A VO2 heterojunction optoelectronic neuromorphic device, its fabrication method and application
By developing a structure and fabrication method for VO2 heterojunction optoelectronic neuromorphic devices, the problems of insufficient uniformity and multimodal capability in the large-scale fabrication of VO2 neuromorphic devices were solved. This enabled efficient sensing and coordinated control of optical and electrical signals, expanding the device's functionality and making it suitable for smart sensors and neuromorphic chips.
Patent Information
- Application Number
- CN202611094490.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing VO2 neuromorphic computing devices suffer from poor uniformity, limited process compatibility, and insufficient multimodal capabilities during large-scale fabrication, making it difficult to achieve multimodal information fusion and functional expansion.
The VO2 heterojunction optoelectronic neuromorphic device structure includes a substrate layer, a vanadium dioxide thin film layer, and an optoelectronic material layer. Through in-situ vacuum magnetron sputtering and annealing, a heterojunction is formed by combining a wide bandgap semiconductor optoelectronic material layer and a vanadium dioxide thin film layer to achieve efficient sensing, conversion, and coordinated control of optical and electrical signals. Furthermore, the device's functionality is broadened by combining photoelectric response with metal-insulator phase transition.
It achieves uniformity and multimodal capability in the large-scale fabrication of VO2 neuromorphic devices. Through the coordinated control of multiple physical fields such as electricity, heat, and light, it breaks through the limitations of traditional single-processing of electrical signals, dynamically adjusts the threshold of neurons, expands the computational dimension, and is suitable for smart sensors and neuromorphic chips.
Smart Images

Figure CN123124671A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of neuromorphic device technology, and in particular to a VO2 heterojunction optoelectronic neuromorphic device, its fabrication method, and its application. Background Technology
[0002] With the slowdown of Moore's Law and the arrival of the big data era, the "memory wall" and "power wall" problems caused by the physical separation of computing and storage units in the traditional von Neumann architecture are becoming increasingly severe, becoming a core bottleneck for improving the computing power of artificial intelligence. Neuromorphic computing, as a new generation of revolutionary computing paradigm, achieves in-memory computing by simulating the parallel processing mechanism and plastic structure of neurons and synapses in the human brain, providing a key path to overcome the bottlenecks in computing power and energy efficiency. Among them, vanadium dioxide (VO2), with its unique metal-insulator phase transition (MIT) characteristics, sub-nanosecond response speed, high resistance change amplitude, and intrinsic memristor behavior, has become a core candidate material for building next-generation neuromorphic hardware. Its physical properties are highly compatible with the biological synaptic weight regulation and neuronal integral-discharge dynamics, which is crucial for meeting the high energy efficiency and low latency requirements of edge computing, autonomous driving, and complex AI tasks.
[0003] Despite the promising prospects of VO2 neuromorphic computing, its practical application still faces numerous challenges, including: High costs of advanced methods (such as ALD and low-temperature epitaxy) for large-scale integration, difficulties in achieving large-area uniform deposition, reliance on lattice-matched substrates (such as Al2O3) leading to industrialization difficulties, uneven phase transition thresholds and resistance distributions between devices, resulting in poor array reliability and limited processing capabilities for complex tasks; mature processes with good uniformity, such as magnetron sputtering, struggle to precisely control the fabricated material, resulting in poor reproducibility. Furthermore, existing research largely focuses on electrical signal processing, lacking multimodal coupling capabilities involving light, heat, and pressure, limiting functional expansion and hindering the realization of brain-like cross-modal information fusion, leading to limited functionality; simultaneously, the correlation mechanism between microstructural evolution during phase transitions (such as lattice distortion and carrier behavior) and macroscopic performance is not fully understood, restricting precise design and performance optimization.
[0004] Therefore, existing technologies still need to be improved and developed. Summary of the Invention
[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a VO2 heterojunction optoelectronic neuromorphic device, its fabrication method and application, aiming to solve the problems of poor uniformity, limited process compatibility and lack of multimodality in the large-scale fabrication of existing neuromorphic devices.
[0006] The technical solution of the present invention is as follows: A VO2 heterojunction optoelectronic neuromorphic device includes a substrate layer, a vanadium dioxide thin film layer, a photoelectric material layer, and a top electrode layer stacked sequentially from bottom to top; the vanadium dioxide thin film layer and the photoelectric material layer form a heterostructure; the top electrode layer includes a first top electrode layer in contact with the photoelectric material layer and a second top electrode layer in contact with the vanadium dioxide thin film layer.
[0007] In the VO2 heterojunction optoelectronic neuromorphic device, the thickness of the vanadium dioxide thin film layer is greater than 20 nm.
[0008] The VO2 heterojunction optoelectronic neuromorphic device, wherein the thickness of the optoelectronic material layer is greater than 60 nm.
[0009] In the aforementioned VO2 heterojunction optoelectronic neuromorphic device, the optoelectronic material layer is selected from one of indium gallium oxide, indium zinc oxide, zinc oxide, indium oxide, cadmium sulfide, and molybdenum oxide.
[0010] The VO2 heterojunction optoelectronic neuromorphic device, wherein the thickness of the top electrode layer is 60nm~100nm; the material of the top electrode layer is selected from one or more of Au, Cu, Ag, Pt, Ti, and Mo.
[0011] A method for fabricating a VO2 heterojunction optoelectronic neuromorphic device includes the following steps: The substrate was placed on the sample stage, and vanadium dioxide was used as the target material. After in-situ vacuum magnetron sputtering, vacuum annealing was performed to obtain the first product with a vanadium dioxide thin film layer. After patterning one side of the vanadium dioxide thin film layer of the first product, magnetron sputtering is performed in an oxygen-containing atmosphere using optoelectronic material as the target material, followed by annealing to obtain a second product with an optoelectronic material layer. After patterning one side of the vanadium dioxide thin film layer of the second product, a top electrode layer is grown on the vanadium dioxide thin film layer and the optoelectronic material layer by magnetron sputtering to obtain a VO2 heterojunction optoelectronic neuromorphic device.
[0012] The fabrication method of the VO2 heterojunction optoelectronic neuromorphic device, wherein the parameters of the in-situ vacuum magnetron sputtering process include: a vacuum degree of 3e -4 ~5e -4 Pa, argon flow rate of 25 sccm~40 sccm, magnetron sputtering power of 80 W~140 W, sputtering time of 14 min~40 min; the rotation speed of the sample stage is 10 rad / min~30 rad / min.
[0013] The method for fabricating the VO2 heterojunction optoelectronic neuromorphic device includes a vacuum annealing process at a temperature of 450°C to 550°C, a heating rate of no more than 10°C / min, and a vacuum annealing time of 45 min to 80 min.
[0014] The method for fabricating the VO2 heterojunction optoelectronic neuromorphic device, wherein the parameters of the magnetron sputtering coating include: the sputtering gas is a mixture of argon and oxygen, the magnetron sputtering power is 60W~120W, and the sputtering time is 15min~60min. Preferably, the annealing temperature is 300℃~400℃, the annealing time is 30min~90min, and the heating rate of the annealing is 5℃ / min~10℃ / min.
[0015] Application of a VO2 heterojunction opto-neuromorphic device in smart sensors or neuromorphic chips.
[0016] Beneficial Effects: This invention provides a VO2 heterojunction optoelectronic neuromorphic device, its fabrication method, and its application. The VO2 heterojunction optoelectronic neuromorphic device comprises a substrate layer, a vanadium dioxide thin film layer, a photoelectric material layer, and a top electrode layer stacked sequentially from bottom to top. The vanadium dioxide thin film layer and the photoelectric material layer constitute a heterostructure. The top electrode layer includes a first top electrode layer in contact with the photoelectric material layer and a second top electrode layer in contact with the vanadium dioxide thin film layer. This invention utilizes a wide-bandgap semiconductor photoelectric material layer and a vanadium dioxide thin film layer to form a heterojunction. Combined with the physical characteristics of the functional layers, it can extract multimodal features in real time, achieving efficient sensing, conversion, and coordinated control of optical and electrical signals. Simultaneously, by combining photoelectric response with the metal-insulator phase transition of vanadium dioxide, it can achieve independent sensing and decoupling of optical and electrical signals, broadening the functionality of a single device and facilitating neuromorphic computing. Furthermore, the fabrication method, by selecting a suitable target material and controlling the power, argon gas, and vacuum level during sputtering, along with annealing, can obtain a high-purity vanadium dioxide thin film layer. Therefore, this invention systematically solves the bottlenecks in the large-scale fabrication uniformity and multimodal capabilities of VO2 neuromorphic devices through synergistic improvements in materials, structure, and processes. By synergistically regulating the phase transition state of VO2 through multiple physical fields such as electricity, heat, and light, dynamic neuron threshold adjustment is achieved, breaking through the limitations of traditional single-processing of electrical signals. Through multi-dimensional optimization, a quantitative correlation between materials, structure, and function is established, providing a technical path for neuromorphic computing systems and possessing broad prospects for industrial applications. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the structure of a VO2 heterojunction optoelectronic neuromorphic device according to the present invention; Figure 2 This is a schematic diagram of a heterojunction formed by gallium oxide as an optoelectronic material layer and a vanadium dioxide thin film layer; Figure 3 This is a schematic diagram of the process flow for fabricating a VO2 heterojunction optoelectronic neuromorphic device according to the present invention. Figure 4 This is a flowchart illustrating the overall fabrication process of the VO2 heterojunction optoelectronic neuromorphic device in Example 1. Figure 5 This is a DC test diagram of the VO2 heterojunction opto-neuromorphic device of Example 1; Explanation of reference numerals in the attached figures: Substrate layer 10, vanadium dioxide thin film layer 20, optoelectronic material layer 30, top electrode layer 40. Detailed Implementation
[0018] This invention provides a VO2 heterojunction optoelectronic neuromorphic device, its fabrication method, and its application. To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention is further described in detail below. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0019] It will be understood by those skilled in the art that, unless otherwise defined, all terms used herein (including technical and scientific terms) have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as in the context of the prior art, and should not be interpreted in an idealized or overly formal sense unless specifically defined as herein.
[0020] The physical properties of VO2 exhibit a reversible first-order phase transition at approximately 68°C, transforming its crystal structure from a monoclinic phase (VO2(M)) at low temperatures to a tetragonal rutile phase (VO2(R)) at high temperatures. This structural reconstruction is accompanied by dramatic abrupt changes in physical properties: resistivity changes by orders of magnitude, infrared transmittance changes significantly, and strong nonlinear conductivity and memristor effects are observed. The phase transition mechanism is generally considered to be driven by a combination of electron-electron correlation (Mott mechanism) and electron-phonon coupling (Peierls mechanism). In the low-temperature insulating state, VV ion dimerization leads to band splitting, forming a Peierls gap; while in the high-temperature metallic state, lattice symmetry is restored, the gap closes, and electron delocalization results in a sharp increase in conductivity. This phase transition possesses ultrafast sub-nanosecond response speeds and good volatility, providing a solid physical basis for simulating the "leaky integration-and-fire" dynamics of biological neurons at the hardware level.
[0021] To construct efficient neuromorphic systems, the core materials of neurons must meet the following stringent standards: they must possess threshold switching characteristics or negative differential resistance effects to enable the "integration-firing" and signal reset functions of the neuron model. VO2's intrinsic memristor properties naturally meet these requirements: its abrupt changes in resistance can be used to simulate threshold triggering in neurons; its intrinsic memristor behavior supports volatile computation; and its nonlinear conductance during phase transitions further enriches the functional dimensions of the device, enabling it to perform complex logic operations and signal processing with a single device.
[0022] Currently, the fabrication process and device design of VO2 thin films face diverse technical paths and challenges: magnetron sputtering is a mature process with fast deposition rates, but it requires precise control of the argon-oxygen ratio and gas flow rate, and is prone to introducing impurities; the sol-gel method is low-cost and offers flexible composition control, but it has high porosity and poor film density, requiring long-term heat treatment to optimize the structure; hydrothermal / solvothermal methods can precisely control nanostructures, but the high-temperature and high-pressure conditions are harsh, making it difficult to achieve large-area uniform deposition; pulsed laser deposition (PLD) can accurately replicate the target material composition, but it is costly, has a low deposition rate, and is prone to surface sputtering particles. Other studies have also attempted to lower the VO2 phase transition temperature (to near room temperature) by doping with elements such as W, Mo, and Nb, thereby improving the thermal hysteresis loop width, but these dopants may introduce lattice distortion, leading to a decrease in infrared modulation capability; doping uniformity is difficult to guarantee, affecting the overall performance consistency of the film. Current efforts need to break through low-temperature compatible processes, optimize post-processing techniques to balance film quality and production efficiency, and explore new deposition technologies to promote the application of flexible electronics and integrated devices.
[0023] Based on current fabrication technologies, the research status of VO2 neuromorphic devices presents both breakthroughs and challenges: Researchers have achieved precise phase transition control of VO2 thin films by optimizing processes such as magnetron sputtering and PLD, constructing biomimetic neurons and synaptic arrays, and verifying low-power information processing capabilities in scenarios such as single-pulse coding and chaotic edge computing. However, process compatibility remains a core bottleneck—uniformity in large-scale fabrication and device performance are mutually exclusive. Current research focuses on developing low-temperature deposition processes (such as in-situ annealing PLD), introducing doping to control phase transition temperature, constructing heterogeneous synapses by combining oxides such as HfO2, and improving system robustness through algorithm-device co-design.
[0024] The unique integral-discharge characteristics of VO2 material provide a core foundation for its simulation of biological neuron behavior. In biomimetic neuron design, VO2 devices simulate the membrane potential integration mechanism of biological neurons through the process of accumulating charge via voltage pulses: when an external input signal (voltage pulse) is applied continuously, charge gradually accumulates within the VO2 film, and its internal electric field strength increases accordingly. This process is highly similar to the gradual increase in membrane potential after a neuron receives synaptic input. When the accumulated voltage exceeds the phase transition threshold of VO2, the material undergoes an insulator-metal phase transition (IMT), the resistivity drops sharply, and a sudden current pulse is generated. This behavior accurately simulates the characteristic of a neuron triggering an action potential and generating a pulse signal output after its membrane potential reaches the threshold. This threshold switching behavior not only realizes the "integration-firing" function of neurons, but also has the following key advantages: 1) Nanosecond-level phase transition speed: matching the rapid response requirements of biological neurons; 2) Low-energy phase transition mechanism: subthreshold accumulation and overthreshold triggering can be achieved by adjusting the voltage pulse amplitude, with energy efficiency far exceeding that of traditional CMOS devices; 3) Multi-physics coupling characteristics: allowing phase transition behavior to be synergistically controlled by electrical, thermal, and optical signals, expanding the perception dimension of biomimetic neurons. Current research has optimized the phase transition temperature and threshold voltage tunability of VO2 through doping engineering (such as W and Mo doping), and enhanced charge trapping ability by using amorphous / polycrystalline composite structures to simulate the time integration characteristics of neurons. In addition, VO2 neuromorphic chips constructed with memristor arrays have successfully realized brain-like computing functions such as pattern recognition and spiking neural networks, but their cyclic stability and threshold consistency still face challenges from material defects and process fluctuations, requiring further optimization through interface engineering and device structure design.
[0025] Therefore, although VO2-based neuromorphic computing technology has shown unique advantages, existing research still has significant shortcomings in terms of material stability, process compatibility, functional accuracy, integration scale and multimodal capabilities.
[0026] Based on this, such as Figure 1 As shown, the present invention provides a VO2 heterojunction optoelectronic neuromorphic device, comprising a substrate layer 10, a vanadium dioxide thin film layer 20, a photoelectric material layer 30, and a top electrode layer 40 stacked sequentially from bottom to top; the vanadium dioxide thin film layer and the photoelectric material layer constitute a heterostructure; the top electrode layer includes a first top electrode layer in contact with the photoelectric material layer and a second top electrode layer in contact with the vanadium dioxide thin film layer.
[0027] In this embodiment, a heterojunction is constructed using a wide-bandgap semiconductor optoelectronic material layer and a vanadium dioxide thin film layer. Combined with the physical properties of the functional layer, multimodal features can be extracted in real time, enabling efficient sensing, conversion, and coordinated control of optical and electrical signals. Simultaneously, by combining photoelectric response with the metal-insulator phase transition of vanadium dioxide, independent sensing and decoupling of optical and electrical signals can be achieved, broadening the functionality of a single device and facilitating neuromorphic computing. Furthermore, the fabrication method, by selecting a suitable target material and controlling power, argon gas, and vacuum during sputtering, along with annealing, yields a high-purity vanadium dioxide thin film layer. Therefore, this invention, through synergistic improvements in materials, structure, and processes, systematically solves the bottlenecks in the uniformity and multimodal capabilities of VO2 neuromorphic devices in large-scale fabrication. By synergistically controlling the phase transition state of VO2 through multiple physical fields (electric, thermal, and optical), dynamic neuron threshold adjustment is achieved, overcoming the limitations of traditional single-processing of electrical signals. Through multi-dimensional optimization, a quantitative correlation between materials, structure, and function is established, providing a technical path for neuromorphic computing systems and possessing broad industrial application prospects.
[0028] Specifically, by utilizing a photoelectric material layer as a wide bandgap semiconductor, the conduction band bottom and valence band positions of the photoelectric material layer differ significantly from those of vanadium dioxide (with a bandgap of approximately 0.7 eV), promoting the separation of photogenerated carriers. Simultaneously, due to the injection of photogenerated carriers, the non-volatile phase transition process of vanadium dioxide can be controlled to a certain extent, achieving multi-modal synergistic control of light, electricity, and heat, greatly expanding the control dimensions of neuromorphic computing. Furthermore, by introducing the photoelectric material layer, dynamic bandgap alignment and phase transition control are achieved. Utilizing the metal-insulator phase transition characteristics of vanadium dioxide, combined with the wide bandgap characteristics of the photoelectric material layer, a dynamically tunable type II heterojunction or Schottky contact can be formed, enabling the device to simultaneously process multiple physical signals such as heat, light, and electricity. Moreover, by combining the Mott phase transition of vanadium dioxide with the photoelectric properties of another material, similar effects can be achieved as long as the bandgap widths of both are sufficient to form a heterojunction and there are no interface contact issues. Even if interface problems exist, the interface contact can be improved to a certain extent by growing an Al2O3 buffer layer.
[0029] In some embodiments, the thickness of the vanadium dioxide thin film layer is greater than 20 nm. A vanadium dioxide thin film layer with a thickness greater than 20 nm can simultaneously optimize the overall performance of the device from multiple dimensions, including lattice strain, metal-insulator phase transition characteristics, opto-electric coupling response, and synaptic biomimetic function. Moreover, the lattice stress inside the film can be fully released, the crystal structure is close to the intrinsic monoclinic phase of bulk VO2, and the intrinsic metal-insulator phase transition behavior near 340 K is completely preserved. The phase transition hysteresis width is narrowed, and the high and low resistance switching ratio is increased by more than two orders of magnitude, laying a structural foundation for the stable realization of pulse-controlled resistive synaptic plasticity of the device.
[0030] In a preferred embodiment, the thickness of the vanadium dioxide thin film layer can be, but is not limited to, 21nm, 25nm, 28nm, 30nm, 32nm, 35nm, etc., and is not limited to integers.
[0031] In some embodiments, the thickness of the optoelectronic material layer is greater than 60 nm. The optoelectronic material layer with a thickness greater than 60 nm can improve the overall performance of the device from multiple dimensions, such as light absorption efficiency, carrier transport regulation, interface recombination suppression, device photoelectric response stability, and realization of biomimetic neuromorphic functions. Furthermore, the optoelectronic material layer with a thickness greater than 60 nm can effectively isolate the defect states at the interface of the upper and lower heterojunctions, reduce the nonradiative recombination loss of photogenerated electron-hole pairs at the interface, and extend the carrier transport lifetime.
[0032] In a preferred embodiment, the thickness of the optoelectronic material layer is not limited to 61nm, 62nm, 65nm, 68nm, 70nm, 72nm, 75nm, 80nm, 82nm, etc., and is not limited to integers.
[0033] In some embodiments, the photoelectric material layer is selected from one of indium gallium oxide (IGO), indium zinc oxide (IZO), zinc oxide (ZnO), indium oxide (In2O3), cadmium sulfide, and molybdenum oxide. The photoelectric material layer of the above materials can form a heterostructure with the vanadium dioxide thin film layer, enhancing the interface modulation capability. Specifically, the photoelectric material layer of the above materials can be combined with the Mott phase transition of vanadium dioxide, and through the functional combination of vanadium dioxide and the above materials, decoupling and synergistic modulation of photo-electric stimulation can be achieved, thereby broadening the multimodal functionality of a single device within the neuromorphic computing system. Simultaneously, the VO2 heterojunction photoelectric neuromorphic device primarily serves the neuromorphic computing system, and the intrinsic Mott phase transition brought about by its VO2 material remains a usable physical characteristic of volatile neurons.
[0034] In a preferred embodiment, the photoelectric material layer is made of indium gallium oxide (IGO), and the gallium oxide (IGO) forms a heterojunction with the vanadium dioxide thin film layer, as shown in the schematic diagram below. Figure 2 As shown.
[0035] Specifically, taking IGO as an example, as a wide bandgap semiconductor (bandgap width of about 4.4~4.9 eV), the conduction band bottom and valence band top positions of IGO are significantly different from those of VO2 (bandgap width of about 0.7 eV), which promotes the separation of photogenerated carriers. At the same time, due to the injection of photogenerated carriers, the non-volatile phase transition process of VO2 can be controlled to a certain extent, realizing multi-modal synergistic control of light, electricity and heat, and greatly expanding the control dimension of neuromorphic computing.
[0036] In some embodiments, the thickness of the top electrode layer is 60 nm to 100 nm; the material of the top electrode layer is selected from one or more of Au, Cu, Ag, Pt, Ti, and Mo. A top electrode layer with a thickness between 60 nm and 100 nm can form a dense, defect-free, and complete conductive metal film, while the internal stress of the film is within a controllable range, making it less prone to delamination failure during thermal cycling.
[0037] In some embodiments, the substrate layer is made of, but is not limited to, silicon dioxide, sapphire, quartz glass, silicon, etc.
[0038] In addition, such as Figure 3 As shown, the present invention also provides a method for fabricating a VO2 heterojunction optoelectronic neuromorphic device, comprising the following steps: Step S10: Place the substrate on the sample stage, use vanadium dioxide as the target material, perform in-situ vacuum magnetron sputtering, and then perform vacuum annealing to obtain the first product with a vanadium dioxide thin film layer. Step S20: After patterning one side of the vanadium dioxide thin film layer of the first product, magnetron sputtering is performed using optoelectronic material as the target material in an oxygen-containing atmosphere, followed by annealing to obtain a second product with an optoelectronic material layer. Step S30: After patterning one side of the vanadium dioxide thin film layer of the second product, a top electrode layer is grown on the vanadium dioxide thin film layer and the optoelectronic material layer by magnetron sputtering to obtain a VO2 heterojunction optoelectronic neuromorphic device.
[0039] In this embodiment, by selecting a suitable target material and controlling the energy, argon gas, and vacuum level during sputtering, combined with annealing, a high-purity vanadium dioxide thin film layer can be obtained. Compared to other processes, magnetron sputtering has the potential for large-scale expansion, and its sputtering uniformity and rate are also superior. Furthermore, by selecting a suitable target material and sputtering in a pure argon atmosphere, this invention effectively avoids many uncontrollable factors during the sputtering process, requiring only vacuum level adjustment. Compared to traditional sputtering processes that adjust the argon-oxygen ratio, this offers higher batch-to-batch controllability. Moreover, the completely oxygen-free VO2 sputtering growth process utilizes the oxygen release from the target material itself to ensure film composition compatibility with the substrate layer, exhibiting high reproducibility and uniformity. Compared to other processes, this invention also ensures controllability for large-scale preparation.
[0040] Specifically, the VO2 heterojunction optoelectronic neuromorphic device prepared by this method realizes a heterojunction using a wide bandgap semiconductor (i.e., a photoelectric thin film layer) and VO2. Combined with the physical characteristics of the functional layer, it achieves real-time multimodal feature extraction, enabling efficient sensing, conversion, and coordinated control of optical and electrical signals. By combining the photoelectric response with the metal-insulator phase transition of VO2, it achieves independent sensing and decoupling of optical and electrical signals, broadening the functionality of a single device and facilitating neuromorphic computing.
[0041] In some embodiments, the parameters of the in-situ vacuum magnetron sputtering process include: a vacuum level of 3e -4 ~5e - 4 Pa, argon flow rate of 25 sccm~40 sccm, magnetron sputtering power of 80 W~140 W, sputtering time of 14 min~40 min; the rotation speed of the sample stage is 10 rad / min~30 rad / min.
[0042] Specifically, step S10 includes: fixing the substrate on a tray, then feeding the sample onto the sample stage in the reaction chamber, rotating the sample stage at a constant speed of 20 rad / min to 40 rad / min, which can significantly improve the uniformity of sputtering. Throughout the entire growth process of the vanadium dioxide thin film layer, the sample stage needs to rotate at a constant speed of 10 rad / min to 30 rad / min, and the vacuum level needs to be evacuated to 3°C. -4 ~5e -4 Pa, then turn on the RF power supply, adjust the Ar flow rate to 25 sccm~40 sccm, adjust the magnetron sputtering chamber pressure to 5 Pa, and adjust the sputtering power of the target material to 80W-140W to make the vanadium dioxide target material glow, then adjust the pressure to 0.68 Pa; perform the pre-sputtering process, the pre-sputtering time is 15min~20min, use pre-sputtering to bombard the oxide layer and adsorbed impurities on the target material surface to remove the contamination layer, stabilize the sputtering process, and ensure the purity of the film; then open the vanadium dioxide target baffle and start the coating, the coating time is 14min~40min, after the coating is completed, turn off the RF power supply, take out the sample, and obtain the in-situ grown vanadium dioxide film.
[0043] In a preferred embodiment, the parameters of the in-situ vacuum magnetron sputtering process include: a vacuum level of 5e. - 4 The parameters are: Pa, argon flow rate 30 sccm, magnetron sputtering power 120 W, sputtering time 15 min; and the rotation speed of the sample stage 20 rad / min.
[0044] In some embodiments, in step S10, the temperature of the vacuum annealing process is 450°C to 550°C, the heating rate of the vacuum annealing process does not exceed 10°C / min, and the time of the vacuum annealing process is 45min to 80min.
[0045] In some embodiments, step S10, the vacuum annealing process includes the following steps: before annealing, purging is performed using argon gas with a purity of 99.99% to ensure that there is little residual oxygen in the annealing furnace; specifically, the annealing furnace is first evacuated, and then argon gas is introduced, and this process is repeated three times; the temperature of the vacuum annealing process is controlled at 450℃~550℃, the heating rate does not exceed 10℃ / min, and the time is 45min~80min, which can improve the crystal quality of the vanadium dioxide thin film layer; and the vacuum environment is maintained throughout the entire annealing process, and after annealing, the sample is taken out after natural cooling to below 200℃.
[0046] In a preferred embodiment, in step S10, the temperature of the vacuum annealing treatment is 500°C, the heating rate of the vacuum annealing treatment is 10°C / min, and the time of the vacuum annealing treatment is 60min.
[0047] In some embodiments, in step S20, the parameters of the magnetron sputtering coating include: the sputtering gas is a mixture of argon and oxygen, the magnetron sputtering power is 60W~120W, and the sputtering time is 15min~60min.
[0048] In some embodiments, the annealing temperature is 300℃~400℃, the annealing time is 30min~90min, and the heating rate of the annealing is 5℃ / min~10℃ / min.
[0049] Specifically, step S20 includes: patterning using positive photoresist lithography before sputtering the optoelectronic material layer; then, magnetron sputtering of the thin film using a 99.9% pure optoelectronic material target and 99.99% pure argon and oxygen as sputtering gases. The specific steps include: fixing the sample on a tray, then feeding the sample into the sample stage of the reaction chamber, rotating the sample stage at a uniform speed of 20 rad / min. Vacuuming is then performed to 5°C. -4Pa was applied, then the RF power supply was turned on, the argon flow rate was adjusted to 10 sccm, the oxygen flow rate to 20 sccm, the magnetron sputtering chamber pressure was adjusted to 5 Pa, and the target sputtering power was adjusted to 80 W to ignite the target. The pressure was then adjusted to 0.5 Pa. A pre-sputtering process was performed for 15 min, followed by opening the target baffle and starting the coating process for 20 min. After coating, the RF power supply was turned off, the sample was removed, and the grown IGO film was obtained. The sample was then immersed in acetone and alcohol, and ultrasonic stripping was applied simultaneously. After stripping, the sample was placed in an annealing furnace for annealing. Before annealing, the sample was purged with 99.99% pure argon. The annealing atmosphere was argon, the annealing temperature was set to 300 degrees Celsius, the heating rate was 10 degrees Celsius / min, and the temperature was held at 300 degrees Celsius for 30 min. After annealing, the sample was allowed to cool naturally to below 200 degrees Celsius before removal.
[0050] In some embodiments, in step S30, the electrode structure adopts a planar two-terminal electrode, and the electrode material is selected as Mo; before sputtering growth, patterning is performed using positive photolithography. Subsequently, a 99.9% pure Mo target is used, and the sputtering gas is 99.99% pure argon gas for magnetron sputtering deposition. The specific steps are as follows: the sample is fixed on a tray, and then fed into the sample stage of the reaction chamber, where the sample stage rotates uniformly at 20 rad / min. A vacuum is then drawn to 5°C. -4 Pa, then the DC power supply was turned on, the argon gas flow rate was adjusted to 50 sccm, the magnetron sputtering chamber pressure was adjusted to 5 Pa, and the target sputtering power was adjusted to 120 W to ignite the target. The pressure was then adjusted to 0.35 Pa. A pre-sputtering process was performed for 15 min, followed by opening the target baffle and starting the coating process for 8 min. After coating, the RF power supply was turned off, the sample was removed, and the grown Mo thin film was obtained. Subsequently, the sample was immersed in acetone and alcohol, and ultrasonic stripping of the photoresist was performed to obtain a VO2 heterojunction optoelectronic neuromorphic device.
[0051] In addition, the present invention also provides an application of a VO2 heterojunction opto-neuromorphic device in smart sensors or neuromorphic chips.
[0052] The following examples further illustrate the present invention in detail. It should also be understood that the following examples are only for further explanation of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention are within the scope of protection of the present invention.
[0053] Example 1 This embodiment provides a method such as Figure 1 The overall fabrication process of the VO2 heterojunction opto-neuromorphic device shown is as follows: Figure 4As shown, the details are as follows: 1) In-situ growth of VO2 thin films In the magnetron sputtering system, a vanadium dioxide target with a purity of 99.99% is used, and a 2cm × 2cm silicon dioxide substrate is selected. The oxide layer thickness is 300nm, and the sputtering gas is argon gas with a purity of 99.99%. In-situ vacuum magnetron sputtering deposition is then performed. The specific steps are as follows: The silicon dioxide substrate was fixed on the tray, and then the sample was fed into the sample stage of the reaction chamber, which was rotated at a constant speed of 20 rad / min. It should be noted that since the spatial distribution of atoms ejected from the target is non-uniform, the tray rotation aims to significantly improve the uniformity of sputtering; the sample stage needs to rotate at a constant speed of 20 rad / min throughout the entire film growth process. A vacuum was then drawn to 5°C. -4 Pa was applied, then the RF power supply was turned on, the Ar flow rate was adjusted to 30 sccm, the magnetron sputtering chamber pressure was adjusted to 5 Pa, and the target sputtering power was adjusted to 120 W to ignite the vanadium dioxide target. The pressure was then adjusted to 0.68 Pa. A pre-sputtering process was then performed for 15 minutes. The purpose of pre-sputtering was to bombard the oxide layer and adsorbed impurities on the target surface, remove the contamination layer, stabilize the sputtering process, and ensure film purity. Subsequently, the vanadium dioxide target baffle was opened, and film deposition began for 15 minutes. After deposition, the RF power supply was turned off, the sample was removed, and an in-situ grown vanadium dioxide film was obtained.
[0054] 2) Vacuum annealing of VO2 thin films The sample obtained in step 1) was sent to an annealing furnace for vacuum annealing. Before annealing, the furnace was purged with 99.99% pure argon gas to ensure minimal oxygen residue. The specific procedure involved first evacuating the furnace, then introducing argon gas, repeating this process three times. The annealing temperature was set to 500℃, with a heating rate of 10℃ / min, followed by holding at 500℃ for 1 hour. A vacuum environment was maintained throughout the annealing process. After annealing, the sample was allowed to cool naturally to below 200℃ before being removed.
[0055] 3) IGO thin film growth Before sputtering growth, patterning was performed using positive photoresist lithography. Subsequently, magnetron sputtering deposition was performed using a 99.9% pure IGO (65:35) target and a sputtering gas mixture of 99.99% pure argon and oxygen. The specific steps are as follows: The sample obtained in step 2) is fixed on the tray and then fed into the sample stage of the reaction chamber, where the sample stage is rotated at a constant speed of 20 rad / min. A vacuum of 5°C is then applied. -4Pa was applied, followed by turning on the RF power supply, adjusting the argon flow rate to 10 sccm and the oxygen flow rate to 20 sccm, adjusting the magnetron sputtering chamber pressure to 5 Pa, and adjusting the target sputtering power to 80 W to ignite the target. The pressure was then adjusted to 0.5 Pa. A pre-sputtering process was performed for 15 minutes, after which the target baffle was opened, and coating began for 20 minutes. After coating, the RF power supply was turned off, the sample was removed, and the grown IGO film was obtained. The sample was then immersed in acetone and alcohol, and simultaneously subjected to ultrasonic exfoliation to obtain a patterned IGO film.
[0056] 4) Annealing of IGO thin films After the peeling is completed in step 4), the sample is sent to an annealing furnace for annealing. Before annealing, the sample is purged with argon gas of 99.99% purity. The annealing atmosphere is argon, the annealing temperature is set to 300℃, the heating rate is 10℃ / min, and then it is held at 300℃ for 30min. After annealing, the sample is allowed to cool naturally to below 200℃ before being removed.
[0057] 5) Mo thin film growth The top electrode layer features a planar two-terminal electrode structure, with Mo as the electrode material. Before sputtering growth, patterning is performed using positive photoresist lithography. Subsequently, magnetron sputtering deposition is performed using a 99.9% pure Mo target and 99.99% pure argon gas. The specific steps are as follows: Secure the sample from step 4) onto the tray, then transfer it to the sample stage in the reaction chamber, rotating the stage at a constant speed of 20 rad / min. Evacuate to 5°C. -4 Pa was applied, then the DC power supply was turned on, the argon gas flow rate was adjusted to 50 sccm, the magnetron sputtering chamber pressure was adjusted to 5 Pa, and the target sputtering power was adjusted to 120 W to ignite the target. The pressure was then adjusted to 0.35 Pa. A pre-sputtering process was performed for 15 minutes. The target baffle was then opened, and film deposition began for 8 minutes. After deposition, the RF power supply was turned off, the sample was removed, and the grown Mo film was obtained. The sample was then immersed in acetone and alcohol, and simultaneously subjected to ultrasonic exfoliation to obtain a patterned Mo film.
[0058] This embodiment achieves a deep integration of material properties and device functions through material process optimization, utilizing the unique design of the VO2 / IGO heterojunction and its application in multimodal neuromorphic computing. Furthermore, in terms of material process optimization, compared to the current mainstream VO2 epitaxial growth process, the optimized process has significant advantages: compared to advanced processes such as PLD, this process has lower substrate requirements, can be adapted to various substrates such as Si, SiO2, and Al2O3, and exhibits better uniformity in large-scale fabrication, possessing the potential for large-scale integration; compared to traditional magnetron sputtering processes, this process simplifies variables, eliminates oxygen involvement in the fabrication process through target selection, making the composition of the thin film more controllable, the effect more stable, and the repeatability stronger, while having lower substrate requirements, reducing process costs and manufacturing complexity.
[0059] Furthermore, by introducing IGO, dynamic bandgap alignment and phase transition modulation are achieved. Utilizing the metal-insulator phase transition characteristics of VO2 and combining them with the wide bandgap of IGO, a dynamically tunable type II heterojunction or Schottky contact is formed. This enables the device to simultaneously process multiple physical signals, including thermal, optical, and electrical signals. The DC test diagram of the VO2 heterojunction opto-neuromorphic device fabricated in this embodiment is shown below. Figure 5 As shown, this enables efficient perception and fusion of multimodal signals, providing a hardware foundation for intelligent decision-making in complex environments.
[0060] Meanwhile, this VO2 heterojunction optoelectronic neuromorphic device possesses dynamic reconfigurable computing capabilities. By changing illumination conditions, the metal-insulator phase transition characteristics of VO2 can be dynamically adjusted, enabling real-time switching of device characteristics and enhancing system flexibility and adaptability. Therefore, this heterostructure makes the device more flexible and scalable in neuromorphic computing systems. The device forms a type II heterojunction in the high-resistivity state, promoting photogenerated carrier separation, combined with VO2 phase transition modulation of the interface barrier. Dynamic threshold adjustment: By controlling the VO2 phase transition through temperature or electric field, the neuron activation threshold can be adaptively adjusted, enhancing the flexibility of neuromorphic computing. On one hand, tunable optical response can be achieved by utilizing the different infrared transmittance of VO2 in the high-resistivity and low-resistivity states to achieve the affinity modulation of optical signals by electrical signals. On the other hand, the phase transition state (MIT) of VO2 can be modulated by applying an external electric field, thereby changing the band structure and light absorption characteristics of the heterojunction. For example, by inducing VO2 to transition from an insulating phase to a metallic phase through illumination, the device can switch from a high-resistivity state to a low-resistivity state, achieving the modulation of electrical performance by optical signals, such as... Figure 5 As shown, after being illuminated, the high-resistivity state at 6V will change to a low-resistivity state.
[0061] In summary, this invention provides a VO2 heterojunction optoelectronic neuromorphic device, its fabrication method, and its application. The VO2 heterojunction optoelectronic neuromorphic device comprises a substrate layer, a vanadium dioxide thin film layer, a photoelectric material layer, and a top electrode layer stacked sequentially from bottom to top. The vanadium dioxide thin film layer and the photoelectric material layer constitute a heterostructure. The top electrode layer includes a first top electrode layer in contact with the photoelectric material layer and a second top electrode layer in contact with the vanadium dioxide thin film layer. This invention utilizes a wide-bandgap semiconductor photoelectric material layer and a vanadium dioxide thin film layer to form a heterojunction. Combined with the physical characteristics of the functional layers, it can extract multimodal features in real time, achieving efficient sensing, conversion, and coordinated control of optical and electrical signals. Simultaneously, by combining photoelectric response with the metal-insulator phase transition of vanadium dioxide, it can achieve independent sensing and decoupling of optical and electrical signals, broadening the functionality of a single device and facilitating neuromorphic computing. Furthermore, the fabrication method, by selecting a suitable target material and controlling the power, argon gas, and vacuum level during sputtering, along with annealing, can obtain a high-purity vanadium dioxide thin film layer. Therefore, this invention systematically solves the bottlenecks in the large-scale fabrication uniformity and multimodal capabilities of VO2 neuromorphic devices through synergistic improvements in materials, structure, and processes. By synergistically regulating the phase transition state of VO2 through multiple physical fields such as electricity, heat, and light, dynamic neuron threshold adjustment is achieved, breaking through the limitations of traditional single-processing of electrical signals. Through multi-dimensional optimization, a quantitative correlation between materials, structure, and function is established, providing a technical path for neuromorphic computing systems and possessing broad prospects for industrial applications.
[0062] It should be understood that the application of the present invention is not limited to the examples above. Those skilled in the art can make improvements or modifications based on the above description, and all such improvements and modifications should fall within the protection scope of the appended claims.
Claims
1. A VO2 heterojunction optoelectronic neuromorphic device, characterized in that, It includes a substrate layer, a vanadium dioxide thin film layer, a photoelectric material layer and a top electrode layer stacked sequentially from bottom to top; the vanadium dioxide thin film layer and the photoelectric material layer form a heterostructure; the top electrode layer includes a first top electrode layer in contact with the photoelectric material layer and a second top electrode layer in contact with the vanadium dioxide thin film layer.
2. The VO2 heterojunction optoelectronic neuromorphic device according to claim 1, characterized in that, The thickness of the vanadium dioxide thin film is greater than 20 nm.
3. The VO2 heterojunction optoelectronic neuromorphic device according to claim 1, characterized in that, The thickness of the optoelectronic material layer is greater than 60 nm.
4. The VO2 heterojunction optoelectronic neuromorphic device according to claim 1, characterized in that, The material of the optoelectronic material layer is selected from one of indium gallium oxide, indium zinc oxide, zinc oxide, indium oxide, cadmium sulfide, and molybdenum oxide.
5. The VO2 heterojunction optoelectronic neuromorphic device according to claim 1, characterized in that, The thickness of the top electrode layer is 60nm~100nm; the material of the top electrode layer is selected from one or more of Au, Cu, Ag, Pt, Ti, and Mo.
6. A method for fabricating a VO2 heterojunction optoelectronic neuromorphic device as described in any one of claims 1-5, characterized in that, Including the following steps: The substrate was placed on the sample stage, and vanadium dioxide was used as the target material. After in-situ vacuum magnetron sputtering, vacuum annealing was performed to obtain the first product with a vanadium dioxide thin film layer. After patterning one side of the vanadium dioxide thin film layer of the first product, magnetron sputtering is performed in an oxygen-containing atmosphere using optoelectronic material as the target material, followed by annealing to obtain a second product with an optoelectronic material layer. After patterning one side of the vanadium dioxide thin film layer of the second product, a top electrode layer is grown on the vanadium dioxide thin film layer and the optoelectronic material layer by magnetron sputtering to obtain a VO2 heterojunction optoelectronic neuromorphic device.
7. The method for fabricating the VO2 heterojunction optoelectronic neuromorphic device according to claim 6, characterized in that, The parameters for the in-situ vacuum magnetron sputtering process include: a vacuum level of 3e. -4 ~5e -4 Pa, argon flow rate of 25 sccm~40 sccm, magnetron sputtering power of 80 W~140 W, sputtering time of 14 min~40 min; the rotation speed of the sample stage is 10 rad / min~30 rad / min.
8. The method for fabricating the VO2 heterojunction optoelectronic neuromorphic device according to claim 6, characterized in that, The vacuum annealing process is performed at a temperature of 450℃ to 550℃, with a heating rate not exceeding 10℃ / min, and a duration of 45min to 80min.
9. The method for fabricating the VO2 heterojunction optoelectronic neuromorphic device according to claim 6, characterized in that, The parameters of the magnetron sputtering coating include: the sputtering gas is a mixture of argon and oxygen, the magnetron sputtering power is 60W~120W, and the sputtering time is 15min~60min; Preferably, the annealing temperature is 300℃~400℃, the annealing time is 30min~90min, and the heating rate of the annealing is 5℃ / min~10℃ / min.
10. The application of a VO2 heterojunction opto-neuromorphic device as described in any one of claims 1-5 in a smart sensor or neuromorphic chip.