 20:3:3. S3. A polyethylene microporous membrane with a thickness of 9 μm (air permeability of 85 s / 100 mL and porosity of 55%) was selected as the base membrane. The above slurry was coated on both sides of the base membrane using a microgravure coating process at a coating speed of 30 m / min. After coating, the membrane was dried at 60℃ for 1 min, 70℃ for 1 min, and 80℃ for 1 min, respectively. After drying, a lithium-ion battery separator was obtained with a single-sided coating thickness of 2 μm.

[0067] The lithium-ion battery separators prepared in Examples 1-22 and Comparative Examples 1-7 were subjected to the following performance tests: (1) Air permeability increase: The lithium-ion battery separator was placed on the Asahi Seiko air permeability tester of Japan and tested at 10 points evenly. The average value was taken to obtain the air permeability increase of the separator. (2) Breakdown voltage: The lithium-ion battery separator is laid flat on the test conductive plate, and 50 breakdown points are tested for each sample to obtain the average breakdown voltage; (3) Thermal shrinkage rate: The lithium-ion battery separator was cut into 4cm×6cm pieces, and its area change was measured after being dried in an oven at 150℃ for 1h. (4) Ionic conductivity: The lithium-ion battery separator was immersed in the electrolyte (1 mol / L lithium hexafluorophosphate). The impedance of the 1st to 4th layers of the separator was measured sequentially, and the corresponding impedance was obtained by fitting. Finally, the corresponding ionic conductivity was obtained from the thickness. The calculation formula is as follows:

[0068] σ: Ionic conductivity of the membrane, in mS / cm; d: The actual thickness of the lithium battery separator being tested, in cm; R: Bulk ionic resistance of the membrane obtained by resistance testing, in Ω; S: Effective contact area between the diaphragm and the electrode, in cm²; (5) Liquid absorption rate and liquid retention rate: Cut a lithium-ion battery separator with a size of 50mm×50mm, weigh the cut sample and record the mass as m1, and immerse the weighed separator in the electrolyte (1mol / L). Soak the lithium-ion battery separator sample in lithium hexafluorophosphate for 30 minutes. Lay a clean industrial wiping paper (size > 150mm × 150mm) on a flat table. Take out the soaked lithium-ion battery separator sample and quickly place it on the industrial wiping paper. Use another industrial wiping paper to gently press and wipe the free electrolyte on the surface of the lithium-ion battery separator sample until no particulate electrolyte is visible to the naked eye. Weigh the dried lithium-ion battery separator sample and record the mass as m2. After 1 hour, weigh it again and record the mass as m3. Calculate the liquid absorption rate and liquid retention rate of the separator according to the following formula: Liquid absorption rate (%) = (m2-m1) / m1 × 100%, Liquid retention rate (%) = (m3-m1) / m1 × 100%. The liquid absorption rate and liquid retention rate test results are the average values ​​of 3 parallel separator samples. (6) Long cycle stability time: The lithium-ion battery separator is cut into circular pieces with a diameter of 20 mm. Before assembly, it is dried in a vacuum oven to remove adsorbed moisture. All batteries are assembled in an argon glove box. Two lithium metal sheets are used as the positive and negative electrodes of the symmetrical battery. The lithium sheet diameter is 15 mm and the thickness is 0.5 mm. The assembly structure is: stainless steel shell - gasket - lithium sheet - composite separator - lithium sheet - spring sheet - shell. After the lithium-ion battery separator is aligned with the electrode, electrolyte is dripped into the center of the lithium-ion battery separator to completely wet the lithium-ion battery separator. After encapsulation, it is left to stand for 5 hours to preserve the battery's stability. To ensure sufficient wetting and interface stability of the electrolyte, the electrolyte concentration was 1.0 mol / L, the solute was LiPF6, and the solvent was a mixed solution of ethylene carbonate: dimethyl carbonate: methyl ethyl carbonate in a volume ratio of 1:1:1. After the battery was packaged and allowed to stand and wet, a constant current lithium plating / stripping cycle test was performed at room temperature using a battery testing system. The test adopted a constant current mode, and the current density was set to 1 mA / cm2. The battery voltage-time curve was recorded. When the battery discharge capacity decayed to 80% of the initial capacity, the corresponding cycle time or number of cycles was the end point of the separator's lifespan. (7) Diaphragm peel strength: Cut the diaphragm into samples with a width of 15mm and a length of 150mm. Use 3M tape to stick it to the sample coating surface, leaving a peel end of at least 20mm. Use a standard roller to evenly press the sample 3 times. Fix both ends of the sample in the upper and lower clamps respectively. The peel direction is 180°. Use a stretching machine to tear off a section of the 3M transparent tape to obtain the coating adhesion.

[0069] The test results are shown in Table 1 below.

[0070] Table 1. Test results of lithium-ion battery separator performance

[0071] A comparison of Examples 1 and Comparative Examples 1-2 shows that when the algebraic range of the amino-containing dendritic macromolecules is 1-3, the internal adhesion and electrochemical performance of the coating can be significantly improved. A comparison of Examples 1 and Comparative Examples 3-4 shows that when the loading of amino-containing dendritic macromolecules relative to organic fibers is 0.5wt%-15wt%, the internal adhesion and electrochemical performance of the coating can be significantly improved. A comparison of Examples 1 and Comparative Examples 5-7 shows that modifying organic fibers with amino-containing dendritic macromolecules can significantly improve the internal adhesion and electrochemical performance of the coating.

[0072] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A fiber-ceramic composite lithium-ion battery separator, characterized in that, The coating comprises a base film and a coating disposed on at least one surface of the base film, the coating comprising organic fibers, inorganic ceramic particles and a binder in a mass ratio of 3~25:20~70:3~20; The surface of the organic fiber is loaded with amino-containing dendritic macromolecules, which form an interface modification layer on the surface of the organic fiber. The amino-containing dendritic macromolecules include a first terminal amino group, which serves as a lithium ion coordination site. The organic fiber is distributed in a three-dimensional network in the coating, and the amino-containing dendritic macromolecules form a bridging structure between the organic fiber and the inorganic ceramic particles. The mass ratio of the organic fiber to the amino-containing dendritic macromolecules is 100:0.5~15, and the algebraic range of the amino-containing dendritic macromolecules is 1~3.

2. The fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, The length L and diameter D1 of the organic fiber satisfy the condition that the median particle size D50 of the inorganic ceramic particles is 0.05 nm. -1 ≤L / (D1×D50)≤0.1nm -1 ; Where L is 30~50μm, D1 is 300~500nm, and D50 is 1~2μm.

3. The fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, The amino-containing dendritic macromolecule also includes a second terminal amino group, which is cross-linked by a cross-linking agent to form a three-dimensional cross-linked network; The mass ratio of the amino-containing dendritic macromolecule to the crosslinking agent is 100:0.05~2.

4. The fiber-ceramic composite lithium-ion battery separator according to claim 3, characterized in that, The crosslinking agent includes at least one of glutaraldehyde, epichlorohydrin, genipin, and polyisocyanate.

5. The fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, The organic fibers include at least one of polyimide fibers, aramid fibers, polyphenylene sulfide fibers, and polytetrafluoroethylene fibers.

6. The fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, The amino-containing dendritic macromolecules include at least one of polyamide-amine dendritic macromolecules, polypropylene imine dendritic macromolecules, and lysine dendritic macromolecules.

7. The fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, The inorganic ceramic particles include at least one of alumina, silicon dioxide, boehmite, titanium dioxide, and barium sulfate.

8. The fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, The adhesive includes at least one of acrylate copolymers, vinylidene fluoride copolymers, aramid nanofibers, polyvinyl alcohol, and waterborne polyurethane.

9. The method for preparing a fiber-ceramic composite lithium-ion battery separator according to claim 1, characterized in that, include: The organic fibers are immersed in a solution containing amino dendritic macromolecules, mixed evenly, and dried to obtain modified organic fibers. The modified organic fibers, inorganic ceramic particles, binder, and dispersion medium are mixed evenly to obtain a slurry; The slurry is coated onto at least one surface of the base film and dried to obtain the lithium-ion battery separator.

10. A battery, characterized in that, The lithium-ion battery separator includes the lithium-ion battery separator according to any one of claims 1 to 8 or the lithium-ion battery separator prepared by the preparation method according to claim 9.