Semiconductor substrate manufacturing methods, manufacturing apparatus, and epitaxial growth methods

By setting multiple substrates and forming a temperature gradient in the thickness direction in the SiC semiconductor substrate manufacturing method, efficient raw material delivery and epitaxial growth are achieved, solving the problem of low production efficiency and improving the production volume and quality of SiC semiconductor devices.

CN123124676APending Publication Date: 2026-11-17KWANSEI GAKUIN EDUCTIONAL FOUND +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611470571.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-04-26
Filing Date
2020-04-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the current technology, the production volume of SiC semiconductor devices is low, and it is difficult to improve production efficiency by processing multiple substrates at the same time.

Method used

Multiple semiconductor substrates are stacked in a setup step, and a temperature gradient is formed in the thickness direction of the substrates through a heating step to achieve material delivery and epitaxial growth.

Benefits of technology

This increased the production volume of semiconductor substrates, optimized production efficiency, reduced surface defect density, and improved the quality of SiC semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124676A_ABST
    Figure CN123124676A_ABST
Patent Text Reader

Abstract

The purpose of this invention is to provide a novel method and apparatus for manufacturing a semiconductor substrate. A method for manufacturing a semiconductor substrate and an apparatus for using the method are provided. The method includes: a setting step of stacking a plurality of workpieces having a semiconductor substrate; and a heating step of heating each of the plurality of workpieces to create a temperature gradient along the thickness direction of the semiconductor substrate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese Patent Application No. 202080030894.2, filed on April 24, 2020, entitled "Method for Manufacturing a Semiconductor Substrate, Manufacturing Apparatus Thereof, and Epitaxial Growth Method Thereof". This Chinese Patent Application is based on International Application PCT / JP2020 / 017643 and claims priority to Japanese Patent Application No. 2019-086714, filed on April 26, 2019, the contents of which are incorporated herein by reference. Technical Field

[0002] This invention relates to a method for manufacturing a SiC substrate, an apparatus for manufacturing the substrate, and an epitaxial growth method thereof. Background Technology

[0003] SiC (silicon carbide) semiconductor devices have attracted attention as high-performance semiconductor devices due to their higher voltage withstand and efficiency compared to Si (silicon) and GaAs (gallium arsenide) semiconductor devices, as well as their ability to operate at high temperatures.

[0004] Typically, SiC semiconductor devices are manufactured through the growth of SiC crystals. Various growth methods have been proposed for SiC crystals.

[0005] In the vapor phase epitaxial growth method described in Patent Document 1, a SiC container made of a polycrystalline SiC material is placed inside a TaC container made of a TaC material, and a bottom substrate is placed inside the SiC container. The TaC container is heated in an environment that generates a temperature gradient, with Si vapor pressure inside the TaC container. As a result, C atoms sublimated by etching the inner surface of the SiC container bond with Si atoms in the atmosphere, thereby growing a 3C-SiC single crystal epitaxial layer on the bottom substrate.

[0006] Existing technical documents Patent documents Patent Document 1: Japanese Re-evaluation No. 2017-188381 Summary of the Invention

[0007] The problem the invention aims to solve However, in the invention described in Patent Document 1, there is room for improvement from the viewpoint of increasing production volume by processing multiple substrates together.

[0008] The problem of this invention is to provide a novel method and apparatus for manufacturing a semiconductor substrate, as well as an epitaxial growth method.

[0009] means for solving problems To solve the above problems, the semiconductor substrate manufacturing method of the present invention includes: a setting step, in which a plurality of processed objects having a semiconductor substrate are stacked; and a heating step, in which each of the plurality of processed objects is heated such that a temperature gradient is formed in the thickness direction of the semiconductor substrate.

[0010] This enables a method for manufacturing semiconductor substrates that promises to increase production volume.

[0011] In a preferred embodiment of the present invention, the setting step involves placing the object to be processed within a quasi-enclosed space.

[0012] Therefore, it is possible to optimize the delivery of raw materials, including epitaxial growth and etching.

[0013] In a preferred embodiment of the invention, the setting step involves setting the processed body such that adjacent semiconductor substrates are opposite each other.

[0014] This enables the delivery of raw materials, including epitaxial growth and etching, between adjacent semiconductor substrates.

[0015] In a preferred embodiment of the invention, the heating step involves heating a plurality of the processed bodies in an atmosphere containing atomic species constituting the semiconductor substrate.

[0016] Therefore, material transport can be achieved in a vapor pressure environment containing gaseous species that constitute the atomic species of the semiconductor substrate.

[0017] To solve the above problems, the semiconductor substrate manufacturing apparatus of the present invention includes: a plurality of processed bodies having a semiconductor substrate and a setting device; and a heating furnace capable of forming a temperature gradient in the thickness direction of the semiconductor substrate in each of the plurality of processed bodies.

[0018] This enables the development of a semiconductor substrate manufacturing apparatus with the potential to increase production volume.

[0019] In a preferred embodiment of the present invention, the material of the setting device is the material of the semiconductor substrate.

[0020] Therefore, material transport can be achieved in a vapor pressure environment containing gaseous species that constitute the atomic species of the semiconductor substrate.

[0021] In a preferred embodiment of the invention, the setting device has a through hole.

[0022] Therefore, the object being processed can be configured such that adjacent semiconductor substrates are opposite each other.

[0023] In a preferred embodiment of the invention, the object to be processed has a main container capable of accommodating the semiconductor substrate and the setting device.

[0024] This makes the processing of the object easier.

[0025] In a preferred embodiment of the invention, the main container has an upper container and a lower container that can fit together, and a gap formed at the fitting portion of the upper and lower containers.

[0026] This allows for the formation of a quasi-enclosed space.

[0027] In a preferred embodiment of the invention, the object to be processed has a vapor supply source made of a material comprising at least one of the atomic species constituting the semiconductor substrate.

[0028] Therefore, raw material transport can be achieved in a vapor pressure environment containing gaseous species that constitute the atomic species of the semiconductor substrate.

[0029] In a preferred embodiment of the invention, the semiconductor substrate manufacturing apparatus further includes a high-melting-point container capable of receiving the workpiece.

[0030] This allows the vapor pressure environment to be maintained.

[0031] Furthermore, the present invention also relates to an epitaxial growth method. Specifically, one aspect of the epitaxial growth method of the present invention involves arranging multiple semiconductor substrates along the thickness direction of the semiconductor substrates and heating them to create a temperature gradient along the thickness direction of the semiconductor substrates, thereby transporting raw materials from a semiconductor substrate disposed on a high-temperature side to a semiconductor substrate disposed on a low-temperature side, continuing the polymorphism of the low-temperature side semiconductor substrate and causing its crystal growth.

[0032] In a preferred embodiment of the invention, multiple semiconductor substrates are subjected to crystal growth simultaneously.

[0033] In a preferred embodiment of the invention, a dummy substrate is disposed at approximately the ends of the plurality of semiconductor substrates arranged thereon.

[0034] In a preferred embodiment of the invention, the semiconductor substrate is disposed within a material delivery space and grown thereon. This material delivery space is vented by gaseous species (containing atomic species constituting the semiconductor substrate). In a preferred embodiment of the invention, the semiconductor substrate is silicon carbide, and the semiconductor substrate is disposed in a raw material transport space that is vented through the Si vapor pressure space and grown there.

[0035] In a preferred embodiment of the invention, the semiconductor substrate is disposed in a quasi-enclosed space with a Si / C atomic ratio exceeding 1 and heated.

[0036] In a preferred embodiment of the invention, the semiconductor substrate is disposed in a quasi-enclosed space with a Si / C atomic ratio of less than 1 and heated.

[0037] The effects of the invention According to the disclosed technology, a novel method for manufacturing a semiconductor substrate, its manufacturing apparatus, and an epitaxial growth method can be provided.

[0038] Other problems, features, and advantages will become apparent from reading the following description of the manner in which the invention is practiced, taken in conjunction with the accompanying drawings and claims. Attached Figure Description

[0039] Figure 1 This is an explanatory diagram of a semiconductor substrate manufacturing method according to an embodiment of the present invention.

[0040] Figure 2 This is an explanatory diagram of a semiconductor substrate manufacturing method according to an embodiment of the present invention.

[0041] Figure 3 This is an explanatory diagram of a semiconductor substrate manufacturing method according to an embodiment of the present invention.

[0042] Figure 4 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0043] Figure 5 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0044] Figure 6 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0045] Figure 7 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0046] Figure 8 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0047] Figure 9 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0048] Figure 10 This is an explanatory diagram of a semiconductor substrate manufacturing apparatus according to an embodiment of the present invention.

[0049] Figure 11 This is an explanatory diagram related to the evaluation of the BPD number in the SiC substrate of Reference Example 1.

[0050] Figure 12This is an SEM image of the SiC substrate surface in Reference Example 2.

[0051] Figure 13 This is an SEM image of the SiC substrate surface in Reference Example 2.

[0052] Figure 14 The graph shows the relationship between the growth rate and heating temperature of the SiC substrate in Example 3.

[0053] Figure 15 This is an illustrative diagram of a semiconductor substrate manufacturing apparatus according to another embodiment of the present invention. Detailed Implementation

[0054] The following uses Figures 1 to 14 A preferred embodiment of the invention illustrated in the accompanying drawings will be described in detail below. The scope of the invention is not limited to the embodiment shown in the drawings, and can be appropriately modified within the scope set forth in the claims.

[0055] Semiconductor Substrate Manufacturing Methods Hereinafter, a method for manufacturing a semiconductor substrate according to an embodiment of the present invention (hereinafter referred to as the manufacturing method) will be described in detail.

[0056] This invention can be understood as a manufacturing method including a setting step and a heating step.

[0057] <Setup Steps> The setup steps involve stacking the workpieces, which have semiconductor substrates, in a layered manner.

[0058] In one embodiment of the present invention, a plurality of processed objects are provided such that a semiconductor substrate 11 and a component made of the material of the semiconductor substrate 11 are positioned opposite each other. Furthermore, in another embodiment of the present invention, a plurality of processed objects are provided such that adjacent semiconductor substrates 11 and 12 are positioned opposite each other. In this case, a material transport space S0 is formed between the semiconductor substrate 11 and the component, or between the semiconductor substrates 11 and 12.

[0059] In this specification, raw material delivery refers to the delivery of a raw material gas containing atomic species that constitute the semiconductor substrate. This raw material gas is preferably a gaseous gas containing only the atomic species.

[0060] <Semiconductor substrate> The details of the semiconductor substrates, including semiconductor substrates 11 and 12, are described below.

[0061] In one embodiment of the present invention, an example is given where the semiconductor substrate is a SiC semiconductor substrate.

[0062] Examples of semiconductor substrates 11 and 12 include SiC wafers obtained by cutting ingots manufactured by methods such as sublimation into disk shapes, and SiC semiconductor substrates obtained by processing SiC single crystals into thin plates. Furthermore, any polymorph can be used as the crystal polymorph of the SiC single crystal.

[0063] As a semiconductor substrate surface, an example can be a surface with an offset angle of several degrees (e.g., 0.4 to 8°) set from the (0001) surface or the (000-1) surface (in addition, in the Miller index notation in this specification, the dash "-" indicates that what follows is the index).

[0064] A step-plateau structure was confirmed on the surface of a SiC single-crystal substrate planarized at atomic energy levels. This step-plateau structure is a stepped structure consisting of alternating steps (i.e., steps and {0001} planes) exposed above a molecular layer and flat regions (i.e., platforms).

[0065] In the steps of a SiC semiconductor substrate, a single molecular layer (0.25 nm) is the minimum height (minimum unit), and this single molecular layer is superimposed on multiple layers to form various step heights. In this specification, step bundling that enlarges the step and has a height exceeding that of a single unit lattice of each polymorph is called macro step bundling (MSB).

[0066] That is, MSB is a step formed by more than 4 molecular layers (more than 5 molecular layers) in the case of 4H-SiC, and a step formed by more than 6 molecular layers (more than 7 molecular layers) in the case of 6H-SiC.

[0067] Since defects caused by MSB occur at the surface during the formation of the growth layer, and are one of the factors hindering the reliability of oxide films in SiC semiconductor devices, it is desirable to avoid the formation of MSB at the surface of SiC single crystal substrates.

[0068] The dimensions of semiconductor substrates 11 and 12 can range from chip sizes of a few centimeters square, such as 6 inches (approximately 15.24 cm), 8 inches (approximately 20.32 cm), and larger wafer sizes.

[0069] Semiconductor substrate 11 has a main surface 113 (not shown) and a back surface 114. In addition, semiconductor substrate 12 has a main surface 123 and a back surface 124 (not shown).

[0070] In this specification, "surface" refers to both the main surface and the back surface. "One side" refers to either the main surface or the back surface, and "other side" refers to the side of the same substrate opposite to that side.

[0071] In this specification, growth layer 111 refers to the layer formed on semiconductor substrate 11 before processing. Growth layer 121 refers to the layer formed on semiconductor substrate 12 before processing.

[0072] For the surface of the growth layer formed on the semiconductor substrate, preferably, the basal plane dislocation (BPD) density is reduced infinitely. Therefore, for the semiconductor substrate surface, preferably, the BPD density is reduced infinitely. Furthermore, during the formation of the growth layer, BPDs are preferably converted into other defects / dislocations including threading edge dislocations (TED).

[0073] The material of the semiconductor substrate according to an embodiment of the present invention is not particularly limited.

[0074] Materials for semiconductor substrates include, for example, compound semiconductor materials such as AlN (aluminum nitride) and GaN (gallium nitride).

[0075] In addition, materials commonly used in the manufacture of semiconductor substrates can also be used. Semiconductor substrate materials include, for example, well-known group IV materials such as silicon (Si), germanium (Ge), and diamond (C). Furthermore, semiconductor substrate materials include, for example, well-known group IV-IV compound materials such as silicon carbide (SiC). Additionally, semiconductor substrate materials are well-known group II-VI compound materials such as zinc oxide (ZnO), zinc sulfide (ZnS), zinc selenide (ZnSe), cadmium sulfide (CdS), and cadmium telluride (CdTe). Furthermore, semiconductor substrate materials are well-known group III-V compound materials such as boron nitride (BN), gallium arsenide (GaAs), gallium nitride (GaN), aluminum nitride (AlN), indium nitride (InN), gallium phosphide (GaP), indium phosphide (InP), and indium antimonide (InSb). Finally, semiconductor substrate materials are, for example, oxide materials such as aluminum oxide (Al2O3) and gallium oxide (Ga2O3). Alternatively, semiconductor substrates can also be configured to have appropriately added atoms of known composition depending on the material.

[0076] The distance D0 between the semiconductor substrate 11 and the component or semiconductor substrate 12 made of the material of the semiconductor substrate 11 during the setting step, i.e., the transport distance D0, is preferably 100 mm or less, more preferably 50 mm or less, more preferably 20 mm or less, more preferably 10 mm or less, even more preferably 7 mm or less, even more preferably 5 mm or less, even more preferably 3.5 mm or less, even more preferably 3 mm or less, and even more preferably 2.7 mm or less. The transport distance D0 is preferably 0.7 mm or more, more preferably 1.0 mm or more, even more preferably 1.2 mm or more, even more preferably 1.5 mm or more, and even more preferably 1.7 mm or more.

[0077] <Heating Steps> According to an embodiment of the invention, the heating step heats each of the plurality of processed bodies, thereby forming a temperature gradient in the thickness direction of the semiconductor substrates 11 and / or 12.

[0078] In addition, this specification provides a detailed description of the case where the semiconductor substrates including semiconductor substrates 11 and 12 are SiC semiconductor substrates.

[0079] For example, the heating step forms a material delivery space S0 with a temperature gradient, such that the semiconductor substrate 11 is the high-temperature side and the semiconductor substrate 12 or a component made of the material of the semiconductor substrate 11 is the low-temperature side. Therefore, it can be understood that the heating step includes the material delivery step.

[0080] In another embodiment of the present invention, the semiconductor substrate 11 may be the low-temperature side, and the semiconductor substrate 12 or a component made of the material of the semiconductor substrate 11 may be the high-temperature side.

[0081] Figures 1 to 3 The material delivery is described in the case where adjacent semiconductor substrates 11 and 12 are opposite each other according to an embodiment of the present invention.

[0082] like Figure 1 As shown, by placing the semiconductor substrate 11 on the high-temperature side of the temperature gradient, the back side 114 is etched and the growth layer 121 in the main surface 123 is formed simultaneously.

[0083] like Figure 2 As shown, by placing the semiconductor substrate 11 on the low-temperature side of the temperature gradient, the growth layer 111 in the back surface 114 and the etching of the main surface 123 are performed simultaneously.

[0084] The heating step is preferably performed by heating the semiconductor substrates 11 and 12 in a semi-enclosed space.

[0085] In this specification, a semi-enclosed space is a space that, while capable of being evacuated, can also contain at least a portion of the vapor generated within it.

[0086] (Raw material conveying steps) like Figure 3 As shown, it can be understood that in the raw material transport space S0 according to an embodiment of the present invention, raw material transport based on the following reactions 1) to 5) is continuously carried out, and for example, a growth layer 121 is formed.

[0087] 1) SiC(s)→Si(v)+C(s) 2) 2C(s)+Si(v)→SiC 2 (v) 3) C(s)+2Si(v)→Si 2 C(v) 4) Si(v)+SiC 2 (v)→2SiC (s) 5) Si 2 C(v)→Si(v)+SiC(s) 1) Explanation: As the back side 114 of the semiconductor substrate 11 is thermally decomposed, Si atoms (Si(v)) are removed from the back side 114.

[0088] Explanation of 2) and 3): The C (C(s)) remaining at the back side 114 due to the detachment of Si atoms (Si(v)) reacts with the Si vapor (Si(v)) in the raw material transport space S0 to become Si2C or SiC2, etc., and sublimates in the raw material transport space S0.

[0089] Explanation of 4) and 5): The sublimated Si2C or SiC2, etc., reach and diffuse to the platform of the main surface 123 of the semiconductor substrate 12 due to the temperature gradient, and reach the step, thereby continuing the polymorphism of the main surface 123 and growing and forming the growth layer 121 (step flow growth).

[0090] The material delivery steps include: a Si atom sublimation step, in which Si atoms are thermally sublimated from the semiconductor substrate 11; and a C atom sublimation step, in which C atoms remaining on the back side 114 of the semiconductor substrate 11 are bonded to Si atoms in the material delivery space S0 to sublimate.

[0091] The material delivery steps include: an etching step, which etches the surface of the semiconductor substrate, which serves as the material delivery source, based on the Si atom sublimation step and the C atom sublimation step.

[0092] The material delivery step includes a growth step, in which a growth layer is formed on the surface of a semiconductor substrate, which serves as the destination for material delivery, based on the aforementioned step flow growth.

[0093] The growth step can be understood as the Si2C or SiC2 that diffuses into the raw material transport space S0 and condenses at the transport destination due to supersaturation.

[0094] The growth process can be understood as being based on physical vapor transport.

[0095] According to one embodiment of the present invention, the driving force for material delivery can be understood as the vapor pressure difference between semiconductor substrates 11 and 12 caused by the formed temperature gradient.

[0096] Therefore, it can be understood that not only the temperature difference at the surfaces of semiconductor substrates 11 and 12, but also the chemical potential difference caused by the crystal structure of the relative SiC materials is also a driving force for raw material transport.

[0097] In the material transport according to one embodiment of the present invention, the transport source or transport destination may not be a semiconductor substrate. Specifically, all semiconductor substrate materials forming the quasi-enclosed space can serve as the transport source or transport destination.

[0098] That is, raw material can also be transported between the semiconductor substrate 11 and the component made of the material of the semiconductor substrate 11.

[0099] In the raw material delivery according to one embodiment of the present invention, the doping concentration of the growth layer 111 can be adjusted by supplying doping gas into the quasi-closed space using a doping gas supply device. On the other hand, without supplying doping gas, the growth layer 111 or 121 is formed by maintaining the doping concentration within the quasi-closed space.

[0100] According to one embodiment of the present invention, the raw material transport is preferably carried out in an environment having gaseous species containing Si and gaseous species containing C, more preferably in a SiC-Si equilibrium vapor pressure environment, and even more preferably in a SiC-C equilibrium vapor pressure environment.

[0101] In this specification, the SiC-Si vapor pressure environment refers to the vapor pressure environment when SiC (solid phase) and Si (liquid phase) are in phase equilibrium through the gas phase. Furthermore, the SiC-C equilibrium vapor pressure environment refers to the vapor pressure environment when SiC (solid phase) and C (solid phase) are in phase equilibrium through the gas phase.

[0102] According to one embodiment of the present invention, the SiC-Si equilibrium vapor pressure environment is formed by heating a quasi-closed space with an atomic number ratio of Si / C exceeding 1. Furthermore, according to another embodiment of the present invention, the SiC-C equilibrium vapor pressure environment is formed by heating a quasi-closed space with an atomic number ratio of Si / C less than 1.

[0103] According to an embodiment of the present invention, the heating temperature is preferably set in the range of 1400 to 2300°C, and more preferably in the range of 1600 to 2000°C.

[0104] According to one embodiment of the present invention, the heating time can be set to any time to obtain the desired etching amount. For example, when the etching rate is 1 μm / min, the heating time is 1 minute if the etching amount is to be set to 1 μm.

[0105] According to one embodiment of the invention, the temperature gradient is set in the range of 0.1 to 5 °C / mm.

[0106] Ideally, the temperature gradient according to an embodiment of the present invention should be the same in the raw material conveying space S0.

[0107] The etching amount and growth amount according to one embodiment of the present invention are, for example, in the range of 0.1 to 20 μm, but can be appropriately changed as needed.

[0108] According to one embodiment of the present invention, the etching rate and the growth rate of the growth layer can be controlled by the above-mentioned temperature range, for example, it can be set in the range of 0.001 to 2 μm / min.

[0109] It can be understood that the etching amount and the growth amount are the same according to one embodiment of the present invention.

[0110] The heating step according to one embodiment of the present invention can be understood to include: a clustering and decomposition step, which decomposes / suppresses the formation of MSBs on the surface of a semiconductor substrate based on an etching step.

[0111] The surface layer on the semiconductor substrate etched in the etching step according to an embodiment of the present invention can be understood as a processing-modified layer that has been subjected to mechanical processing (e.g., slicing, grinding / polishing) or laser processing, resulting in processing damage such as scratches or latent scratches, strain, etc.

[0112] Semiconductor Substrate Manufacturing Equipment The following uses Figures 4 to 10 A semiconductor substrate manufacturing apparatus (hereinafter referred to as the manufacturing apparatus) according to one embodiment of the present invention will be described in detail. Furthermore, structural elements that are substantially the same as those shown in the manufacturing method described above will be given the same reference numerals to simplify the description.

[0113] The manufacturing apparatus according to one embodiment of the present invention includes at least a workpiece, a heating furnace 30, and a high-melting-point container 40.

[0114] According to one embodiment of the present invention, the object to be processed refers to the assembly 10 and the main container 20. Furthermore, according to one embodiment of the present invention, the object to be processed may also be the assembly 10.

[0115] <Collection> The assembly 10 includes: a material transport space S0, a semiconductor substrate 11, a component made of a semiconductor substrate 12 or the material of the semiconductor substrate 11, and a mounting device 13. Furthermore, the processing unit 100 includes the mounting device 13 and the semiconductor substrates 11, 12, or a dummy substrate 14 described later. Details of the material transport space S0, the semiconductor substrates 11 and 12 are as described above.

[0116] Additionally, assembly 10 includes a semiconductor substrate 11 or one or more processing units 100. In the following description, examples are given of the case where assembly 10 includes multiple processing units 100.

[0117] <Setup Tools> The fixture 13 has an upper edge 13A and a lower edge 13B or a bottom 13C.

[0118] The upper edge 13A and lower edge 13B have through holes at approximately the center. Figure 5 In the example shown, the inner diameter of the through hole at the lower edge 13B is formed to be smaller than the inner diameter of the through hole at the upper edge 13A.

[0119] The upper edge 13A and lower edge 13B with such through holes are stacked in multiple layers to form a multi-level semiconductor substrate 11 capable of being disposed in multiple stages. That is, at least a portion of the upper bottom surface of the lower edge 13B is configured to serve as a contact surface with the semiconductor substrate 11.

[0120] The upper edge 13A supports the mounting fixture 13 above. The lower edge 13B supports at least a portion of the outer periphery of the semiconductor substrate. If necessary, the bottom edge 13C is disposed at the lowest point or the upper section of the lowest point, etc., instead of the lower edge 13B.

[0121] The upper bottom surface of the upper edge 13A and the lower bottom surface of the lower edge 13B can also be configured to each be equipped with a protrusion and a groove for setting different setting tools 13 by fitting or the like.

[0122] The mounting device 13 may also be configured to have a cover portion 13D opposite to the semiconductor substrate 11, 2 or the dummy substrate 14, in addition to the bottom portion 13C.

[0123] The mounting device 13 is positioned such that the semiconductor substrate 11 is adjacent to and substantially parallel to a component made of the semiconductor substrate 12, the dummy substrate 14, or the material of the semiconductor substrate 11, and is spaced apart by a transport distance D0. The details of the transport distance D0 are as described above. Alternatively, the transport distance D0 may be set to be small or large at approximately the end of the assembly 10.

[0124] One or more dummy substrates 14 are provided at approximately the end of the assembly 10. In addition, the number of dummy substrates 14 is not limited, and the assembly 10 may also be configured not to include dummy substrates 14.

[0125] The material of the dummy substrate 14 is preferably the same as that of the semiconductor substrates 11 and 12, but its crystallinity may not be the same as that of the semiconductor substrates 11 and 12. Specifically, it may also have the following structure: the semiconductor substrates 11 and 12 are single-crystal substrates, and the dummy substrate 14 is a polycrystalline substrate.

[0126] like Figure 4 As shown, a processing unit 100 according to an embodiment of the present invention includes: a semiconductor substrate 11 or a dummy substrate 14, and a mounting device 13 consisting of an upper edge 13A and a bottom edge 13C. A material transport space S0 is formed between the semiconductor substrate 11 or the dummy substrate 14 and the bottom edge 13C. Furthermore, an abutment surface 131 is formed on the entire surface of the semiconductor substrate 11 or the dummy substrate 14.

[0127] like Figure 5 As shown, a processing unit 100 according to an embodiment of the present invention includes: a semiconductor substrate 11, 12 or a dummy substrate 14; a mounting device 13 composed of an upper edge 13A and a lower edge 13B; and a mounting device 13 composed of an upper edge 13A and a bottom edge 13C. In this case, the mounting device 13 at the end of the processing unit 100 is composed of an upper edge 13A and a bottom edge 13C. Therefore, the semiconductor substrates 11 and 12 face each other, and a material delivery space S0 is formed between the semiconductor substrates 11 and 12. Furthermore, an abutment surface 131 is formed on the entire surface or the entire outer periphery of the semiconductor substrates 11, 12 or the dummy substrate 14.

[0128] like Figure 6 As shown, a processing unit 100 according to an embodiment of the present invention includes: a semiconductor substrate 11, 12 or a dummy substrate 14, and a mounting device 13 composed of an upper edge 13A and a lower edge 13B. At this time, the semiconductor substrates 11 and 12 face each other, and a material transport space S0 is formed between the semiconductor substrates 11 and 12. Furthermore, an abutment surface 131 is formed on the entire outer periphery of the semiconductor substrate 11 or the dummy substrate 14.

[0129] like Figure 7As shown, a processing unit 100 according to an embodiment of the present invention includes: a semiconductor substrate 11, 12 or a dummy substrate 14, and a mounting device 13 composed of an upper edge 13A and a lower edge 13B. At this time, the semiconductor substrates 11 and 12 face each other, and a material transport space S0 is formed between the semiconductor substrates 11 and 12. Furthermore, an abutment surface 131 is formed in a portion of the outer periphery of the semiconductor substrate 11 or the dummy substrate 14. Any conventional support device, such as a structure for holding the semiconductor substrates 11, 12 and the dummy substrate 14 and supporting or clamping at least a portion of the outer periphery, can be used.

[0130] The width of the outer periphery including the abutment surface 131 according to an embodiment of the present invention can be appropriately determined.

[0131] <Main Container> like Figure 8 As shown, the main container 20 can accommodate the assembly 10. Multiple main containers 20 according to one embodiment of the present invention can also be arranged in a stacked manner.

[0132] The main container 20 is a fitted container including an upper container 21 and a lower container 22 that can fit together. A small gap 24 is formed at the fitting part of the upper container 21 and the lower container 22, which is configured to allow air to be vented (vacuumed) from the main container 20 through the gap 24.

[0133] Ideally, the environment within the main container 20 after heat treatment should become a vapor pressure environment of a mixed system of gaseous species containing Si and gaseous species containing C. Examples of gaseous species containing Si include Si, Si2, Si3, Si2C, SiC2, and SiC. Examples of gaseous species containing C include Si2C, SiC2, SiC, and C.

[0134] This structure can be used as long as it generates vapor pressures of gaseous species containing Si and gaseous species containing C in the internal space during the heat treatment of the main container 20. For example, a structure in which SiC polycrystalline material is exposed at a portion of the inner surface, or a structure in which SiC polycrystalline material is separately disposed within the main container 20, can be shown.

[0135] The main container 20 has a steam supply source 23.

[0136] The steam supply source 23 is used to adjust the Si / C atomic ratio in the semi-enclosed space within the main container 20 to be greater than 1.

[0137] The steam supply source 23 can also be configured to be installed in the internal space of the assembly 10. Specifically, the steam supply source 23 is installed on the inner wall of the upper edge 13A or lower edge 13B of the fixture 13.

[0138] As a vapor supply source 23, examples include solid Si (Si particles such as Si single crystal wafers and Si powder) and Si compounds.

[0139] For example, as in one embodiment of the present invention, when the main container 20 is entirely composed of SiC polycrystalline material, by providing a vapor supply source 23, the Si / C atomic ratio within the main container 20 exceeds 1. Specifically, when a semiconductor substrate 11 and 12 with a stoichiometric ratio of 1:1 and a vapor supply source 23 are provided within a SiC polycrystalline main container 20 with a SiC polycrystalline material having a stoichiometric ratio of 1:1, the Si / C atomic ratio within the main container 20 exceeds 1.

[0140] In this way, by heating a space with an atomic ratio of Si / C greater than 1, it is possible to approach the vapor pressure environment when SiC (solid phase) and Si (liquid phase) are in phase equilibrium through the gas phase (SiC-Si equilibrium vapor pressure environment).

[0141] The dopant and doping concentration of the main container 20 can be selected based on the dopant and doping concentration of the growth layer 111 or 121 to be formed. For example, element N can be used as a dopant.

[0142] <Heating Furnace> like Figure 9 As shown, the heating furnace 30 is configured to heat to create a temperature gradient, such that the temperature decreases / increases from the upper container 21 of the main container 20 toward the lower container 22. That is, for example, a temperature gradient is formed in the thickness direction of the semiconductor substrate 11.

[0143] The heating furnace 30 includes: a main heating chamber 31, capable of heating the assembly 10 to a temperature above 1000°C and below 2300°C; a preheating chamber, capable of preheating the assembly 10 to a temperature above 500°C; a high melting point container 40, capable of housing the main container 20; and a moving device 33, capable of moving the high melting point container 40 from the preheating chamber 32 to the main heating chamber 31.

[0144] The main heating chamber 31 is equipped with, for example, a heater 34 (mesh heater). Furthermore, multiple layers of heat-reflective metal plates are fixed to the side walls or ceiling of the main heating chamber 31. These multiple layers of heat-reflective metal plates are configured to reflect the heat from the heater 34 towards approximately the center of the main heating chamber 31.

[0145] The heater 34 is configured to surround the high-melting-point container 40 containing the assembly within the main heating chamber 31. In this case, by providing multiple layers of heat-reflective metal plates on the outside of the heater 34, it becomes possible to raise the temperature within a range of 1000°C to 2300°C.

[0146] Heater 34 can be, for example, a resistance heater or a high-frequency induction heater.

[0147] The heater 34 may also employ a structure capable of creating a temperature gradient within the high-melting-point container 40. For example, the heater 34 may be configured to have multiple heaters disposed on the upper (or lower) side. Furthermore, the heater 34 may be configured such that its width increases as it moves upward (or downward). Alternatively, the heater 34 may be configured to increase the supplied power for heating as it moves upward (or downward).

[0148] The main heating chamber 31 is connected to: a vacuum forming valve 35 for venting the main heating chamber 31; an inert gas injection valve 36 for introducing inert gas into the main heating chamber 31; and a vacuum gauge 37 for measuring the vacuum level in the main heating chamber 31.

[0149] The vacuum forming valve 35 can be connected to a vacuum pump for venting and evacuating the main heating chamber 31. Through this vacuum forming valve 35 and the vacuum pump, the vacuum level in the main heating chamber 31 can be adjusted to preferably 10 Pa or less, more preferably 1 Pa or less, and even more preferably 10 Pa or less. -3 Pa or less. Examples of this vacuum pump include turbomolecular pumps or rotary pumps.

[0150] An inert gas injection valve 36 is connected to an inert gas supply source. Through this inert gas injection valve 36 and the inert gas supply source, inert gas can be injected into the main heating chamber 31 at a rate of 10... -5 Up to 10 4 Inert gas is introduced within the range of Pa.

[0151] The inert gas injection valve 36 is a doped gas supply device capable of supplying doped gas into the main container 20. That is, by selecting a doped gas (e.g., N2, etc.) as the inert gas, the doping concentration of the growth layer 111 can be increased.

[0152] The preparation chamber 32 is connected to the main heating chamber 31 and is configured to allow the high-melting-point container 40 to be moved by the moving device 33. Furthermore, in one embodiment of the present invention, the preparation chamber 32 is configured to utilize the residual heat from the heater 34 of the main heating chamber 31 for heating. For example, when the main heating chamber 31 is heated to 2000°C, the preparation chamber 32 is heated to approximately 1000°C, allowing for degassing of the assembly 10 and the main container 20.

[0153] The moving device 33 is configured to place and hold the high-melting-point container 40 and move it between the main heating chamber 31 and the preparatory chamber 32. At this time, the moving platform holding the high-melting-point container 40 moves vertically via a motor or the like. The moving device for placing and holding the high-melting-point container 40 can also be configured to rotate around an axis extending vertically. Furthermore, the components constituting the moving device 33 are preferably made of a semiconductor substrate material.

[0154] Since the transfer between the main heating chamber 31 and the preparatory chamber 32 using the moving device 33 is completed in as little as about 1 minute, it is possible to achieve a heating / cooling rate of 1~1000℃ / min.

[0155] Therefore, because rapid heating and cooling are possible, it is possible to observe surface morphologies that do not have a low-temperature growth history during heating and cooling. Furthermore, in Figure 9 In this configuration, a preparatory chamber 32 is provided above the main heating chamber 31, but it is not limited to this configuration and can be provided in any direction.

[0156] According to one embodiment of the present invention, the moving device 33 is, for example, a moving platform for placing a high-melting-point container 40. The contact portion between the moving platform and the high-melting-point container 40 becomes a heat propagation path.

[0157] Therefore, a temperature gradient can be formed inside the high melting point container 40, so that the contact side between the moving stage and the high melting point container 40 is the low temperature side.

[0158] In a heating furnace 30 according to one embodiment of the present invention, since the bottom of the high melting point container 40 is in contact with the moving stage, the temperature gradient is set such that the temperature decreases from the upper container 41 of the high melting point container 40 toward the lower container 42.

[0159] The direction of the temperature gradient can be set arbitrarily by changing the position of the contact portion between the moving stage and the high-melting-point container 40. For example, if the moving stage is a suspended type and the contact portion is located at the top of the high-melting-point container 40, heat escapes upwards. Therefore, the temperature gradient is set so that the temperature rises from the upper container 41 to the lower container 42 of the high-melting-point container 40. Furthermore, as described above, the temperature gradient can also be formed according to the structure of the heater 34.

[0160] The heating furnace 30 includes a gate valve 38 between the main heating chamber 31 and the preparatory chamber 32.

[0161] The gate valve 38 is a transport system gate valve that has the dimensions to allow the assembly 10 to be moved in and out via the moving device 33 and to maintain the vacuum level of the main heating chamber 31. The gate valve 38 can be any conventional device, including a valve plate for opening and closing the gate opening to the main heating chamber 31, a valve shaft on which the valve plate is mounted, and a cylinder for driving the valve shaft.

[0162] High melting point containers like Figure 10 As shown, the high melting point container 40 can accommodate the main container.

[0163] Like the main container 20, the high-melting-point container 40 is a fitted container comprising an upper container 41 and a lower container 42 that can fit together, and is configured to accommodate the main container 20. A small gap 43 is formed at the fitting part of the upper container 41 and the lower container 42, which allows for venting (vacuuming) of the high-melting-point container 40 through the gap 43.

[0164] The high melting point container 40 has a vapor supply material 44 capable of supplying vapor pressure of gaseous species containing Si into the high melting point container 40.

[0165] The vapor supply material 44 can be any structure that generates Si vapor in the high melting point container 40 during heat treatment, such as a thin film covering the inner wall of the high melting point container 40.

[0166] In the case that the high-melting-point container 40 is a metal compound such as TaC, the vapor supply material 44 is, for example, a silicide material that constitutes the metal atoms and Si atoms of the high-melting-point container 40.

[0167] The high-melting-point container 40, by having a vapor supply material 44 on its inner side, can maintain the vapor pressure environment of the gaseous species containing Si within the main container 20. This can be understood as the vapor pressure of the gaseous species containing Si within the main container 20 being balanced with the vapor pressure of the gaseous species containing Si outside the main container 20.

[0168] According to one embodiment of the present invention, the vapor pressure environment of gaseous species containing Si in the heating furnace 30 is formed using a high melting point container 40 and a vapor supply material 44. For example, any method that can form a vapor pressure environment of gaseous species containing Si around the main container 20 can be used in the structure of the present invention.

[0169] The high-melting-point container 40 is preferably configured as a high-melting-point material including the material whose melting point is equal to or higher than that of the material constituting the main container 20.

[0170] Examples of the high-melting-point container 40 include C as a general heat-resistant member, W, Re, Os, Ta, Mo as high-melting-point metals, Ta9C8, HfC, TaC, NbC, ZrC, Ta2C, TiC, WC, MoC as carbides, HfN, TaN, BN, Ta2N, ZrN, TiN as nitrides, HfB2, TaB2, ZrB2, NB2, TiB2 as borides, and SiC polycrystal, etc.

[0171] The member made of the material of the semiconductor substrate 11 according to one embodiment of the present invention refers to the installation tool 13 and the main container 20. That is, the materials of the installation tool 13 and the main container 20 are the materials of the semiconductor substrates 11 and 12. Therefore, at least a part of the installation tool 13 or the main container 20 can serve as a transport source or a transport destination in raw material transport according to one embodiment of the present invention.

[0172] Reference Examples 1 to 3 are shown below.

[0173] 《Reference Example 1》 Under the following conditions, the SiC single crystal substrate E10 is housed in the main container 20, and the main container 20 is housed in the high-melting-point container 40.

[0174] <SiC Single Crystal Substrate E10> Polymorph: 4H-SiC Substrate dimensions: transverse width (10 mm), longitudinal width (10 mm), thickness (0.3 mm) Off direction and off angle: 4° off in the <11-20> direction Growth surface: (0001) plane Presence or absence of MSB: Absent <Main Container 20> Material: SiC polycrystal Container dimensions: diameter (60 mm), height (4 mm) Distance between the SiC single crystal substrate E10 and the SiC material: 2 mm Si / C atomic ratio in the container: 1 or less <High-Melting-Point Container 40> Material: TaC Container dimensions: diameter (160 mm), height (60 mm) Vapor supply material 44 (Si compound): TaSi2 The SiC single crystal substrate E10 arranged under the above conditions is subjected to a heat treatment under the following conditions.

[0175] Heating temperature: 1700°C Heating time: 300 min Temperature gradient: 1℃ / mm Growth rate: 5 nm / min Vacuum level of main heating chamber 31: 10 -5 Pa Figure 11 This is an illustration of a method for determining the conversion rate from BPD to other defects / dislocations (TED, etc.) in growth layer E11.

[0176] Figure 11 (a) shows the growth of growth layer E11 through a heating step. In this heating step, BPD present in the SiC single crystal substrate E10 is converted to TED with a certain probability. Therefore, unless 100% conversion occurs, TED and BPD will be mixed at the surface of growth layer E11.

[0177] Figure 11 (b) shows the condition of defects in the growth layer E11 as confirmed using the KOH dissolution etching method. This KOH dissolution etching method involves immersing the SiC single-crystal substrate E10 in a dissolved salt (such as KOH) heated to approximately 500°C, forming etching pits at dislocations and defects, and identifying the type of dislocation based on the size and shape of these etching pits. This method yields the number of BPDs present on the surface of the growth layer E11.

[0178] Figure 11 (c) shows the removal of the growth layer E11 after KOH dissolution etching. In this method, after planarization to the depth of the etch pits by mechanical polishing, CMP, etc., the growth layer E11 is removed by thermal etching, exposing the surface of the SiC single crystal substrate E10.

[0179] Figure 11 (d) shows the condition of defects in the SiC single crystal substrate E10 obtained after removing the growth layer E11, confirmed using the KOH dissolution etching method. The number of BPDs present on the surface of the SiC single crystal substrate E10 was obtained using this method.

[0180] according to Figure 11 The sequence shown represents the number of BPDs present on the surface of growth layer E11 (refer to...). Figure 11 (b) and the number of BPDs present on the surface of the SiC single crystal substrate E10. Figure 11 By comparing (d) in the above, the BPD conversion rate from BPD to other defects / dislocations during the heating step can be obtained.

[0181] The number of BPDs present on the surface of growth layer E11 in Reference Example 1 is approximately 0 cm. -2, the number of BPDs present at the surface of the SiC single crystal substrate E10 is 1000 per cm -2 .

[0182] That is, it can be understood that BPDs are reduced / removed by disposing the SiC single crystal substrate E10 having no MSB on the surface thereof in a quasi-enclosed space with a Si / C atomic ratio of 1 or less and performing heating.

[0183] In Reference Example 1, a SiC-C equilibrium vapor pressure environment is formed inside the main vessel 20, so that the Si / C atomic ratio inside the main vessel 20 is 1 or less.

[0184] It can be understood that since the heating step including the etching step in the above method and the heating step including the etching step according to one embodiment of the present invention are based on the same reaction process, BPDs can be reduced / removed even in the etching step according to one embodiment of the present invention.

[0185] (Reference Example 2) Under the following conditions, the SiC single crystal substrate E10 is housed in the main vessel 20, and the main vessel 20 is housed in the high melting point vessel 40.

[0186] <SiC Single Crystal Substrate E10> Polytype: 4H-SiC Substrate dimensions: lateral width (10 mm), longitudinal width (10 mm), thickness (0.3 mm) Off-direction and off-angle: 4° off in the <11-20> direction Growth surface: (0001) plane Presence or absence of MSB: Present <Main Vessel 20> Material: SiC polycrystal Vessel dimensions: diameter (60 mm), height (4 mm) Distance between SiC single crystal substrate E10 and SiC material: 2 mm Vapor supply source 23: Si piece Si / C atomic ratio inside the vessel: more than 1 By housing the Si piece together with the SiC single crystal substrate in the main vessel 20, the Si / C atomic ratio inside the vessel becomes more than 1.

[0187] <High Melting Point Vessel 40> Material: TaC Vessel dimensions: diameter 160 mm × height 60 mm Vapor supply material 44 (Si compound): TaSi₂ The SiC single crystal substrate E10 configured under the above conditions will be subjected to heat treatment under the following conditions.

[0188] Heating temperature: 1800℃ Heating time: 60 min Temperature gradient: 1℃ / mm Growth rate: 68 nm / min Vacuum level of main heating chamber 31: 10 -5 Pa Figure 12 This is an SEM image of the surface of the SiC single crystal substrate E10 before the growth of the growth layer E11. Figure 12 (a) is a SEM image observed at magnification ×1000. Figure 12 (b) is the SEM image observed at magnification × 100000.

[0189] This can be understood as follows: an MSB is formed on the surface of the SiC single-crystal substrate E10 before the growth of the growth layer E11, and steps with a height of 3 nm or more are arranged with a platform width of an average of 42 nm. In addition, the step height is measured by AFM.

[0190] Figure 13 This is an SEM image of the surface of the SiC single crystal substrate E10 after the growth of the growth layer E11. Figure 13 (a) is a SEM image observed at magnification ×1000. Figure 13 (b) is the SEM image observed at magnification × 100000.

[0191] This can be understood as follows: no MSB was formed on the surface of the growth layer E11 in Reference Example 2, and the 1.0 nm (full cell) steps were regularly arranged with a platform width of 14 nm. Furthermore, the step height was measured using AFM.

[0192] Therefore, it can be understood that the growth layer E11 after the MSB is decomposed is formed by placing the SiC single crystal substrate E10 with MSB on the surface in a quasi-closed space with an atomic ratio of more than 1 Si / C and heating it.

[0193] In Reference Example 2, since the Si vapor supply source 26 is configured such that the Si / C atomic ratio in the main container 20 exceeds 1, a SiC-Si equilibrium vapor pressure environment is formed in the main container 20.

[0194] It can be understood that since the heating step including the etching step in the above method and the heating step including the etching step according to an embodiment of the present invention are based on the same reactant process, MSB on the surface of the SiC single crystal substrate can be decomposed even in the etching step according to an embodiment of the present invention.

[0195] Reference Example 3 Figure 14 This is a graph showing the relationship between heating temperature and growth rate obtained by the manufacturing method of SiC single crystal substrate according to the present invention. The horizontal axis of the graph is the reciprocal of temperature, and the vertical axis is the logarithmic representation of growth rate. The result of growing layer E11 on SiC single crystal substrate E10 in a space (within the main container 20) where the Si / C atomic ratio is greater than 1 is indicated by ○. Furthermore, the result of growing layer E11 on SiC single crystal substrate E10 in a space (within the main container 20) where the Si / C atomic ratio is less than 1 is indicated by ×.

[0196] In addition, Figure 14 In the curves, the thermodynamic calculation results of SiC substrate growth in the SiC-Si equilibrium vapor pressure environment are represented by the dashed line (Arrhenius diagram), and the thermodynamic calculation results of SiC substrate growth in the SiC-C equilibrium vapor pressure environment are represented by the double-dotted line (Arrhenius diagram).

[0197] In this method, under conditions where the vapor pressure environment between the SiC raw material and the SiC substrate is either a SiC-C equilibrium vapor pressure environment or a SiC-C equilibrium vapor pressure environment, the chemical potential difference or temperature gradient is used as the growth driving force to grow E10 on a SiC single crystal substrate. This chemical potential difference can be exemplified by the partial pressure difference of gaseous species generated on the surface of SiC polycrystalline and SiC single crystals.

[0198] Here, the SiC growth rate is calculated using Equation 1 below, with the partial pressure difference of the vapor generated from the SiC raw material (supply source) and the SiC substrate (supply destination) set as the growth rate.

[0199] [Formula 1] Here, T is the temperature on the SiC raw material side, m i For gaseous species (Si) x C y The molecular weight of ), where k is the Boltzmann constant.

[0200] In addition, P 输送源i -P 输送目的地i The raw material gas is in a supersaturated state and is used as the growth amount of SiC precipitation. As the raw material gas, SiC, Si2C, and SiC2 are envisioned.

[0201] That is, the dashed line represents the thermodynamic calculation results of growing SiC single crystals using SiC polycrystalline material in a vapor pressure environment where SiC (solid phase) and Si (liquid phase) are in phase equilibrium through the gas phase.

[0202] Specifically, thermodynamic calculations were performed using Equation 1 under the following conditions (i) to (iv): (i) a constant volume SiC-Si equilibrium vapor pressure environment; (ii) the growth driving force is the temperature gradient within the main container 20 and the vapor pressure difference (chemical potential difference) between the SiC polycrystalline and SiC single crystals; (iii) the feed gases are SiC, Si2C, and SiC2; and (iv) the adsorption coefficient of the feed gas adsorbed onto the step of the SiC single crystal substrate E10 is 0.001.

[0203] Furthermore, the double-dotted line represents the thermodynamic calculation results of growing SiC single crystals using SiC polycrystalline material in a vapor pressure environment where SiC (solid phase) and C (solid phase) are in phase equilibrium through the gas phase.

[0204] Specifically, thermodynamic calculations were performed using Equation 1 under the following conditions (i) to (iv): (i) a constant volume SiC-C equilibrium vapor pressure environment; (ii) the growth driving force is the temperature gradient within the main container 20 and the vapor pressure difference (chemical potential difference) between the SiC polycrystalline and SiC single crystals; (iii) the feed gases are SiC, Si2C, and SiC2; and (iv) the adsorption coefficient of the feed adsorbed onto the step of the SiC single crystal substrate E10 is 0.001.

[0205] In addition, the data for each chemical species used in the thermodynamic calculations are based on the values ​​from the JANAF thermochemical tables.

[0206] According to this Figure 14 The curves show that the results obtained by placing the SiC single crystal substrate E10 in a space (within the main container 20) with an atomic ratio of Si / C greater than 1 and growing the growth layer E11 on the SiC single crystal substrate E10 (marked with ○) are consistent with the thermodynamic calculation results of SiC growth in the SiC-Si equilibrium vapor pressure environment.

[0207] Furthermore, it can be understood that the results obtained by placing the SiC single crystal substrate E10 in a space (within the main container 20) with an atomic ratio of Si / C of less than 1 and growing the growth layer E11 on the SiC single crystal substrate E10 (× mark) tend to be consistent with the thermodynamic calculation results of SiC growth in the SiC-C equilibrium vapor pressure environment.

[0208] Under SiC-Si equilibrium vapor pressure conditions, a growth rate of over 1.0 μm / min is estimated to be achieved at a heating temperature of 1960 °C. Furthermore, a growth rate of over 2.0 μm / min is estimated to be achieved at heating temperatures above 2000 °C.

[0209] On the other hand, under SiC-C equilibrium vapor pressure conditions, a growth rate of 1.0 μm / min or higher is estimated to be achieved at a heating temperature of 2000 °C. Furthermore, a growth rate of 2.0 μm / min or higher is estimated to be achieved at a heating temperature of 2030 °C or higher.

[0210] According to the present invention, it is possible to increase the production volume in the manufacturing of semiconductor substrates.

[0211] also, Figure 15 This is an illustrative diagram of a semiconductor substrate manufacturing apparatus according to another embodiment of the present invention.

[0212] Such as Figure 15 As shown, the heater 34, which serves as a heating source, can be arranged in a direction intersecting the main surface of the semiconductor substrate 11. Furthermore, a temperature gradient can be formed between the heater 34 located at the upper part and the heater 34 located at the lower part by setting a temperature difference.

[0213] Furthermore, it is desirable that the heater 34 has a heating portion that generates heat, and the area of ​​the heating portion is set to be greater than or equal to the area of ​​the semiconductor substrate 11.

[0214] In this way, by arranging heaters 34 at the top and bottom, the temperature distribution on the surface of a semiconductor substrate 11 can be heated in a substantially uniform manner.

[0215] Explanation of reference numerals in the attached figures S0 Raw material conveying space D0 Conveying distance 10. Collective 100 processing units 11 Semiconductor substrate Growth layers 111 and 121 113, 123 main surface 114, 124 Back side 12 Semiconductor substrates 123 Main side 124 Back 13 Setting tools 13A Upper edge 13B Lower edge 131 Contact surface 14. Dummy Substrate 20 Main Containers Containers 21 and 41 Containers 22 and 42 23 Steam supply source 24, 43 gap 30 Heating Furnace 31 Main Heating Chamber 32. Preparation Room 33 Mobile devices 34 Heaters 36. Valve for inert gas injection 37 Vacuum gauge 38 Gate valve 40 High melting point containers 44 Steam supply materials

Claims

1. A method for manufacturing a SiC semiconductor substrate, comprising: In the setup step, multiple processed objects having SiC semiconductor substrates are stacked in the thickness direction of the SiC semiconductor substrates with adjacent SiC semiconductor substrates facing each other, forming a raw material transport space between adjacent SiC semiconductor substrates. and The heating step involves heating each of the plurality of processed objects to create a temperature gradient along the thickness direction of the SiC semiconductor substrate, thereby continuously conveying the raw material in the material conveying space. The heating step includes: The etching step involves etching the surface of the SiC semiconductor substrate, which serves as a raw material delivery source, located on the high-temperature side of the temperature gradient, thereby generating a raw material gas containing atomic species constituting the SiC semiconductor substrate. as well as In the growth step, the raw material gas is transported via the raw material transport space to the surface of the SiC semiconductor substrate, which is located on the low-temperature side of the temperature gradient and serves as the raw material transport source, to form a growth layer on the surface of the SiC semiconductor substrate, which serves as the raw material transport destination.

2. The manufacturing method according to claim 1, wherein, The surface of the SiC semiconductor substrate, which serves as the source of the raw material, and the surface of the SiC semiconductor substrate, which serves as the destination of the raw material, are opposite each other across the raw material transport space.

3. The manufacturing method according to claim 1, wherein, The driving force for the material transport is the vapor pressure difference between the SiC semiconductor substrate, which serves as the source of the material transport, and the SiC semiconductor substrate, which serves as the destination of the material transport, caused by the temperature gradient.

4. The manufacturing method according to claim 1, wherein, The etching step is a step of removing the processed modified layer on the surface of the SiC semiconductor substrate, which serves as a raw material delivery source, located on the high-temperature side of the temperature gradient, by etching.

5. The manufacturing method according to claim 1, wherein, During the heating step, the back side of the first SiC semiconductor substrate is etched simultaneously, and a growth layer is formed on the main surface of the second SiC semiconductor substrate adjacent to the first SiC semiconductor substrate. or Simultaneously, the formation of a growth layer on the back side of the first SiC semiconductor substrate and the etching of the main surface of the second SiC semiconductor substrate are performed.

6. The manufacturing method according to claim 1, wherein, The amount of etching of the SiC semiconductor substrate in the etching step is the same as the amount of growth of the growth layer in the growth step.

7. The manufacturing method according to claim 1, wherein, The material transport distance D0 between the SiC semiconductor substrate, which serves as the source of the material transport, and the SiC semiconductor substrate, which serves as the destination of the material transport, is less than 10 mm.

8. The manufacturing method according to claim 7, wherein, The material conveying distance D0 is 0.7 mm or more and 5 mm or less.

9. The manufacturing method according to any one of claims 1 to 8, wherein, Each of the plurality of said processed objects has a setting means for holding the SiC semiconductor substrate in a manner that the setting means holds the SiC semiconductor substrate in a manner that is substantially parallel to adjacent SiC semiconductor substrates.

10. The manufacturing method according to any one of claims 1 to 8, wherein, In the setup step, multiple SiC semiconductor substrates are placed inside a main container that is entirely composed of SiC polycrystalline materials.

Citation Information

Patent Citations

  • Electrode for short arc discharge lamp

    JP2017188381A

  • Label sheet

    JP2019086714A