Methods and related systems for treating metal or ceramic surfaces with continuous wave laser beams
By using a continuous wave laser beam of less than 100 µm to treat the surface of metal and ceramic materials, the problem of balancing strength and ductility in the prior art has been solved, and the overall performance of materials has been improved.
Patent Information
- Application Number
- CN202580017407.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-02-26
- Filing Date
- 2025-02-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to simultaneously improve strength, ductility, and fatigue limit when treating metal and ceramic surfaces, and conventional methods may lead to degradation of another physical property.
A continuous wave laser beam of less than 100 µm is used to scan the material surface. By combining appropriate processing power, scanning speed and atmospheric conditions, the material is ensured to reach the melting temperature on the surface and be processed.
It significantly improves the microstructure of the material, enhances its strength, ductility, and fatigue limit, while reducing surface roughness and improving the overall performance of the material.
Smart Images

Figure CN123125066A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of methods for treating the surface of metals or ceramics to improve their physical properties. More particularly, this invention relates to a treatment method using continuous wave lasers. Background Technology
[0002] Methods for treating metal, alloy, or ceramic surfaces are known in the prior art. For example, these treatments aim to improve strength or achieve higher ductility and fatigue limits than the "original" (i.e., untreated) material.
[0003] These materials are characterized by their microstructure, and the aim is to design such microstructures that exhibit greater strength, ductility, and fatigue limits than currently possible, while reducing energy and material consumption.
[0004] The advent of metal 3D printing, or additive manufacturing, has enabled the production of manufactured parts with microstructures possessing unprecedented strength compared to their conventionally manufactured counterparts. However, this increase in strength is often accompanied by reduced ductility and a worse fatigue response.
[0005] The strength-ductility tradeoff stems from the multi-layered microstructure resulting from the highly unbalanced processes occurring during additive manufacturing. Thermo-mass interactions, caused by molten pool kinetics, rapid solidification, and thermal cycling in the solid state, lead to a microstructure exhibiting physical and chemical inhomogeneities ranging from tens of nanometers to hundreds of micrometers. The major contributions to the material's strength come from the smaller of these features, which in stainless steel are precipitates, micro-segregated cells, and dislocation structures.
[0006] "Plain" or initial material (before processing) has a crystalline grain structure, with numerous smaller dislocation structures within each grain. Dislocations are linear crystal defects resulting from the lack of atomic planes. Microscopic segregated cells have cell walls that exhibit a higher concentration of one or more elements than the cell interior.
[0007] As a general rule, it is known that the smaller the size (and the higher the density) of these microscopic segregated cells / dislocation structures, the higher their strength and the lower their ductility.
[0008] Annealing is a common method used to improve ductility. It is an isothermal heat treatment process that causes metastable microstructures to move toward equilibrium by minimizing stored energy. However, this process inadvertently leads to an increase in cell / structure size and a decrease in density, which inevitably results in a reduction in strength.
[0009] Furthermore, the fatigue response of dense parts (with negligible porosity / void) depends largely on their surface roughness. During additive manufacturing, unmelted powder particles sinter at the surface and become the primary contributor to the surface roughness of the manufactured part. Under fatigue loading, failure is mainly due to the initiation (if not already present) and propagation of surface cracks.
[0010] The fatigue response of manufactured parts can be improved by post-manufacturing surface treatments, the most common of which are mechanical (pre-stressed shot peening, polishing, etc.), which reduce surface roughness and introduce compressive stress in the plane of the surface.
[0011] Laser-based treatments have also been used, utilizing industrially available lasers with large spot diameters ranging from approximately 500 µm to several millimeters. For example, the publication “Effects of quench-tempering and laser hardening treatment on wear resistance of gray cast iron” by B. Wang et al. (JMR&T 2020, 9(4)8163-8171) describes an implementation of laser treatment using a 2 mm spot to improve the wear resistance of gray cast iron.
[0012] Therefore, the effectiveness of these various post-manufacturing treatments may prove insufficient, or may improve one physical property only by degrading another.
[0013] The purpose of this invention is to overcome the above-mentioned shortcomings by proposing a method for treating the surface of a sample made of metal or ceramic material using a continuous wave laser, which allows for a significant and simultaneous improvement in several physical properties of the treated sample. Summary of the Invention
[0014] This invention relates to a method for treating the surface of a sample made of a metallic or ceramic material, the method comprising a treatment step of scanning the surface to be treated with a continuous-wave laser beam (referred to as a treatment laser beam), the treatment laser beam having a treatment power and a treatment spot on the surface, the treatment spot having a diameter (referred to as a treatment diameter), the treatment spot moving on the surface at a scanning speed (referred to as a treatment speed). - The processing diameter is less than or equal to 100 µm. The processing power, the processing diameter, and the processing scanning speed are determined such that point reception on the surface of the sample is determined such that the material at that point in the sample reaches the processing surface energy density at that point. - The processing method is carried out under an inert atmosphere or vacuum.
[0015] According to one embodiment, the scanning is configured such that there is at least 50% overlap between two processing spots associated with two adjacent scanning paths.
[0016] According to one embodiment, the method according to the invention includes the step of characterizing a sample using a scanning microscope, which is performed after a processing step, wherein the characterization is carried out without removing the sample from an inert atmosphere or a vacuum.
[0017] According to another aspect, the present invention relates to a method for manufacturing said sample made of a metallic or ceramic material and for treating the surface of said sample, said method comprising: - The steps for manufacturing the sample using additive manufacturing technology. - Processing steps of a processing method according to one aspect of the present invention.
[0018] According to one embodiment, the manufacturing and processing method according to the present invention further includes a characterization step.
[0019] According to one embodiment of the manufacturing and processing method of the present invention, it includes an additive manufacturing step performed using a manufacturing beam, said manufacturing beam being a laser beam.
[0020] According to one embodiment of the manufacturing and processing method of the present invention, the additive manufacturing step is performed by a laser powder bed melting method.
[0021] In another embodiment of the manufacturing and processing method according to the present invention, the additive manufacturing step is performed by a laser-directed energy deposition method.
[0022] According to one embodiment of the manufacturing and processing method of the present invention, the manufacturing laser beam has a manufacturing spot with a manufacturing diameter greater than or equal to the processing diameter.
[0023] According to one embodiment of the manufacturing and processing method of the present invention, the manufacturing laser beam and the processing laser beam are generated by the same continuous wave laser source.
[0024] According to another aspect, the present invention relates to a processing system configured to process the surface of a sample made of a metallic or ceramic material, the system comprising: - A laser source configured to generate a continuous-wave laser beam, called a processing laser beam, which has processing power. - A focusing device configured to focus the processing laser beam onto the surface of the sample according to a spot called the processing spot, the processing spot exhibiting a processing diameter of less than or equal to 100 µm. - A scanning device configured to move the processing spot on the surface of the sample at a processing scanning speed. - A sealing section, configured to provide an inert atmosphere or vacuum around the sample, and including a window. The processing power, the processing diameter, and the processing scanning speed are determined such that the point acceptance on the surface of the sample is determined such that the material of the sample at that point reaches the melting temperature of the processed surface energy density.
[0025] According to one embodiment of the processing system of the present invention, the laser source, the scanning device and the focusing device are placed in a housing, and the system further includes a coupling component configured to interface between the housing and the enclosure.
[0026] According to one embodiment of the processing system of the present invention, it further includes: - A device configured to generate an electron beam and focus the electron beam onto the sample. - At least one detector configured to detect electrons from the sample. - The apparatus for generating the electron beam and the detector are arranged together with the enclosure to form a scanning electron microscope.
[0027] According to the last aspect, the present invention relates to an additive manufacturing and surface treatment system configured to manufacture a sample made of a metallic or ceramic material and treat the surface of said sample, said system comprising: - A laser source configured to generate a continuous-wave laser beam with adjustable power to produce power known as manufacturing power or processing power over a given area. - A device for properly positioning metal powder relative to the laser beam. - A focusing device configured to focus the laser beam onto the powder with a manufacturing spot having a manufacturing diameter, and once manufactured, to focus the laser beam onto the sample surface with a processing spot exhibiting a processing diameter of less than or equal to 100 µm. - A scanning device configured to move the manufacturing spot over the powder at a manufacturing scanning speed to manufacture the sample, and once the sample is made, to move the processing spot over the surface of the sample at a processing scanning speed. - A sealing section, configured to provide an inert atmosphere or vacuum around the sample, and including a window. - The laser source, the scanning device, and the focusing device are configured such that: During manufacturing, the manufacturing power, manufacturing diameter, and manufacturing scanning speed are determined to cause the powder to solidify in order to manufacture the sample via additive manufacturing. During processing, the processing power, the processing diameter, and the processing scan speed are determined such that point reception on the sample surface is determined to be the processing surface energy density that allows the material at that point in the sample to reach its melting temperature.
[0028] According to one embodiment of the additive manufacturing and surface treatment system of the present invention, the system further includes: - A device configured to generate an electron beam and focus the electron beam onto the sample. - At least one detector configured to detect electrons from the sample. The apparatus for generating an electron beam and the detector are arranged together with the enclosure to form a scanning electron microscope.
[0029] According to one embodiment of the system for additive manufacturing of a sample and processing the surface of the sample, the manufacturing diameter is greater than or equal to the processing diameter.
[0030] The following description provides several exemplary embodiments of the apparatus of the present invention; these examples do not limit the scope of the invention. These exemplary embodiments include not only the features necessary for the invention, but also additional features related to the described embodiments. Attached Figure Description
[0031] The invention will be better understood from the following detailed description with reference to the accompanying drawings, in which: Figure 1 A transmission electron microscope image of the surface of the wall region of a sample before treatment according to the present invention is shown.
[0032] Figure 2 Transmission electron microscopy images of the same region of a sample after applying the method according to the invention are shown.
[0033] Figure 3 An energy-dispersive X-ray spectral image of a region of the sample before treatment according to the present invention is shown.
[0034] Figure 4 Energy dispersive X-ray spectra of the same region of a sample after applying the method according to the invention are shown.
[0035] Figure 5 The results show three different energies: A: 0.4 J / mm 2 B: 1.6 J / mm 2 C: 8 J / mm 2 A cross-sectional profile image of the trajectory of the laser beam along the wall of the sample.
[0036] Figure 6 A side view of the sample before applying the method according to the invention is shown.
[0037] Figure 7 As shown Figure 6 Side profile of the same sample after applying the method according to the present invention.
[0038] Figure 8 A system according to the invention is shown for implementing the method according to the invention.
[0039] Figure 8bis An embodiment of a system including a connecting component according to the present invention is shown.
[0040] Figure 9 An embodiment of a system incorporating a scanning electron microscope according to the present invention is shown.
[0041] Figure 10 An embodiment of a method for manufacturing a sample and treating the sample surface according to another aspect of the present invention is shown.
[0042] Figure 11 An additive manufacturing and surface treatment system according to another aspect of the invention is shown, which is configured to manufacture a sample and treat the surface of the sample. Detailed Implementation
[0043] The embodiments described below refer to stainless steel in a non-limiting manner, but the considerations and results obtained can be extrapolated to any type of sample made of metal (including alloys) or ceramic. Therefore, the method according to the invention is applicable to all such types of samples.
[0044] The implementation of method 100 according to the invention is the result of extensive observation and experimentation. The inventors have noted that prior art continuous laser-based surface treatments typically use spot sizes larger than 500 µm on the sample surface, while smaller diameter spots are only used for additive manufacturing of the samples. The inventors have demonstrated that using small diameter spots less than 100 µm, combined with appropriate scanning parameters, it is possible to deeply alter the dislocation structure and microscopic segregation cells of the material, leading to improvements in certain properties of the irradiated (treated) material.
[0045] Therefore, the method 100 according to the present invention for treating the surface S of a sample SAM made of a metallic or ceramic material (denoted as MM) includes a treatment step ETAt, which involves scanning the surface S to be treated with a continuous-wave laser beam (referred to as the treatment laser beam LBT). The treatment laser beam has a power Pt and a spot ST (referred to as the treatment spot) on the surface S, the treatment spot ST having a diameter referred to as the treatment diameter DST. The spot ST moves on the surface at a scanning speed referred to as the treatment velocity vt.
[0046] Metallic materials are understood to refer to pure metallic materials (single compounds) or alloys.
[0047] The diameter of the DST is less than or equal to 100 µm. However, using the required small diameter is insufficient to properly modify the dislocation structure, and the inventors have established additional conditions to be verified to achieve material performance improvements. The power Pt, the diameter DST of the processing spot ST, and the processing scan speed vt should be determined such that the point reception on the sample surface is determined such that the processed surface energy Est density at that point in the sample, under the illumination of the moving laser beam, reaches the melting temperature of the material MM.
[0048] The relationship between the different variables of the laser beam is as follows: Est = Pt / (vt·DST) (1) In other words, the energy Est should be greater than or equal to the minimum surface energy Estmin density at which a point on the surface reaches its melting temperature.
[0049] The condition Est ≥ Estmin ensures surface melting of the material. Furthermore, the inventors have demonstrated that the small diameter of the processing spot ST (less than 100 µm) associated with material melting ensures a very high thermal gradient, which induces a high cooling rate after the material MM in the sample melts. Specifically, when the processing spot is wider, the time required to release the energy supplied by the laser is longer and the cooling rate is reduced.
[0050] Furthermore, it has been confirmed that the higher the cooling rate, the smaller the dislocation structure formed by recombination. By applying the treatment according to the invention, a smaller and denser structure than the initial size can be obtained. In addition, during the solidification period after melting, the dendrites formed in the material have smaller microsegregated cells than the initial size.
[0051] Another advantage of the method of the present invention has been found: the roughness of the treated surface is reduced, which improves the fatigue response of the material. This is especially true for metal samples produced by additive manufacturing based on metal powders. These samples exhibit residual powder sintered at the surface after their manufacture, resulting in increased roughness. Due to melting that occurs at the surface of the sample, the method according to the invention allows for the melting and subsequent solidification of these residual powders (see below).
[0052] To avoid the infiltration of unwanted atoms or molecules present in the sample's environment during melting, the method according to the invention is carried out under an inert atmosphere or vacuum. In an inert atmosphere, the pressure should not be too high to ensure that inert gas molecules do not infiltrate the molten material. Specifically, certain atoms or molecules injected into the sample may alter its properties, causing degradation. The method according to the invention is a general surface treatment method that does not change the chemical composition of the sample material, but rather alters its microstructure near the surface being treated. To carry out the method under a vacuum or inert atmosphere, the sample is placed in a sealed enclosure.
[0053] In order to make the processing according to the present invention effective, it is sought to achieve melting at a depth of at least a few micrometers in the sample.
[0054] These physical considerations apply to samples produced by additive manufacturing, as well as to any other type of sample made of metal (pure metal or alloy) or ceramic manufactured by other methods.
[0055] To illustrate the physical reasoning and results obtained using the method according to the invention, consider an E316L sample with thin walls made of 316L stainless steel, manufactured by an additive manufacturing method. These walls are arranged on a substrate also made of hot-rolled 316L stainless steel.
[0056] The wall was fabricated using laser-directed energy deposition (LDED). The laser used for fabricating the sample wall via LDED was a 250 W laser with a scanning speed of 33 mm / s and a spot size of 0.7 mm on the powder surface. These parameters resulted in a fabricated surface energy density (Esf) of 10.7 J / mm² received by the sample. 2 (Formula (1)).
[0057] Figure 1 An image of the surface of a region of the wall of an E316L sample before treatment according to the present invention, obtained by transmission electron microscopy (TEM), is shown, with the contrast magnified to clearly show the bright and dark areas. The dark areas correspond to dislocation structures. Figure 2 A TEM image of the same region of the surface after applying the method according to the invention is shown. It can be seen that the dark areas are denser and smaller in size on the processed sample.
[0058] Figure 3 The following are energy-dispersive X-ray spectra of a region of the E316L sample before processing. Figure 4Images of the same type on the surface after applying the method according to the invention are shown. Contrast has been magnified to make the bright and dark areas more clearly visible. Energy-dispersive X-ray spectroscopy identifies specific types of atoms, in this case chromium, in clustered areas. The bright areas show the aforementioned microscopic segregation cells. It can be seen that these cells are more compact and smaller in size after treatment. The same effect was obtained for iron, nickel, molybdenum, manganese, silicon, etc., which are also present in the sample.
[0059] In respectively Figure 1 and Figure 2 Bright areas 11 and 22 are visible in the image, and respectively in... Figure 3 and Figure 4 Dark areas 33 and 44, visible in the image, correspond to microscopic segregation cells observed from above. These cells form when the molten, liquefied metal returns to a solid state. The cells are respectively located in... Figure 1 and Figure 2 Dark dislocation structures 12 and 23 were separated, and intercellular chemical segregation was also observed, respectively in Figure 3 and Figure 4 For chromium, the bright areas are 34 and 45.
[0060] As the cooling rate increases, the size of the microsegregated cells decreases; therefore, by the method according to the invention, a very significant reduction in the dislocation structure and the size of the microsegregated cells in the treated sample is obtained. Dislocations and microsegregation occur at the interface between two grown microsegregated cells during curing.
[0061] As mentioned above, smaller (tens of nanometers) and denser feature-enhancing materials are recognized.
[0062] The energy Estmin that melts the surface of the material to be treated cannot be precisely calculated. The known formula is: Q = m·ΔHf Where Q is the energy required to achieve melting, m is the mass of the sample, and ΔHf is the latent heat of melting. Transforming this volumetric formula into the surface energy Estmin required for a sample of a given shape (surface area and thickness) is not a simple analytical process.
[0063] With a sufficiently small spot size, i.e., less than or equal to 100 µm, the power Pt and velocity vt must be determined to obtain material melting at least on the surface. This can be determined experimentally, for example, as described below.
[0064] Different laser treatments were performed on the E316L sample using constant power Pt, a beam diameter of 60 µm on the surface, and a variable scanning speed: Pt = 24 W, vt = 50 (8), 100 (4), 250 (1.6), 500 (0.8), and 1000 (0.4) mm / s. The values in parentheses are the corresponding surface energy Est densities in J / mm². 2 count. Figure 5 The following is shown for three energies: A: 0.4 J / mm 2 B: 1.6 J / mm 2 C: 8 J / mm 2 Cross-sectional profile images of the trajectory of the laser beam along the sample wall obtained by scanning at three corresponding speeds vt (with the z-axis in depth relative to the sample surface S, and the scanning speed vt perpendicular to the plane of the image).
[0065] The image was obtained using backscattered electron (BSE) imaging. Figure 5 It is easy to see from A that the energy is insufficient to cause melting because the sample was not affected by the laser scan. Figure 5 As can be seen in B, the laser has penetrated the sample in region 50 to a maximum depth pmax of approximately 10 µm, causing local melting and resulting in changes to the sample's microstructure. Region 51 was unaffected by the laser beam. Regions 50 and 51 are separated by interface 52, which shows the boundary between the region (50) that has reached the melting temperature and the region (51) that has not melted.
[0066] In the molten region 50, the basic feature size is smaller. In C, the laser penetration is deeper (pmax approximately 25 µm deep), and the volume of the molten region 50 is larger. This experiment clearly demonstrates that, for this stainless steel sample, 0.4 J / mm... 2 The energy Es is insufficient, while 1.6 J / mm 2 The energy Es is higher than the energy Estmin that allows the surface region of the sample to exceed the melting temperature. Therefore, 1.6 and 8 J / mm 2 The energy Es is compatible with the method according to the invention.
[0067] Therefore, in order to identify the laser parameters suitable for implementing the method according to the invention to achieve surface melting, preliminary experimental measurements should be performed on a sample of the same material and shape as the sample to be treated, or even on the sample itself, while changing at least one of the parameters (Pt, vt, DST). If Pt and / or vt can also be changed, then a change in diameter is not necessary, as long as it is less than 100 µm. Since the laser power is usually adjustable, changes in Pt can be easily obtained. Changes in vt are also easily achieved, as the scanning device usually has a speed setting. Experimental identification of the presence (or absence) of melting on the sample surface can be performed, for example, by BSE imaging, such as... Figure 5As shown. Therefore, the result consisting of the presence (or absence) of melting on the surface of the sample can be verified by the above experiments.
[0068] Once a set of values (DST0, Pt0, vt0) that can achieve the desired effect (surface melting) is identified, the treatment is carried out by scanning the light spot on the surface of the sample to be treated.
[0069] According to one embodiment, and in order to achieve uniform processing across the entire surface being processed, the scanning is configured such that there is at least 50% overlap between two processing spots associated with two adjacent scanning paths. This ensures that the sample up to p... max The entire volume has been melted, resulting in a processed layer of uniform thickness. For example, in the case of a spot with a diameter of 60 µm, the parallel scan trajectories are preferably spaced at a maximum of 30 µm apart.
[0070] The E316L sample was characterized to measure the performance gain resulting from the treatment according to the invention. The treatment according to the invention was performed under the following conditions: PT = 70 W, DST = 60 µm, vt = 100 mm / s, i.e., the energy density of the treated surface: Est = 11.7 J / mm 2 .
[0071] The process was performed under vacuum. Scans were performed with 50% overlap.
[0072] Tensile tests showed that the average yield strength in the untreated area was 360 MPa and in the treated area it was 1157 MPa.
[0073] The ductility was not affected by the laser passage. An increase of approximately 9% in ductility was even measured in the treated sample. Both the initial and treated samples met the consideration criteria, meaning that all microstructures reached their full deformability before failure.
[0074] Fatigue strength (constant amplitude uniaxial fatigue) before and after treatment (as before, with Est = 11.7 J / mm) 2 The same conditions were applied to approximately thirty samples, and measurements (Δσ) were performed under the same conditions.
[0075] For the failure cycle number N = 3.10 6 The measured Δσ was 182 MPa before treatment and 227 MPa after treatment, meaning the fatigue limit Δσ increased by approximately 25%. Regarding surface roughness, the roughness (arithmetic mean height Sa) measured before treatment was 16.6 µm, while after treatment under the above conditions, the roughness was 0.9 µm. The surface roughness after treatment is significantly better. This is due to... Figure 6 and Figure 7 The images shown depict side-view profiles of the samples before and after the aforementioned treatment. Contrast enhancement has been applied to improve visibility. These images are secondary electron (SE) microscope images. Figure 6 In the middle, the upper white area 60 represents powder residue that appeared during additive manufacturing. Figure 7 As can be seen, the residual powder is compacted (region 70) because it has melted. Furthermore, the surface of the sample is... Figure 6 The surface of the medium sample appears smoother and better compared to the medium sample. Figure 7 Region 71, corresponding to the area of the surface treated by the laser, is shown.
[0076] Therefore, several physical properties of material MM are improved by this treatment. Yield strength, roughness, and fatigue strength can be listed in an inexhaustible manner.
[0077] According to one embodiment, the processing method according to the invention includes a step ETAc of characterizing the sample using a scanning electron microscope (SEM) at least after the processing step. The characterization is performed without removing the sample from an inert atmosphere or vacuum, i.e., by holding the sample in a closed environment in which the processing is carried out. The method according to the invention thus makes it possible to process and characterize material samples according to the invention in the same instrument including a laser and an SEM. According to a variation, the characterization of the sample is also performed before processing so that the samples before and after processing can be compared. Such an instrument is described in patent application FR 2213567, which has not yet been published.
[0078] According to another aspect, the present invention relates to a system 80 for implementing the method according to the invention, such as... Figure 8 As shown. System 80 includes a laser source LS configured to generate a processing laser beam LBT having a processing power Pt on the surface of sample SAM. It also includes a scanning device DS configured to move the processing laser beam across the sample surface S at a processing scanning speed vt. Finally, it includes a focusing device DFOC configured to focus (or defocus) the laser beam onto the sample surface S such that the diameter of the spot (referred to as the processing diameter DST) is less than 100 µm.
[0079] System 80 also includes a closure E in which the sample is placed, configured to maintain an inert atmosphere or vacuum around the sample. The closure includes a window H to allow the laser beam to enter the closure. The sample to be processed, SAM, is placed on a support, Sup.
[0080] Furthermore, the laser source LS, the scanning device DS, and the focusing device DFOC are configured such that the parameters (Pt, vt, DST) satisfy the above conditions, i.e., generate sufficient surface energy density so that the material MM of the sample reaches the melting temperature at the point on the surface irradiated by the moving laser beam.
[0081] according to Figure 8bis In one embodiment shown, the laser source, the scanning device, and the focusing device are housed within a housing BT, and the system further includes a coupling component PA configured to interface between the housing and the enclosure. Therefore, the laser beam and the various optical elements constituting the focusing device are enclosed and protected.
[0082] Figure 9 An embodiment of a system 80 according to the invention is shown, which also allows for sample characterization after processing and optionally before processing. System 80 includes a device COL configured to generate an electron beam FE and focus the electron beam onto the sample, and at least one detector Det configured to detect electrons from the sample. The device COL and detector Det are arranged together with a closure E to form a scanning electron microscope (SEM).
[0083] As described above, the method according to the invention is applicable to any type of sample made of metal (pure metal or alloy) or ceramic.
[0084] The method according to the invention is particularly suitable for (metal or ceramic) materials produced from (metal or ceramic) powders by additive manufacturing (or 3D printing).
[0085] Metal additive manufacturing involves creating parts by sequentially adding (metal) materials based on 3D digital files. The material is molded by solidifying metal powder. The metal materials constituting the powder can be selected from, for example, stainless steel, titanium-based alloys, aluminum-based alloys, nickel-based alloys, etc.
[0086] The first method, known as powder bed metal additive manufacturing (MAM-PB), is implemented from a powder bed. A powder bed (PB) should be understood as powder with a controlled thickness (MP) having a flat surface. Manufacturing is performed by layer-by-layer spreading of thin powder layers (typically between 10 and 100 µm thick), with a selective consolidation step of the material occurring between each layer deposition. Selective consolidation is performed, for example, by one or more laser beams, electron beams, laser sintering, or binder jetting. Consolidation should be understood as hardening the material by binding powder particles together.
[0087] The second method, known as LDED (mentioned above), involves generating a powder jet directly melted by a laser to fabricate a sample. The LDED method typically uses a spot diameter between 200 µm and 1 mm.
[0088] According to another aspect, the present invention relates to a method 200 for manufacturing a metal sample SAM and treating the surface of the sample, the method comprising the step ETAf of manufacturing the sample using an additive manufacturing technique that solidifies metal powder. The method further includes the processing step ETAt of implementing the above-described method 100 of the present invention.
[0089] According to one embodiment, the additive manufacturing step ETAf of method 200 is performed using a manufacturing beam LBM of a laser beam, such as... Figure 10 As shown.
[0090] Method 200 is compatible with embodiments of method 100 that incorporate the steps of characterizing the manufactured and processed sample using a scanning electron microscope as described above. Optionally, the sample is also characterized prior to processing.
[0091] According to one embodiment, the manufacturing and processing steps are performed using a manufacturing laser beam (LBM) and a processing laser beam (LBT) generated by the same continuous-wave laser source, respectively. This is possible because the continuous power required for each step is on the same order of magnitude, and the spot size and / or scanning speed can be adjusted for each step using deflection devices and, where appropriate, beam focusing devices.
[0092] Therefore, method 200 enables the use of the same laser to perform manufacturing and processing without moving the sample. It also allows for reduced surface treatment costs because it uses the same laser.
[0093] According to one embodiment, the additive manufacturing step is performed using a laser powder bed melting (LPBF) method. According to another embodiment, the additive manufacturing step is performed using a laser-directed energy deposition (LDED) method.
[0094] The manufacturing laser beam LBM has a manufacturing power Pf and a manufacturing spot SF defined when the laser encounters the powder to solidify it. The spot SF has a manufacturing diameter DSF. The spot moves across the powder at a manufacturing scanning speed vf. The manufacturing surface energy density Esf is achieved at points on the powder surface during solidification.
[0095] According to one embodiment, in order to obtain a more effective surface treatment of the sample, the diameter DSF is manufactured to be greater than or equal to the treatment diameter DST.
[0096] DSF ≥ DST (2) Based on extensive experiments, the preferred method has been determined as follows: DSF ≥ 2·DST or DST ≤ 0.5×DSF (2bis) Specifically, when the processing diameter DST is substantially equal to the manufacturing diameter DSF, the defects in the material caused by the microstructure size remain substantially the same size, and the microstructure does not change significantly during the processing.
[0097] When the processing diameter is significantly smaller than the manufacturing diameter, the volume heated during processing is smaller than the volume used during manufacturing, and therefore cooling is faster. These faster cooling kinetics during processing (compared to manufacturing) induce a finer microstructure in the processed material compared to the microstructure at the end of manufacturing, leading to improved material mechanical properties. Therefore, such a diameter condition of 2bis allows for microstructure refinement through processing, resulting in improved material mechanical properties.
[0098] According to another aspect, the present invention relates to an additive manufacturing and surface treatment system 10, configured to manufacture a sample SAM made of a metallic or ceramic material MM, and to treat the surface S of the sample SAM, such as... Figure 11 As shown schematically.
[0099] The system includes a laser source LS configured to generate a continuous-wave laser beam with adjustable power to produce a so-called manufacturing power Pf or a so-called processing power Pt on a defined surface. It also includes a device PPD for properly positioning metal powder relative to the laser beam. This could be, for example, a nozzle and associated elements for implementing the LDED method, or a set of tanks with the device for implementing the LPBF method.
[0100] System 10 also includes: - The focusing device DFOC is configured to focus a laser beam onto the powder according to a manufacturing spot SF having a manufacturing diameter DSF, and once the sample has been made, to focus a laser beam onto the surface S of the sample according to a processing spot DST having a processing diameter less than or equal to 100 µm.
[0101] - A scanning device DS, which is configured to move the manufacturing spot SF on the powder at a manufacturing scanning speed vf to manufacture the sample, and once the sample is made, to move the processing spot ST on the surface S of the sample at a processing scanning speed vt.
[0102] Finally, system 10 includes a closure E, which is configured to ensure an inert atmosphere or vacuum around the sample during processing. According to one embodiment, the sample is moved into the closure after manufacturing, while manufacturing takes place outside the closure. Figure 11 In another embodiment shown, manufacturing also takes place in the closed section E.
[0103] The laser source LS, the scanning device DS, and the focusing device DFOC are further configured such that: During manufacturing, manufacturing power Pf, manufacturing diameter DSF, and manufacturing scan speed vf were determined to cause powder consolidation in order to manufacture samples via additive manufacturing. During processing, the processing power Pt, processing diameter DST, and processing scan speed vt are determined such that point reception on the sample surface is determined such that the processing surface energy Est density at that point in the sample reaches the melting temperature of the material MM.
[0104] System 10 thus allows for the fabrication and post-fabrication of samples using the same laser source, ensuring reduced speed and processing costs.
[0105] According to one embodiment not shown, system 10 includes the device COL and detector Det as described above.
Claims
1. A method (100) for treating the surface (S) of a sample (SAM) made of a metallic or ceramic material (MM), the method comprising a treatment step (ETAt) of scanning the surface (S) to be treated with a continuous-wave laser beam called a treatment laser beam (LBT), the treatment laser beam having a treatment power (Pt) and a treatment spot (ST) on the surface, the treatment spot having a diameter (DST) called a treatment diameter, the treatment spot moving on the surface at a scanning speed (vt) called a treatment speed. - The processing diameter (DST) is less than or equal to 100 µm. - The processing power (Pt), the processing diameter (DST), and the processing scan speed (vt) are determined such that the point acceptance on the sample surface is determined such that the material (MM) in the sample at that point reaches the melting temperature of the processed surface energy (Est) density. - The processing method is carried out under an inert atmosphere or vacuum.
2. The processing method according to the preceding claim, wherein, The scanning is configured such that there is at least 50% overlap between two processing spots associated with two adjacent scanning paths.
3. The processing method according to any one of the preceding claims, the method comprising a step of characterizing the sample with a scanning microscope (ETAc), the step being performed after the processing step, the characterization being performed without removing the sample from an inert atmosphere or vacuum.
4. A method (200) for manufacturing a sample made of a metallic or ceramic material and for treating the surface of said sample, said method comprising: - The step of manufacturing the sample using additive manufacturing technology (ETAf). - The processing steps (ETAt) according to claim 1 or 2.
5. The manufacturing and processing method (200) according to the preceding claim further includes the characterization step according to claim 3.
6. The manufacturing and processing method according to any one of claims 4 or 5, wherein, The additive manufacturing step is performed using a manufacturing beam (LBM) of a laser beam.
7. The manufacturing and processing method according to the preceding claim, wherein, The additive manufacturing step is performed using the laser powder bed melting (LPBF) method.
8. The manufacturing and processing method according to claim 6, wherein, The additive manufacturing step is performed using the laser-directed energy deposition (LDED) method.
9. The manufacturing and processing method according to any one of claims 6 to 8, wherein, The manufacturing laser beam (LBM) has a manufacturing spot (SF) with a manufacturing diameter (DSF), which is greater than or equal to the processing diameter (DST).
10. The method according to any one of claims 6 to 9, wherein, The manufacturing laser beam (LBM) and the processing laser beam (LBT) are generated by the same continuous wave laser source.
11. A processing system (80) configured to process the surface (S) of a sample (SAM) made of a metallic or ceramic material (MM), said system comprising: - A laser source (LS) configured to generate a continuous-wave laser beam called a processing laser beam (LBT) with processing power (Pt). - A focusing device (DFOC) is configured to focus the processing laser beam onto the surface of the sample according to a so-called processing spot (ST), the processing spot exhibiting a processing diameter (DST) of less than or equal to 100 µm. - A scanning device (DS) configured to move the processing spot on the surface (S) of the sample at a processing scanning speed (vt). - A sealing section (E), which is configured to provide an inert atmosphere or vacuum around the sample and includes a window (H). - The processing power (Pt), the processing diameter (DST), and the processing scan speed (vt) are determined such that point reception on the sample surface is determined such that the material (MM) of the sample at that point reaches the melting temperature of the processed surface energy (Est) density.
12. The processing system (80) according to the preceding claim, wherein, The laser source, the scanning device, and the focusing device are housed in a housing (BT). The system also includes a coupling component (PA) configured to interface between the housing and the enclosure.
13. The processing system (80) according to the preceding claim further includes: - A device (COL) configured to generate an electron beam (FE) and focus the electron beam onto the sample. - At least one detector (Det) configured to detect electrons from the sample. - The device for generating the electron beam and the detector are arranged together with the enclosure to form a scanning electron microscope (SEM).
14. An additive manufacturing and surface treatment system (10) configured to manufacture samples (SAMs) made of metallic or ceramic materials (MMs) and treat the surfaces of said samples, said system comprising: - A laser source (LS) is configured to generate a continuous-wave laser beam with tunable power to produce so-called manufacturing power (Pf) or so-called processing power (Pt) over a given area. - A device (PPD) for properly positioning metal powder relative to the laser beam. - A focusing device (DFOC) configured to focus the laser beam onto the powder with a manufacturing spot (SF) having a manufacturing diameter (DSF), and once manufacturing is complete, to focus the laser beam onto the surface of the sample with a processing spot (ST) exhibiting a processing diameter (DST) less than or equal to 100 µm. - A scanning device (DS) configured to move the manufacturing spot over the powder at a manufacturing scanning speed (vf) to manufacture the sample, and once the sample is manufactured, to move the processing spot over the surface (S) of the sample at a processing scanning speed (vt). - A sealing section (E), which is configured to provide an inert atmosphere or vacuum around the sample and includes a window (H). - The laser source (LS), the scanning device (DS), and the focusing device (DFOC) are configured such that: During manufacturing, the manufacturing power (Pf), the manufacturing diameter (DSF), and the manufacturing scan speed (vf) are determined to cause the powder to solidify in order to manufacture the sample by additive manufacturing. - During processing, the processing power (Pt), the processing diameter (DST), and the processing scan rate (vt) are determined such that the point acceptance on the surface of the sample is determined such that the material (MM) at the point in the sample reaches the melting temperature of the processed surface energy (Est) density.
15. The additive manufacturing and surface treatment system (10) according to the preceding claim further includes: - A device (COL) configured to generate an electron beam (FE) and focus the electron beam onto the sample. - At least one detector (Det) configured to detect electrons from the sample. - The device for generating the electron beam and the detector are arranged together with the enclosure to form a scanning electron microscope (SEM).
16. The system for additively manufacturing a sample and treating the surface of said sample according to any one of claims 14 or 15, wherein, The manufacturing diameter (DSF) is greater than or equal to the processing diameter (DST).
Citation Information
Patent Citations
FR2213567A1