Etching methods and semiconductor process equipment

By using layer-by-layer etching and oxidizing plasma treatment of the etching interface, combined with inert plasma to form a sealing layer, the problem of side-holeing of oxide semiconductor material layers is solved, improving the structural integrity and production yield of the device.

CN123124669APending Publication Date: 2026-11-17BEIJING NAURA MICROELECTRONICS EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611235303.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, oxide semiconductor material layers are easily side-cut during the etching process, leading to a decrease in device performance, reliability, and production yield.

Method used

A layer-by-layer etching method is adopted. After etching the second material layer with halogen gas, an oxidizing plasma is introduced to treat the etching interface. The halogen free radicals are consumed through chemical reaction and a passivation layer is formed. Combined with inert plasma, a sealing layer is formed to prevent lateral erosion.

Benefits of technology

It effectively prevents corrosion of the sidewalls of oxide semiconductor material layers, improves the integrity of device structure and process reliability, avoids side-hole phenomenon, and improves production yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124669A_ABST
    Figure CN123124669A_ABST
Patent Text Reader

Abstract

This application provides an etching method and semiconductor process equipment, belonging to the field of semiconductor technology. In this method, when etching a stacked structure including a first material layer and a second material layer layer by layer, the process gas used to etch the second material layer includes a halogen gas. After etching the second material layer, an oxidizing plasma is introduced to treat the etching interface. The oxidizing plasma in this application works synergistically at the etching interface through a triple mechanism of chemical reaction consumption, surface passivation, and plasma gas flow entrainment activation-desorption, preventing the first material layer from being side-exposed and improving the integrity of the device structure and the reliability of the process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor technology, specifically to an etching method and semiconductor process equipment. Background Technology

[0002] Resistive Random Access Memory (RRAM) is a novel type of non-volatile memory. Its core principle is to store information by utilizing the reversible change in the resistance state of a material under an applied electric field. In RRAM, oxide semiconductor materials such as indium gallium zinc oxide (IGZO) are commonly used as the resistive switching functional layer. IGZO has higher electron mobility, which helps improve the on-state current and speed of RRAM devices. IGZO-based RRAM devices typically have lower operating voltage and power consumption, contributing to extended battery life in electronic devices.

[0003] In RRAM devices, HfO2 layers are typically formed on the upper and lower surfaces of the IGZO layer as dielectric protective layers. These layers regulate interface oxygen vacancies, passivate interface defects in the IGZO layer, reduce leakage current, improve resistive switching window, and enhance durability and data retention. During fabrication, the IGZO layer and its HfO2 layers on both surfaces need to be patterned and etched. A common approach is to use dry plasma etching to etch the HfO2 layer. Since the HfO2 layer and other dielectric protective layers are usually made of high-melting-point metal oxide materials, the process gases typically include halogen gases such as Cl2 and BCl3. Highly active chlorine plasma reacts chemically with the metal oxide material, and ion bombardment is used to assist in anisotropic etching. However, this process can cause side-holeing of the IGZO layer during HfO2 etching. This side-holeing not only affects the quality of subsequent trench filling processes, leading to incomplete filling or voids, but also weakens the structure at the trench opening edges, making them prone to fracture during subsequent heat treatment. Ultimately, this damages the device's performance, reliability, and production yield. Summary of the Invention

[0004] In view of this, the embodiments of this application aim to provide an etching method and semiconductor process equipment to solve the problem that oxide semiconductor material layers are easily side-cut in the prior art.

[0005] This application provides an etching method, including: A stacked structure is provided, the stacked structure comprising a stacked first material layer and a second material layer, wherein the first material layer is made of an oxide semiconductor material; and... The stacked structure is etched layer by layer in the order of film layer stacking. The process gas for etching the second material layer includes halogen gas, and after etching the second material layer, the etching interface is treated with oxidizing plasma.

[0006] In some embodiments, it also includes: After treating the etched interface with the oxidizing plasma, a passivation layer is formed at least on the sidewall of the first material layer.

[0007] In some embodiments, the stacked structure has one layer of the second material, which is located on the upper or lower surface of the first material layer; or, the stacked structure has two layers of the second material, with the first material layer located between the two layers of the second material.

[0008] In some embodiments, after each of the second material layers is etched, the etched interface is treated with the oxidizing plasma.

[0009] In some embodiments, the oxidizing gas is ionized to generate the oxidizing plasma. When the oxidizing plasma is used to treat the etched interface, the flow rate of the oxidizing gas is 100 sccm to 200 sccm, the gas pressure is 10 mT to 20 mT, the temperature of the substrate carrier is 40°C to 60°C, the power of the on-board RF power supply is 900 W to 1100 W, and the process time is 10 s to 20 s.

[0010] In some embodiments, the second material layer is located at least on the lower surface of the first material layer. When etching the stacked structure, a portion of the thickness of the second material layer on the lower surface of the first material layer is removed. After etching the stacked structure, the surface of the second material layer is bombarded with inert plasma to form a sealing layer at least on the sidewall of the first material layer.

[0011] In some embodiments, the material of the sealing layer is the same as the material of the second material layer; and / or, the thickness of the sealing layer is 3 angstroms to 5 angstroms.

[0012] In some embodiments, the inert gas is ionized to generate the inert plasma. When the surface of the second material layer is bombarded with the inert plasma, the flow rate of the inert gas is 150 sccm to 350 sccm, the gas pressure is 8 mT to 20 mT, the power of the upper RF power supply is 350 W to 600 W, the power of the lower RF power supply is 200 W to 400 W, the temperature of the substrate carrier is 50 °C to 65 °C, and the process time is set to 15 s to 30 s.

[0013] In some embodiments, the process gas for etching the second material layer includes halogen gas and / or halide gas; during etching of the second material layer, the flow rate of the halogen gas and / or the halide gas is 150 sccm to 200 sccm, the gas pressure is 5 mT to 10 mT, the power of the on-board RF power supply is 900 W to 1100 W, the temperature of the substrate carrier is 60°C to 80°C, and the process time is 10 s to 20 s; and / or, The process gas used to etch the first material layer includes a hydrocarbon gas. When etching the first material layer, the flow rate of the hydrocarbon gas is 30 sccm to 50 sccm, the gas pressure is 8 mT to 15 mT, the power of the upper RF power supply is 300 W to 500 W, the power of the lower RF power supply is 30 W to 70 W, the temperature of the substrate carrier is 50 °C to 65 °C, and the process time is 15 s to 25 s.

[0014] In some embodiments, the stacked structure is a resistive switching functional layer, the first material layer is a dielectric material layer, and the second material layer is a metal oxide semiconductor layer.

[0015] This application also provides a semiconductor process apparatus, including a process chamber and a controller, the controller including at least one processor and at least one memory, the memory storing a computer program, the computer program being executed by the processor to implement the etching method.

[0016] This application provides an etching method and semiconductor process equipment. After forming a stacked structure of a first material layer and a second material layer, etching is performed layer by layer along the stacking sequence. The process gas for etching the second material layer includes halogen gases. After etching the second material layer, oxidizing plasma is introduced to treat the etching interface. On the one hand, the oxidizing plasma can chemically react with residual halogen free radicals and other active groups at the etching interface, converting them into stable and easily removed gaseous products, thus eliminating the corrosion source from the chemical root. On the other hand, the oxidizing plasma performs in-situ passivation of the etching interface, effectively suppressing the lateral erosion of the first material layer by subsequent process steps or environmental factors. In addition, the high-flow-rate oxidizing plasma can form a directional gas flow field, replacing the etching exhaust gas, trace by-products, and adsorbed halogen particles retained on the etching interface. Through gas flow entrainment and vacuum pumping, the stable products and unreacted residues after the reaction are carried out of the process chamber, reducing the concentration of halogen particles on the etching interface. Oxidizing plasma works synergistically on the etching interface through a triple mechanism of chemical reaction consumption, surface passivation, and plasma gas flow entrainment activation and desorption, avoiding the side-cutting of the first material layer and improving the integrity of the device structure and the reliability of the process. Attached Figure Description

[0017] Figure 1 Electron micrograph of the IGZO layer with side cutouts.

[0018] Figure 2 A flowchart of an etching method provided in an embodiment of this application.

[0019] Figure 3 This is a schematic diagram of a stacked structure provided in an embodiment of this application.

[0020] Figure 4 This is a schematic diagram of the structure of the etched upper second material layer provided in an embodiment of this application.

[0021] Figure 5 This is a schematic diagram of the structure for etching the first material layer according to an embodiment of this application.

[0022] Figure 6 This is a schematic diagram of the structure of the etched lower second material layer provided in an embodiment of this application.

[0023] Figure 7 This is a schematic diagram of a structure provided in an embodiment of this application, which utilizes inert plasma to bombard a lower second material layer.

[0024] Figure 8 An electron microscope image of a stacked structure etched using the etching method provided in this application, provided as an embodiment of this application.

[0025] Figure 9 This is a schematic diagram of the structure of a semiconductor process equipment provided in an embodiment of this application.

[0026] The attached figures are labeled as follows: 100 - Substrate; 200 - Stacked structure; 201 - First material layer; 202a - Lower second material layer; 202b - Upper second material layer; 300 - Mask layer; 401 - Sealing layer; 10 - Object to be etched; 20 - Process chamber; 20A - Inlet assembly; 20B - Upper electrode assembly; 20C - Lower electrode assembly; 21 - RF coil; 22 - Wafer carrier structure; 23 - Upper RF power supply; 24 - Lower RF power supply; 25 - Upper matching unit; 26 - Lower matching unit. Detailed Implementation

[0027] To achieve high-precision patterning etching of stacked structures with HfO2 and IGZO layers, the HfO2 layer is typically etched using halogen gases, while the IGZO layer is etched using hydrocarbon gases. Specifically, this method etches the HfO2 layer by introducing halogen gases (such as Cl2 and BCl3) into the process chamber. The basic working principle is that the halogen gas dissociates into highly reactive halogen radicals, which react chemically with the HfO2 material to generate volatile products. Simultaneously, anisotropic etching is achieved by bombardment with plasma (such as Ar plasma). For the IGZO layer, free radicals (such as CH3 radicals) dissociated from hydrocarbon gases (such as CH4) react with the metal elements in the IGZO layer (such as...). The reaction of indium (In), gallium (Ga), and zinc (Zn) produces low-boiling-point organometallic compounds (such as trimethylindiumIn(CH3)3, trimethylgalliumGa(CH3)3, and dimethylzincZn(CH3)2). These compounds are then desorbed into the gas phase through physical bombardment and simultaneously bombarded with plasma (such as Ar plasma). Through momentum transfer, the metal-oxygen bonds on the surface of the IGZO layer are physically broken, leaving the surface atoms in an "activated" or "damaged" state, making them more susceptible to reaction with free radicals.

[0028] However, since electrically neutral halogen radicals are not constrained by the direction of the electric field, they can diffuse both vertically and laterally, and adsorb onto the sidewalls of the exposed or soon-to-be-exposed IGZO layer. Because the metal components in the IGZO layer have strong reactivity with halogen radicals, they easily weaken and destroy metal-oxidation bonds (such as In–O, Ga–O, and Zn–O bonds). When the sidewalls of the IGZO layer are exposed to a halogen radical atmosphere for extended periods, the reaction products (such as InCl3, GaCl3, and ZnCl2) are all volatile gaseous / easily sublimable products. Under vacuum, heating, and plasma bombardment, these products rapidly detach from the IGZO layer surface and are removed by the system. Fresh IGZO surfaces are then re-exposed, continuing the adsorption reaction and persistent lateral halogenation corrosion, ultimately leading to the side-penetration of the IGZO layer. Meanwhile, after etching, highly active halogen particles, active groups, and etching byproducts will remain on the sidewalls and other etching interfaces of the IGZO layer. These residual substances will generate weak acids when they come into contact with air and moisture in subsequent processes (such as removing the wafer into the air or wet cleaning), which will continue to erode the sidewalls of the IGZO layer and further aggravate the side-penetration of the IGZO layer.

[0029] Figure 1 This is a schematic diagram of an IGZO layer being side-cut. (Example) Figure 1As shown, after the side-hole occurs, the effective support cross-sectional area of ​​the IGZO layer is greatly reduced. The edge of the HfO2 layer loses the lateral support of the IGZO layer and is only maintained by the film itself in suspension. The mechanical load-bearing capacity is significantly reduced, which directly causes the edge structure to become locally thinner. This makes it easy for voids and fractures to occur during subsequent filling or heat treatment, affecting the integrity and yield of the device.

[0030] To overcome the above problems, this application provides an etching method and semiconductor process equipment: during the layer-by-layer etching process along the film stacking sequence, after each step of etching the dielectric protective layer using a process gas containing halogen gas is completed, a step of treating the etching interface using oxidizing plasma is immediately introduced. On the one hand, oxidizing plasma can chemically react with residual halogen free radicals and other active groups at the etching interface, converting them into stable and easily removable gaseous products. This chemically quenches and physically removes residual halogen active particles after etching, eliminating the source of corrosion at its chemical origin. On the other hand, oxidizing plasma performs in-situ passivation of the etching interface, constructing a protective barrier at the exposed etching interface. This fundamentally interrupts the lateral erosion process and effectively enhances the sidewall resistance of the oxide semiconductor material film in subsequent processes. Furthermore, high-flow-rate oxidizing plasma can form a directional airflow field, replacing the etching exhaust gas, trace by-products, and adsorbed halogen particles retained on the etching interface. Through airflow entrainment and vacuum pumping, the stable products and unreacted residues after the reaction are carried out of the process chamber, reducing the concentration of halogen particles on the etching interface. In other words, by introducing an oxidizing plasma treatment process after the etching step containing halogen gases, the sidewalls of the oxide semiconductor material film are not scooped out through the synergistic effect of the three mechanisms of chemical reaction consumption, surface passivation, and plasma gas flow entrainment activation and desorption at the etching interface, thereby improving the integrity of the device structure and the reliability of the process.

[0031] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0032] This application provides an etching method that can be applied to the manufacturing process of various semiconductor devices, especially in process steps that require precise patterning etching of multilayer thin films containing oxide semiconductor materials, such as the patterning etching of the resistive switching functional layer of resistive random access memory, but is not limited thereto. Figure 2 This is a flowchart illustrating an etching method provided in an embodiment of this application. Figure 2 As shown, the etching methods include: Step S100: Provide a stacked structure, the stacked structure including a stacked first material layer and a second material layer, wherein the material of the first material layer is an oxide semiconductor material; and, Step S200: Etch the stacked structure layer by layer in the order of film layer stacking. The process gas for etching the second material layer includes halogen gas. After etching the second material layer, the etching interface is treated with oxidizing plasma.

[0033] Figures 3-7 This is a schematic diagram of the structure corresponding to the steps of the etching method provided in an embodiment of this application. Next, we will combine... Figures 3-7 The etching method provided in one embodiment of this application will be described in detail.

[0034] like Figure 3 As shown, in step S100, a substrate 100 is provided. The substrate 100 can be a silicon substrate, a silicon-on-insulator (SOI) substrate, or any other suitable substrate, on which a bottom electrode or other functional layer (not shown) may have been formed. A stacked structure 200 has been formed on the substrate 100. The stacked structure 200 includes a stacked first material layer 201 and at least one second material layer. The material of the first material layer 201 is an oxide semiconductor material, such as indium gallium zinc oxide (IGZO), indium zinc oxide (IZO), indium gallium oxide (IGO), or other suitable oxide semiconductor materials; the material of the second material layer is typically a dielectric material, such as hafnium oxide (HfO2), zirconium oxide (ZrO2), aluminum oxide (Al2O3), titanium oxide (TiO2), or other high-k dielectric or low-k dielectric materials.

[0035] In some embodiments, the stacked structure is a resistive switching functional layer, the first material layer 201 is a dielectric material layer, and the second material layer is a metal oxide semiconductor layer, but this should not be limited thereto.

[0036] Furthermore, the stacked structure 200 has two second material layers, with the first material layer 201 sandwiched between the two second material layers, forming a sandwich-like structure. For ease of distinction, the second material layer on the upper surface of the first material layer 201 is referred to as the upper second material layer 202b, and the second material layer on the lower surface of the first material layer 201 is referred to as the lower second material layer 202a. The materials of the upper second material layer 202b and the lower second material layer 202a can be the same or different.

[0037] Of course, in some embodiments, the stacked structure 200 may include only one second material layer, which may be located on the upper or lower surface of the first material layer 201. That is, the stacking order of the first material layer 201 and the second material layer is not restricted.

[0038] In some embodiments, the top surface of the stacked structure 200 has a mask layer 300, which is a patterned film layer used to pattern the stacked structure 200.

[0039] like Figures 4-7 As shown, in step S200, using the mask layer 300 as a mask, the stacked structure 200 is etched layer by layer along the order of film layer stacking to form trenches in the stacked structure 200. In the step of etching the second material layer, the process gas utilizes oxidizing plasma to treat the etching interface. This step of treating the etching interface with oxidizing plasma can effectively solve the problem of side-cutting of the first material layer 201. Step S200 will be described in more detail below with reference to a specific embodiment of the etching method applied to a structure with two second material layers.

[0040] like Figure 4 As shown, the upper second material layer 202b is first etched to open a window that exposes the first material layer 201. During the etching of the upper second material layer 202b, the process gas includes halogen gases. In some embodiments, assuming the material of the upper second material layer 202b is HfO2, the gas used for etching the upper second material layer 202b includes halogen gases (such as Cl2) and / or halide gases (such as BCl3), and an inert gas (such as Ar) is added as a dilution and bombardment gas. Under the action of plasma, Cl2 and BCl3 dissociate to generate highly reactive chlorine radicals (Cl·) and boron-containing chlorine reactive groups (BCl2·, BCl·). These reactive particles react chemically with HfO2 to generate volatile products, which are then removed by a vacuum pump, thereby achieving anisotropic etching.

[0041] When etching the upper second material layer 202b, the flow rate of halogen gas and / or halide gas can be 150 sccm to 200 sccm; the flow rate of inert gas can be 100 sccm to 200 sccm; the gas pressure in the process chamber can be 5 mT to 10 mT; the power of the upper RF power supply (source power) can be 900 W to 1100 W; the power of the lower RF power supply (bias power) can be 200 W to 400 W; the temperature of the substrate support disk used to support the wafer can be 60 °C to 80 °C; and the etching process duration can be 10 s to 20 s. These parameters are selected to ensure effective and uniform etching of the upper second material layer 202b while controlling plasma damage.

[0042] After the etching step is completed, the predetermined area of ​​the upper second material layer 202b is removed, exposing the interface area of ​​the lower first material layer 201. At this time, a large amount of active residues from the etching gas, especially chlorine free radicals, chloride ions, and boron-containing chlorine active groups, will be physically adsorbed and retained on the sidewalls of the etched trench, the exposed surface of the first material layer 201, and in the chamber environment.

[0043] After etching the upper second material layer 202b, the etching interface is treated with oxidizing plasma. In this step, oxidizing gases (such as O2 and / or O3) are introduced into the process chamber and ionized by applying radio frequency power to generate oxidizing plasma (such as oxygen plasma).

[0044] When oxidizing plasma is used to treat the etched interface, on the one hand, the oxidizing plasma reacts chemically with residual halogen free radicals and other active groups (such as boron-containing chlorine groups BCl2·, BCl·, etc.) on the etched interface. For example, it oxidizes chlorine free radicals (such as Cl·) to generate ClO. x Stable, non-corrosive, and easily extracted gaseous compounds oxidize boron-containing chlorine active groups (such as BCl2·, BCl·, etc.) to generate BO. x Stable inert products containing elements such as B, O, and Cl consume and neutralize the corrosion source at its chemical origin. On the other hand, the highly active oxidizing plasma will at least slightly oxidize the surface of the exposed first material layer 201, growing an ultra-thin and dense passivation layer in situ. Of course, the oxidizing plasma can also slightly oxidize the sidewalls of the second material layer, allowing an ultra-thin and dense passivation layer to grow in situ on the sidewalls of the second material layer as well. This passivation layer is a physical barrier with high chemical stability, which can effectively inhibit the lateral erosion of the first material layer 201 by subsequent process steps or environmental factors. In addition, the high-flow-rate oxidizing plasma can also form a directional airflow field in the process chamber, replacing the etching exhaust gas, trace by-products, and adsorbed halogen particles retained on the etching interface (especially the sidewalls of the first material layer 201), entraining and carrying away the stable products generated by the reaction and unreacted residues, further reducing the concentration of halogen particles on the etching interface. Oxidizing plasma works synergistically on the etching interface through a triple mechanism of chemical reaction consumption, surface passivation, and plasma gas flow entrainment activation and desorption, preventing the first material layer 201 from being side-cut, thus improving the integrity of the device structure and the reliability of the process.

[0045] In some embodiments, when using oxidizing plasma to treat the etched interface, the flow rate of the oxidizing gas can be 100 sccm to 200 sccm, such as 101 sccm, 113 sccm, 125 sccm, 138 sccm, 150 sccm, 162 sccm, 175 sccm, 188 sccm, 198 sccm, etc. This ensures that sufficient active oxidizing plasma participates in the halogen quenching reaction, while forming a stable directional gas flow field, balancing chemical reaction efficiency and physical purging and replacement effects, and ensuring uniform and continuous growth of the passivation layer. If the flow rate of the oxidizing gas is too low, the amount of oxidizing plasma generated will be insufficient to fully neutralize the residual halogen particles, and the gas flow purging and replacement ability will also be weak, resulting in incomplete residue removal, and the formed passivation layer may be discontinuous, failing to provide good protection and barrier effects. If the flow rate of the oxidizing gas is too high, it may excessively dilute the plasma concentration, leading to plasma instability, a decrease in the mean free path of ions, and potentially causing gas flow turbulence, which in turn causes by-product redeposition and increases process costs.

[0046] In some embodiments, when using oxidizing plasma to treat the etched interface, the gas pressure can be 10mT~20mT, such as 11mT, 12mT, 13mT, 14mT, 15mT, 16mT, 17mT, 18mT, 19mT, 20mT, etc. This can match the plasma dissociation efficiency and directional transport characteristics, ensuring sufficient generation of oxidizing plasma to penetrate deep into the etched interface for residue removal, while also controlling anisotropy to avoid over-oxidation and structural damage. If the gas pressure is too low, the mean free path of the particles is too long, the collision probability is low, the dissociation efficiency of the oxidizing gas is insufficient, the reactivity is weak, and it cannot fully neutralize the residual halogen particles; if the gas pressure is too high, particle scattering is aggravated, the isotropy of the oxidizing plasma is enhanced, which may lead to non-selective, excessively large-area oxidation, or even damage to the upper second material layer 202b.

[0047] In some embodiments, when treating the etching interface with oxidizing plasma, the temperature of the substrate carrier can be 40°C to 60°C, such as 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C, 59°C, etc. Appropriately increasing the wafer temperature helps reduce the surface adsorption force of halogen particles, promotes their desorption, and improves the surface diffusion and migration ability of oxidizing plasma, which is beneficial for forming a uniform, dense, and defect-free passivation layer without introducing additional thermal stress damage. If the wafer temperature is too low, halogen particles and etching byproducts are easily and firmly adsorbed at the etching interface, the surface diffusion reaction rate of oxidizing plasma is low, and the passivation layer grows slowly and has poor density. If the wafer temperature is too high, it will introduce additional thermal stress to the second material layer, and at the same time, it will aggravate the germination of intrinsic defects at the etching interface, and even cause problems such as coarsening of the already formed passivation layer grains and deterioration of interface flatness.

[0048] In some embodiments, when using oxidizing plasma to treat the etched interface, the power of the upper radio frequency power supply can be 900W~1100W, such as 920W, 940W, 960W, 980W, 1000W, 1020W, 1040W, 1060W, 1080W, 1095W, etc., to stably excite high-density oxidizing plasma, ensuring sufficient dissociation of the oxidizing gas, meeting the requirements of halogen particle chemical reaction quenching and interface passivation, while controlling the ion bombardment intensity to avoid sputtering damage to the existing thin film structure. If the power of the upper radio frequency power supply is too low, the efficiency of generating oxidizing plasma from the dissociation of the oxidizing gas will be low, the concentration of active species will be insufficient, and halogen quenching and interface passivation cannot be completed efficiently; if the power of the upper radio frequency power supply is too high, the ion bombardment energy will be too strong, which may cause sputtering damage to the existing structure, destroy the integrity of the thin film structure, and generate too many high-energy ions, triggering unnecessary side reactions.

[0049] In some embodiments, when using oxidizing plasma to treat the etched interface, the process duration can be 10s to 20s, such as 11s, 12s, 13s, 14s, 15s, 16s, 17s, 18s, 19s, 20s, etc. This provides an optimal process window for the saturation of the residual chemical reaction of halogen particles, the activation and desorption by the plasma gas flow, and the uniform formation of the passivation layer. This can fully achieve the functions of residue removal and interface protection, while avoiding morphological distortion and stress defects caused by overprocessing. If the process duration is too short, the residual chemical reaction of halogen particles, the activation and desorption by the plasma gas flow, and the growth of the passivation layer will not reach saturation, resulting in incomplete residue removal, insufficient passivation layer thickness, and weak protection. If the process duration is too long, it can easily cause over-oxidation, excessively thick passivation layer, changes in trench morphology and size, introduction of additional interface stress, and reduction of the process window and production efficiency.

[0050] It is understandable that after the etching of the upper second material layer 202b is completed, the lower first material layer 201 is exposed (the first material layer 201 may have been etched as well). Since the first material layer 201 is subjected to oxidizing plasma treatment after etching, the first material layer 201 can be prevented from being side-cut.

[0051] It should be noted that, since the sidewalls of the first material layer 201 may not be exposed or only a very small portion may be exposed after etching the upper second material layer 202b, the erosion ability of halogen residual particles and etching byproducts on the sidewalls of the first material layer 201 is limited. In some embodiments, the step of oxidizing plasma treatment after etching the upper second material layer 202b can be omitted.

[0052] like Figure 5As shown, the first material layer 201 is etched continuing along the order of film stacking. Since the first material layer 201 is an oxide semiconductor material, such as IGZO, this etching step uses a different process gas formulation than the etching of the upper second material layer 202b. For example, assuming the first material layer 201 is IGZO, the process gas used for etching the first material layer 201 can include hydrocarbon gases (such as CH4) and can be supplemented with an inert gas (such as Ar). Under the action of plasma, CH4 dissociates into methyl radicals (CH3·), which react chemically with metal atoms such as indium (In), gallium (Ga), and zinc (Zn) in IGZO to generate corresponding low-boiling-point organometallic compounds, such as trimethylindium, trimethylgallium, and dimethylzinc. These products are easily desorbed from the surface and extracted. At the same time, the Ar plasma physically bombards the surface of the first material layer 201 under the action of bias voltage, promoting the breaking of chemical bonds and the desorption of products, thus achieving precise and low-damage etching of the first material layer 201.

[0053] In some embodiments, when etching the first material layer 201, the flow rate of the hydrocarbon gas can be 30 sccm to 50 sccm; the flow rate of the inert gas can be 50 sccm to 100 sccm; the gas pressure in the process chamber can be 8 mT to 15 mT; the power of the upper RF power supply can be 300 W to 500 W; the power of the lower RF power supply can be 30 W to 70 W; the temperature of the substrate carrier can be 50 °C to 65 °C; and the process duration can be 15 s to 25 s. These parameters are selected to ensure high-precision and high-uniformity etching of the first material layer 201, while controlling the damage caused by the plasma and avoiding exacerbation of side-cutting.

[0054] like Figure 6 As shown, the lower second material layer 202a is etched. The process formulation for this step is basically the same as that for etching the upper second material layer 202b. The process gases can also include halogen gases (such as Cl2 and BCl3), with the addition of inert gases (such as Ar) as dilution and bombardment gases. The process parameters can be selected within a similar range to the process conditions for etching the upper second material layer 202b. For example: the flow rates of halogen and halide gases can be 150 sccm to 200 sccm; the flow rate of inert gases can be 100 sccm to 200 sccm; the gas pressure in the process chamber can be 5 mT to 10 mT; the power of the upper RF power supply can be 900 W to 1100 W; the power of the lower RF power supply can be 200 W to 400 W; the temperature of the substrate support disk used to support the wafer can be 60℃ to 80℃; and the etching process duration can be 10 s to 20 s.

[0055] It is worth noting that during the etching of the lower second material layer 202a, the etching process can be controlled so that only a portion of the thickness of the lower second material layer 202a is removed, rather than being completely etched away. This means that after this etching step, a certain thickness of the lower second material layer 202a remains at the bottom of the trench. The purpose of this retention step will be explained in the following description.

[0056] After removing a portion of the thickness of the lower second material layer 202a, the etching step again uses halogen gases, inevitably introducing and leaving highly reactive halogen particles, active groups, and etching byproducts on the etching interface (especially the newly exposed sidewalls of the first material layer 201). To prevent these residual particles from causing lateral erosion of the sidewalls of the first material layer 201, the etching interface is treated again with oxidizing plasma after etching the lower second material layer 202a. The treatment method, mechanism, and range of process conditions are the same as those described above for the oxidizing plasma treatment after etching the upper second material layer 202b, and will not be repeated here. Through the second oxidizing plasma treatment, the chemical corrosion source is removed again and the passivation layer of the sidewalls of the first material layer 201 is strengthened, ensuring continuous protection of the sidewalls of the first material layer 201 throughout the entire etching process of the multi-layer second material layers, and minimizing the risk of the first material layer 201 being eroded laterally.

[0057] Furthermore, although the halogen residue particles are removed and a passivation layer is formed in situ through oxidizing plasma treatment, the first material layer 201 may still face slow erosion from air, water vapor or other pollutants during subsequent process transfers, exposure to the atmosphere or subsequent wet processes, posing a long-term reliability risk.

[0058] Based on this, such as Figure 7 As shown, after the overall etching step of the stacked structure 200 is completed, the surface of the lower second material layer 202a can be bombarded with inert plasma to form a sealing layer 401 at least on the sidewall of the first material layer 201.

[0059] Specifically, an inert gas (such as Ar) is introduced into the process chamber and ionized to generate inert plasma. Under the directional bombardment of the inert plasma, the surface material of the lower second material layer 202a will be physically sputtered. The atoms or atomic groups (such as HfO2 particles) of the lower second material layer 202a that are bombarded out migrate to the exposed sidewall of the first material layer 201 and are redeposited, thereby forming a closed layer 401. Since this sputtering migration and redeposition process is isotropic, the sealing layer 401 may eventually form a continuous, dense and conformal sealing layer 401 on the sidewalls and bottom of the entire trench. That is, the sealing layer 401 can completely cover and isolate the exposed and sensitive sidewalls of the first material layer 201, the sidewalls of the upper second material layer 202b, and the sidewalls of the lower material layer, forming a robust inert protective barrier that completely blocks the path of air, water vapor, and any residual active particles to intrude and corrode, eliminating the causes of subsequent side-cutting, hydration deterioration, or thermal stress cracking. Figure 8 An electron microscope image of the stacked structure 200 etched using the etching method provided in this application, as an embodiment of this application, is shown below. Figure 8 As can be seen, the sealing layer 401 continuously covers the sidewalls of the first material layer 201, the sidewalls of the upper second material layer 202b, and the sidewalls of the lower material layer, and may even cover the sidewalls of the mask layer 300, thus achieving a good protective effect.

[0060] It is understandable that the material of the sealing layer 401 formed in this way is the same as that of the lower second material layer 202a, which serves as the sputtering source, such as HfO2. This ensures that the sealing layer 401 has a high degree of lattice compatibility, matching coefficient of thermal expansion, and strong interfacial bonding with the original stacked materials, avoiding the introduction of additional interfacial mismatch, lattice distortion, or thermal stress concentration. Alternatively, the material of the sealing layer 401 can be adaptively changed according to the material of the lower second material layer 202a. For example, if the lower second material layer 202a is ZrO2, Al2O3, or TiO2, then the sealing layer 401 formed by sputtering redeposition will also be composed of these materials accordingly.

[0061] In some embodiments, the thickness of the sealing layer 401 can be 3 to 5 angstroms, such as 3.1 angstroms, 3.3 angstroms, 3.5 angstroms, 3.7 angstroms, 3.9 angstroms, 4.1 angstroms, 4.3 angstroms, 4.5 angstroms, 4.7 angstroms, 4.9 angstroms, etc. This thickness range is sufficient to form a continuous and pinhole-free dense physical barrier to effectively isolate external corrosive substances. At the same time, due to its extremely thin characteristics, it hardly changes the original critical dimensions of the trench and does not introduce significant additional stress, thereby providing robust protection while maximizing the maintenance of the dimensional accuracy and mechanical integrity of the device structure. If the thickness of the sealing layer 401 is less than 3 angstroms, a continuous film layer may not be formed, resulting in localized exposed defects and leading to protection failure. If the thickness of the sealing layer 401 is greater than 5 angstroms, although the protective capability is enhanced, it may begin to affect the morphology and dimensions of the trench and may generate additional interfacial stress.

[0062] In some embodiments, when bombarding the surface of the lower second material layer 202a with inert plasma, the flow rate of the inert gas can be 150 sccm to 350 sccm, such as 160 sccm, 180 sccm, 205 sccm, 230 sccm, 255 sccm, 280 sccm, 305 sccm, 330 sccm, 345 sccm, etc. This flow rate range can stably maintain the inert plasma ignition and provide a moderate ion concentration to ensure a mild sputtering efficiency, while taking into account both the continuity of the sealing layer 401 and the fidelity of the original etched morphology. If the flow rate of the inert gas is too low, the inert plasma ignition is unstable, the ion concentration is too low, the sputtering bombardment flux is insufficient, the sputtering migration redeposition amount is small, and a continuous and dense sealing layer 401 cannot be formed. If the flow rate of the inert gas is too high, the inert plasma density is too large, the ion collision scattering is aggravated, and excessive bombardment causes excessive wear and morphology distortion of the lower second material layer 202a. At the same time, the process airflow turbulence is prone to microparticle recontamination.

[0063] In some embodiments, when bombarding the surface of the lower second material layer 202a with inert plasma, the gas pressure can be 8mT~20mT, such as 9mT, 10mT, 12mT, 14mT, 16mT, 18mT, 19mT, etc., to control the mean free path and bombardment angle of the inert plasma, achieving gentle and directional sputtering, which is beneficial for uniform redeposition of the sidewalls, forming a closed layer 401 without damaging the existing stacked structure morphology. If the gas pressure is too low, the mean free path of the ions in the inert plasma is too long, and the directional bombardment is too strong, which can easily cause hard bombardment damage to the trench sidewalls; if the gas pressure is too high, particle scattering is severe, and the anisotropic sputtering becomes disordered, making it difficult to form a uniform and continuous closed layer 401 on the trench sidewalls.

[0064] In some embodiments, when bombarding the surface of the lower second material layer 202a with inert plasma, the power of the upper radio frequency power supply can be 350W~600W, such as 370W, 400W, 430W, 460W, 490W, 520W, 550W, 580W, 595W, etc., to generate stable and moderately energetic plasma, achieving controllable temperature sputtering redeposition, performing only surface reconstruction and sealing, without generating additional etching damage. If the power of the upper radio frequency power supply is too low, the inert plasma density is insufficient, the inert plasma ignition is weak and the quantity is small, the sputtering migration efficiency is insufficient, and the sealing layer 401 is thin and discontinuous; if the power of the upper radio frequency power supply is too high, the inert plasma energy is too strong, the high-energy ions generate a strong physical etching effect, reverse etching the sidewalls of the second material layer and the first material layer 201, which aggravates the morphology damage.

[0065] In some embodiments, when the surface of the lower second material layer 202a is bombarded with inert plasma, the power of the lower radio frequency power supply can be 200W~400W, such as 220W, 240W, 260W, 280W, 300W, 320W, 340W, 360W, 380W, 395W, etc., to precisely control the ion incident energy and angle, ensuring that the sealing layer 401 can fully cover the sidewalls of the high aspect ratio trench. If the power of the lower radio frequency power supply is too low, the orientation of the inert plasma is poor, making it difficult to focus sputtering, resulting in uneven film formation of the sealing layer 401; if the power of the lower radio frequency power supply is too high, the ion bombardment energy is too large, causing deep lattice damage and interface stress concentration, introducing leakage and reliability risks.

[0066] In some embodiments, when the surface of the lower second material layer 202a is bombarded with inert plasma, the temperature of the substrate support disk can be 50°C to 65°C, such as 51°C, 53°C, 55°C, 57°C, 59°C, 61°C, 63°C, 64°C, etc., to optimize the surface adsorption and migration characteristics of sputtered particles, which is beneficial for forming a dense, low-stress, and well-adhesive sealing layer 401. If the temperature of the substrate support disk is too low, the surface adsorption energy of the etching interface is large, and the sputtered particles are not easy to adhere to the trench sidewalls and are easy to detach, making it difficult to form a dense sealing layer 401. If the temperature of the substrate support disk is too high, the thermal stress of the thin film increases, and the sputtered redeposited sealing layer 401 is prone to grain coarsening and interface mismatch, and subsequent heat treatment is prone to peeling and cracking.

[0067] In some embodiments, when bombarding the surface of the lower second material layer 202a with inert plasma, the process duration can be 15s to 30s, such as 16s, 18s, 20s, 22s, 24s, 26s, 28s, 29s, etc., to ensure the full completion of sputtering, migration, and film formation processes, forming a process window with controllable dimensions and optimal stress. If the process duration is too short, sputtering migration, surface wetting and spreading, and film coverage will be insufficient, resulting in local exposed gaps in the sealing layer 401 and failure of protection. If the process duration is too long, excessive sputtering and redeposition will occur, resulting in an excessively thick sealing layer 401, misalignment of critical trench dimensions, and accumulation of additional interfacial stress.

[0068] Furthermore, the steps of etching the stacked structure 200, treating the etching interface with oxidizing plasma, and bombarding the surface of the lower second material layer 202a with inert plasma are all performed in situ within the same process chamber without transferring the wafer. This not only eliminates the risks of contamination, oxidation, and particle adsorption that may result from wafer exposure to the atmosphere, but also avoids the negative impact of thermal history and vacuum environment changes caused by cross-cavity transfer on thin film stress. At the same time, it significantly shortens the process cycle and improves production capacity and equipment utilization.

[0069] The above embodiments are illustrated using a stacked structure 200 having two second material layers with a first material layer 201 sandwiched between them. However, the application of this method is not limited to this. In other embodiments, the stacked structure 200 may have only one second material layer, which may be located only on the upper surface of the first material layer 201 or only on the lower surface of the first material layer 201. When there is only an upper second material layer 202b, the interface is treated with oxidizing plasma after etching this layer, and then the first material layer 201 is etched. When there is only a lower second material layer 202a, the first material layer 201 can be etched first, then the second material layer can be etched, and the oxidizing plasma treatment step can be performed after etching the second material layer. If there is a lower second material layer 202a and it is desired to form a sealing layer 401, a portion of the thickness is also retained when etching the lower second material layer 202a, and an inert plasma bombardment step is performed at the end. Regardless of the structure, as long as the etching of a second material layer containing halogen gases is performed, followed by an oxidizing plasma treatment step, the effect of preventing the first material layer 201 from being side-penetrated can be achieved. Furthermore, whenever necessary, an oxidizing plasma treatment step can be performed after etching each second material layer to ensure protection throughout the entire process.

[0070] Based on this, one embodiment of this application also provides a semiconductor process apparatus. Figure 9 This is a schematic diagram of the structure of a semiconductor process equipment provided in an embodiment of this application, as shown below. Figure 9As shown, the semiconductor process equipment includes a process chamber 20, an inlet assembly 20A, an upper electrode assembly 20B, a lower electrode assembly 20C, and a controller. Figure 9 (Not shown in the image), the controller includes at least one processor and at least one memory, the memory storing a computer program that, when executed by the processor, implements the etching method described above.

[0071] For example, the controller can be a host computer or a slave computer. The controller can open the valve of the air inlet assembly 20A to introduce the corresponding process gas into the process chamber 20; the controller can also control the flow rate of the process gas by controlling the opening and closing degree of the valve of the air inlet assembly 20A. The controller can also control the air extraction assembly to evacuate the interior of the process chamber 20, thereby controlling the pressure inside the process chamber 20 and removing reaction byproducts.

[0072] The upper electrode assembly 20B includes an RF coil 21, an upper RF power supply 23, and an upper matching unit 25. The controller is also used to control the upper RF power supply 23 to provide upper electrode power to the RF coil 21 through the upper matching unit 25, so that the RF coil 21 excites the process gas inside the process chamber 20 to generate plasma.

[0073] The lower electrode assembly 20C includes a wafer carrier 22, a lower RF power supply 24, and a lower matching unit 26. The controller is also used to control the lower RF power supply 24 to provide lower electrode power to the lower electrode of the wafer carrier 22 through the lower matching unit 26, so that the lower electrode of the wafer carrier 22 is provided with RF bias voltage to attract plasma above the object to be etched 10 to bombard the object to be etched 10.

[0074] The semiconductor process equipment in this embodiment can be either an inductively coupled plasma (ICP) etching apparatus or a capacitively coupled plasma (CCP) etching apparatus. This application does not limit the type of semiconductor process equipment.

[0075] It should be noted that the various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. For the systems disclosed in the embodiments, since they correspond to the methods disclosed in the embodiments, the descriptions are relatively simple, and relevant parts can be referred to the method section.

[0076] It should also be noted that although preferred embodiments have been disclosed above, these embodiments are not intended to limit this application. Any person skilled in the art can make many possible variations and modifications to the technical solutions of this application, or modify them into equivalent embodiments, without departing from the scope of the technical solutions of this application. Therefore, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of this application, without departing from the content of the technical solutions of this application, shall still fall within the scope of protection of the technical solutions of this application.

[0077] It should also be understood that, unless otherwise specified or indicated, the terms “first,” “second,” “third,” etc., in the specification are used only to distinguish the various components, elements, and steps in the specification, and not to indicate the logical or sequential relationships between the various components, elements, and steps.

[0078] Furthermore, it should be recognized that the terminology described herein is used only to describe particular embodiments and is not intended to limit the scope of this application. It must be noted that the singular forms “a” and “an” as used herein include plural bases unless the context clearly indicates the opposite. For example, a reference to “a step” or “an apparatus” means a reference to one or more steps or apparatuses, and may include secondary steps and secondary apparatuses. All conjunctions used should be understood in the broadest sense. Also, the word “or” should be understood as having the definition of logical “or”, not logical “exclusive OR”, unless the context clearly indicates the opposite. Furthermore, implementations of the methods and / or devices in the embodiments of this application may include performing selected tasks manually, automatically, or in combination.

Claims

1. An etching method, characterized in that, include: A stacked structure is provided, the stacked structure comprising a stacked first material layer and a second material layer, wherein the material of the first material layer is an oxide semiconductor material; as well as, The stacked structure is etched layer by layer in the order of film layer stacking. The process gas for etching the second material layer includes halogen gas, and after etching the second material layer, the etching interface is treated with oxidizing plasma.

2. The etching method according to claim 1, characterized in that, Also includes: After treating the etched interface with the oxidizing plasma, a passivation layer is formed at least on the sidewall of the first material layer.

3. The etching method according to claim 1, characterized in that, The stacked structure has one layer of the second material, which is located on the upper or lower surface of the first material layer; or, the stacked structure has two layers of the second material, with the first material layer located between the two layers of the second material.

4. The etching method according to claim 3, characterized in that, After etching each of the second material layers, the etched interface is treated with the oxidizing plasma.

5. The etching method according to any one of claims 1 to 4, characterized in that, The oxidizing gas is ionized to generate the oxidizing plasma. When the oxidizing plasma is used to treat the etched interface, the flow rate of the oxidizing gas is 100 sccm to 200 sccm, the gas pressure is 10 mT to 20 mT, the temperature of the substrate carrier is 40°C to 60°C, the power of the on-board RF power supply is 900 W to 1100 W, and the process time is 10 s to 20 s.

6. The etching method according to any one of claims 1 to 4, characterized in that, The second material layer is located at least on the lower surface of the first material layer. When etching the stacked structure, a portion of the thickness of the second material layer on the lower surface of the first material layer is removed. After etching the stacked structure, the surface of the second material layer is bombarded with inert plasma to form a sealing layer at least on the sidewall of the first material layer.

7. The etching method according to claim 6, characterized in that, The material of the sealing layer is the same as that of the second material layer; and / or, the thickness of the sealing layer is 3 to 5 angstroms.

8. The etching method according to claim 6, characterized in that, The inert gas is ionized to generate the inert plasma. When the surface of the second material layer is bombarded with the inert plasma, the flow rate of the inert gas is 150 sccm to 350 sccm, the gas pressure is 8 mT to 20 mT, the power of the upper RF power supply is 350 W to 600 W, the power of the lower RF power supply is 200 W to 400 W, the temperature of the substrate carrier is 50 °C to 65 °C, and the process time is set to 15 s to 30 s.

9. The etching method according to claim 1, characterized in that, The halogen gas includes halogen gas and / or halide gas; during etching of the second material layer, the flow rate of the halogen gas and / or the halide gas is 150 sccm to 200 sccm, the gas pressure is 5 mT to 10 mT, the power of the on-board RF power supply is 900 W to 1100 W, the temperature of the substrate carrier is 60°C to 80°C, and the process time is 10 s to 20 s; and / or, The process gas used to etch the first material layer includes a hydrocarbon gas. When etching the first material layer, the flow rate of the hydrocarbon gas is 30 sccm to 50 sccm, the gas pressure is 8 mT to 15 mT, the power of the upper RF power supply is 300 W to 500 W, the power of the lower RF power supply is 30 W to 70 W, the temperature of the substrate carrier is 50 °C to 65 °C, and the process time is 15 s to 25 s.

10. The etching method according to claim 1, characterized in that, The stacked structure is a resistive switching functional layer, the first material layer is a dielectric material layer, and the second material layer is a metal oxide semiconductor layer.

11. A semiconductor process apparatus, characterized in that, The method includes a process chamber and a controller, characterized in that the controller includes at least one processor and at least one memory, the memory storing a computer program, which, when executed by the processor, implements the etching method as described in any one of claims 1 to 10.