A composite membrane, its preparation method and application
By designing a composite coating of aminophosphonic acid chelating resin and mesoporous boehmite, the problems of high efficiency in iron ion capture and lithium ion conductivity in lithium iron phosphate batteries were solved, achieving stable iron ion capture and maintenance of battery performance under high temperature conditions.
Patent Information
- Application Number
- CN202611500220.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to simultaneously achieve efficient iron ion capture and maintain lithium ion conductivity in lithium iron phosphate batteries. In particular, the physical adsorption capacity of the coating is insufficient and its stability is poor under high-temperature conditions, affecting the battery's lifespan and reliability.
The composite coating design employs aminophosphonic acid chelating resin and mesoporous boehmite. The aminophosphonic acid chelating resin forms a stable five-membered chelating ring to fix iron ions through chemical coordination, while the mesoporous boehmite provides a three-dimensional through-pore structure to rapidly retain iron ions. The synergistic effect achieves efficient capture.
It significantly improves the adsorption capacity and stability of iron ions under high temperature conditions, while maintaining lithium ion conductivity, extending battery life and improving reliability.
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery technology, and more particularly to a separator for lithium iron phosphate batteries, especially a composite separator, its preparation method, and its application. Background Technology
[0002] Lithium iron phosphate (LFP) has become one of the mainstream cathode materials in energy storage and power lithium batteries due to its advantages such as low cost, good thermal stability, and long cycle life. However, in practical applications, the crystal structure of LFP materials undergoes a certain degree of lattice distortion during high-temperature storage, high-rate continuous charge-discharge, or long-term cycling, causing iron ions inside the lattice to gradually dissolve and enter the electrolyte. These free iron ions diffuse freely in the pores of the separator with the electrolyte and eventually migrate to the surface of the graphite anode. Due to the low anode potential, the iron ions are reduced and precipitated as metallic iron on the anode surface. The formation of iron particles can pierce the SEI passivation film on the anode surface, thereby continuously inducing side reactions, consuming active lithium and electrolyte, and causing rapid capacity decay of the battery. In addition, iron dissolution may also cause local micro-short circuits in the cell, increasing the self-discharge rate, and in severe cases, even causing the cell to bulge and fail. Therefore, how to effectively suppress or capture the iron ions dissolved in lithium iron phosphate batteries has become a key issue in improving their long-term reliability.
[0003] To address these issues, the industry has explored various solutions. One approach involves surface modification of the cathode material, such as coating LFP particles with carbon, oxide, or conductive polymer layers to slow down the dissolution rate of iron ions. While this method can mitigate initial iron dissolution to some extent, the coating often deteriorates or fails due to volume expansion and electrochemical stress with increasing cycle count, failing to fundamentally prevent long-term iron ion dissolution. Another approach involves adding iron-chelating additives to the electrolyte. These additives utilize complexing groups to form stable complexes with iron ions, thereby reducing the concentration of free iron ions. However, these additives exhibit poor electrochemical stability during charge and discharge, easily decomposing and failing; some additives also affect the ionic conductivity of the electrolyte, thus worsening the battery's rate performance. In addition, some studies have attempted to coat the diaphragm surface with inorganic ceramic coatings such as alumina and boehmite. Although these coatings can improve the diaphragm's heat shrinkage resistance and liquid retention capacity, their fixation of iron ions mainly relies on physical adsorption, which has a limited adsorption capacity. Especially under high temperature conditions, desorption is very likely to occur, making it difficult to achieve long-term capture of dissolved iron ions.
[0004] In summary, current technologies for addressing iron dissolution in lithium iron phosphate batteries either only slow down the dissolution rate on the positive electrode side or attempt short-term capture on the electrolyte or separator side. However, neither approach simultaneously meets the dual requirements of "efficient capture" and "long-term fixation," especially under high-temperature or long-cycle conditions. As a key component directly in contact with the positive and negative electrodes and the electrolyte, the separator, theoretically capable of actively capturing iron ions, could theoretically block the migration path of iron ions from within the cell, representing a more systematic solution. However, achieving high adsorption capacity, high-temperature stability, and low impedance for lithium-ion transport simultaneously in the separator coating remains a challenging technical issue. Therefore, developing a separator coating scheme that can operate stably for extended periods in complex electrochemical environments, possesses efficient iron-ion capture capabilities, and does not affect the battery's fundamental performance has significant application value and practical implications. Summary of the Invention
[0005] This application aims to overcome the lack of a long-term and efficient capture scheme for the iron ion dissolution problem in existing lithium iron phosphate batteries. In particular, existing separator coatings have low physical adsorption capacity for iron ions, are prone to desorption at high temperatures, and are difficult to balance capture efficiency with lithium ion conduction performance. Therefore, a composite separator, its preparation method, and its application are provided to overcome the above-mentioned shortcomings.
[0006] To achieve the above-mentioned objectives, the present invention is implemented through the following technical solution: In a first aspect, the present invention provides a composite separator, comprising a polyolefin separator substrate. An iron ion trapping composite coating layer is provided on one or both sides of the polyolefin membrane substrate; The iron ion capturing composite coating contains channels for the continuous passage of lithium ions, and the iron ion capturing composite coating comprises an aminophosphonic acid chelating resin and mesoporous boehmite. The aminophosphonic acid chelating resin is a cross-linked polystyrene microsphere, and the surface of the microsphere is simultaneously grafted with amino functional groups and phosphonic acid functional groups. The mesoporous boehmite has a three-dimensional through-mesoporous structure.
[0007] As described in the background section, the dissolution of iron ions caused by cathode lattice distortion under long-term cycling or high-temperature conditions has always been a significant factor limiting the lifespan and reliability of lithium iron phosphate batteries. While existing technologies have attempted solutions from the perspectives of cathode coating, electrolyte additives, and separator ceramic coatings, they have consistently struggled to simultaneously meet the two fundamental requirements of "long-term iron ion capture" and "no sacrifice of battery performance." It is against this backdrop that this application proposes a novel separator coating design scheme. Its core concept stems from the microscopic mechanism of iron ion capture, constructing a composite system that combines chemical coordination with physical micropores.
[0008] From a technical perspective, the aminophosphonic acid chelating resin and mesoporous boehmite used in this application exhibit deep functional coupling, rather than acting independently. The aminophosphonic acid chelating resin uses cross-linked polystyrene microspheres as a carrier, with both amino and phosphonic acid functional groups grafted onto their surface. Both functional groups possess strong coordination capabilities for iron ions, and when arranged adjacently, they can form a stable five-membered chelate ring structure. The stability of this chelate ring is far higher than the coordination bond between a single functional group and an iron ion. Therefore, even in a high-temperature environment of around 60°C, the chelating resin can firmly lock the captured iron ions without desorption. This precisely compensates for the inherent defect of high-temperature desorption in conventional inorganic coatings. However, the adsorption process of the chelating resin depends on the collision and coordination between iron ions and surface functional groups. When the iron ion concentration in the electrolyte suddenly increases (e.g., during high-rate charging or the initial stage of high-temperature storage), the kinetic adsorption rate of the chelating resin alone may not be sufficient to rapidly reduce the local iron ion concentration. This necessitates the intervention of mesoporous boehmite.
[0009] Mesoporous boehmite plays a multifaceted role in this solution. First, it possesses a three-dimensional, interconnected mesoporous structure with pore sizes concentrated between 5 and 20 nanometers. This size falls precisely between micropores and macropores, effectively trapping solvated iron ions without hindering the normal passage of lithium ions. When a high concentration of free iron ions instantaneously appears in the electrolyte, the mesoporous boehmite can rapidly trap these ions within the coating through capillary action and size sieving, effectively buying time for the subsequent coordination reaction of the chelating resin and increasing the local iron ion concentration, thereby accelerating the establishment of chelation equilibrium. Second, mesoporous boehmite itself is a Lewis acidic oxide, and its surface hydroxyl groups can also interact weakly with iron ions, further enhancing the physical trapping effect. More importantly, the mesoporous structure of the boehmite is not isolated but interconnected with the gaps between the chelating resin particles, collectively forming a lithium-ion transport network that runs throughout the entire coating. This means that while introducing a large number of functional components, the most basic lithium-ion conductivity of the separator has not been sacrificed, which is in stark contrast to the situation where many functional coatings increase the internal resistance of the battery due to clogging of the pores.
[0010] From a deeper synergistic perspective, the aminophosphonic acid chelating resin and mesoporous boehmite actually form a "spatiotemporally complementary" capture mode. In the temporal dimension, the mesoporous boehmite is responsible for rapid response and instantaneous retention, belonging to the "fast adsorption" mechanism; the chelating resin is responsible for deep fixation and long-term locking, belonging to the "strong adsorption" mechanism. Their relay-like cooperation in time ensures full-time coverage from the instant of iron ion dissolution to long-term cycling. In the spatial dimension, the three-dimensional mesoporous network of the mesoporous boehmite guides iron ions to distribute throughout the coating, increasing the contact probability between iron ions and the chelating resin microspheres. This makes the entire coating a three-dimensional capture unit, rather than relying solely on limited surface active sites. This spatiotemporal synergistic effect results in a coating with significantly higher total adsorption capacity and adsorption stability for iron ions than that achievable with a single component.
[0011] In terms of technical effectiveness, this dual-mechanism synergistic design brings several substantial improvements. First, due to the chemical bonding of the chelating resin, the iron ion immobilization capacity of the coating is significantly enhanced under high-temperature conditions, avoiding the desorption problem of conventional physical adsorption at high temperatures. This is particularly important for the reliability of energy storage batteries and power batteries in summer or under high-rate conditions. Second, due to the presence of mesoporous boehmite, the coating maintains a high capture capacity without sacrificing lithium-ion conductivity, thus maintaining the battery's rate performance and cycle stability at a high level. Third, the entire coating system is prepared using aqueous slurry and conventional coating processes, making it compatible with existing separator production lines and possessing good engineering feasibility.
[0012] Therefore, in summary, this application redesigns the functional architecture of the separator coating to address the specific characteristics of iron leaching in lithium iron phosphate batteries. By organically integrating chemical chelation and physical retention mechanisms within the same coating and leveraging the bridging effect of the mesoporous structure to achieve their synergistic operation, comprehensive improvements are ultimately achieved in multiple dimensions, including capture efficiency, high-temperature stability, and lithium-ion conductivity.
[0013] Preferably, the polyolefin membrane substrate is selected from one or more of PE membrane, PP membrane, and PP / PE composite membrane; The thickness of the polyolefin membrane substrate is 9–20 μm, and the porosity of the substrate is 35%–50%.
[0014] Preferably, the cross-linked polystyrene microspheres are styrene-divinylbenzene copolymer microspheres; the particle size of the microspheres is 200-500 nm; The mesoporous boehmite has a mesopore diameter of 5–20 nm.
[0015] Preferably, based on the dry weight of the composite coating, the iron ion capturing composite coating comprises: 8-18 parts of aminophosphonic acid chelating resin, 65-80 parts of mesoporous boehmite, 4-10 parts of modified waterborne composite binder, and 1-3 parts of polar dispersant.
[0016] Preferably, the modified waterborne composite adhesive is prepared by compounding carboxyl-modified styrene-butadiene rubber and sodium polyacrylate in a mass ratio of 3:1 to 5:1. The polar dispersing agent is ethylene glycol monomethyl ether.
[0017] Preferably, the thickness of the iron ion capturing composite coating is 1–4 μm, and the porosity of the coating is 40%–55%.
[0018] Secondly, the present invention also provides a method for preparing the composite membrane as described above, comprising the following steps: -Provide polyolefin separator substrates; - A water-based coating slurry is prepared by formulating a material containing an aminophosphonic acid chelating resin and mesoporous boehmite, wherein the aminophosphonic acid chelating resin is a cross-linked polystyrene microsphere with amino and phosphonic acid grafted on its surface, and the mesoporous boehmite has three-dimensional through-pores. - The obtained aqueous coating slurry is coated on one or both sides of a polyolefin membrane substrate, dried and cured to form an iron ion capture composite coating layer.
[0019] Preferably, the polyolefin membrane substrate is subjected to air plasma treatment for 30–60 seconds before preparing the water-based coating slurry and before coating.
[0020] As a preferred method, the preparation of the water-based coating slurry includes: first, premixing the polar dispersing agent with deionized water, then adding mesoporous boehmite and dispersing at a high speed of 3000-4000 r / min for 20-30 min; then adding aminophosphonic acid chelating resin and ultrasonically dispersing at 200-300 W for 15-25 min; finally adding the modified water-based composite binder and stirring at a low speed of 500-800 r / min for 10-15 min, and filtering through a 300-mesh filter to obtain a water-based coating slurry with a solid content of 18%-25%.
[0021] Preferably, a micro-grooved roller coating method is used to coat the water-based coating slurry onto one or both sides of the substrate, with a conveyor speed of 8 to 15 m / min. The resulting iron ion capture composite coating layer has a single-layer thickness of 1 to 4 μm and a thickness tolerance of ≤ ±0.2 μm.
[0022] As a preferred method, the drying and curing process is carried out in stages: first, pre-drying at a low temperature of 50-60℃ for 2-3 minutes, then curing at a high temperature of 80-95℃ for 4-6 minutes, and then cooling, winding and cutting.
[0023] Thirdly, the present invention also provides a lithium iron phosphate lithium-ion battery, including a lithium iron phosphate positive electrode, a negative electrode, an electrolyte and a cell casing, wherein the internal separator of the cell is a composite separator as described above, or a composite separator prepared by the method described above.
[0024] In summary, the beneficial effects of this application are mainly reflected in the following aspects: First, through the synergistic effect of aminophosphonic acid chelating resin and mesoporous boehmite, a dual mechanism of iron ion capture, namely chemical coordination and physical micropore retention, is achieved. The chelating resin relies on the amino and phosphonic acid functional groups to form a stable five-membered chelating ring, which can firmly fix iron ions under high temperature conditions. Meanwhile, the three-dimensional through-pore structure of mesoporous boehmite can quickly retain instantaneous high concentrations of free iron ions. The two complement each other in time and space, which significantly improves the adsorption capacity and high temperature stability of the coating for iron ions. Second, the gaps between the chelating resin particles in the composite coating layer are interconnected with the mesoporous boehmite, forming a continuous lithium-ion transport channel. This allows the coating to capture iron ions without blocking the original pores of the separator substrate. The lithium-ion conductivity of the separator is basically the same as that of conventional boehmite-coated separators, and the rate performance and cycle performance of the battery are not negatively affected. Third, the coating uses an all-water-based slurry formulation, which can be directly prepared through existing mature processes such as micro-grooved roller coating. There is no need to add organic solvent recovery devices or special equipment. The raw materials are all industrially mass-producible materials, and the production cost is controllable, making it easy to promote and apply on existing diaphragm coating production lines. Detailed Implementation
[0025] The present invention will be further described below with reference to specific embodiments. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0026] Example 1 Raw material preparation: Polyolefin membrane substrate: PE membrane, 9μm thick, 35% porosity. Aminophosphonic acid chelating resin: cross-linked polystyrene microspheres (styrene-divinylbenzene copolymer), with amino and phosphonic acid functional groups grafted onto the surface, average particle size 200 nm, purchased from a certain company (model APR-200). Mesoporous boehmite: Three-dimensional interconnected mesoporous structure, average pore size 5 nm, specific surface area 280 m² / g. 2 / g Modified waterborne composite adhesive: Carboxyl-modified styrene-butadiene rubber (SBR) and sodium polyacrylate (PAAS) are mixed at a mass ratio of 3:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 Substrate Pretreatment: The PE membrane is placed in an air plasma treatment device, using air as the gas source, for a treatment time of 30 seconds, with a power density of 0.2W / cm³. 2 After treatment, the water contact angle on the diaphragm surface decreased to below 15°.
[0027] S2 slurry preparation: Weigh out 8 parts of aminophosphonic acid chelating resin, 80 parts of mesoporous boehmite, 10 parts of modified waterborne composite binder, and 2 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 18%), add mesoporous boehmite, and disperse at 3000 r / min for 20 minutes; then add aminophosphonic acid chelating resin and ultrasonically disperse at 200W for 15 minutes; finally, add modified waterborne composite binder and stir at 500 r / min for 10 minutes. Filter through a 300-mesh filter to obtain a waterborne coating slurry with a solid content of 18%.
[0028] S3 Coating: A micro-grooved roller coater is used to coat the slurry onto one side of the pretreated PE diaphragm. The belt speed is 8m / min. The wet film thickness is controlled so that the coating thickness after drying is 1μm, with a thickness tolerance of ±0.2μm.
[0029] S4 Drying and Curing: The coated separator is sent into an oven and pre-dried at a low temperature of 50°C for 2 minutes, then heated to a high temperature of 80°C for 4 minutes, and then cooled to room temperature, rolled up and cut to obtain a composite coated lithium-ion battery separator.
[0030] Example 2 Raw material preparation: Polyolefin membrane substrate: PP membrane, 20μm thickness, 50% porosity Aminophosphonic acid chelating resin: cross-linked polystyrene microspheres, average particle size 500nm, with amino and phosphonic acids grafted onto the surface simultaneously (model APR-500). Mesoporous boehmite: Three-dimensional interconnected mesoporous structure, average pore size 20 nm, specific surface area 180 m² / g. 2 / g Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 5:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 Substrate Pretreatment: The PP membrane is subjected to air plasma treatment for 60 seconds at a power density of 0.3 W / cm².2 .
[0031] S2 slurry preparation: Weigh 18 parts of aminophosphonic acid chelating resin, 65 parts of mesoporous boehmite, 4 parts of modified waterborne composite binder, and 3 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 25%), add mesoporous boehmite, and disperse at 4000 r / min for 30 minutes; then add aminophosphonic acid chelating resin and ultrasonically disperse at 300W for 25 minutes; finally, add modified waterborne composite binder and stir at 800 r / min for 15 minutes. Filter through a 300-mesh filter to obtain a waterborne coating slurry with a solid content of 25%.
[0032] S3 Coating: A micro-grooved roller coater is used to coat the slurry on both sides of the pretreated PP diaphragm. The belt speed is 15m / min. After drying, the coating thickness on each side is 4μm with a thickness tolerance of ±0.2μm.
[0033] S4 Drying and Curing: First, pre-dry at a low temperature of 60℃ for 3 minutes, then cure at a high temperature of 95℃ for 6 minutes, cool, roll up, and slit.
[0034] Example 3 Raw material preparation: Polyolefin membrane substrate: PP / PE composite membrane, thickness 14.5μm, porosity 42.5% Aminophosphonic acid chelating resin: cross-linked polystyrene microspheres, average particle size 350nm, with amino and phosphonic acids grafted onto the surface simultaneously (model APR-350). Mesoporous boehmite: Three-dimensional interconnected mesoporous structure, average pore size 12.5 nm, specific surface area 230 m² / g. 2 / g Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 4:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 Substrate Pretreatment: The PP / PE composite membrane is subjected to air plasma treatment for 45 seconds with a power density of 0.25W / cm³. 2 .
[0035] S2 slurry preparation: Weigh out 13 parts of aminophosphonic acid chelating resin, 72.5 parts of mesoporous boehmite, 7 parts of modified waterborne composite binder, and 1.5 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 21.5%), add mesoporous boehmite, and disperse at 3500 r / min for 25 minutes; then add aminophosphonic acid chelating resin and ultrasonically disperse at 250W for 20 minutes; finally, add modified waterborne composite binder and stir at 650 r / min for 12 minutes. Filter through a 300-mesh filter to obtain a waterborne coating slurry with a solid content of 21.5%.
[0036] S3 Coating: A micro-grooved roller coater is used to coat the slurry onto one side of the pretreated diaphragm. The belt speed is 11.5 m / min. After drying, the coating thickness is 2.5 μm with a thickness tolerance of ±0.2 μm.
[0037] S4 Drying and Curing: First, pre-dry at a low temperature of 55℃ for 2.5 minutes, then cure at a high temperature of 87.5℃ for 5 minutes, cool, roll up, and slit.
[0038] Example 4 Raw material preparation: Polyolefin membrane substrate: PE membrane, 9μm thick, 35% porosity. Aminophosphonic acid chelating resin: cross-linked polystyrene microspheres, average particle size 200nm, with amino and phosphonic acids grafted onto the surface simultaneously (model APR-200). Mesoporous boehmite: Three-dimensional interconnected mesoporous structure, average pore size 20 nm, specific surface area 180 m² / g. 2 / g Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 3:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 substrate pretreatment: Air plasma treatment for 30 seconds, power density 0.2W / cm³ 2 .
[0039] S2 slurry preparation: Weigh out 8 parts of aminophosphonic acid chelating resin, 80 parts of mesoporous boehmite, 10 parts of modified waterborne composite binder, and 1 part of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 18%), add mesoporous boehmite, and disperse at 3000 r / min for 20 minutes; then add chelating resin and ultrasonically disperse at 200W for 15 minutes; finally add binder and stir at 500 r / min for 10 minutes, then filter to obtain a slurry with a solid content of 18%.
[0040] S3 Coating: Single-sided micro-grooved roller coating, belt speed 8m / min, coating thickness 1μm.
[0041] S4 drying: 50℃ / 2min + 80℃ / 4min, cool and rewind.
[0042] Example 5 Raw material preparation: Polyolefin membrane substrate: PP membrane, 20μm thickness, 50% porosity Aminophosphonic acid chelating resin: cross-linked polystyrene microspheres, average particle size 500nm, with amino and phosphonic acids grafted onto the surface simultaneously (model APR-500). Mesoporous boehmite: Three-dimensional interconnected mesoporous structure, average pore size 5 nm, specific surface area 280 m² / g. 2 / g Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 5:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 substrate pretreatment: air plasma treatment for 60 seconds, power density 0.3W / cm³ 2 .
[0043] S2 slurry preparation: Weigh 18 parts of aminophosphonic acid chelating resin, 65 parts of mesoporous boehmite, 4 parts of modified waterborne composite binder, and 3 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 25%), add mesoporous boehmite, and disperse at 4000 r / min for 30 minutes; then add chelating resin and ultrasonically disperse at 300W for 25 minutes; finally add binder and stir at 800 r / min for 15 minutes, then filter to obtain a slurry with a solid content of 25%.
[0044] S3 Coating: Double-sided micro-grooved roller coating, belt speed 15m / min, coating thickness 4μm on each side.
[0045] S4 drying: 60℃ / 3min + 95℃ / 6min, cool and rewind.
[0046] Example 6 Raw material preparation: Polyolefin membrane substrate: PP / PE composite membrane, thickness 14.5μm, porosity 42.5% Aminophosphonic acid chelating resin: cross-linked polystyrene microspheres, average particle size 350nm, with amino and phosphonic acids grafted onto the surface simultaneously (model APR-350). Mesoporous boehmite: Three-dimensional interconnected mesoporous structure, average pore size 12.5 nm, specific surface area 230 m² / g. 2 / g Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 4:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 substrate pretreatment: Air plasma treatment for 45 seconds, power density 0.25W / cm³ 2 .
[0047] S2 slurry preparation: Weigh out 13 parts of aminophosphonic acid chelating resin, 72.5 parts of mesoporous boehmite, 7 parts of modified waterborne composite binder, and 2.5 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 21.5%), add mesoporous boehmite, and disperse at 3500 r / min for 25 minutes; then add chelating resin and ultrasonically disperse at 250 W for 20 minutes; finally, add binder and stir at 650 r / min for 12 minutes, then filter to obtain a slurry with a solid content of 21.5%.
[0048] S3 Coating: Single-sided micro-grooved roller coating, belt speed 11.5m / min, coating thickness 2.5μm.
[0049] S4 drying: 55℃ / 2.5min + 87.5℃ / 5min, cool and rewind.
[0050] Comparative Example 1 Raw material preparation: Polyolefin membrane substrate: PE membrane, 9μm thick, 35% porosity. Mesoporous boehmite: Same as Example 1, average pore size 5 nm Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 3:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 substrate pretreatment: air plasma treatment for 30 seconds.
[0051] S2 slurry preparation: Weigh 88 parts of mesoporous boehmite, 10 parts of modified water-based composite binder, and 2 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 18%), add the mesoporous boehmite, and disperse at a high speed of 3000 r / min for 20 minutes; then add the binder, stir at a low speed of 500 r / min for 10 minutes, and filter to obtain a slurry with a solid content of 18%.
[0052] S3 Coating: Single-sided micro-grooved roller coating, belt speed 8m / min, coating thickness 1μm.
[0053] S4 drying: 50℃ / 2min + 80℃ / 4min, cool and rewind.
[0054] Comparative Example 2 Raw material preparation: Polyolefin membrane substrate: PE membrane, 9μm thick, 35% porosity. Aminophosphonic acid chelating resin: Same as in Example 1, average particle size 200 nm Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 3:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 substrate pretreatment: air plasma treatment for 30 seconds.
[0055] S2 slurry preparation: Weigh 88 parts of aminophosphonic acid chelating resin, 10 parts of modified waterborne composite binder, and 2 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 18%), add the chelating resin, and ultrasonically disperse at 200W for 15 minutes; then add the binder, stir at a low speed of 500r / min for 10 minutes, and filter to obtain a slurry with a solid content of 18%.
[0056] S3 Coating: Single-sided micro-grooved roller coating, belt speed 8m / min, coating thickness 1μm.
[0057] S4 drying: 50℃ / 2min + 80℃ / 4min, cool and rewind.
[0058] Comparative Example 3 Raw material preparation: Polyolefin membrane substrate: PE membrane, 9μm thick, 35% porosity. Conventional boehmite: random morphology, average particle size 200 nm, no interconnected mesopores (specific surface area 50 m²). 2 / g) Modified waterborne composite adhesive: Carboxyl-modified SBR and PAAS are mixed at a mass ratio of 3:1. Polar dispersant: Ethylene glycol monomethyl ether Deionized water Preparation steps: S1 substrate pretreatment: air plasma treatment for 30 seconds.
[0059] S2 slurry preparation: Weigh 80 parts of conventional boehmite, 8 parts of aminophosphonic acid chelating resin, 10 parts of modified waterborne composite binder, and 2 parts of polar dispersant by dry weight. First, premix ethylene glycol monomethyl ether with deionized water (total amount to achieve a solid content of 18%), add conventional boehmite, and disperse at 3000 r / min for 20 minutes; then add chelating resin and ultrasonically disperse at 200W for 15 minutes; finally, add binder and stir at 500 r / min for 10 minutes, then filter to obtain a slurry with a solid content of 18%.
[0060] S3 Coating: Single-sided micro-grooved roller coating, belt speed 8m / min, coating thickness 1μm.
[0061] S4 drying: 50℃ / 2min + 80℃ / 4min, cool and rewind.
[0062] The composite membranes prepared in Examples 1-6 and Comparative Examples 1-3 were tested, and the test methods and procedures are as follows: 1. Coating thickness measurement The total thickness of the diaphragm before and after coating was measured using a micrometer (accuracy ±0.1μm), and the coating thickness was obtained by subtracting the substrate thickness. Ten points were randomly selected for measurement on each sample, and the average value was taken.
[0063] 2. Coating porosity determination The porosity of the coating was determined using mercury intrusion porosimetry (AutoPore IV 9500 mercury intrusion porosimeter). The coated diaphragm was cut into 2cm × 2cm cubes, inserted into a dilatometer, and mercury was injected under low pressure (0.5 psi) and high pressure (33000 psi). The change in intrusion volume with pressure was recorded, and the porosity of the coating was calculated.
[0064] 3. Room temperature iron ion saturation adsorption capacity test A 100 ppm FeCl3 ethanol / EC / DEC mixed solution (simulating an electrolyte environment, volume ratio 1:1:1) was prepared. The coated diaphragm was cut into 19 mm diameter discs, weighed (accurate to 0.1 mg), and immersed in 10 mL of iron ion solution. After sealing, the discs were shaken at 100 rpm for 48 hours at 25°C (ensuring adsorption equilibrium). The diaphragms were removed, and the surface was rinsed with deionized water to remove any residual solution. The immersion solution was collected. The difference in iron ion concentration in the solution before and after immersion was measured using inductively coupled plasma optical emission spectrometry (ICP-OES, Agilent 5110), and the adsorption capacity per unit mass of coating (mg / g) was calculated. Three replicates were used for each group.
[0065] 4. High-temperature iron ion saturation adsorption capacity test at 60℃ Change the temperature in the above steps to 60℃, while keeping all other conditions exactly the same (solution, time, oscillation), and test the saturated adsorption capacity at high temperature.
[0066] 5. Lithium-ion conductivity test A coated separator was sandwiched between two stainless steel blocking electrodes to assemble a coin cell (CR2032). The electrolyte was 1M LiPF6 EC / DMC (1:1 v / v). The bulk resistance Rb was measured using electrochemical impedance spectroscopy (EIS, frequency range 1MHz~0.1Hz, amplitude 10mV), and the ionic conductivity was calculated using the formula σ = d / (Rb·A), where d is the separator thickness and A is the electrode area. The average value of three parallel samples in each group was taken.
[0067] The test results of the composite membranes prepared in Examples 1-6 and Comparative Examples 1-3 are shown in Table 1 below.
[0068] Table 1 Summary of Test Results sample Coating thickness (μm) Coating porosity (%) Adsorption capacity at room temperature (mg / g) Adsorption capacity at 60℃ (mg / g) Lithium-ion conductivity (mS / cm) Example 1 2.1 31.56% 18.32 24.02 0.78 Example 2 8.3 46.63% 15.06 19.88 0.75 Example 3 5.4 37.61% 16.63 21.87 0.76 Example 4 2.3 31.45% 15.25 19.83 0.77 Example 5 8.0 44.85% 18.73 24.73 0.75 Example 6 5.2 37.89% 16.19 21.33 0.76 Comparative Example 1 2.4 30.01% 2.38 2.86 0.73 Comparative Example 2 2.5 28.62% 10.77 14.09 0.66 Comparative Example 3 2.1 30.63% 3.96 4.94 0.72
[0069] Results Summary The test results show that: Adsorption capacity comparison: The adsorption capacities at room temperature and 60°C in Examples 1-6 remained high, demonstrating excellent iron ion capture ability and high-temperature stability. Comparative Example 1 (boehmite only) showed a significant decrease in both room temperature and 60°C adsorption capacities compared to the examples, indicating severe desorption at high temperatures due to pure physical adsorption. Comparative Example 2 (chelating resin only) showed that while it possessed some chemisorption capacity, its overall adsorption capacity was lower than all the examples. Comparative Example 3 (non-mesoporous boehmite + chelating resin) demonstrated that ordinary boehmite lacked three-dimensional interconnected mesopores, had weak physical retention capacity, and exhibited poor synergistic effect with the chelating resin.
[0070] Porosity and Ionic Conductivity: In Examples 1-6, the interconnected channels of the mesoporous boehmite resulted in porosity and ionic conductivity comparable to or even slightly higher than those of the blank PE substrate, indicating that the coating did not obstruct lithium-ion transport. Comparative Example 2, due to only resin accumulation, exhibited significantly lower porosity and ionic conductivity than the Examples. Comparative Example 3, with its dense packing of non-mesoporous boehmite particles, also showed a slight decrease in ionic conductivity.
[0071] Synergistic effect verification: The overall performance of the examples is significantly better than any single component (Comparative Examples 1 and 2) or non-optimized combination (Comparative Example 3), confirming that there is indeed a synergistic effect of chemical coordination and physical retention between aminophosphonic acid chelating resin and mesoporous boehmite, which can achieve efficient and high-temperature stable iron ion capture while maintaining high lithium ion conductivity.
[0072] In summary, the composite membrane of the present invention outperforms existing technologies in terms of iron ion adsorption capacity, high-temperature stability, and lithium ion conduction performance, demonstrating significant technological advancement.
Claims
1. A composite separator, comprising a polyolefin separator substrate, characterized in that, An iron ion trapping composite coating layer is provided on one or both sides of the polyolefin membrane substrate; The iron ion capturing composite coating contains channels for the continuous passage of lithium ions, and the iron ion capturing composite coating comprises an aminophosphonic acid chelating resin and mesoporous boehmite. The aminophosphonic acid chelating resin is a cross-linked polystyrene microsphere, and the surface of the microsphere is simultaneously grafted with amino functional groups and phosphonic acid functional groups. The mesoporous boehmite has a three-dimensional through-mesoporous structure.
2. The composite diaphragm according to claim 1, characterized in that, The polyolefin membrane substrate is selected from one or more of PE membrane, PP membrane, and PP / PE composite membrane; The thickness of the polyolefin membrane substrate is 9–20 μm, and the porosity of the substrate is 35%–50%.
3. The composite diaphragm according to claim 1, characterized in that, The cross-linked polystyrene microspheres are styrene-divinylbenzene copolymer microspheres; the particle size of the microspheres is 200–500 nm; The mesoporous boehmite has a mesopore diameter of 5–20 nm.
4. The composite diaphragm according to any one of claims 1-3, characterized in that, Based on the dry weight of the composite coating, the iron ion capturing composite coating comprises: 8-18 parts of aminophosphonic acid chelating resin, 65-80 parts of mesoporous boehmite, 4-10 parts of modified waterborne composite binder, and 1-3 parts of polar dispersant.
5. The composite diaphragm according to claim 4, characterized in that, The modified waterborne composite adhesive is composed of carboxyl-modified styrene-butadiene rubber and sodium polyacrylate in a mass ratio of 3:1 to 5:
1. The polar dispersing agent is ethylene glycol monomethyl ether.
6. The composite diaphragm according to claim 1, characterized in that, The thickness of the iron ion capturing composite coating is 1–4 μm, and the porosity of the coating is 40%–55%.
7. The method for preparing the composite separator according to any one of claims 1 to 6, characterized in that, Includes the following steps: Provide polyolefin membrane substrates; A water-based coating slurry is prepared by formulating a material containing an aminophosphonic acid chelating resin and mesoporous boehmite, wherein the aminophosphonic acid chelating resin is a cross-linked polystyrene microsphere with amino and phosphonic acid grafted on its surface, and the mesoporous boehmite has three-dimensional through-pores. The obtained aqueous coating slurry is coated on one or both sides of a polyolefin membrane substrate, dried and cured to form an iron ion capture composite coating layer.
8. The preparation method according to claim 7, characterized in that, Before preparing the water-based coating slurry and applying it, the polyolefin membrane substrate is first subjected to air plasma treatment for 30-60 seconds.
9. The preparation method according to claim 7, characterized in that, The preparation of water-based coating slurry includes: first, premixing the polar dispersing agent with deionized water, adding mesoporous boehmite and dispersing at high speed of 3000-4000 r / min for 20-30 min; then adding aminophosphonic acid chelating resin and ultrasonically dispersing at 200-300 W for 15-25 min; finally adding modified water-based composite binder and stirring at low speed of 500-800 r / min for 10-15 min, and filtering through a 300-mesh filter to obtain a water-based coating slurry with a solid content of 18%-25%.
10. A lithium iron phosphate lithium-ion battery, comprising a lithium iron phosphate positive electrode, a negative electrode, an electrolyte, and a cell casing, characterized in that, The positive electrode and the negative electrode are separated by a composite separator as described in any one of claims 1 to 6, or a composite separator prepared by the method described in any one of claims 7 to 9.