Methods for manufacturing metal-carbon catalysts

By preparing nickel or cobalt metal-carbon catalysts, the problems of high cost and insufficient safety of precious metal catalysts have been solved, achieving inexpensive and efficient hydrogenation and hydrogen generation catalysis.

CN123125044APending Publication Date: 2026-11-17MITSUBISHI GAS CHEM CO INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580029252.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-03
Filing Date
2025-06-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, precious metal catalysts are expensive and have complex manufacturing processes, while cheap and highly active hydrogenation catalysts are not safe enough to meet the needs of large-scale hydrogen production and chemical reactions.

Method used

A metal-carbon catalyst containing nickel or cobalt is prepared by mixing a nitric acid solution of nickel or cobalt with a specific amine compound, precipitating and calcining the mixture, and then combining it with carbon black to enhance catalytic activity.

Benefits of technology

A low-cost and highly active metal-carbon catalyst was prepared, suitable for hydrogen generation and hydrogenation reactions, and exhibited excellent catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

A method for manufacturing a metal-carbon catalyst includes: step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor containing the amine (A) and the metal (M); and step 2, separating the catalyst precursor from the solution and calcining it.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing metal-carbon catalysts. Background Technology

[0002] Catalysts play a crucial role in various chemical reactions, either promoting the reaction or inhibiting side reactions. Among them, noble metal catalysts such as platinum are widely used.

[0003] Hydrogen production via water electrolysis has a very low environmental impact and is an important technology for a circular economy. The biggest challenge in water electrolysis is the high cost of hydrogen production. In this regard, catalyst materials are one of the most important factors significantly affecting the overall cost.

[0004] Platinum (Pt) catalysts have high and excellent catalytic activity as catalysts for hydrogen generation reaction (HER), but they are expensive, which significantly increases the cost of hydrogen production.

[0005] Therefore, the development of HER catalysts using inexpensive metals is underway.

[0006] For example, in Patent Document 1, as an alternative to the transition metal matrix that is abundant on Earth, a HER catalyst is disclosed: a catalyst metal species such as nickel and / or cobalt containing an active catalyst species, and a vanadium species, wherein the catalyst metal species and the vanadium species are embedded in the catalyst.

[0007] Furthermore, hydrogenation is a crucial chemical reaction, with the hydrogenation of unsaturated bonds, ketone groups, aldehyde groups, nitro groups, and others used in the synthesis of various chemical products. While noble metal catalysts such as Pt and palladium (Pd) are well-known for hydrogenation, their high cost is a significant drawback. Therefore, Raney nickel, which is relatively inexpensive and exhibits high hydrogenation catalytic activity, is widely used.

[0008] Existing technical documents

[0009] Patent documents

[0010] Patent Document 1: Japanese Patent Publication No. 2022-508971 Summary of the Invention

[0011] The problem the invention aims to solve

[0012] As mentioned above, catalysts that do not use precious metals such as platinum have been developed, but catalysts with sufficient performance have not yet been obtained. Furthermore, the preparation of HER catalysts that combine multiple metals, as in Patent Document 1, requires complex manufacturing processes and is unsuitable for large-scale hydrogen production. On the other hand, Raney nickel, in particular, used as a hydrogenation catalyst, can generate heat and ignite in a dry state, requiring careful handling. Therefore, there is a demand for hydrogenation catalysts that exhibit both low cost and high activity, as well as high safety.

[0013] As mentioned above, there is a need for a catalyst that is highly active as a HER catalyst and is also inexpensive and easy to manufacture, and can be used as a chemical reaction catalyst (e.g., a hydrogenation catalyst).

[0014] Therefore, the object of the present invention is to provide a method for manufacturing a metal-carbon catalyst that is inexpensive and has high catalytic activity, and an inexpensive metal-carbon catalyst that has high catalytic activity.

[0015] Solution for solving the problem

[0016] The inventors discovered that the above-mentioned problems can be solved by a manufacturing method that involves calcining a precursor obtained from a nitric acid solution of nickel or cobalt and a specific amine, thus completing the present invention.

[0017] That is, the present invention is a method for manufacturing a metal-carbon catalyst, comprising: step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor containing the amine (A) and the metal (M); and step 2, separating the catalyst precursor from the solution and calcining it. Additionally, the present invention is a metal-carbon catalyst containing 0.5 to 70% by mass of at least one metal (M) selected from the group consisting of nickel and cobalt.

[0018] The effects of the invention

[0019] According to the present invention, a method for manufacturing a metal-carbon catalyst that yields an inexpensive catalyst with high catalytic activity, and an inexpensive metal-carbon catalyst with high catalytic activity, are provided. The obtained metal-carbon catalyst is particularly excellent as a catalyst for hydrogen generation reactions and hydrogenation reactions. Attached Figure Description

[0020] Figure 1 This is an example of a linear sweep voltammetry (LSV) curve in a hydrogen generation test (Example 1-2 and Comparative Example 1) using the catalysts of Examples 1-2 and Comparative Example 1. Detailed Implementation

[0021] [Preparation methods for metal-carbon catalysts]

[0022] The method for manufacturing the metal-carbon catalyst of the present invention comprises the following steps: Step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor containing amine (A) and metal (M); and Step 2, separating the catalyst precursor from the solution and calcining it. Alternatively, the method for manufacturing the metal-carbon catalyst of the present invention preferably comprises the following steps: Step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor containing amine (A) and metal (M); and Step 2, separating the catalyst precursor from the solution, drying it, and calcining it.

[0023] According to the method for manufacturing the metal-carbon catalyst of the present invention, a catalyst with low cost and high catalytic activity can be obtained.

[0024] The specific method is as follows.

[0025] <Process 1: The process of precipitating the catalyst precursor (catalyst precursor precipitation process)>

[0026] The method for manufacturing the metal-carbon catalyst of the present invention includes the following step 1 as the initial step: mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having at least one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor containing amine (A) and metal (M).

[0027] (Solution)

[0028] A solution (hereinafter also simply referred to as a solution) comprising at least one metal (M) selected from the group consisting of nickel and cobalt and comprising nitric acid or nitrate comprises the metal (M), nitric acid or nitrate, and solvent.

[0029] Here, water and lower alcohols are examples of solvents, with lower alcohols being preferred. By using lower alcohols, the amount of amine (A) used can be suppressed. As a lower alcohol, aliphatic alcohols with 1 to 4 carbon atoms are preferred, and aliphatic alcohols with 1 to 3 carbon atoms are more preferred. Specifically, methanol, ethanol, and isopropanol are preferred, with methanol being more preferred. As a solvent, at least one selected from the group consisting of water and methanol is preferred, with methanol being more preferred. It should be noted that a mixture of methanol and water is also preferred.

[0030] The metal (M) is at least one selected from the group consisting of nickel and cobalt.

[0031] From the viewpoint of hydrogenation catalyst performance, the metal (M) is preferably selected from at least one of nickel and a mixture of nickel and cobalt, more preferably a mixture of nickel and cobalt.

[0032] Furthermore, from the viewpoint of selectively obtaining unsaturated alcohols by hydrogenating unsaturated aldehydes, the metal (M) is preferably cobalt.

[0033] Furthermore, from the viewpoint of HER catalyst performance, the metal (M) is preferably selected from at least one of nickel and a mixture of nickel and cobalt, and more preferably nickel.

[0034] When the metal (M) is a mixture of nickel and cobalt, the mixing ratio of nickel and cobalt (nickel / cobalt) is not particularly limited, but is preferably 0.1 to 10.0 in molar ratio, more preferably 0.2 to 5, and even more preferably 0.25 to 4.

[0035] The metal (M) is preferably contained in the solution in the form of metal ions. Specifically, the metal ions contained in the solution are preferably at least one selected from the group consisting of nickel ions and cobalt ions.

[0036] From the viewpoint of hydrogenation catalyst performance, the metal ions contained in the solution are more preferably selected from at least one of the group consisting of nickel ions and a mixture of nickel ions and cobalt ions, and more preferably a mixture of nickel ions and cobalt ions.

[0037] Furthermore, from the viewpoint of selectively obtaining unsaturated alcohols by hydrogenating unsaturated aldehydes, the metal ions contained in the solution are more preferably cobalt ions.

[0038] Furthermore, from the viewpoint of HER catalyst performance, the metal ions contained in the solution are more preferably selected from at least one of nickel ions and a mixture of nickel ions and cobalt ions, and more preferably nickel ions.

[0039] The content of metal (M) in the solution, calculated as metal ions, is preferably 0.1~50 g / L, more preferably 0.1~30 g / L, even more preferably 0.2~25 g / L, and even more preferably 1~20 g / L.

[0040] The solution contains nitric acid or a nitrate, preferably nitric acid. When nitric acid is included, it is also preferred to contain it in the form of nitrate ions. It should be noted that even when the solvent is a lower alcohol and completely anhydrous, the possibility of non-free nitrate ions is considered, but in this case, it is still preferred to contain it as a nitrate in the form of nitrate ions. As a nitrate, at least one is preferably selected from the group consisting of sodium nitrate, potassium nitrate, and calcium nitrate.

[0041] The concentration of nitric acid or nitrate in the solution, calculated in terms of nitrate ions, is preferably 0.005~8 mol / L, more preferably 0.008~6 mol / L, even more preferably 0.1~5 mol / L, and even more preferably 0.1~3 mol / L.

[0042] Furthermore, as a precursor by reacting the metal (M) with nitric acid, at least one of nickel nitrate and cobalt nitrate, selected from the group consisting of nickel and cobalt nitrates, can be used. Using nickel and cobalt nitrates is simple and preferred. Nickel nitrate is more preferred.

[0043] As a method for preparing the solution, it is sufficient to mix the metal (M), nitric acid or nitrate, and the solvent. The order of mixing can be arbitrary, and pre-mixing and reaction can also be used. Specifically, the following combinations are considered. As a method for pre-mixing nitric acid and solvent, a method of mixing nickel hydroxide and an aqueous solution of nitric acid can be cited. As a method for pre-reacting nitric acid with the metal, a method of mixing a metal nitrate salt containing metal (M) (ions) and nitric acid (ions) with methanol can be cited.

[0044] (Amine(A))

[0045] The amine (A) is an amine having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, preferably an amine having one or two benzylamino groups, and more preferably an amine having two benzylamino groups.

[0046] The amine (A) is preferably an amine having two amino groups, and more preferably a diamine.

[0047] The amine (A) preferably has 3 to 8 carbon atoms, more preferably 4 to 8, and even more preferably 6 to 8.

[0048] By giving amine (A) the structure described above, the resulting catalyst has high activity, and is particularly excellent as a catalyst for hydrogen generation reaction and hydrogenation reaction.

[0049] As an amine having a benzylamino group, at least one can be selected from the group consisting of phenylenediamine and benzylamine, with phenylenediamine being preferred.

[0050] As an amine having an aliphatic amino group, at least one can be selected from the group consisting of bis(aminomethyl)cyclohexane, hexamethylenediamine, 2-ethylhexylamine, and propylamine.

[0051] The amine (A) is preferably at least one selected from the group consisting of phenylenediamine, bis(aminomethyl)cyclohexane, hexamethylenediamine, 2-ethylhexylamine and propylamine, more preferably at least one selected from the group consisting of phenylenediamine and bis(aminomethyl)cyclohexane, and even more preferably phenylenediamine.

[0052] The preferred bis(aminomethyl)cyclohexane is at least one selected from the group consisting of 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane, more preferably 1,4-bis(aminomethyl)cyclohexane.

[0053] The phenylenediamine is preferably selected from at least one of the group consisting of m-phenylenediamine and p-phenylenediamine, and more preferably m-phenylenediamine.

[0054] (Mixture of solution and amine (A))

[0055] In this process, the solution is mixed with amine (A) to precipitate a catalyst precursor containing amine (A) and metal (M).

[0056] In this process, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 0.5 to 500, more preferably 1 to 400, further preferably 1 to 300, even more preferably 2 to 200, even more preferably 2 to 100, even more preferably 2 to 80, and even more preferably 2 to 50.

[0057] It should be noted that when metal (M) is a mixture of nickel and cobalt, the molar amount of metal (M) is the total molar amount of nickel and the molar amount of cobalt.

[0058] In particular, when the solvent is water, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 1 to 500, more preferably 2 to 400, even more preferably 5 to 300, even more preferably 10 to 200, and even more preferably 20 to 100.

[0059] Furthermore, when the solvent is a lower alcohol, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 0.5 to 100, more preferably 1 to 50, even more preferably 1 to 30, even more preferably 2 to 20, and even more preferably 2 to 10.

[0060] It should be noted that when metal (M) is a mixture of nickel and cobalt, the molar amount of metal (M) is the total molar amount of nickel and the molar amount of cobalt.

[0061] In this process, the molar ratio of amine (A) (amino equivalent) to nitrate ions (amino / nitrate ions of amine (A)) is preferably 1 to 3.

[0062] The mixing method in this process can be any method that enables the solution to mix well with the amine (A). The amine (A) can be added to the solution, or the solution can be added to the amine (A). Stirring or shaking can be used to mix the mixture.

[0063] The mixing time (stirring time or shaking time) can be adjusted appropriately according to the concentration of the components of the solution, the type of solvent, the amount of amine (A), the temperature of the solution, etc., preferably 1 minute or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. Mixing can be stopped when the precipitation of the catalyst precursor containing amine (A) and metal (M) is completed.

[0064] As described above, a precipitate containing an amine (A) and a metal (M) can be obtained.

[0065] Furthermore, in this process, it is preferable to mix carbon black. Specifically, preferred step 1 involves mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt, and containing nitric acid or nitrate, with carbon black and an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor composition containing amine (A), metal (M), and carbon black. It should be noted that carbon black may be contained in the solution. That is, step 1 can be a process of mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt, carbon black, and containing nitric acid or nitrate, with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor composition containing amine (A), metal (M), and carbon black.

[0066] It should be noted that in this specification, when the catalyst precursor is obtained in the form of a catalyst precursor composition containing carbon black, the catalyst precursor composition may be considered synonymous with the catalyst precursor.

[0067] The carbon black used in this process can be categorized as furnace black, channel black, acetylene black, and thermal cracking black, with furnace black being the preferred option.

[0068] The amount of carbon black relative to 100 parts by mass of metal (M) (metal element, metal ion) is preferably 50 to 5000 parts by mass, more preferably 100 to 3000 parts by mass, further preferably 100 to 2000 parts by mass, and even more preferably 200 to 1000 parts by mass.

[0069] When mixing carbon black, the preferred molar ratio of amine (A) to metal (M) is also as described above.

[0070] Furthermore, the mixing method for mixing carbon black can be any method that can effectively mix the solution, carbon black, and amine (A), and any component can be added. Preferred methods include: adding carbon black to the solution and then adding amine (A); and adding carbon black to the dispersion after mixing the solution with amine (A) to obtain a precipitate. More preferably, the method of adding carbon black to the solution and then adding amine (A) is used. To achieve overall mixing, stirring or shaking can be performed.

[0071] The mixing time (stirring time or shaking time) can be adjusted appropriately according to the concentration of the components of the above solution, the type of solvent, the amount of amine (A), the type and / or amount of carbon black, the temperature of the solution, etc., preferably 1 minute or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. Mixing can be stopped when the precipitation of the catalyst precursor composition containing amine (A), carbon black and metal (M) is completed.

[0072] As described above, a precipitate comprising a catalyst precursor composition containing an amine (A), carbon black, and a metal (M) can be obtained.

[0073] A catalyst can be obtained by calcining a precipitate containing carbon black, as described below. The catalyst obtained in this way exhibits excellent catalytic activity, particularly its hydrogenation catalytic activity. The reason for this is not yet certain, but it can be attributed to the fact that supporting the metal-carbon catalyst with carbon black can inhibit catalyst aggregation and increase the specific surface area of ​​the catalyst.

[0074] <Step 2: Separating the catalyst precursor from the solution and calcining it (catalyst precursor recovery step and calcination step)>

[0075] The method for manufacturing the metal-carbon catalyst of the present invention includes, following step 1, a step 2 in which the catalyst precursor is separated from the solution and calcined. Step 2 is preferably a step following step 1 in which the catalyst precursor is separated from the solution, dried, and calcined.

[0076] In this process, firstly, the catalyst precursor is separated from the solution. If carbon black is used in the previous process, the catalyst precursor composition containing carbon black is separated from the solution. In this case, step 2 is a process following step 1 where the catalyst precursor composition is separated from the solution and calcined.

[0077] There are no particular limitations on the method for separating catalyst precursors or catalyst precursor compositions from solution; various solid-liquid separation methods can be used. For example, filtration and centrifugation can be listed.

[0078] Next, the obtained precipitate (catalyst precursor or catalyst precursor composition) is preferably dried. Drying is preferably carried out before calcination. There are no restrictions on the drying method.

[0079] Next, the catalyst precursor or catalyst precursor composition is calcined to obtain a metal-carbon catalyst.

[0080] In step 2, the firing temperature is preferably 250~1000℃, more preferably 300~1000℃, even more preferably 300~900℃, even more preferably 400~900℃, even more preferably 450~850℃, and even more preferably 450~800℃.

[0081] The firing time can be adjusted according to the firing temperature, etc., preferably 5 minutes to 10 hours, more preferably 10 minutes to 5 hours, and even more preferably 15 minutes to 2 hours.

[0082] Firing is preferably carried out in the presence of an inert gas. Nitrogen is more preferably an inert gas.

[0083] By calcining under the above conditions, the catalytic activity of the obtained catalyst can be improved.

[0084] [Catalyst precursors and methods for manufacturing catalyst precursors]

[0085] The catalyst precursor of the present invention is a catalyst precursor comprising at least one metal (M) selected from the group consisting of nickel and cobalt and comprising an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups.

[0086] The catalyst can be obtained by calcining the catalyst precursor.

[0087] The metal (M) contained in the catalyst precursor is at least one selected from the group consisting of nickel and cobalt.

[0088] From the viewpoint of hydrogenation catalyst performance, the metal (M) is preferably selected from at least one of nickel and a mixture of nickel and cobalt, more preferably a mixture of nickel and cobalt.

[0089] Furthermore, from the viewpoint of selectively obtaining unsaturated alcohols by hydrogenating unsaturated aldehydes, the metal (M) is preferably cobalt.

[0090] Furthermore, from the viewpoint of HER catalyst performance, the metal (M) is preferably selected from at least one of nickel and a mixture of nickel and cobalt, and more preferably nickel.

[0091] When the metal (M) contained in the catalyst precursor is a mixture of nickel and cobalt, the mixing ratio of nickel to cobalt (nickel / cobalt) is preferably 0.1 to 10, more preferably 0.2 to 5, and even more preferably 0.25 to 4 in molar ratio.

[0092] The content of metal (M) can be adjusted appropriately according to the type of metal and amine used as raw materials. In the catalyst precursor, it is preferably 3 to 40% by mass, more preferably 5 to 35% by mass, even more preferably 5 to 25% by mass, and even more preferably 5 to 20% by mass.

[0093] When the catalyst precursor is obtained in the form of a catalyst precursor composition containing carbon black, the content of metal (M) can be appropriately adjusted according to the type of metal and amine used as raw materials. In the catalyst precursor composition, it is preferably 0.1 to 20% by mass, more preferably 0.3 to 15% by mass, even more preferably 0.5 to 10% by mass, and even more preferably 1 to 7% by mass.

[0094] The amine (A) contained in the catalyst precursor or catalyst precursor composition having at least one amino group selected from the group consisting of benzylamino and aliphatic amino groups is an amine having at least one amino group selected from the group consisting of benzylamino and aliphatic amino groups, preferably an amine having one or two benzylamino groups, more preferably an amine having two benzylamino groups.

[0095] The amine (A) is preferably an amine having two amino groups, and more preferably a diamine.

[0096] The amine (A) preferably has 3 to 8 carbon atoms, more preferably 4 to 8, and even more preferably 6 to 8.

[0097] By giving the amine (A) the structure described above, the catalyst obtained using the catalyst precursor or catalyst precursor composition has high activity, and is particularly excellent as a catalyst for hydrogen generation reaction and hydrogenation reaction.

[0098] As an amine having a benzylamino group, at least one can be selected from the group consisting of phenylenediamine and benzylamine, with phenylenediamine being preferred.

[0099] As an amine having an aliphatic amino group, at least one can be selected from the group consisting of bis(aminomethyl)cyclohexane, hexamethylenediamine, 2-ethylhexylamine, and propylamine.

[0100] The amine (A) is preferably at least one selected from the group consisting of phenylenediamine, bis(aminomethyl)cyclohexane, hexamethylenediamine, 2-ethylhexylamine and propylamine, more preferably at least one selected from the group consisting of phenylenediamine and bis(aminomethyl)cyclohexane, and even more preferably phenylenediamine.

[0101] The preferred bis(aminomethyl)cyclohexane is at least one selected from the group consisting of 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane, more preferably 1,4-bis(aminomethyl)cyclohexane.

[0102] The phenylenediamine is preferably selected from at least one of the group consisting of m-phenylenediamine and p-phenylenediamine, and more preferably m-phenylenediamine.

[0103] The molar ratio (metal(M) / amine(A)) of the metal (M) to amine (A) contained in the catalyst precursor is preferably 5 / 0.2 to 0.2 / 5, more preferably 3 / 0.5 to 0.5 / 3, and even more preferably 2 / 1 to 1 / 2. More specifically, the molar ratio (metal(M) / amine(A)) varies depending on the type of metal (M) and amine (A). For example, the molar ratio of nickel to phenylenediamine (nickel / phenylenediamine) is preferably about 1 / 2, the molar ratio of nickel to bis(aminomethyl)cyclohexane (nickel / bis(aminomethyl)cyclohexane) is preferably about 1 / 2, the molar ratio of cobalt to phenylenediamine (cobalt / phenylenediamine) is preferably about 2 / 1, the molar ratio of cobalt to benzylamine (cobalt / benzylamine) is preferably about 1 / 1, and the molar ratio of cobalt to 2-ethylhexylamine (cobalt / 2-ethylhexylamine) is preferably about 1 / 1. In addition, when the metal (M) is a mixture of nickel and cobalt, the molar ratio of nickel·cobalt to phenylenediamine (nickel·cobalt / phenylenediamine) is preferably about 1 / 1.

[0104] The preferred method for manufacturing the catalyst precursor of the present invention is a method comprising: step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating the catalyst precursor containing the amine (A) and the metal (M); and step 3, separating the catalyst precursor into solid and liquid components. More preferably, the method for manufacturing the catalyst precursor of the present invention is a method comprising: step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating the catalyst precursor containing the amine (A) and the metal (M); step 3, separating the catalyst precursor into solid and liquid components; and step 4, drying.

[0105] Step 1 of the method for manufacturing the catalyst precursor of the present invention is the same as <Step 1: Step of precipitating the catalyst precursor (catalyst precursor precipitation step)> in the [method for manufacturing a metal-carbon catalyst], and the preferred conditions are also the same. The specific conditions are as follows.

[0106] A solution (hereinafter also simply referred to as a solution) comprising at least one metal (M) selected from the group consisting of nickel and cobalt and comprising nitric acid or nitrate comprises the metal (M), nitric acid or nitrate, and solvent.

[0107] Here, water and lower alcohols are examples of solvents, with lower alcohols being preferred. By using lower alcohols, the amount of amine (A) used can be suppressed. As a lower alcohol, aliphatic alcohols with 1 to 4 carbon atoms are preferred, and aliphatic alcohols with 1 to 3 carbon atoms are more preferred. Specifically, methanol, ethanol, and isopropanol are preferred, with methanol being more preferred. As a solvent, at least one selected from the group consisting of water and methanol is preferred, with methanol being more preferred. It should be noted that a mixture of methanol and water is also preferred.

[0108] The metal (M) is at least one selected from the group consisting of nickel and cobalt. From the viewpoint of hydrogenation catalyst performance, the metal (M) is preferably at least one selected from the group consisting of nickel and mixtures of nickel and cobalt, and more preferably a mixture of nickel and cobalt.

[0109] Furthermore, from the viewpoint of selectively obtaining unsaturated alcohols by hydrogenating unsaturated aldehydes, the metal (M) is preferably cobalt.

[0110] Furthermore, from the viewpoint of HER catalyst performance, the metal (M) is preferably selected from at least one of nickel and a mixture of nickel and cobalt, and more preferably nickel.

[0111] When the metal (M) is a mixture of nickel and cobalt, the mixing ratio of nickel and cobalt (nickel / cobalt) is not particularly limited, but is preferably 0.1 to 10 in molar ratio, more preferably 0.2 to 5, and even more preferably 0.25 to 4.

[0112] The metal (M) is preferably contained in the solution in the form of metal ions. Specifically, the metal ions contained in the solution are preferably at least one selected from the group consisting of nickel ions and cobalt ions.

[0113] From the viewpoint of hydrogenation catalyst performance, the metal ions contained in the solution are more preferably selected from at least one of the group consisting of nickel ions and a mixture of nickel ions and cobalt ions, and more preferably a mixture of nickel ions and cobalt ions.

[0114] Furthermore, from the viewpoint of selectively obtaining unsaturated alcohols by hydrogenating unsaturated aldehydes, the metal ions contained in the solution are more preferably cobalt ions.

[0115] Furthermore, from the viewpoint of HER catalyst performance, the metal ions contained in the solution are more preferably selected from at least one of nickel ions and a mixture of nickel ions and cobalt ions, and more preferably nickel ions.

[0116] The content of metal (M) in the solution, calculated as metal ions, is preferably 0.1~50 g / L, more preferably 0.1~30 g / L, even more preferably 0.2~25 g / L, and even more preferably 1~20 g / L.

[0117] The solution contains nitric acid or a nitrate, preferably nitric acid. When nitric acid is included, it is also preferred to contain it in the form of nitrate ions. It should be noted that even when the solvent is a lower alcohol and completely free of water, the absence of free nitrate ions is considered, but in this case, it is still preferred to contain it as a nitrate in the form of nitrate ions. As a nitrate, at least one is preferably selected from the group consisting of sodium nitrate, potassium nitrate, and calcium nitrate.

[0118] The concentration of nitric acid or nitrate in the solution, calculated in terms of nitrate ions, is preferably 0.005~8 mol / L, more preferably 0.008~6 mol / L, even more preferably 0.1~5 mol / L, and even more preferably 0.1~3 mol / L.

[0119] Furthermore, as a precursor by reacting the metal (M) with nitric acid, at least one of nickel nitrate and cobalt nitrate, selected from the group consisting of nickel and cobalt nitrates, can be used. Using nickel and cobalt nitrates is convenient and preferred. Nickel nitrate is more preferred.

[0120] As a method for preparing the solution, it is sufficient to mix the metal (M), nitric acid or nitrate, and the solvent. The order of mixing can be arbitrary, and pre-mixing and reaction can also be used. Specifically, the following combinations are considered. As a method for pre-mixing nitric acid and solvent, a method of mixing nickel hydroxide with an aqueous solution of nitric acid can be listed; as a method for pre-reacting nitric acid with the metal, a method of mixing a metal nitrate salt containing metal (M) (ions) and nitric acid (ions) with methanol can be listed, etc.

[0121] (Amine(A))

[0122] The amine (A) is an amine having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, preferably an amine having one or two benzylamino groups, and more preferably an amine having two benzylamino groups.

[0123] The amine (A) is preferably an amine having two amino groups, and more preferably a diamine.

[0124] The amine (A) preferably has 3 to 8 carbon atoms, more preferably 4 to 8, and even more preferably 6 to 8.

[0125] By giving amine (A) the structure described above, the resulting catalyst has high activity, and is particularly excellent as a catalyst for hydrogen generation reaction and hydrogenation reaction.

[0126] As an amine having a benzylamino group, at least one can be selected from the group consisting of phenylenediamine and benzylamine, with phenylenediamine being preferred.

[0127] As an amine having an aliphatic amino group, at least one can be selected from the group consisting of bis(aminomethyl)cyclohexane, hexamethylenediamine, 2-ethylhexylamine, and propylamine.

[0128] The amine (A) is preferably at least one selected from the group consisting of phenylenediamine, bis(aminomethyl)cyclohexane, hexamethylenediamine, 2-ethylhexylamine and propylamine, more preferably at least one selected from the group consisting of phenylenediamine and bis(aminomethyl)cyclohexane, and even more preferably phenylenediamine.

[0129] The preferred bis(aminomethyl)cyclohexane is at least one selected from the group consisting of 1,3-bis(aminomethyl)cyclohexane and 1,4-bis(aminomethyl)cyclohexane, more preferably 1,4-bis(aminomethyl)cyclohexane.

[0130] The phenylenediamine is preferably selected from at least one of the group consisting of m-phenylenediamine and p-phenylenediamine, and more preferably m-phenylenediamine.

[0131] (Mixture of solution and amine (A))

[0132] In this process, the solution is mixed with amine (A) to precipitate a catalyst precursor containing amine (A) and metal (M).

[0133] In this process, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 0.5 to 500, more preferably 1 to 400, further preferably 1 to 300, even more preferably 2 to 200, and even more preferably 2 to 100. That is, in step 1, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 0.5 to 500, more preferably 1 to 400, further preferably 1 to 300, even more preferably 2 to 200, even more preferably 2 to 100, even more preferably 2 to 80, and even more preferably 2 to 50.

[0134] It should be noted that when metal (M) is a mixture of nickel and cobalt, the molar amount of metal (M) is the total molar amount of nickel and the molar amount of cobalt.

[0135] In particular, when the solvent is water, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 1 to 500, more preferably 2 to 400, even more preferably 5 to 300, even more preferably 10 to 200, and even more preferably 20 to 100.

[0136] Furthermore, when the solvent is a lower alcohol, the molar ratio (number of amine molecules / number of metal atoms) of amine (A) to metal (M) is preferably 0.5 to 100, more preferably 1 to 50, even more preferably 1 to 30, even more preferably 2 to 20, and even more preferably 2 to 10.

[0137] It should be noted that when metal (M) is a mixture of nickel and cobalt, the molar amount of metal (M) is the total molar amount of nickel and the molar amount of cobalt.

[0138] In this process, the molar ratio of amine (A) (amino equivalent) to nitrate ions (amino / nitrate ions of amine (A)) is preferably 1 to 3.

[0139] The mixing method in this process can be any method that enables the solution to mix well with the amine (A). The amine (A) can be added to the solution, or the solution can be added to the amine (A). Stirring or shaking can be used to mix the mixture.

[0140] The mixing time (stirring time or shaking time) can be adjusted appropriately according to the concentration of the components of the solution, the type of solvent, the amount of amine (A), the temperature of the solution, etc., preferably 1 minute or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. Mixing can be stopped when the precipitation of the catalyst precursor containing amine (A) and metal (M) is completed.

[0141] As described above, a precipitate containing an amine (A) and a metal (M) can be obtained.

[0142] Furthermore, in this process, it is preferable to mix carbon black. Specifically, preferred step 1 involves mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt, and containing nitric acid or nitrate, with carbon black and an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor composition containing amine (A), metal (M), and carbon black. It should be noted that carbon black may be contained in the solution. That is, step 1 can be a process of mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt, carbon black, and containing nitric acid or nitrate, with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor composition containing amine (A), metal (M), and carbon black.

[0143] It should be noted that the catalyst precursor in this specification does not contain carbon black. When carbon black is included, it is referred to as a catalyst precursor composition containing both catalyst precursor and carbon black.

[0144] The carbon black used in this process can be categorized as furnace black, channel black, acetylene black, and thermal cracking black, with furnace black being the preferred option.

[0145] The amount of carbon black relative to 100 parts by mass of metal (M) (metal element, metal ion) is preferably 50 to 5000 parts by mass, more preferably 100 to 3000 parts by mass, further preferably 100 to 2000 parts by mass, and even more preferably 200 to 1000 parts by mass.

[0146] When mixing carbon black, the preferred molar ratio of amine (A) to metal (M) is also as described above.

[0147] Furthermore, the mixing method for mixing carbon black can be any method that can effectively mix the solution, carbon black, and amine (A), and any component can be added. Preferred methods include: adding carbon black to the solution and then adding amine (A); and adding carbon black to the dispersion after mixing the solution with amine (A) to obtain a precipitate. More preferably, the method of adding carbon black to the solution and then adding amine (A) is used. To achieve overall mixing, stirring or shaking can be performed.

[0148] The mixing time (stirring time or shaking time) can be adjusted appropriately according to the concentration of the components of the above solution, the type of solvent, the amount of amine (A), the type and / or amount of carbon black, the temperature of the solution, etc., preferably 1 minute or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. Mixing can be stopped when the precipitation of the catalyst precursor composition containing amine (A), carbon black and metal (M) is completed.

[0149] As described above, a precipitate comprising a catalyst precursor composition containing an amine (A), carbon black, and a metal (M) can be obtained.

[0150] The method for manufacturing the catalyst precursor of the present invention includes, following step 1, step 3, separating the catalyst precursor from the solution.

[0151] In this process, firstly, the catalyst precursor is separated from the solution. If carbon black is used in the previous process, the catalyst precursor composition containing carbon black is separated from the solution. In this case, step 3 is the step of separating the catalyst precursor composition from the solution following step 1.

[0152] There are no particular limitations on the method for separating catalyst precursors or catalyst precursor compositions from solution; various solid-liquid separation methods can be used. For example, filtration and centrifugation can be listed.

[0153] Next, step 4 can be performed as an optional step. Step 4 is a drying step, which involves drying the obtained precipitate (catalyst precursor or catalyst precursor composition). Drying is preferably performed before calcination to obtain the catalyst. There are no limitations on the drying method.

[0154] As described above, catalyst precursors or catalyst precursor compositions can be obtained.

[0155] [Metal-Carbon Catalyst]

[0156] The metal-carbon catalyst of the present invention comprises 0.5 to 80% by mass, preferably 1 to 80% by mass, more preferably 10 to 80% by mass, further preferably 15 to 80% by mass, even more preferably 20 to 80% by mass, even more preferably 30 to 80% by mass, and even more preferably 40 to 75% by mass of at least one metal (M) selected from the group consisting of nickel and cobalt.

[0157] The metal-carbon catalyst of the present invention is a metal-carbon catalyst that, when carbon black is included, contains preferably 0.5 to 60% by mass, more preferably 1 to 60% by mass, even more preferably 5 to 50% by mass, even more preferably 5 to 40% by mass, even more preferably 5 to 35% by mass, and even more preferably 5 to 30% by mass of at least one metal (M) selected from the group consisting of nickel and cobalt.

[0158] With the structure described above, it becomes inexpensive and has high catalytic activity, especially as a catalyst for hydrogen generation reaction and hydrogenation reaction.

[0159] The metal (M) content in the metal-carbon catalyst is preferably 0.5 to 80% by mass, more preferably 0.5 to 70% by mass, and even more preferably 1 to 60% by mass.

[0160] The metal-carbon catalyst of the present invention has metal-carbon bonds. Therefore, the metal-carbon catalyst of the present invention is a metal-carbon catalyst comprising 0.5 to 80% by mass of at least one metal (M) selected from the group consisting of nickel and cobalt, and having a bond (metal (M)-carbon bond) between at least one metal (M) selected from the group consisting of nickel and cobalt and carbon.

[0161] The metal-carbon catalyst of the present invention is preferably obtained by the aforementioned [method of manufacturing metal-carbon catalyst]. That is, the metal-carbon catalyst of the present invention is preferably obtained by a manufacturing method comprising the following steps: step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate with an amine (A) having one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, thereby precipitating a catalyst precursor containing amine (A) and metal (M); and step 2, separating the catalyst precursor into solid and liquid phases and calcining it.

[0162] Furthermore, in step 1, carbon black is preferably used. When carbon black is used, the metal-carbon catalyst of the present invention is preferably a metal-carbon catalyst obtained by a manufacturing method comprising the following steps: step 1, mixing a solution containing at least one metal (M) selected from the group consisting of nickel and cobalt and containing nitric acid or nitrate, with carbon black, and with an amine (A) having at least one or two amino groups selected from the group consisting of benzylamino and aliphatic amino groups, to precipitate a catalyst precursor composition containing amine (A), metal (M) and carbon black; and step 2, separating the catalyst precursor composition into solid and liquid phases and calcining it.

[0163] Example

[0164] The present invention will be specifically described based on the embodiments shown below, but the present invention is not limited to these embodiments.

[0165] [Preparation of metal-carbon catalysts]

[0166] Example 1 (Preparation of Nickel-Carbon Catalyst)

[0167] <Process 1: Catalyst Precipitation Process>

[0168] In a methanol solution containing nickel nitrate at a concentration of 10 g / L, m-phenylenediamine was added in an amount twice the amount (mol / mol) relative to nickel. The solution was then shaken at 25 °C for 1 hour to obtain a precipitate.

[0169] <Process 2-1: Catalyst Precursor Recovery Process>

[0170] The resulting precipitate and solution were separated by filtration. The resulting solid was dried under reduced pressure to obtain the catalyst precursor as a bluish-white powder.

[0171] <Process 2-2: Firing Process>

[0172] 0.1 g of the catalyst precursor was added to a tubular electric furnace (FT-02VAC-03, manufactured by FULLTEC Corporation), and calcined at a calcination temperature of 900°C for 15 minutes while nitrogen gas was flowing at a rate of 100-200 mL / min, to obtain a nickel-carbon catalyst in the form of a black powder.

[0173] Example 2 (Preparation of nickel-carbon catalyst)

[0174] In Example 1, m-phenylenediamine was replaced with 1,4-bis(aminomethyl)cyclohexane, and otherwise a nickel-carbon catalyst was obtained in the same manner as in Example 1.

[0175] Examples 3 and 4 (Preparation of nickel-carbon catalysts)

[0176] The firing temperature in <Step 2-2: Firing Step> of Example 1 was changed from 900°C to the temperature recorded in Table 2. Otherwise, the nickel-carbon catalyst was obtained in the same manner as in Example 1.

[0177] Example 5 (Preparation of a nickel-carbon catalyst using carbon black)

[0178] <Process 1: Precipitation of Catalyst Precursor Composition>

[0179] Add 50 mg of carbon black (Vulcan XC-72, manufactured by Cabot Corporation) to 30 mL of a methanol solution containing nickel nitrate at a concentration of 1 g / L. Then add 2 mL of methanol to dissolve m-phenylenediamine in an amount three times the amount of nickel (mol / mol). Shake at 25 °C for 15 minutes to obtain a precipitate.

[0180] <Process 2-1: Catalyst Precursor Composition Recovery Process>

[0181] The resulting precipitate and solution were separated by filtration. The resulting solid was dried under reduced pressure to obtain the catalyst precursor composition as a black powder.

[0182] <Process 2-2: Firing Process>

[0183] 0.1 g of the catalyst precursor composition was added to a tubular electric furnace (FT-02VAC-03, manufactured by FULLTEC Corporation), and calcined at a calcination temperature of 500°C for 15 minutes while nitrogen flowed at a rate of 100-200 mL / min, to obtain a nickel-carbon catalyst in the form of a black powder.

[0184] Example 6 (Preparation of cobalt-carbon catalyst)

[0185] <Process 1: Catalyst Precipitation Process>

[0186] In a methanol solution containing cobalt nitrate at a concentration of 10 g / L, m-phenylenediamine was added in an amount twice the amount (mol / mol) relative to cobalt. The solution was then shaken at 25 °C for 1 hour to obtain a precipitate.

[0187] <Process 2-1: Catalyst Precursor Recovery Process>

[0188] The resulting precipitate and solution were separated by filtration. The resulting solid was dried under reduced pressure to obtain the catalyst precursor as a pale red powder.

[0189] <Process 2-2: Firing Process>

[0190] 0.1 g of the catalyst precursor was added to a tubular electric furnace (FT-02VAC-03, manufactured by FULLTEC Corporation), and calcined at a calcination temperature of 500°C for 15 minutes while nitrogen flowed at a rate of 100-200 mL / min, to obtain a cobalt-carbon catalyst in the form of a black powder.

[0191] Example 7 (Preparation of Nickel-Cobalt-Carbon Catalyst)

[0192] <Process 1: Catalyst Precipitation Process>

[0193] To methanol solutions containing nickel nitrate and cobalt nitrate at concentrations of 5 g / L, m-phenylenediamine was added in an amount twice the total amount of nickel and cobalt (mol / mol). The mixture was then shaken at 25°C for 1 hour to obtain a precipitate.

[0194] <Process 2-1: Catalyst Precursor Recovery Process>

[0195] The resulting precipitate and solution were separated by filtration. The resulting solid was dried under reduced pressure to obtain a catalyst precursor as a gray powder.

[0196] Here, taking nickel in the filtrate after solid-liquid separation in step 2-1 as an example, the difference X (the amount of nickel in the catalyst precursor) between the amount of nickel quantified using a microwave plasma atomic emission spectrometry (Agilent 4210, manufactured by Agilent Technologies, Ltd.) and the amount of nickel contained in the methanol solution of step 1 is calculated. Similarly, taking cobalt in the filtrate after solid-liquid separation in step 2-1 as an example, the difference Y (the amount of cobalt in the catalyst precursor) between the amount of cobalt quantified using the same microwave plasma atomic emission spectrometry and the amount of cobalt contained in the methanol solution of step 1 is calculated. Based on the calculated differences X (the amount of nickel in the catalyst precursor) and Y (the amount of cobalt in the catalyst precursor), the molar ratio of nickel to cobalt in the catalyst precursor is 1:1.

[0197] <Process 2-2: Firing Process>

[0198] 0.1 g of the catalyst precursor was added to a tubular electric furnace (FT-02VAC-03, manufactured by FULLTEC Corporation), and calcined at a calcination temperature of 500°C for 30 minutes while nitrogen flowed at a rate of 100-200 mL / min, to obtain a nickel-cobalt-carbon catalyst as a black powder.

[0199] Example 8 (Preparation of cobalt-carbon catalyst)

[0200] The firing temperature in <Step 2-2: Firing Step> of Example 6 was changed from 500°C to 900°C. Otherwise, the cobalt-carbon catalyst was obtained in the same manner as in Example 6.

[0201] Example 9 (Preparation of Nickel-Cobalt-Carbon Catalyst)

[0202] The firing temperature in <Step 2-2: Firing Step> of Example 7 was changed from 500°C to 900°C. Otherwise, the nickel-cobalt-carbon catalyst was obtained in the same manner as in Example 7.

[0203] Comparative Example 1 (Preparation of Nickel Catalyst)

[0204] 0.1 g of nickel hydroxide (manufactured by Fujifilm and Kohden Chemical Co., Ltd.) was calcined under the same conditions as in <Step 2-2: calcination step> of Example 1 to obtain a nickel catalyst.

[0205] [Analysis of Catalysts]

[0206] (1) The amount of metal contained in the catalyst precursor

[0207] The amount of metal contained in the catalyst precursors obtained in Examples 1-9 was quantified by thermogravimetric analysis (TG).

[0208] The catalyst precursors obtained in Examples 1-9 were heated to 800°C at a rate of 10°C / min while air was flowing at a rate of 200 mL / min using a thermogravimetric analysis apparatus (STA7300, manufactured by Hitachi High-Tech Science Corporation). Since the residue after heating was a metal oxide, the amount of zero-valent metal was calculated from the amount of residue and compared with the amount of the original catalyst precursor to determine the amount of metal in the catalyst precursor.

[0209] The catalyst precursors of Examples 1, 3, and 4 contain 7.5% nickel by mass, while the catalyst precursor of Example 2 contains 10% nickel by mass. The catalyst precursor of Example 5 contains 6% nickel by mass, the catalyst precursors of Examples 6 and 8 contain 32% cobalt by mass, and the catalyst precursors of Examples 7 and 9 contain 20% nickel and cobalt by mass.

[0210] (2) The amount of metal contained in the metal-carbon catalyst

[0211] The amount of metal contained in the metal-carbon catalysts obtained in Examples 1 to 9 was also determined in the same manner as above, and the values ​​of the amount of metal contained in the catalysts of Examples 1 to 9 are shown in Tables 1 to 8.

[0212] (3) The molar ratio of metal (M) to amine (A) contained in the catalyst precursor (metal (M) / amine (A))

[0213] Elemental analysis (CE-440, EGZETER Analytical) was performed on the catalyst precursors obtained in Examples 1-9 to determine the proportions of carbon, nitrogen, and hydrogen. The molar ratio (metal (M) / amine (A)) was calculated from the results of the elemental analysis and the metal content in the catalyst precursors determined above.

[0214] The molar ratio (metal (M) / amine (A)) of Examples 1, 3, and 4 is 1 / 2, the molar ratio (metal (M) / amine (A)) of Example 2 is 1 / 2, the molar ratio (metal (M) / amine (A)) of Example 5 is 1 / 2, the molar ratio (metal (M) / amine (A)) of Examples 6 and 8 is 2 / 1, and the molar ratio (metal (M) / amine (A)) of Examples 7 and 9 is 1 / 1.

[0215] [Catalyst Evaluation 1]

[0216] Test Examples 1-2, 12-13 and Comparative Test Example 1 (Hydrogen Generation Test and Overvoltage Measurement (as an Evaluation of HER Catalyst))

[0217] 100 μL of a mixture of distilled water and 2-propanol (2:3) was added to 1 mg of the catalyst obtained in Examples 1-2, 6, 7 and Comparative Example 1, and the mixture was dispersed by ultrasound to obtain a dispersion. This dispersion was then measured to be 255 μg / cm³ in metal conversion. 2 The electrode was coated with 5 μL of 0.25% Nafion (registered trademark) solution, dried at 25°C, and then coated again to obtain the electrode for measurement.

[0218] Hydrogen generation tests and overvoltage measurements were performed using an electrochemical analyzer (ALS model 600E, manufactured by BAS Corporation).

[0219] The determination was performed using a three-electrode system with 1M KOH solution. An alkaline reference electrode (Hg / HgO / 1M NaOH) was used as the reference electrode, a Pt coil as the counter electrode, and a 5mm diameter glassy carbon rotating electrode (RDE) as the working electrode. Measurements were performed after bubbling with nitrogen to remove dissolved gases. The reversible hydrogen electrode (RHE) reference potential was obtained by adding 0.950V to the reference electrode reference potential.

[0220] The hydrogen generation test was conducted using a linear sweep voltammetry (LSV) method with the rotating electrode rotated at 1600 rpm. In the overvoltage determination, an iR guarantee (85%) was performed to remove the resistance of the solution.

[0221] In the hydrogen generation experiment, a decrease in current density along with a scan to lower potential is desirable. In particular, a significant decrease in current density near 0V (RHE reference) in the LSV curve indicates excellent hydrogen generation catalytic activity. The LSV curves of Examples 1, 2, and Comparative Example 1 are shown below. Figure 1 .

[0222] Current density reaches -10 mA / cm 2 The absolute value of the potential (RHE reference) at that time is the hydrogen overvoltage, and a lower overvoltage is considered better. In particular, overvoltages below 300mV are even better. The results are shown in Table 1.

[0223] Experimental Examples 3-5 (Hydrogenation of furfural (Evaluation as a hydrogenation catalyst))

[0224] The reaction of hydrogenating furfural to obtain furfuryl alcohol and tetrahydrofurfuryl alcohol was evaluated.

[0225] In a 20 mL portable reactor (TPR2 type, manufactured by Pressure Glass Industry Co., Ltd.), 2.5 mg of the catalyst from Examples 1, 3, or 4 (based on the mass of metal), 2 mL of 2-propanol, and 0.32 mmol of furfural were added. The reactor was pressurized to 4 MPa with hydrogen and heated at 140 °C for 2 hours to carry out the reaction. The reaction was then carried out using deuterated chloroform as a solvent. 1 The proportions of each product in the reaction were determined by H-NMR, and the reaction rate and selectivity were calculated. The results are shown in Table 2.

[0226] Test Example 6 and Comparative Test Example 2 (Hydrogenation of Furfural (Comparison with Raney Nickel))

[0227] Under the same conditions as in the example using Raney nickel as a catalyst for the hydrogenation of furfural (Molecular Catalysis, 2018, 445, 52-60), the hydrogenation of furfural was carried out using the catalyst of Example 4, and the conversion and selectivity were compared.

[0228] In a 20 mL portable reactor (TPR2 type, manufactured by Pressure Glass Industry Co., Ltd.), 12.6 mg of the catalyst from Example 4 or Comparative Example 2 (based on the mass of metal), 1.8 mL of 2-propanol, and 0.66 mmol of furfural were added. The reactor was pressurized to 3 MPa with hydrogen and heated at 180 °C for 1.25 hours to carry out the reaction. The reaction was then carried out using deuterated chloroform as a solvent. 1 The proportions of each product in the reaction were determined by H-NMR, and the reaction rate and selectivity were calculated. Raney nickel was used as a comparative example, Example 2. The results are shown in Table 3.

[0229] [Table 1]

[0230]

[0231] [Table 2]

[0232]

[0233] [Table 3]

[0234]

[0235] As shown in Table 1, the nickel-carbon catalysts of Examples 1 and 2 exhibited low hydrogen generation overvoltages during hydrogen generation experiments. Figure 1 As shown, LSV curves were obtained showing a decrease in current density as the potential decreased with increasing scanning. On the other hand, in the nickel catalyst of Comparative Example 1, which does not contain carbon, in the hydrogen generation test of Comparative Example 1, as... Figure 1 As shown, no decrease in current density was observed in the LSV curve. Furthermore, as shown in Table 1, low hydrogen generation overvoltage and decreased current density were also observed for the cobalt-carbon catalyst of Example 8 and the nickel-cobalt-carbon catalyst of Example 9. Therefore, it can be seen that the metal-carbon catalyst of the present invention is useful as a HER catalyst.

[0236] Furthermore, as shown in Table 2, the hydrogenation reaction of furfural using the nickel-carbon catalysts of Examples 1, 3, and 4 exhibited high reaction rates. Therefore, it can be seen that the nickel catalysts of Examples 1, 3, and 4 are also useful as hydrogenation catalysts. Furthermore, it can be seen that the nickel-carbon catalysts of Examples 1, 3, and 4 selectively hydrogenate furfural to obtain tetrahydrofurfuryl alcohol.

[0237] Furthermore, as shown in Table 3, the nickel-carbon catalyst of Example 4 exhibits higher selectivity for tetrahydrofurfuryl alcohol compared to the case using the Raney nickel catalyst (Comparative Example 2). This demonstrates that the metal-carbon catalyst of the present invention offers superior safety and hydrogenation catalytic activity compared to widely used Raney nickel catalysts.

[0238] Thus, the metal-carbon catalyst obtained from the catalyst precursor of the present invention via the manufacturing method of the present invention does not use precious metals, is inexpensive, and has high activity, making it particularly excellent as a catalyst for hydrogen generation reactions and hydrogenation reactions. Furthermore, the metal-carbon catalyst of the present invention does not use precious metals, is inexpensive, and has high activity, making it particularly excellent as a catalyst for hydrogen generation reactions and hydrogenation reactions.

[0239] [Catalyst Evaluation 2]

[0240] Experimental Examples 7-9 (Hydrogenation of furfural (Evaluation as a hydrogenation catalyst))

[0241] The reaction of hydrogenating furfural to obtain furfuryl alcohol and tetrahydrofurfuryl alcohol was evaluated.

[0242] In a 20 mL portable reactor (TPR2 type, manufactured by Pressure Glass Industry Co., Ltd.), 2.5 mg of the catalyst from Example 4 or 5 (based on the mass of metal), 2 mL of 2-propanol, and furfural were added. The reactor was pressurized to 4 MPa with hydrogen and heated at 140 °C for 2 hours to carry out the reaction. It should be noted that the reaction was carried out with two amounts of furfural: 0.32 mmol (nickel / furfural (mass) ratio = 0.08) and 0.16 mmol (nickel / furfural (mass) ratio = 0.04). The reaction was carried out using deuterated chloroform as a solvent. 1 The proportions of each product in the reaction were determined by H-NMR, and the reaction rate and selectivity were calculated. The results are shown in Table 4.

[0243] [Table 4]

[0244]

[0245] As shown in Table 4, the hydrogenation reaction of furfural using the nickel-carbon catalysts of Examples 4 and 5 exhibited high reaction rates. Therefore, it can be seen that the nickel-carbon catalysts of Examples 4 and 5 are also useful as hydrogenation catalysts. Furthermore, it can be seen that the nickel-carbon catalyst of Example 5, which used carbon black, selectively hydrogenated furfural to obtain tetrahydrofurfuryl alcohol despite the low amount of metal used.

[0246] Thus, the metal-carbon catalyst obtained from the catalyst precursor of the present invention via the manufacturing method of the present invention does not use precious metals, is inexpensive, and has high activity, making it particularly excellent as a catalyst for hydrogenation reactions. Furthermore, the metal-carbon catalyst of the present invention does not use precious metals, is inexpensive, and has high activity, making it particularly excellent as a catalyst for hydrogenation reactions.

[0247] [Catalyst Evaluation 3]

[0248] Experimental Example 10 (Hydrogenation of furfural (Evaluation as a hydrogenation catalyst))

[0249] The reaction of hydrogenating furfural to obtain furfuryl alcohol and tetrahydrofurfuryl alcohol was evaluated.

[0250] In a 20 mL portable reactor (TPR2 type, manufactured by Pressure Glass Industry Co., Ltd.), 2.5 mg of the catalyst from Example 6 (based on the mass of metal), 2 mL of 2-propanol, and 0.32 mmol of furfural were added. The reactor was pressurized to 4 MPa with hydrogen and heated at 140 °C for 2 hours to carry out the reaction. The reaction was then carried out using deuterated chloroform as a solvent. 1 The proportions of each product in the reaction were determined by H-NMR, and the reaction rate and selectivity were calculated. The results are shown in Table 5.

[0251] [Table 5]

[0252]

[0253] As shown in Table 5, the hydrogenation rate of furfural using the cobalt-carbon catalyst of Example 6 was high. Therefore, it can be seen that the cobalt-carbon catalyst of Example 6 is also useful as a hydrogenation catalyst. Furthermore, it can be seen that the cobalt-carbon catalyst of Example 6 selectively hydrogenates furfural to obtain tetrahydrofurfuryl alcohol.

[0254] Thus, the metal-carbon catalyst obtained from the catalyst precursor of the present invention via the manufacturing method of the present invention does not use precious metals, is inexpensive, and has high activity, making it particularly excellent as a catalyst for hydrogenation reactions. Furthermore, the metal-carbon catalyst of the present invention does not use precious metals, is inexpensive, and has high activity, making it particularly excellent as a catalyst for hydrogenation reactions.

[0255] [Catalyst Evaluation 4]

[0256] Experimental Example 11 (Hydrogenation of furfural (Evaluation as a hydrogenation catalyst))

[0257] The reaction of hydrogenating furfural to obtain furfuryl alcohol and tetrahydrofurfuryl alcohol was evaluated.

[0258] In a 20 mL portable reactor (TPR2 type, manufactured by Pressure Glass Industry Co., Ltd.), 2.5 mg of the catalyst from Example 7 (based on the mass of metal), 2 mL of 2-propanol, and 0.32 mmol of furfural were added. The reactor was pressurized to 4 MPa with hydrogen and heated at 140 °C for 2 hours to carry out the reaction. The reaction was then carried out using deuterated chloroform as a solvent. 1 The proportions of each product in the reaction were determined by H-NMR, and the reaction rate and selectivity were calculated. The results are shown in Table 6.

[0259]

[0260] As shown in Table 6, the hydrogenation rate of furfural using the nickel-cobalt-carbon catalyst of Example 7 was high. Therefore, it can be seen that the nickel-cobalt-carbon catalyst of Example 7 is also useful as a hydrogenation catalyst. Furthermore, it can be seen that the nickel-cobalt-carbon catalyst of Example 7 selectively hydrogenates furfural to obtain tetrahydrofurfuryl alcohol.

[0261] [Catalyst Evaluation 5]

[0262] Experimental Examples 14-19 (Hydrogenation of Furfural (Evaluation of Hydrogenation Catalysts Used in the Selective Hydrogenation of Unsaturated Aldehydes))

[0263] To compare the performance of hydrogenation catalysts used in the selective hydrogenation of unsaturated aldehydes using the nickel-carbon catalyst of Example 4, the cobalt-carbon catalyst of Example 6, and the nickel-cobalt-carbon catalyst of Example 7, the reaction of hydrogenating furfural to obtain furfuryl alcohol and tetrahydrofurfuryl alcohol at a lower temperature was evaluated.

[0264] In a 20 mL portable reactor (TPR2 type, manufactured by Pressure Glass Industry Co., Ltd.), 2.5 mg of the catalyst from Examples 4, 6, or 7 (based on the mass of metal), 2 mL of 2-propanol, and 0.32 mmol of furfural were added. The reactor was pressurized to 4 MPa with hydrogen and heated at 100°C or 120°C for 2 hours to carry out the reaction. The reaction was then carried out using deuterated chloroform as a solvent. 1 The proportions of each product obtained from the H-NMR analysis were used to determine the proportions of the compounds present after the reaction. The results are shown in Tables 7 and 8.

[0265]

[0266]

[0267] As shown in Tables 7 and 8, it can be seen that regardless of whether the reaction temperature is 100℃ or 120℃, the cobalt-carbon catalyst of Example 6 can selectively hydrogenate furfural to obtain furfuryl alcohol compared with the nickel-carbon catalyst of Example 4 and the nickel-cobalt-carbon catalyst of Example 7.

Claims

1. A method for producing a metal-carbon catalyst, comprising: Process 1, mixing a solution containing at least one metal M selected from the group consisting of nickel and cobalt and containing nitric acid or a nitrate salt, with an amine A having one or two at least one amino group selected from the group consisting of a benzylamino group and an aliphatic amino group, to precipitate a catalyst precursor containing the amine A and the metal M; and Process 2, separating the catalyst precursor from the solution and performing calcination.

2. The method for producing a metal-carbon catalyst according to claim 1, wherein, The amine A is a diamine.

3. The method for producing a metal-carbon catalyst according to claim 1, wherein, The amine A has a carbon number of 3 to 8.

4. The method for producing a metal-carbon catalyst according to claim 1, wherein, The amine A is at least one selected from the group consisting of benzylmethylamine, bis(amino methyl)cyclohexane, hexamethylene diamine, 2-ethylhexylamine, and propylamine.

5. The method for producing a metal-carbon catalyst according to any one of claims 1 to 4, wherein In Process 1, the molar ratio of the amine A to the metal M, that is, the number of amine molecules per number of metal atoms, is 0.5 to 500.

6. The method for producing a metal-carbon catalyst according to any one of claims 1 to 4, wherein In Process 2, the temperature of the calcination is 250 to 1000°C.

7. A catalyst precursor containing at least one metal M selected from the group consisting of nickel and cobalt, and an amine A having one or two at least one amino group selected from the group consisting of a benzylamino group and an aliphatic amino group.

8. The catalyst precursor according to claim 7, containing 3 to 40 mass% of the metal M.

9. A method for producing a catalyst precursor, which is the method for producing the catalyst precursor according to claim 7 or 8, comprising: Process 1, mixing a solution containing at least one metal M selected from the group consisting of nickel and cobalt and containing nitric acid or a nitrate salt, with an amine A having one or two at least one amino group selected from the group consisting of a benzylamino group and an aliphatic amino group, to precipitate a catalyst precursor containing the amine A and the metal M; and Process 3, solid-liquid separating the catalyst precursor.

10. A metal-carbon catalyst containing 0.5 to 80 mass% of at least one metal M selected from the group consisting of nickel and cobalt.

11. The metal-carbon catalyst according to claim 10, obtained by a production method comprising: Process 1, mixing a solution containing at least one metal M selected from the group consisting of nickel and cobalt and containing nitric acid or a nitrate salt, with an amine A having one or two at least one amino group selected from the group consisting of a benzylamino group and an aliphatic amino group, to precipitate a catalyst precursor containing the amine A and the metal M; and Process 2, solid-liquid separating the catalyst precursor and performing calcination.

Citation Information

Patent Citations

  • Hydrogen evolution reaction catalyst