Abrasive pad fixing adhesive sheet, abrasive pad with adhesive layer A, and a method for fixing the abrasive pad to the platen.

By introducing the regular concave-convex structure of the release tab FA and the acrylic adhesive layer into the adhesive sheet for fixing the grinding pad, the problems of air ingress and insufficient adhesion during grinding pad fixing are solved, achieving high-precision, stable grinding performance and rapid position adjustment.

CN123125294APending Publication Date: 2026-11-17아티엔스가부시키가이샤 +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202680000658.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-04-16
Filing Date
2026-02-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the prior art, when the grinding pad is fixed to the table, air enters between the table and the adhesive layer, which leads to a decrease in grinding accuracy. At the same time, insufficient adhesion makes it difficult to adjust the position, and the adhesion performance is unstable during repeated use.

Method used

An adhesive sheet is used to fix the abrasive pad with a release tab FA. The outer surface of the release tab FA has a regular uneven structure with an average height Rc of 5 μm to 25 μm and a Beck smoothness of 0.1 seconds to 500 seconds. The uneven structure of the release tab FA serves as an air flow path to improve air exhaust. An acrylic adhesive layer is used to ensure strong adhesion and chemical resistance.

Benefits of technology

It achieves improved grinding accuracy in high-precision CMP machining, with excellent air expulsion, good adhesion and chemical resistance, easy position adjustment, and the adhesive layer maintains stable performance during repeated use, reducing fluctuations in grinding batches.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125294A_ABST
    Figure CN123125294A_ABST
Patent Text Reader

Abstract

The problem of the present invention can be solved by an adhesive sheet (1) for fixing an abrasive pad with a release tab FA. The adhesive sheet (1) for fixing an abrasive pad with a release tab FA includes an adhesive layer A on one side of a sheet substrate (F) and an adhesive layer B on the other side. The other surface of the adhesive layer A is in contact with the release tab FA. The outer surface of the release tab FA has irregularities and irregularities. The shape is regular and fixed when viewed from above. The average height Rc of the irregularities and irregularities on the front surface is 5 μm to 25 μm. The material of the release tab FA is a plastic film. The Beck smoothness of the outer surface is 0.1 seconds to 30 seconds under specific condition 1 and 1 second to 500 seconds under specific condition 2.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to an adhesive sheet for fixing an abrasive pad with a release tab FA, and an adhesive sheet for fixing an abrasive pad with both a release tab FA and a release tab FB. Additionally, it relates to an abrasive pad with a release tab FA and an adhesive layer A. Furthermore, it relates to a method for fixing an abrasive pad to a platform via the adhesive sheet. Background Technology

[0002] Recent semiconductor development has demanded higher integration and higher quality, requiring wafers, as the material, to achieve even greater polishing precision. Methods have evolved beyond simple grinding with abrasive grains; some utilize chemical mechanical polishing (CMP) to modify the surface through chemical reactions. Within CMP, methods have been developed to achieve even smoother polished surfaces than before.

[0003] When attaching the polishing pad to the worktable, a double-sided adhesive sheet is used. Specifically, one side of the double-sided adhesive sheet is attached to one side of the polishing pad (the side opposite to the side intended for polishing the object), and a polishing pad with a single-sided adhesive layer is prepared in advance and the adhesive layer of the polishing pad with the single-sided adhesive layer is attached to the worktable.

[0004] Various adhesive sheets have been proposed as adhesive sheets for fixing abrasive pads (Patent Documents 1 to 3, etc.).

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2011-122069

[0008] Patent Document 2: Japanese Patent Application Publication No. 2011-168714

[0009] Patent Document 3: Japanese Patent Application Publication No. 2012-057135 Summary of the Invention

[0010] The problem that the invention aims to solve

[0011] The requirements for polishing pads vary depending on the stage of polishing. In particular, polishing pads used in the final finishing process are multi-layered with varying hardness and thickness, resulting in increasingly complex structures. The more complex the structure of the polishing pad, the more difficult it becomes to attach it to the worktable.

[0012] When attaching highly multi-layered, thick polishing pads with single-sided adhesive layers to a worktable, repositioning often requires temporary application, confirmation of position, peeling, and re-application to achieve the desired location. Ideally, this repositioning process should be as quick and frequent as possible to improve productivity. Using adhesive layers with low adhesion is effective in terms of ease of repositioning. However, the adhesive layer used to hold the polishing pad to the worktable must be able to withstand the strong adhesion or cohesion (holding force) required for polishing.

[0013] Furthermore, even if a polishing pad with a single-sided adhesive layer can be quickly and temporarily fixed to the target position on the worktable, there is still a problem of air being trapped between the worktable and the adhesive layer when using rollers or presses to firmly fix the polishing pad to the worktable. If some of the air trapped between the worktable and the adhesive layer remains, the parallelism between the outermost surface of the polishing pad and the surface of the worktable is damaged, making it impossible to polish the object with high precision and smoothness, thus affecting the polishing accuracy.

[0014] One approach to suppress air ingress is to create grooves on the surface of the adhesive layer on the side in contact with the substrate, forming airflow paths. However, even with these airflow paths, the soft adhesive layer can still clog them when the polishing pad is securely attached to the substrate. This can sometimes prevent the removal of voids completely or result in time wasted before air can escape, thus reducing semiconductor production speed. Furthermore, in CMP, polishing pads attached to the substrate are reused approximately 100 to 1000 times. Therefore, maintaining polishing quality (polishing volume) even with additional uses is crucial in terms of manufacturing cost.

[0015] For the adhesive layer constituting the double-sided adhesive sheet used to fix the polishing pad to the platen, strong adhesion, or cohesion (holding force) to withstand the shear forces applied during the polishing process, or chemical resistance to strong alkalis and acids in relation to the polishing fluid used during polishing are required. In particular, in CMP, since strongly alkaline polishing fluids are mostly used, resistance to strong alkalis is strongly required.

[0016] This disclosure is made in view of the aforementioned background, and aims to provide a double-sided adhesive sheet for fixing a polishing pad, which is suitable for high-precision CMP processing, and is easy to reposition based on re-attachment, has excellent air expulsion performance, excellent adhesive properties, and is used to fix a polishing pad that maintains stable polishing performance even during repeated polishing to a stage. Furthermore, it aims to provide a polishing pad with a release tab FA and an adhesive layer A, which is used to obtain a polishing pad that adheres to the stage and maintains stable polishing performance even during repeated polishing use. Finally, it aims to provide a method for fixing a polishing pad to a stage via the adhesive sheet.

[0017] Technical means to solve the problem

[0018] The inventors have conducted repeated and diligent research and have discovered that the problems of this disclosure can be solved in the following forms, thereby completing this disclosure.

[0019] [1]: An adhesive sheet for fixing an abrasive pad with a release tab FA, comprising an adhesive layer A on one side of a sheet-like substrate and an adhesive layer B on the other side of the sheet-like substrate, wherein the surface of the adhesive layer A that is not in contact with the sheet-like substrate is in contact with the release tab FA.

[0020] The adhesive sheet for fixing the abrasive pad with the release tab FA is characterized in that:

[0021] The protrusions on the outer surface of the peeling strip FA have a regular and well-defined shape when viewed from above.

[0022] The average height Rc of the uneven surface on the outer side of the release tab FA is 5 μm to 25 μm.

[0023] The release tab FA is made of plastic.

[0024] The outer surface of the release tab FA, which is not in contact with the adhesive layer A, has irregularities. In the Bekk smoothness test,

[0025] The smoothness of the outer surface of the release tab FA, determined under the following condition 1, is 0.1 seconds to 30 seconds.

[0026] The smoothness of the outer surface of the peeling sheet FA, determined under the following condition 2, is 1 second to 500 seconds.

[0027] Condition 1: The time it takes for the pressure to change from -50.7 kPa to -48.0 kPa.

[0028] Condition 2: The time it takes for the pressure to change from -50.7 kPa to -29.3 kPa.

[0029] [2]: An adhesive sheet for fixing an abrasive pad with a release tab FA as described in [1], wherein the outer side of the release tab FA has the same shape as the inner side of the release tab FA after being reversed.

[0030] [3]: The adhesive sheet for fixing the abrasive pad with the release strip FA as described in [1] or [2] is characterized in that: the average height Rc of the unevenness of the outer surface of the release strip FA is 5 μm to 25 μm, and the average height Rc of the unevenness of the inner surface of the release strip FA is 5 μm to 25 μm.

[0031] [4]: An adhesive sheet for fixing an abrasive pad with a release tab FA according to any one of [1] to [3], characterized in that: the thickness of the release tab FA is 25 μm to 100 μm.

[0032] [5]: An adhesive sheet for fixing an abrasive pad with a release tab FA according to any one of [1] to [4], characterized in that: the cutting level difference Rδc of the contour curve of the outer surface of the release tab FA is 1 μm to 10 μm.

[0033] [6]: An adhesive sheet for fixing an abrasive pad with a release tab FA according to any one of [1] to [5], characterized in that: the adhesive layer A is an acrylic adhesive layer.

[0034] [7]: An adhesive sheet for fixing an abrasive pad with a release strip FA according to any one of [1] to [6], which is wound into a roll and the length of the roll in the width direction is 1000 mm or less.

[0035] [8]: An adhesive sheet for fixing an abrasive pad with a release tab FA and a release tab FB, characterized in that it comprises: an adhesive sheet for fixing an abrasive pad with a release tab FA according to any one of [1] to [7], and a release tab FB.

[0036] The surfaces of the release tab FB and the adhesive layer B that are not in contact with the sheet-like substrate are in contact.

[0037] The release tab FB is made of plastic.

[0038] [9]: The adhesive sheet for fixing the grinding pad with release strip FA and release strip FB as described in [8] is wound into a roll and the length of the roll in the width direction is 1000 mm or less.

[0039]

[10] : An adhesive sheet for fixing an abrasive pad with a release tab FA and a release tab FB as described in [8] or [9], wherein the length of the short side is 1000 mm or less.

[0040]

[11] : An abrasive pad with a release tab FA and an adhesive layer A, comprising an abrasive pad and an adhesive layer for fixing the abrasive pad with a release tab FA according to any one of [1] to [7], wherein,

[0041] The abrasive pad is in contact with the adhesive layer B.

[0042]

[12] : A method for fixing an abrasive pad to a table via an adhesive sheet, characterized in that: the release sheet FA is peeled off from the abrasive pad with release sheet FA and adhesive layer A as described in

[11] , and the adhesive layer A is attached to the table.

[0043] The effects of the invention

[0044] This disclosure provides a double-sided adhesive sheet for fixing a polishing pad to a worktable. It facilitates repositioning based on re-attachment, exhibits excellent air expulsion, and demonstrates superior adhesive properties and resistance to chemicals such as strong alkalis and acids. The adhesive sheet for fixing polishing pads with a release fin FA of this disclosure improves workability during adhesion and significantly enhances polishing accuracy in high-precision CMP processes. Furthermore, the polishing pad with adhesive layer A of this disclosure exhibits the following excellent effects: it adheres to the worktable and maintains stable polishing performance even after repeated polishing applications. Attached Figure Description

[0045] [ Figure 1A [This is a schematic cross-sectional view of an adhesive strip for fixing an abrasive pad with a release tab FA.]

[0046] [ Figure 1B [This is a schematic cross-sectional view of an adhesive pad for fixing an abrasive pad with release tabs FA and FB.]

[0047] [ Figure 1C [This is a schematic cross-sectional view of an abrasive pad with release tab FA and adhesive layer A.]

[0048] [ Figure 1D [This is a schematic cross-sectional view showing the state in which the polishing pad is fixed to the platen via an adhesive sheet.]

[0049] [ Figure 1E [This is a schematic illustration of an example of an adhesive strip for fixing a rolled abrasive pad with a release tab FA.]

[0050] [ Figure 2A [ ] is a schematic diagram illustrating the specimen used in the Beck smoothness test.

[0051] [ Figure 2B [ ] is a schematic diagram illustrating the Beck smoothness test method.

[0052] [ Figure 3A ]~[ Figure 3D [ ] is a schematic cross-sectional view used to illustrate an example of the unevenness (section) of the surface of the release strip FA.

[0053] [ Figure 4A [ ] is a schematic cross-sectional view of the surface irregularities of an example of the release sheet used to illustrate this embodiment.

[0054] [ Figure 4B [ ] is a schematic cross-sectional view used to illustrate the unevenness of the surface of the peel sheet in the comparative example.

[0055] [ Figure 5A(a) and (b) are images of the outer surface of the peeling sheet FA, an example of an embodiment.

[0056] [ Figure 5B ]~[ Figure 5C [ ] is an explanatory diagram illustrating the method for measuring Rc and Rδc on the outer surface of the release FA.

[0057] [ Figure 6A ]~[ Figure 6B [This is a schematic diagram illustrating an example of the "regular" shape (top view) of the uneven surface of the outer side of the release strip FA.]

[0058] [ Figure 6C ]yes Figure 6B Cross-sectional view of the X-X' section.

[0059] [ Figure 6D ] is through Figure 6B A cross-sectional view of the cut section at position X-X' of the laminate of the release liner FA transfer adhesive layer A / sheet substrate.

[0060] [ Figure 6E [This is a schematic diagram illustrating an example of the "regular" shape (top view) of the uneven surface of the outer side of the release strip FA.]

[0061] [ Figure 6F ]yes Figure 6E Cross-sectional view of the Y-Y' section.

[0062] [ Figure 6G ] is through Figure 6E A cross-sectional view of the cut section at the Y-Y' position of the laminate of the release liner FA transfer adhesive layer A / sheet substrate.

[0063] [ Figure 6H ]~[ Figure 6I [This is a schematic diagram illustrating an example of the "regular" shape (when viewed from above) of the surface of the outer side of the release strip FA.]

[0064] [ Figure 7 [This is an explanatory diagram showing an example of the irregular and amorphous patterns and designs (viewed from above) on the outer surface of the release sheet FA.]

[0065] [ Figure 8A [ ] is a manufacturing process diagram illustrating an example of a method for forming the unevenness of a release sheet FA.

[0066] [ Figure 8B ]~[ Figure 8D [This is a schematic cross-sectional view showing the usage of the adhesive pad for fixing the abrasive pad with release tab FA.]

[0067] [ Figure 9[Illustration] is a schematic diagram illustrating the method for evaluating the adhesion performance of this embodiment.

[0068] [ Figure 10 [Illustration] is a schematic diagram illustrating the air exhaust performance evaluation method of this embodiment. Detailed Implementation

[0069] Hereinafter, an example of an embodiment applying the present disclosure will be described. Furthermore, the numerical values ​​"A to B" specifically designated in this specification represent values ​​A or higher and B or lower.

[0070] <Adhesive pads for fixing abrasive pads with release tabs (FA), etc.>

[0071] like Figure 1A As shown, the grinding pad fixing adhesive sheet 1 with release tab FA of this disclosure has a grinding pad fixing adhesive sheet 5 (hereinafter also referred to as adhesive sheet 5) having an adhesive layer A on one side of a sheet substrate F and an adhesive layer B on the other side. The surface of the adhesive layer A of the grinding pad fixing adhesive sheet 5 (the surface not in contact with the sheet substrate F) is covered and protected by the release tab FA. The contact surface of the release tab FA with the adhesive layer A is equivalent to the peeling surface. The material of the release tab FA is a plastic film. It can also be used as... Figure 1E As shown, the abrasive pad fixing adhesive sheet 1 with release tab FA is provided in the following form: the abrasive pad fixing adhesive sheet 1 with release tab FA is wound around a cylindrical member 6 called a core (also called core material), and the outer surface of the release tab FA (the surface not in contact with the adhesive layer A) covers the surface of the adhesive layer B in a roll form. For example, the abrasive pad fixing sheet 1 with release tab FA can be wound into a roll and the length in the width direction of the roll is 1000 mm or less. Furthermore, in Figure 1A In the figures, the unevenness of the surfaces of the release sheet FA and the adhesive layer A is omitted.

[0072] As another form, such as Figure 1B As shown, examples of adhesive sheets 2 for fixing abrasive pads include a release tab FB covering the surface of the adhesive layer B, and a release tab FA and a release tab FB. Examples of adhesive sheets for fixing abrasive pads with release tabs FA and FB include sheets with a short side length of 1000 mm or less, or sheets wound into a roll with a width length of 1000 mm or less.

[0073] like Figure 1C As shown, the abrasive pad 3 (hereinafter also referred to as abrasive pad 3) with release tab FA and adhesive layer A of the present disclosure has abrasive pad PP stacked on the adhesive layer B of the adhesive tab 1 for fixing abrasive pad with release tab FA.

[0074] The polishing pad PP is fixed to the platform SP via the adhesive tab 5. Specifically, the polishing pad 3 (with release tab FA and adhesive layer A) Figure 1C Peel off the release tab FA, and attach the polishing pad 4 with the adhesive layer A to the stage plate SP after exposing the adhesive layer A. Figure 1D In adhesive sheet 5, adhesive layer A is bonded to the platform SP, and adhesive layer B is bonded to the polishing pad PP. That is, the polishing pad PP is fixed to the platform SP via adhesive sheet 5, which has a stacked structure of adhesive layer A / sheet substrate F / adhesive layer B.

[0075] When attaching the polishing pad PP to the worktable SP via the adhesive sheet 5, in most cases up to now, while gently warping and bending the polishing pad PP, the surface of the polishing pad PP is slowly pressed from the end using a roller or scraper, etc., to expel air from the end while attaching it. When attaching the adhesive layer A to the worktable SP, if the adhesive sheet is twisted or uneven force is applied to the adhesive sheet 5, large local air accumulation areas will be generated between the worktable SP and the adhesive layer A.

[0076] Furthermore, recently, there has been an increasing trend in the thickness of polishing pads (PP), as well as extreme hardening or extreme softening. Because the increased thickness or extreme hardening of polishing pads (PP) makes them too rigid, the following problems arise: they cannot bend as much as before, and the rollers or scrapers used for pressing cannot fully act on the surface of the polishing pad (PP).

[0077] On the other hand, because the extremely soft PP abrasive pad is prone to flexing and bending, it is difficult to maintain its flexed state when the surface of the abrasive pad is smoothed using rollers or scrapers. In either case, it is impossible to quickly expel the air at the adhesion interface or achieve uniformity across the entire interface, resulting in large localized air pockets.

[0078] In addition, when the surface of the polishing pad PP is pressed using rollers or scrapers, pressure is applied locally to the surface of the polishing pad PP. In order to ensure that the pressure is applied to the entire surface of the polishing pad PP in sequence, the surface of the polishing pad PP is a predetermined surface that contacts the polishing object (the object being polished), and there is also a requirement that too much force should not be applied.

[0079] The outer surface of the release fin FA (the predetermined surface in contact with the platform SP) of the adhesive sheet 1 for fixing the abrasive pad with the release fin FA disclosed herein has an unevenness specifically specified by the Beck smoothness test and surface height, as described later. The adhesive layer A has the same unevenness as the outer surface of the release fin FA, and the recesses on the surface of the adhesive layer A can be used as air passages (flow paths) to expel air between the platform SP and the adhesive layer A from the periphery to the outside, or to make it uniform across the entire adhesion interface. As a result, the generation of large localized air accumulations between the platform SP and the adhesive sheet 5, such as the surface of the abrasive pad PP (the surface in contact with the abrasive object) being parallel to the platform SP, can be suppressed and prevented.

[0080] The Beck smoothness of the outer surface of the release sheet FA is described. Beck smoothness is specified by Japanese Industrial Standards (JIS) P8119:1998.

[0081] A general description of the sequence of the Beck smoothness test is provided.

[0082] (1) The test piece described later is placed on the plane of a glass (an annular glass component with a circular hole in the center connected to a vacuum container) that has undergone optical plane finishing.

[0083] (2) While applying a pressure of 0.1 MPa to the rubber pressing plate placed on the test piece via the pressure plate, reduce the pressure inside the vacuum container to -50.7 kPa.

[0084] (3) After reaching -50.7 kPa, stop the decompression and draw in atmospheric pressure air between the glass plane and the contact surface of the test piece. Here, for the pressure inside the vacuum container, measure the time it takes for the pressure to change from -50.7 kPa to -48.0 kPa under condition 1 and the time it takes for the pressure to change from -50.7 kPa to -29.3 kPa under condition 2. The ventilability of the surface of adhesive layer A can be evaluated based on these values. That is, under either condition 1 or condition 2, the shorter the time to restore the pressure to the specified pressure, the easier it is to ventilate.

[0085] The test piece was prepared as follows: First, a polyethylene terephthalate (PET) film with a thickness of 100 μm and an Rc of less than 0.5 μm on both sides was adhered to the adhesive layer B of the abrasive pad fixing adhesive sheet 1 with release tab FA. Then, it was cut into 50 mm squares, as shown below. Figure 2A As shown, a laminate formed by overlapping two of these layers is obtained. A circular hole 7 with a radius of 5 mm (smaller than the central hole of the glass component) is made in the center of the obtained laminate to prepare a test sample 8. Then, as... Figure 2B As shown, with the hole 7 of the test sample 8 directly above the central hole 9 of the glass component G, the outer surface of the lowermost release sheet FA in the figure is placed on the surface of the glass component G, and a rubber pressing plate E is placed on the upper surface of the uppermost PET film in the figure. Under the condition of applying a pressure of 0.1 MPa through the pressure plate H, suction and decompression are performed from the lower part of the central hole 9 of the glass component G to determine the smoothness of conditions 1 and 2.

[0086] In the test sample 8, two abrasive pads with release tabs FA are overlapped using adhesive sheets 1. Therefore, half of the measured value is the result of the adhesive layer A of each abrasive pad with release tabs FA using adhesive sheets 1. That is, if the measured value is 2 seconds, the Beck smoothness of the outer surface of the release tab FA is 1 second.

[0087] Regarding the Beck smoothness of the outer surface of the release strip FA, in condition 1, it is important that it is 0.1 seconds to 30 seconds, more preferably 0.5 seconds to 20 seconds, particularly preferably 1.0 seconds to 10 seconds, and most preferably 1.5 seconds to 6 seconds.

[0088] The smoothness of condition 1 is related to the air movement and state in the very initial stage when the adhesive layer A and the platform SP come into contact, and is mainly related to position adjustment. That is, when the smoothness of condition 1 is less than 20 seconds, large local air accumulation is less likely to occur when the adhesive layer A comes into contact with the platform SP, and a tight seal can be achieved by adsorbing the adhesive layer A onto the platform SP. If the position of the adhesive layer A in contact with the platform SP is appropriate and position adjustment is not required, and the smoothness of condition 1 is less than 0.1 seconds, the air permeability is too good, and the position of the adhesive layer A is more likely to shift. That is, when the smoothness of condition 1 is 0.1 seconds or more, it is easy to maintain the position of the abrasive pad 4 with the abrasive pad fixing adhesive sheet adsorbed onto the platform SP.

[0089] In addition, regarding the smoothness of the surface of the outer side of the release sheet FA, in condition 2, it is important to be 1 second to 500 seconds, more preferably 20 seconds to 200 seconds, further preferably 30 seconds to 150 seconds, and most preferably 40 seconds to 100 seconds.

[0090] The smoothness of condition 2 is related to the air movement and state over several minutes to tens of minutes after the adhesive layer A is attached to the platen SP, and is mainly related to the air expulsion of the adhesion interface. With a smoothness of less than 400 seconds in condition 2, even if localized air accumulation occurs between the platen SP and the adhesive layer A, the air is easily uniformly distributed across the adhesion interface via the recesses, or expelled from the periphery. With a smoothness of more than 1 second in condition 2, the adhesive layer A in contact with the platen SP adheres more firmly to the platen SP. By being within the aforementioned preferred range, a smooth and non-distorted high-adhesion state to the platen is demonstrated, while also showing the gradual expulsion of gaps over tens of minutes without special treatment, thus making it suitable for high-precision CMP polishing processes. By being within the preferred range, a vent is provided that exhibits high adhesion and has a degree of venting that can suppress the intrusion of slurry into the space between the adhesive layer A and the platen during grinding. This suppresses the deterioration of the adhesive layer, prevents bubbling or swelling, allows for the reuse of the grinding pad, and reduces batch variation in grinding.

[0091] In addition, the surfaces of the release liner FB and the adhesive layer B (the predetermined surfaces that are in contact with the abrasive pad PP) do not need to have any special irregularities.

[0092] When the polishing pad 3 is attached to the worktable SP, large air pockets are easily formed between the adhesive layer A and the worktable SP because the attachment is done manually. On the other hand, when the polishing pad PP is attached to the adhesive layer B of the polishing pad fixing adhesive sheet 1 with the release tab FA, large air pockets are less likely to form locally because the attachment is done mechanically rather than manually, unlike when the polishing pad 3 is attached to the worktable SP.

[0093] An example of the shape of the surface irregularities (section) of the release liner FA is given by using... Figures 3A to 3D The schematic enlarged cross-sectional view is provided for illustration. Furthermore, regarding the adhesive layer A, since it is printed with a pattern that reverses the outer surface of the release liner FA, it becomes the same shape as the outer surface of the release liner FA. The upper part of the cross-section shown in the figure is in contact with the adhesive layer A, and the lower part shows the outer surface of the release liner FA. For illustration, the surface of the release liner FA in contact with the adhesive layer A is sometimes referred to as the inner side of the release liner FA, and the non-in contact surface is referred to as the outer side of the release liner FA.

[0094] Regarding the aspect that the surface of the adhesive layer A will not be completely flattened even after being bonded to the platform SP, thus ensuring reliable ventilation, the area near the corner of the outer protrusion of the release tab FA is similar to... Figure 3C As shown, a rounded shape is preferred. Figure 3A As shown, it is angular. The reason is that when pressure is applied to the surface of the adhesive layer A, which corresponds to the shape of the protrusion on the outside of the release sheet FA, the pressure will be concentrated at the corner of the protrusion. By taking an angular shape, it can prevent it from being completely flattened.

[0095] Furthermore, the larger the contact area ratio between the adhesive layer A and the platform SP, the better the parallelism between the platform SP and the polishing pad PP is maintained. Therefore, in terms of improving polishing accuracy and suppressing batch fluctuations, the convex portion on the outer side of the release liner FA is wider than the concave portion (i.e., the convex portion of the adhesive layer A is wider). Figure 3A Compare Figure 3B More preferably, Figure 3C Compare Figure 3D More preferably.

[0096] Therefore, in order to improve air expulsion and alignment without reducing grinding accuracy, it is important that the average height Rc (hereinafter referred to as average height Rc) of the roughness curve element on the outer surface of the release sheet FA is 5 μm to 25 μm, preferably 7 μm to 20 μm, and more preferably 10 μm to 15 μm. Within this range, the unevenness of the adhesive layer A can be reproduced with high accuracy. Because the average height Rc of the outer surface of the release sheet FA is 5 μm or more, the recesses are relatively deeper, thus improving air permeability even on the surface of the adhesive layer A under either condition 1 or condition 2 in the Beck smoothness test, thereby improving alignment and air expulsion. In particular, the effect on air expulsion is significant; after grinding, the grinding pad PP along with the adhesive sheet 5 can be easily peeled off from the platform SP. With an average height Rc of 25 μm or less on the outer surface of the release liner FA, the adhesive layer A, which reproduces this average height Rc, is used as a polishing pad PP when attached to the worktable SP for polishing. The uneven shape of this layer minimizes its impact on the outermost surface of the polishing pad PP in contact with the workpiece, resulting in excellent polishing accuracy. Furthermore, the recesses formed on the adhesive surface are less prone to flattening even during adhesion deformation. The recesses on the adhesive layer surface, which serve as vents, remain uniform and are not locally blocked, making the removal of locally infiltrated slurry easier and improving polishing accuracy. Moreover, by being within the preferred range, the polishing accuracy and air expulsion are maintained, and the vents are a size that makes slurry intrusion less likely. Therefore, even with additional polishing batches (polishing a new workpiece without changing the polishing pad), the polishing rate (polishing amount) between batches is less likely to differ, which is preferable.

[0097] Regarding the uneven shape of the outer surface of the release sheet FA disclosed herein, the roundness or inclination of the protrusion, the interval between the protrusions and the shape of the unevenness can be more specifically determined based on the cutting level difference of the contour curve: Rδc.

[0098] The Rδc of the outer surface 11 of the release tab FA is preferably 1 μm to 10 μm, more preferably 2 μm to 7.5 μm, and even more preferably 4 μm to 6 μm. The Rδc is the difference in horizontal distance in the height direction consistent with any two load length rates, as described in the load curve (a curve obtained by plotting the ratio of the length of the solid portion to the measured length in height order). In this disclosure, the two load length rates are defined as 0% and 50%. In particular, the Rδc, representing the load length rate using 0% and 50%, indirectly represents the depth and frequency of the unevenness and the inclination of the protrusion.

[0099] With an Rδc of more than 1 μm on the outer surface 11 of the release sheet FA, it is more difficult to generate air accumulation in the very early stage of attachment, and it is easier to suppress the deviation (batch fluctuation) of each grinding batch.

[0100] In other words, since the adhesive layer A is not so firmly bonded to the platform SP, the adhesive layer A can be peeled off with little resistance when it is temporarily in contact with the platform SP, making position adjustment easy.

[0101] Furthermore, since adhesive layer A adheres, it is assumed that some deformation will occur when adhesive layer A is adhered to the stage plate SP. That is, microscopically, it can be imagined that during adhesion, the small protrusions on the surface of adhesive layer A will be flattened, and the concave areas will become relatively shallower. By ensuring that the Rδc of the outer surface 11 of the release tab FA is less than 10 μm, even if adhesive layer A is flattened, the concave areas can be reliably maintained when adhesive layer A is firmly attached to the stage plate SP, thus improving air expulsion.

[0102] Rc and Rδc are explained using schematic diagrams. Additionally, the following explanation is for the lower side of each diagram (the outer side of the FA with the release tab FA, used to fix the abrasive pad).

[0103] Figure 3A , Figure 3B , Figure 3C This refers to the case where Rc is of the same degree. If Figure 3A This indicates that Rδc is between 1 μm and 10 μm, then the convexity on the lower surface corresponding to the vent is greater than... Figure 3A The recess on the lower surface of the adhesive layer, which is wide and corresponds to the area where it contacts the adhered object, is narrow. Figure 3B In the case of Rδc, Figure 3A The situation is large. In Figure 3C In the case of Rδc, Figure 3B Further increase.

[0104] Rc and Rδc are values ​​determined based on JIS B 0601 (2013), specifically using a laser microscope (Keyence VK-X100). An example of an image obtained by observing the outer surface 11 of the release slab FA using a laser microscope is shown below. Figure 5A . Figure 5A In the image above, the straight lines represent concave areas, while the triangular areas surrounded by the straight lines represent convex areas. When viewed from above, they appear regular and well-defined.

[0105] Specifically, at 100x magnification, six consecutive images were taken in each direction (6 in each direction) for a field of view approximately 950 μm in length and 1300 μm in width (a total of 36 images). The area approximately 5700 μm in length and 7800 μm in width was used as the entire field of view. The central area of ​​approximately 5500 μm in length and 7500 μm in width was used as the measurement field of view (refer to...). Figure 5B), set measurement lines along one and two diagonal directions along the horizontal direction of the measurement field of view, measure Rc and Rδc, and calculate the average value respectively. If in such Figure 5C When the diagonal of the measurement field is located directly above the convex part, the measurement line is set at a position approximately parallel to the diagonal, spanning as many concave and convex parts as possible (e.g., more than 5), and the measurement is performed. Similarly, for lateral measurement lines, the measurement line is set at a position approximately parallel to the lateral side of the measurement field, spanning as many concave and convex parts as possible, and the measurement is performed to avoid measuring only directly above the convex part. The same applies to the measurement of Rc, etc., of the peeling sheet FA, which will be discussed later.

[0106] An image of the uneven cross-section of the outer surface 11 of the release tab FA in this disclosure is shown. Figure 4A The image shown is a cross-sectional view of the uneven surface 11 of the outer side of the so-called "extinct" comparative example peel sheet FA-x. Figure 4B middle.

[0107] The unevenness in this disclosure differs from the so-called "extinction" unevenness intended for optical light removal. The unevenness elements (spacing, depth) on the outer surface of the release liner FA in this disclosure are significantly larger. Since the unevenness elements of "extinction" are significantly smaller, it is difficult to directly transfer the unevenness shape of the outer surface of the release liner FA to the adhesive layer A. Even assuming transfer to the adhesive layer A, the unevenness Rc and Rδc of this disclosure have a larger height difference and wider unevenness spacing compared to the so-called "extinction" unevenness formed on the adhesive layer A, which is good at general optical light removal. Therefore, it exhibits an ideal shape for initial position adjustment, air expulsion during application, and parallel and smooth fixation of the abrasive pad to the platform.

[0108] The "rules" of the surface irregularities (top view) of the outer surface of the release tab FA will be described. Examples of the surface irregularities (top view) of the outer surface of the release tab FA in this disclosure include: Figure 6A The grid pattern shown, or like Figure 6B , Figure 6E The patterns and designs shown are regular, such as water droplet patterns. In the diagram, the gray and shaded areas represent concave areas.

[0109] Figure 6B This indicates that the outer surface of the peeling sheet FA has a regular water droplet pattern consisting of independent circular recesses and continuous convexities. Figure 6C yes Figure 6B A cross-sectional view at point X-X'. Figure 6C The upper surface in the figure represents the outer surface 11 of the release strip FA, and the lower surface in the figure represents the inner surface 12 of the release strip FA. The inner surface 12 of the release strip FA has the same degree of unevenness as the outer surface 11 of the release strip FA. Figure 6D This is a cross-sectional view of the adhesive layer A, which is reverse-transferred and features the raised and recessed surfaces 12 of the inner side of the release liner FA. The raised and recessed surfaces 11 of the outer side of the release liner FA are reproduced on the surface of the adhesive layer A. For example... Figure 6B As shown, on the outer surface 11 of the release tab FA, where the protrusions are continuous, as... Figure 6D As shown, an independent recess is formed in the adhesive layer A.

[0110] On the other hand, such as Figure 6E As shown, when the outer surface of the release liner FA has a regular water droplet pattern including independent circular protrusions and continuous concave portions, the surface of the adhesive layer A formed by the reverse transfer of the protrusions and concavities of the inner surface 12 of the release liner FA, as shown... Figure 6G The surface 11 of the release liner FA has continuous recesses extending to the end of the adhesive layer A. To ensure airflow in the adhesive layer A, the surface 11 of the release liner FA preferably has independent protrusions and continuous recesses extending to the end. This also applies to triangular or polygonal patterns in addition to water droplet patterns.

[0111] Furthermore, such as Figure 6H As shown, examples can also be shown where the same or similar patterns overlap on the outer surface of the peeling sheet FA, with independent convex parts and continuous concave parts.

[0112] In addition, such as Figure 6I As shown, a continuous grid-like concave portion that overlaps with a continuous concave portion other than a circular convex portion can also be used as a release sheet FA.

[0113] An example of an irregular and amorphous surface (viewed from top) on the outer surface 11 of the release strip FA is shown. Figure 7 In the middle, the black parts represent convex parts, and the white parts represent concave parts. Their positions are irregular, and no regularity has been found in their shapes either.

[0114] If the Beck smoothness of the outer surface of the release tab FA in the adhesive pad 1 for fixing the abrasive pad with the release tab FA is within the range described in conditions 1 and 2, then regardless of whether the shape is irregular and amorphous or regular and shaped when viewed from above, there is no difference in terms of position adjustment or air expulsion when pasting onto the platen. However, if the pattern or design is regular and shaped when viewed from above, gaps or unevenness caused by air entering and disrupting the regularity are easily detected during attachment, and can be easily detected as a defect in the process by a charge-coupled device (CCD) camera, etc., therefore, it is preferred.

[0115] As a method for obtaining a polishing pad 1 with a release strip FA that has a Beck smoothness within a specified range, a method using a release strip FA with an uneven surface having an average height Rc of 5 μm to 25 μm can be cited.

[0116] That is, prepare a pre-peeling sheet FA' with a peeling layer (not shown), and then, as follows: Figure 8A As shown, the pre-peeling sheet FA' is passed between a metal roller R1 and a rubber roller R2, both processed to the desired surface shape, at high temperature. This reverses the surface shape of the transfer roller R1, creating a peeling sheet FA with an average height Rc of 5 μm to 25 μm. Furthermore, while the surface shape of the peeling sheet FA is reversed by rotating the metal roller R1, its surface shape exhibits a certain periodicity, but this periodicity differs from the regularity observed in the top view.

[0117] Furthermore, when measuring the Beck smoothness of an adhesive sheet 1 for fixing an abrasive pad with a release tab FA, formed using such an uneven release tab FA, the unevenness of the outer surface of the release tab FA is deformed (flattened) by the pressure applied during the measurement. The deformation of the unevenness of the outer surface of the release tab FA is affected by the thickness or hardness of the adhesive layer A that is in contact with the inner surface of the release tab FA. For example, if it is an adhesive layer of the same type, a thicker layer is easier to mitigate stress, and therefore the unevenness of the outer surface of the release tab FA is flattened in a smoother manner. Therefore, the Beck smoothness value of the adhesive sheet 1 for fixing an abrasive pad with a release tab FA increases. The Beck smoothness of the adhesive sheet 1 for fixing an abrasive pad with a release tab FA is based on the deformation of the unevenness of the outer surface of the release tab FA caused by pressure and the deformation of the unevenness of the adhesive layer A that is in contact with the inner surface of the release tab FA. Therefore, the Beck smoothness value of the adhesive pad 1 for fixing the abrasive pad with release tab FA is related to the adhesion or air expulsion when the adhesive layer A is attached to the platen SP, the adhesion or holding force to the platen, the abrasive precision, etc.

[0118] The adhesive sheet for fixing the abrasive pad with release strips FA and FB disclosed herein can be manufactured, for example, by the following method.

[0119] (1) Apply adhesive a to the release layer of the release sheet FA and dry it as needed to form adhesive layer A.

[0120] (2) On the surface of the adhesive layer A that is not in contact with the release sheet FA, overlap the sheet substrate.

[0121] (3) Apply adhesive b to the peeled surface of the release sheet FB and dry it as needed to form an adhesive layer B.

[0122] (4) On the surface of the sheet substrate that is not in contact with the adhesive layer A, overlap the surface of the adhesive layer B that is not in contact with the release sheet FB.

[0123] As a result, it is possible to produce such as Figure 8B The adhesive sheet 2 for fixing the abrasive pad with a release sheet has a laminated structure as shown, consisting of [release sheet FA / adhesive layer A / sheet substrate F / adhesive layer B / release sheet FB].

[0124] Alternatively, it can be made using the following method: Figure 8B An adhesive sheet for fixing an abrasive pad with a release sheet, as shown in the laminated structure of [release sheet FA / adhesive layer A / sheet substrate F / adhesive layer B / release sheet FB].

[0125] (5) Apply adhesive a to one side of the sheet substrate F and dry it as needed to form an adhesive layer A.

[0126] (6) On the surface of the adhesive layer A that is not in contact with the sheet substrate F, the surface of the release sheet FA that overlaps with the surface of the release treatment has an average height Rc of 5 μm to 25 μm.

[0127] (7) Apply adhesive b to the peeled surface of the release sheet FB and dry it as needed to form an adhesive layer B.

[0128] (8) On the surface of the sheet substrate F that is not in contact with the adhesive layer A, overlap the surface of the adhesive layer B that is not in contact with the release sheet FB.

[0129] Alternatively, it can be made using the following method: Figure 8B An adhesive sheet for fixing an abrasive pad with a release sheet, as shown in the laminated structure of [release sheet FA / adhesive layer A / sheet substrate F / adhesive layer B / release sheet FB].

[0130] (9) Apply adhesive b to the peeled surface of the release sheet FB and dry it as needed to form an adhesive layer B.

[0131] (10) On the surface of the adhesive layer B that is not in contact with the release sheet FB, overlap the sheet substrate F.

[0132] (11) On the surface of the release sheet FA, where the average height Rc of the surface after the peeling treatment is 5 μm to 25 μm, an adhesive a is applied and dried as needed to form an adhesive layer A.

[0133] (12) On the surface of the sheet substrate F that is not in contact with the adhesive layer B, overlap the surface of the adhesive layer A that is not in contact with the release sheet FA.

[0134] Furthermore, in any method, the surface of the adhesive layer B (the predetermined surface in contact with the abrasive pad) is preferably without any unevenness, so the release surface of the release sheet FB for which the adhesive b is applied is preferably smooth.

[0135] The adhesive can be applied using known methods such as roller coating, corner roller coating, die lip coating, die coating, reverse coating, screen printing, and gravure coating. After application, it can be dried using a hot air oven, infrared heater, or similar equipment.

[0136] From the lamination structure of [release sheet FA / adhesive layer A / sheet substrate F / adhesive layer B / release sheet FB] obtained by various methods, the release sheet FB is peeled off from the abrasive pad fixing adhesive sheet with release sheet FA and release sheet FB. Figure 8C As shown, the polishing pad PP is attached to the exposed adhesive layer B, thereby obtaining the polishing pad 3 with the release sheet A and adhesive layer A in the laminated structure of [release sheet FA / adhesive layer A / sheet substrate F / adhesive layer B / polishing pad PP].

[0137] Next, from the obtained polishing pad 3 with release sheet FA and adhesive layer A, the release sheet FA covering the adhesive layer A is peeled off, thereby obtaining a polishing pad 4 with the uneven adhesive layer A on the inner surface of the release sheet FA transferred in reverse. Then, as... Figure 8D As shown, the exposed adhesive layer A is pasted onto the platform SP, thereby fixing the polishing pad PP to the platform SP via the adhesive sheet 5.

[0138] <Adhesive layer>

[0139] In the adhesive sheet 5 for fixing the abrasive pad disclosed herein, adhesive layer A and adhesive layer B are respectively located on the outermost surface of the adhesive sheet 5. The sheet substrate F can be a single layer or can be formed by stacking multiple components, and the number of layers is not particularly limited.

[0140] The thickness of the adhesive layer A of the adhesive sheet 5 for fixing the polishing pad is preferably 15 μm to 100 μm, more preferably 30 μm to 70 μm. By setting the thickness of the adhesive layer A to 15 μm or more, adhesion is easily demonstrated. In addition, the thicker the thickness, the easier it is for the unevenness of the adhesive layer A formed by the release liner FA to be flattened, and the air permeability when attached to the platen SP becomes worse. Therefore, by setting it to 100 μm or less, the unevenness shape required by this disclosure is easily maintained even under pressure during the polishing stroke. By being in the more preferred range, the adhesion is excellent, and the undesirable situation of the adhesive layer shifting in the shear direction is suppressed when the adhesive sheet becomes hot during polishing. Furthermore, the thickness is the average value obtained by measuring five arbitrary points using a Litematic VL-50B thickness gauge manufactured by Mitutoyo, with a Φ7.5 mm measuring head and a pressing pressure of 0.01 N.

[0141] Regarding the thickness of the adhesive layer B, there are no particular restrictions as long as it can fix various abrasive pads. It is set to less than 200 μm by combining it with the thickness of the adhesive layer A after removing the substrate layer. This reduces the proportion of the adhesive layer, which is a low-elasticity material, in the entire adhesive sheet, thereby improving the abrasive precision.

[0142] In the adhesive layers A and B of the adhesive sheet disclosed herein, acrylic adhesives, elastic adhesives, urethane adhesives, silicone adhesives, etc., may be used, or two or more may be used in combination. From the viewpoints of less gel formation, less likelihood of localized poor elastic modulus, and easier control of adhesive force, acrylic adhesive layers using acrylic adhesives are preferred.

[0143] Elastic adhesives or urethane adhesives mostly use metal catalysts during synthesis, and silicone adhesives mostly use metal catalysts during curing. In contrast, acrylic adhesives have a lower content of metal catalysts, so they are less likely to affect CMP processing and have high chemical resistance, making them a preferred choice from this perspective.

[0144] In addition, to accommodate the wide variety of abrasive pad materials, adhesive layer B is preferably made of an acrylic adhesive with a wide range of monomers.

[0145] <Acrylic adhesives>

[0146] Acrylic adhesives contain acrylic copolymers and hardeners. They may also contain adhesive-improving resins. The acrylic copolymers are preferably carboxyl or hydroxyl groups, and more preferably (meth)acrylate resins with hydroxyl groups.

[0147] The (meth)acrylate resin is obtained by copolymerizing a monomer having hydroxyl groups with other monomers that do not have hydroxyl groups. That is, the (meth)acrylate resin is a copolymer comprising units derived from monomers having hydroxyl groups and units derived from other monomers.

[0148] Examples of monomers containing hydroxyl groups include hydroxyalkyl methacrylates, or compounds formed by adding ε-caprolactone to the hydroxyalkyl methacrylates, with hydroxyalkyl methacrylates being preferred.

[0149] Specific examples of hydroxyalkyl methacrylates include 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, and 4-hydroxybutyl methacrylate, where the alkyl group has 1 to 4 carbon atoms. Specific examples of compounds formed by the addition of ε-caprolactone to hydroxyalkyl methacrylates include 1-molar ε-caprolactone adducts of 2-hydroxyethyl methacrylate, 2-molar ε-caprolactone adducts of 2-hydroxyethyl methacrylate, and 3-molar ε-caprolactone adducts of 2-hydroxyethyl methacrylate, where the ε-caprolactone adduct has 1 to 4 carbon atoms, etc., but this disclosure is not limited to the examples described. These hydroxyl-containing monomers can be used individually or in combination. From the viewpoint that crosslinking with isocyanate curing agents results in closer intermolecular distances and improved chemical resistance, 2-hydroxyethyl (meth)acrylate is particularly preferred.

[0150] Other monomers that do not possess a hydroxyl group can be listed as various monomers as shown below. Examples of alkyl methacrylates include: methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, isoamyl methacrylate, 2-ethylhexyl methacrylate, isononyl methacrylate, isodecanyl methacrylate, lauryl methacrylate, stearyl methacrylate, tert-butylhexyl methacrylate, etc., as well as alkyl methacrylates such as 2-acetylacetoxyethyl methacrylate and phenoxyethyl methacrylate.

[0151] The weight average molecular weight (Mw) of the acrylic copolymer is preferably between 200,000 and 1,800,000, more preferably between 500,000 and 1,500,000. With a weight average molecular weight (Mw) of 200,000 or more, the adhesive readily acquires cohesive strength capable of withstanding strong shear forces; with a value of 1,800,000 or less, it exhibits excellent heat resistance and is less prone to degradation in adhesion to abrasive materials; and with an even more preferred range, its performance is further improved.

[0152] Examples of methods for polymerizing monomers include solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization, but this disclosure is not limited to these polymerization methods. Among these polymerization methods, solution polymerization is preferred in terms of the direct usability of the resulting reaction mixture.

[0153] <Elastic System Adhesives>

[0154] The elastic adhesive system comprises an elastomer and an adhesive-improving resin. The elastomer is preferably a styrene-isoprene block copolymer.

[0155] Styrene-isoprene block copolymers exist in both linear and radial structures. In the case of a linear structure, the copolymer exhibits high flexibility, resulting in excellent adhesion to various substrates and superior performance in terms of both adhesion and heat resistance. Therefore, linear structures comprising triblock copolymers (styrene-isoprene-styrene (SIS)) and diblock copolymers (styrene-isoprene (SI)) containing styrene-isoprene blocks are preferred. A linear styrene-isoprene block copolymer refers to a linear copolymer formed by the bonding of styrene blocks and isoprene blocks.

[0156] The styrene content in the styrene-isoprene block copolymer is preferably 20% to 40% by weight per 100% of weight. The diblock content is preferably 15% to 70% by weight. By having the styrene content and diblock content within the aforementioned ranges, it can exhibit excellent cohesive adhesive properties, improved holding power, and enhanced resistance to pharmaceutical solutions in high-humidity environments.

[0157] Examples of styrene-isoprene block copolymers include, but are not limited to, Kraton D1119 (manufactured by Kraton, 22% wt% styrene, 66% wt% diblock), Kraton D1126 (manufactured by Kraton, 21% wt% styrene, 30% wt% diblock), and Kraton D1117 (manufactured by Kraton, 17% wt% styrene, 33% wt% diblock). Two or more copolymers may be used in combination as needed.

[0158] Additionally, natural rubber may be included if the desired performance range is not compromised. There are no particular limitations on the type of natural rubber, but kneading using kneading rollers is preferred to achieve a Mooney viscosity of, for example, 10 to 100. Other elastomers or natural rubbers are not limited to these; one or more may be used alone or in combination.

[0159] <Silicone-based adhesives>

[0160] Silicone-based adhesives can utilize materials known as silicone resins. Specifically, examples include organopolysiloxanes with silanol groups at both ends of the molecular chain, such as those containing R3SiO groups in the molecule. 0.5 Materials obtained by partially dehydrating and condensing organopolysiloxanes with SiO2 units (where R represents a substituted or unsubstituted monovalent hydrocarbon group) represented by the triorganosiloxane unit. These can be obtained as silicone adhesives KR-101-10, KR-120, KR-130, and X-40-3068 (all manufactured by Shin-Etsu Chemical Industry Co., Ltd.). The curing methods for silicone adhesives generally include curing using peroxides such as benzoyl peroxide, and curing using a platinum catalyst reacting with organopolysiloxanes containing Si-H bonds. Either method can be used, or they can be used in combination.

[0161] <Adhesion-improving resin>

[0162] Examples of adhesive-imparting resins include: rosin-based resins such as rosin esters, polymerized rosin, hydrogenated rosin, disproportionated rosin, maleic acid-modified rosin, fumaric acid-modified rosin, and rosin phenol resins; terpene-based resins such as α-pinene resin, β-pinene resin, dipentene resin, aromatic modified terpene resin, hydrogenated terpene resin, terpene phenol resin, acid-modified terpene resin, and styrene-modified terpene resin; alkylphenol resins, coumarone-based resins, styrene-based resins, petroleum-based resins, or copolymers thereof, with terpene phenol resins being particularly preferred. One or more adhesive-imparting resins may be used.

[0163] Hardener

[0164] Hardeners can be added to the adhesive as needed. The peel force during separation from the grinding machine plate varies from high to low adhesion, therefore, hardeners can be added to control adhesion. As hardeners, isocyanate-based hardeners, aziridine-based hardeners, metal chelate-based hardeners, and epoxy-based hardeners can be used as needed, without compromising the desired performance. In particular, from the viewpoint of cohesion and heat resistance, isocyanate-based hardeners are preferred for addition to acrylic adhesives.

[0165] These hardeners can be used alone or in combination of two or more.

[0166] <Other Additives>

[0167] Among the various adhesives used to form the adhesive layer in the adhesive sheet of this disclosure, various additives may be included as needed, such as known antioxidants and other anti-aging agents, fillers, pigments, dyes, diluents, plasticizers, polymerization inhibitors, ultraviolet absorbers, ultraviolet stabilizers, coupling agents, etc. Furthermore, two or more additives may be used in combination. In addition, the amount of additives added is not particularly limited, as long as it is set to the amount that obtains the desired physical properties.

[0168] The adhesive layer A on the SP side of the platen is preferably designed to balance alignment during adhesion and fixation during the grinding process, and the change in adhesive strength is small even after immersion in an alkaline aqueous solution. From this perspective, the adhesive strength of the adhesive layer A on the SP side of the platen before immersion is not particularly limited, but is preferably 5 N / 25 mm to 25 N / 25 mm, and particularly preferably 15 N / 25 mm to 20 N / 25 mm.

[0169] Furthermore, it is preferable to have minimal change in adhesion after grinding. Specifically, the smaller the change in adhesion after immersion in a sodium hydroxide aqueous solution with a pH of 11.5 while still attached to a stainless steel plate, and after being placed at 40°C for 24 hours, the better. Generally, regarding adhesion after immersion in an alkaline aqueous solution, the cohesion decreases due to the swelling of the adhesive layer, and the adhesion tends to increase. However, by using a hardener to increase the crosslinking density, the decrease in cohesion can be suppressed. Increasing the crosslinking density reduces the adhesion before immersion, thus presenting a trade-off. Therefore, balancing these two aspects becomes important.

[0170] Compared to the irregular and amorphous textured surface of the adhesive layer, the grid pattern makes the surface of the raised portion of the adhesive layer A that contacts the substrate SP more flat. Therefore, the contact area ratio with the bonded object is less likely to change due to external factors such as swelling or load from the moment of bonding. Even during multiple wafer polishing processes, the polishing accuracy or polishing rate of the wafer is less likely to change, making it preferable in terms of increasing the number of uses of the polishing pad.

[0171] After adhesion, the polishing pad PP is not easily misaligned. Considering the stability of the polishing process, the initial adhesion is preferably 5 N / 25 mm or more, and in terms of re-adhesion (alignment) during bonding, it is preferably less than 30 N / 25 mm. In terms of ease of alignment, and the fact that it is not easily misaligned or peeled off even when various stresses are applied during the polishing process, it is particularly preferred to be 10 N / 25 mm to 20 N / 25 mm.

[0172] Furthermore, the adhesion force disclosed herein refers to the following value: the surface to be measured is overlapped with a stainless steel plate, a 2 kg roller is pressed back and forth once to press the adhesive layer A onto the stainless steel plate, and after being left for 24 hours, the value is obtained by measuring it using a tensile testing machine at a peel angle of 180 degrees and a peel speed of 0.3 m / min in an environment of 23℃-50%RH according to the test method of JIS Z1528:2009.

[0173] Regarding adhesive layer A, in order to achieve air expulsion and fixation to the tabletop, during bonding, the adhesive layer in close contact with the tabletop is spaced at intervals of 0.5 cm. 2 The grounding area ratio is preferably 60% to 90%, more preferably 62% to 80%, and particularly preferably 65% ​​to 75%. With a grounding area ratio of 60% or higher, the adhesion is less likely to change after initial fixation to the worktable and during grinding. When grinding is repeated on different objects without changing the grinding pad adhered to the worktable, fluctuations in the amount of material ground in each batch are less likely to occur. With a grounding area ratio of 90% or lower, air expulsion is excellent, suppressing gaps during adhesion. As described below, the grounding area ratio is the following average value: Using a hand roller, the adhesive layer A exposed by the peeling off the adhesive sheet FA is bonded to the vapor-deposited surface of the spacer after metal vapor deposition. Then, a 2 kg roller is pressed back and forth once. Afterwards, a digital microscope (Keyence Corporation) is used with a coaxial light source and 20x magnification (field of view approximately 1.0 cm²). 2 Furthermore, three images were taken of any different locations on the surface of the spacer side, and the average value of the three images represents the ratio of the identifiable areas with vapor-deposited film to the areas without vapor-deposited film in the captured images.

[0174] <Resealant FA>, <Resealant FB>

[0175] Release sheets FA and FB, for example, have a release layer formed by coating a release agent onto a sheet substrate such as a plastic film or synthetic paper made primarily of plastics such as polypropylene. In CMP processing, release sheets using a highly cleanable plastic film as the sheet substrate are preferred.

[0176] The plastic film used for the release sheet FA is preferably a polyethylene terephthalate film, which is easy to process with a metal roller and is inexpensive. Furthermore, compared to cutting or laser processing, processing with a metal roller is less likely to introduce foreign matter, resulting in a product with excellent cleanliness, and is therefore preferred. In the embossing process using the exemplified metal roller, a release sheet with a thickness of 25 μm to 100 μm is preferred, more preferably 45 μm to 80 μm. With this range, it is easy to transfer a shape identical to the desired shape formed on the metal surface to the release sheet (transferability), and the shape of the outer side and inner side of the release sheet FA after reversal is identical (reversibility). Moreover, through a series of processes such as coating to the inner side of the release sheet FA and making the pattern on the surface of the resulting adhesive layer A become the shape of the inner side of the release sheet FA, the embossed pattern of the metal roller can be reproduced well on the surface of the adhesive layer A.

[0177] Regarding the transfer of the unevenness of the inner side of the release sheet FA to the surface of the adhesive layer A, the average height Rc of the outer side of the release sheet FA is preferably 5 μm to 25 μm, more preferably 7 μm to 20 μm, and even more preferably 10 μm to 15 μm. By being within the preferred range, its unevenness can be reproduced in the adhesive layer A with high precision.

[0178] The plastic film used for the release sheet FB is preferably made of inexpensive polyethylene terephthalate (PET) film, which has high smoothness. Furthermore, the thickness of the release sheet FB is not particularly limited, but is preferably 10 μm to 200 μm to provide toughness and easy peeling.

[0179] Release agents used in release sheets FA and FB include, for example, silicone resins, alkyd resins, melamine resins, fluorinated resins, and acrylic resins. Among these, silicone resins are preferred.

[0180] <Sheet substrate>

[0181] The sheet substrate F disclosed herein is preferably a non-woven fabric or a plastic film. Examples of plastic films include those comprising polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate, polyphenylene sulfide (PPS), nylon, triacetyl cellulose, cyclic olefins, polyimide, and polyamide. Polyethylene terephthalate films, which are inexpensive to manufacture and exhibit excellent chemical resistance and smoothness, are particularly preferred.

[0182] The thickness of the sheet substrate F is not particularly limited, but is preferably 5 μm to 200 μm, more preferably 25 μm to 75 μm, and particularly preferably 50 μm to 75 μm. By being within the preferred range, the unevenness of the adhesive layer A will not affect the adhesive layer B or the abrasive pad, providing appropriate toughness and improving workability during application. By being within the particularly preferred range, workability is further improved.

[0183] The sheet substrate F in this disclosure can also undergo an easy-bonding treatment to improve the adhesion between adhesive layer A and adhesive layer B. The easy-bonding treatment can be performed using known methods such as a dry method involving corona discharge and a wet method involving the application of an anchoring coating.

[0184] When using acrylic adhesives in the formation of the adhesive layer, it is preferable to use a substrate that has undergone an easy-bond treatment to improve adhesion. On the other hand, in the case of elastic adhesives, if an easy-bond treatment using corona discharge is performed, the adhesive layer is more likely to peel off from the sheet substrate. Therefore, it is preferable to apply the elastic adhesive to the surface where the easy-bond treatment has not been performed.

[0185] The thickness of the adhesive sheet 5 for fixing the abrasive pad, comprising adhesive layer A, sheet substrate F, and adhesive layer B, is preferably 80 μm to 300 μm, more preferably 100 μm to 200 μm. With a thickness of 80 μm or more, processing can be performed uniformly without force bias during lamination when integrated with the abrasive pad PP. With a thickness of 300 μm or less, a roll shape can be used when manufacturing the adhesive sheet 5, increasing productivity. Within the more preferred range, the force of the platform SP is appropriately transmitted to the abrasive pad PP during grinding, improving grinding accuracy.

[0186] <Utilization Form>

[0187] An example of the utilization form of the adhesive sheet for fixing the abrasive pad disclosed herein will be described.

[0188] like Figure 1B , Figure 8B As shown, an adhesive sheet for fixing an abrasive pad with a release tab FA can also be provided, in which each side of the adhesive sheet for fixing the abrasive pad is covered by the release tab FA and the release tab FB, respectively. Figure 1AAs shown, it can also be provided in a state where the release fin FA only covers the adhesive layer A side of the adhesive sheet used to fix the abrasive pad. Figure 1A In the case of its form, it can be like Figure 1E As shown, an adhesive sheet 1 for fixing an abrasive pad with a release tab FA is wound around a cylindrical component 6, which is called the core (also called the core material). The surface of the adhesive layer B is covered by the other side of the release tab FA (the side that is not in contact with the adhesive layer A), thereby providing a rolled adhesive sheet for fixing an abrasive pad with a release tab FA.

[0189] like Figure 1C , Figure 8C As shown, an abrasive pad PP is laminated on the surface of the adhesive layer B of the adhesive sheet for fixing the abrasive pad with release tab FA to form an abrasive pad 3 with release tab FA and adhesive layer A.

[0190] Then, as Figure 1D , Figure 8D As shown, the release tab FA is peeled off to expose the adhesive layer A, and the polishing pad with adhesive layer A is attached to the stage plate SP. The adhesive layer A in the polishing pad fixing adhesive tab 5 is connected to the stage plate SP, and the adhesive layer B is connected to the polishing pad PP.

[0191] Polishing pads (PP), also known as polishing cloths, polishing mats, or polishing PADs, are components that come into contact with the surface of the object being polished and polish it. Polishing pads exist in single-layer types containing a single component and multi-layer types with multiple components stacked together. Examples of raw materials for the outermost layer of the polishing pad include urethane-based, non-woven fabric, and suede-like fabric. In multi-layer types, urethane-based foams, polyethylene-based foams, and polypropylene-based foams are used as cushioning materials in the inner layers.

[0192] Example

[0193] The present disclosure will be described in more detail below through embodiments, but the present disclosure is not limited to the following embodiments. In addition, in the examples, "parts" means "parts by weight" and "%" means "% by weight".

[0194] [Molecular weight]

[0195] In the following examples, molecular weight refers to the weight-average molecular weight of polystyrene determined by gel permeation chromatography (GPC). The determination was performed using a GPC-8020 (manufactured by Tosoh Corporation) with tetrahydrofuran as the eluent. Three TSK gel SuperHM-M (manufactured by Tosoh Corporation) columns were used as the column temperature at 40°C, a flow rate of 0.6 mL / min, a sample concentration of 0.3%, and an injection volume of 10 μL.

[0196] [Non-volatile components]

[0197] Non-volatile components are defined as the mass of a 1 g sample after heating at 170°C for 10 minutes, divided by the mass of the sample before heating. For commercially available products, the value can also be calculated using a method specified by the manufacturer.

[0198] (Adhesive)

[0199] <Preparation of a solution for acrylic adhesive (P-1)>

[0200] In a four-necked flask equipped with a stirrer, reflux condenser, nitrogen inlet tube, and thermometer, 500 g of ethyl acetate was heated in a water bath while nitrogen gas was introduced. Then, a mixture consisting of 360 g of BA (n-butylacrylic acid), 120 g of 2-EHA (2-ethylhexyl acrylic acid), 10 g of AA (acrylic acid), 5 g of HEA (hydroxyethyl acrylate), and 0.5 g of AIBN (azobisisobutyronitrile) as an initiator was added dropwise to the ethyl acetate mixture, and the reaction was carried out under reflux for 8 hours. After the reaction, 110 g of ethyl acetate was added to obtain a solution of (meth)acrylate resin p-1 with a weight average molecular weight (Mw) of 510,000 (45% non-volatile components).

[0201] Then, 100 parts of a solution of (meth)acrylate resin p-1 and 3 parts of an isocyanate-based hardener (Mitsubishi Chemical Corporation (Mytec GP105A): an adduct of toluene diisocyanate and trimethylolpropane) were stirred and mixed, and methyl ethyl ketone was added as a solvent to prepare a solution of acrylic adhesive (P-1) (hereinafter also referred to as adhesive (P-1)) (45% non-volatile component).

[0202] <Preparation of a solution for acrylic adhesive (P-2)>

[0203] In a four-necked flask equipped with a stirrer, reflux condenser, nitrogen inlet tube, and thermometer, 500 g of ethyl acetate was heated in a water bath while nitrogen gas was introduced. Then, a mixture consisting of 120 g of BA (n-butyl acrylate), 360 g of 2-EHA (2-ethylhexyl acrylate), 20 g of AA (acrylic acid), and 0.3 g of AIBN (azobisisobutyronitrile) as an initiator was added dropwise to the ethyl acetate mixture, and the reaction was carried out under reflux for 8 hours. After the reaction, 110 g of ethyl acetate was added to obtain a solution of (meth)acrylate resin p-2 with a weight average molecular weight (Mw) of 800,000 (45% non-volatile components).

[0204] Then, 100 parts of a solution of (meth)acrylate resin p-2 and 3 parts of an isocyanate-based curing agent (Mitsubishi Chemical Corporation (Mytec GP105A): an adduct of toluene diisocyanate and trimethylolpropane) were stirred and mixed, and methyl ethyl ketone was added as a solvent to produce a solution of acrylic adhesive (P-2) (hereinafter also referred to as adhesive (P-2)) (45% non-volatile component).

[0205] <Preparation of a solution for acrylic adhesive (P-3)>

[0206] A solution of acrylic adhesive (P-3) (45% non-volatile component) was prepared by mixing 100 parts of a solution of (meth)acrylate resin p-2, 10 parts of O-130P (manufactured by Adeka Corporation, epoxidized soybean oil), and 3 parts of isocyanate-based hardener (manufactured by Mitsubishi Chemical Corporation (Mytec GP105A: adduct of toluene diisocyanate and trimethylolpropane) with methyl ethyl ketone as a solvent.

[0207] <Preparation of a solution for an elastomer adhesive (P-4)>

[0208] In a four-necked flask equipped with a stirrer, thermometer, reflux cooler, dropping device, and nitrogen inlet tube, 100 parts of Quintac 3270 (manufactured by ZEON Corporation, Japan, with 24% wt% styrene and 67% wt% diblock content), an elastomer, and appropriate amounts of methyl ethyl ketone and toluene were added under a nitrogen atmosphere. The flask was then slowly heated to an internal temperature of approximately 50°C for 3 hours. After heating, the flask was cooled to a temperature below approximately 40°C. Under the stated conditions, 39 parts of YS Polyster T130 (manufactured by Yasuhara Chemical Co., Ltd., softening point 130±5℃, hydroxyl value 60 mgKOH / g), 10 parts of O-130P (manufactured by Adeka Co., Ltd., epoxidized soybean oil), and 2 parts of Irganox 1010 (manufactured by BASF Japan Co., Ltd., anti-aging agent) were added as adhesive-improving resin and diluted with methyl ethyl ketone and toluene. Stirring continued until the adhesive-improving resin dissolved. One part of isocyanate-based curing agent (manufactured by Mitsubishi Chemical Co., Ltd. (Mytec GP105A: adduct of toluene diisocyanate and trimethylolpropane) was then added to obtain a solution of elastomer adhesive (P-4) (hereinafter also referred to as adhesive (P-4)) (40% non-volatile component).

[0209] Manufacturing of the peeling sheet <FA-1>

[0210] As a pre-peeling sheet, a PET peeling sheet "RF2PETCS001-50" (thickness: 50 μm, single-sided silicone peeling treatment, Rc: 0.2 μm) manufactured by IMX Corporation, with a size of approximately 30 cm × 30 cm, was prepared. The pre-peeling sheet was subjected to conditions of temperature: 220°C, pressure: 5 MPa, and speed: 3 m / min, with... Figure 6A The grid pattern shown (area of ​​the grid surface of the mold recess: 2.4 mm) 2 A metal roller (with a mold protrusion line width of 200 μm and a mold protrusion height of 8 μm) passes between a rubber roller and a mold roller to obtain a release sheet FA-1 with the grid pattern transferred on it.

[0211] Using a laser microscope (VK-X100 manufactured by Keyence), the Rc of the outer side of the peeling sheet <FA-1> was measured to be 5.2 μm by the method described above.

[0212] Furthermore, the thickness of the PET release sheet is the average value obtained by measuring any 5 points using a Litematic VL-50B thickness gauge (manufactured by MITUTOYO) with a Φ7.5 mm measuring head and a pressing pressure of 0.01 N.

[0213] Manufacturing of release tablets <FA-2> to <FA-5>

[0214] In addition to further cutting the concave part of the metal roller used in manufacturing the release sheet FA-1 to make the convex part higher, release sheets FA-2 to FA-5 are obtained under the same processing conditions as the release sheet FA-1.

[0215] Manufacturing of the peeling tablet <FA-6>

[0216] Instead of the metal rollers used in manufacturing the FA-1 release sheet, a roller with a surface such as Figure 5A The grid pattern shown, along with the raised sections along the diagonal (the area of ​​the triangular shape representing the mold recess is 0.9 mm). 2 A metal roller (with a mold protrusion line width of 200 μm and a mold protrusion height of 6 μm) passes between a rubber roller and a metal roller under conditions of 220°C, 5 MPa, and 3 m / min to obtain a release sheet FA-6 with the grid pattern transferred on it.

[0217] Manufacturing of release tablets <FA-7> to <FA-10>

[0218] In addition to further cutting the concave part of the metal roller used in manufacturing the release sheet FA-6 to make the convex part higher, release sheets FA-7 to FA-10 are obtained under the same processing conditions as the release sheet FA-6.

[0219] The Rc on the outer side of each stripping sheet FA-1 to stripping sheet FA-10 is described in detail below.

[0220] FA-1: Transferred checkered pattern. Rc: 5.2 μm

[0221] FA-2: Raises the raised portion of the lattice pattern mold used in FA-1 and performs transfer printing. Rc: 7.5 μm

[0222] FA-3: Raises the raised portion of the lattice pattern mold used in FA-1 and performs transfer printing. Rc: 11.1 μm

[0223] FA-4: Raises the raised portion of the lattice pattern mold used in FA-1 and performs transfer printing. Rc: 14.8 μm

[0224] FA-5: Raises the raised portion of the lattice pattern mold used in FA-1 and performs transfer printing. Rc: 18.7 μm

[0225] FA-6: Transfer pattern of checkered and diagonal lines. Rc: 5.4 μm

[0226] FA-7: Raises the raised portions of the molds used in FA-6 for the checkered and diagonal patterns, and then transfers them. Rc: 11.5 μm

[0227] FA-8: Raises the raised portions of the molds used in FA-6 for the checkered and diagonal patterns, and then transfers them. Rc: 14.5 μm

[0228] FA-9: Raises the raised portions of the molds used in FA-6 for the checkered and diagonal patterns, and then transfers them. Rc: 18.1 μm

[0229] FA-10: Raises the raised portions of the molds used in FA-6 for the checkered and diagonal patterns, and then transfers them. Rc: 23.6 μm

[0230] <Flattening Tablets>

[0231] FB-1: RF2PETCS001-50, manufactured by IMX, PET release sheet (thickness: 50 μm, single-sided silicone release treatment, Rc: 0.2 μm)

[0232] <Other peeling tablets>

[0233] FH-21: Using a coil bar, apply BYK's silicone treatment agent "BYK 300" at a concentration of 0.1 g / m³. 2 A film is formed by coating a matte-grade polyester film (Unitika, Emblet "PTH-38") onto the glossy side opposite to the matte side and then creating a release surface. Rc: 0.1 μm

[0234] FH-22: Using a wire rod, apply BYK's silicone treatment agent "BYK 300" at a concentration of 0.1 g / m³.2 A film is formed by coating a matte-grade polyester film (Unitika, Emblet "PTH-38") onto the matte side opposite to the glossy side and then creating a release surface. Rc: 1.5 μm

[0235] FH-23: The release sheet FH-23 is obtained in the same manner as FA-1, except that the temperature during the passage of the pre-release sheet between the metal and rubber rollers is set to 175°C. Rc: 3.2 μm

[0236] FH-24: Raises the raised portion of the lattice pattern mold used in FA-1 and performs transfer printing. Rc: 43.2 μm

[0237] <Sheet substrate F>

[0238] Sheet substrate F-1: PET25 PET film manufactured by Unitika (thickness: 25 μm)

[0239] Sheet substrate F-2: PET75 PET film manufactured by Unitika (thickness: 75 μm)

[0240] Sheet substrate F-3: PET5 PET film manufactured by Unitika (thickness: 5 μm)

[0241] <Example 1> Manufacturing of an adhesive sheet for fixing abrasive pads and an adhesive sheet for fixing abrasive pads with a release tab.

[0242] On the release surface (inner surface) of the release sheet FA-1, a solution of adhesive P-1 is applied using a doctor blade to a thickness of 50 μm after drying. The solution is then dried in an oven at 80°C to form an adhesive layer A-1. On the surface of the adhesive layer A-1, a sheet substrate F-1 is bonded together using a hand roller.

[0243] Separately, on the release surface of the release sheet FB-1, a solution of adhesive P-2 was applied using a doctor blade to achieve a thickness of 50 μm after drying, and then dried in an oven at 80°C to form an adhesive layer B-1.

[0244] Next, the sheet-like substrate F-1, on the side opposite to the adhesive layer A-1, is pressed together with a hand roller to the side opposite to the release tab FB-1 of the adhesive layer B-1, thereby obtaining an adhesive sheet for fixing a polishing pad with a laminated structure of [adhesive layer A-1 / sheet-like substrate F-1 / adhesive layer B-1], wherein the release tab FA-1 is attached to the adhesive layer A-1 and the release tab FB-1 is attached to the adhesive layer B-1.

[0245] Following the method described later, determine the properties of the obtained adhesive sheet (Beck smoothness of the outer surface of the release sheet FA, average height Rc, and cut-off level difference Rδc of the profile curve).

[0246] In addition, the performance of the obtained adhesive sheet (adhesion workability, air expulsion, adhesion, alkali resistance, holding power, and grinding accuracy) is evaluated according to the method described later.

[0247] <Examples 2-10>

[0248] Instead of release sheet FA-1, as shown in Table 1, release sheets for coating adhesive P-1 solution are set as FA-2 to FA-10. Otherwise, in the same manner as in Example 1, an adhesive sheet for fixing abrasive pad with release sheet is obtained.

[0249] <Examples 11-15>

[0250] Instead of release tab FA-1, release tab FA-3 or release tab FA-4 is used. Furthermore, as shown in Table 1, instead of adhesive P-1, adhesive P-4 is used. The thickness of adhesive layer A is changed, or the sheet substrate is changed, or the type or thickness of adhesive layer B is changed. Otherwise, in the same manner as in Example 1, an adhesive sheet for fixing an abrasive pad with release tab is obtained.

[0251] <Comparative Examples 1-4>

[0252] Instead of release sheet FA-1, as shown in Table 1, release sheets for coating adhesive P-1 solution are set as FH-21 to FH-24. Otherwise, in the same manner as in Example 1, an adhesive sheet for fixing abrasive pad with release sheet is obtained.

[0253] [Properties of adhesive sheets]

[0254] <Beck Smoothness>

[0255] The release sheet FB covering the adhesive layer B is peeled off from the abrasive pad fixing adhesive sheet prepared in the examples and comparative examples, and the exposed adhesive layer B is bonded to a 100 μm PET film (Rc: 0.2 μm) and cut to a size of 50 mm square.

[0256] Next, two samples are overlapped, and a hole is formed in the center using a Thomson mold with a radius of 5 mm to create a test sample.

[0257] The test sample was placed on a glass plate with the outer surface of the peeling strip FA of the test sample in contact with the glass plate of the Beck smoothness meter (manufactured by Kumagai Riki Kogyo Co., Ltd.), and the hole of the test sample was located directly above the central circular hole on the glass plate. A rubber pressing plate was placed on the upper surface of the PET film at the top of the test sample. Under a pressure of 0.1 MPa applied via the pressing plate, suction was performed from the bottom of the central circular hole of the glass component to reduce the pressure to -50.7 kPa. After reaching -50.7 kPa, the decompression was stopped, and the time for the change from -50.7 kPa to -48.0 kPa under condition 1 and the time for the change from -50.7 kPa to -29.3 kPa under condition 2 were measured five times. The average value was calculated and then divided by the number of overlapping strips, i.e., 2. In addition, if any of the five measurements exceeded 1000 seconds, the measurement was stopped, which was recorded as ">1000" in the table. In addition, if there is one instance of poor smoothness and measurement time of less than 0.1 seconds in 5 measurements, or if the air inflow is too large and the vacuum degree cannot be raised to -50.7 kPa, it will be recorded as "0" in the table.

[0258] <Rc、Rδc>

[0259] For the surface of the sample being measured, a vapor-deposited film of approximately 20 nm thickness was formed using a vacuum device (MSP15) with a Pt-Pd target and a working time of 1 minute, by means of laser reflection from the outermost surface of the sample using a laser microscope (Keyence VK-X100). Measurements were performed using a laser microscope based on JIS B 0601 (2013).

[0260] [Evaluation of adhesive sheet]

[0261] <Attachment Operation (Position Adjustment)>

[0262] according to Figure 9 Explain the order.

[0263] like Figure 9As shown in (a), the adhesive sheet for fixing the abrasive pad with a release liner prepared in the examples and comparative examples was cut to a size of 210 mm square. The release liner FB was peeled off to expose the adhesive layer B. Under an environment of 23°C-50%RH, it was adhered to a smooth glass plate G1 (approximately 300 g) with a thickness of 3 mm and a square diameter of 200 mm. The adhesive sheet 5 extending from the four sides of the glass plate G1 was removed using a cutter, resulting in a 200 mm square sample (hereinafter referred to as sample) 21 for evaluating the adhesion workability of the structure [glass plate G1 / adhesive sheet 5 / release liner FA]. Furthermore, in Figure 9 The diagrams showing the stacking state of the adhesive sheet and the stacking state of the adhesive sheet and the release sheet FA are omitted.

[0264] like Figure 9 As shown in (b), two types of frames, 200 mm square and 150 mm square, are written on approximately the center of one side of a 300 mm square glass plate, i.e., the substrate G2, to create an evaluation substrate (hereinafter referred to as the substrate).

[0265] like Figure 9 As shown in (c), the release tab FA of sample 21 is peeled off to expose the adhesive layer A, and the sample is placed such that each side of the 200 mm square sample extends at least 10 mm beyond the two sides of the 200 mm square outer frame written on the substrate. Furthermore, the surface on which the sample is placed is the opposite side to the surface with the two frames written on it.

[0266] Immediately after placement, peel the sample off the substrate G2, as follows: Figure 9 As shown in (d), the position was adjusted to match the 200 mm square frame of the object being adhered to, and the time until re-application was measured (placement ~ peeling ~ re-application). Furthermore, five randomly selected individuals performed the work, and each was scored as follows, with the overall score from the five individuals used to evaluate the adhesion performance.

[0267] The score for the application of the adhesive is calculated as follows.

[0268] 3 points: Can be easily aligned with the frame line within 10 seconds.

[0269] 2 points: Can be aligned within 10 seconds to less than 15 seconds.

[0270] 1 point: Can be aligned within 15 seconds to less than 30 seconds.

[0271] 0 points: It will take more than 30 seconds.

[0272] The evaluation criteria for adhesion workability are as follows.

[0273] S: 13-15 points

[0274] A: 10 points-12 points

[0275] B: 7-9 points

[0276] C: 4-6 points

[0277] D: 0-3 points

[0278] <Evaluation of air exhaust performance>

[0279] like Figure 10 As shown in (a), immediately after the evaluation of the adhesion workability, a 500 g weight 22 (41 mm in diameter × 63 mm in height) for a pan balance was placed at the center of each of the five evaluation samples 21, and allowed to stand for 180 seconds. Then, as... Figure 10 As shown in (b), after removing weight 22, the number of air pockets with a diameter of 5 mm or more existing inside the 150 mm square frame line on the side of the adhered object G2 (the back of the 300 mm square glass plate) and the presence or absence of air pockets with a diameter of 10 mm or more are scored as follows. Furthermore, the air expulsion performance is evaluated based on the total score of the 5 pieces.

[0280] The air emission performance score is scored as follows.

[0281] 3 points: There are 0 air pockets with a diameter of 5 mm or more inside the frame.

[0282] 2 points: There are 1 to 2 air accumulation sections with a diameter of 5 mm or more inside the frame, and there are no air accumulation sections with a diameter of 10 mm or more.

[0283] 1 point: There are 3 to 5 air pockets with a diameter of 5 mm or more inside the frame, and there are no air pockets with a diameter of 10 mm or more.

[0284] 0 points: There are more than 5 air pockets with a diameter of 5 mm or more inside the frame, and some of them have an air pocket with a diameter of 10 mm or more.

[0285] The evaluation criteria for air emission performance are as follows.

[0286] S: 13-15 points

[0287] A: 10 points-12 points

[0288] B: 7-9 points

[0289] C: 4-6 points

[0290] D: 0-3 points

[0291] [Preparation of adhesive samples for determining adhesive properties]

[0292] <Evaluation of the initial adhesion of adhesive layer A>

[0293] Under conditions of 23℃-50%RH, the release tab FB was peeled off from the abrasive pad with a release tab, and the exposed adhesive layer B was laminated to a 25 μm PET film. The film was then cut into specimens 25 mm wide and 100 mm long to prepare samples for adhesion evaluation. Subsequently, the release tab FA was peeled off, and the exposed adhesive layer A was overlapped onto a stainless steel plate. A 2 kg roller was used to press adhesive layer A onto the stainless steel plate once, and the plate was left to stand for 24 hours. Then, according to the test method of JIS Z1528:2009, the adhesion of adhesive layer A (to steel use stainless steel, SUS) was measured using a tensile testing machine at a peel angle of 180 degrees and a peel speed of 0.3 m / min under conditions of 23℃ and 50%RH. The obtained test values ​​are shown in Table 1.

[0294] <Evaluation of chemical resistance>

[0295] For the adhesion evaluation sample, the release liner FA was peeled off, and the exposed adhesive layer A was overlapped onto a stainless steel plate. A 2 kg roller was then applied once to press adhesive layer A onto the stainless steel plate. Subsequently, while remaining adhered to the stainless steel plate for no more than 30 minutes, the sample was immersed in a sodium hydroxide aqueous solution with a pH of 11.5 and placed at 60°C for 12 hours. Afterward, the sample was removed from the sodium hydroxide aqueous solution, washed with water, and placed at 23°C and 50% RH for 1 hour.

[0296] The adhesive force is measured using the same method as described in the "Determination of Initial Adhesion Force," and denoted as "Adhesion Force After Impregnation." The difference between the initial adhesive force and the adhesion force after impregnation is calculated. The smaller the difference, the better the chemical resistance.

[0297] The evaluation criteria for chemical resistance are as follows.

[0298] S: The difference in adhesion is less than 1.0 N / 25 mm

[0299] A: The difference in adhesion is greater than 1.0 N / 25 mm and less than 1.5 N / 25 mm.

[0300] B: The difference in adhesion is greater than 1.5 N / 25 mm and less than 2.0 N / 25 mm.

[0301] C: The difference in adhesion is greater than 2.0 N / 25 mm and less than 3.0 N / 25 mm.

[0302] D: The difference in adhesion is 3.0 N / 25 mm or more.

[0303] In CMP processes where various chemicals are used depending on the object being ground, chemical resistance is strongly required. S is the best, A is suitable, B is generally usable, C has limited applications, and D is unusable.

[0304] <Evaluation of retention>

[0305] For the adhesion evaluation sample, the release tab FA was peeled off, and only a 25 mm wide × 25 mm long area of ​​the exposed adhesive layer A was overlapped onto the stainless steel plate. A 2 kg roller was then applied back and forth once to press adhesive layer A onto the stainless steel plate. Afterward, the sample was placed at 23°C and 50% RH for 20 minutes. Subsequently, at 80°C, a 1 kg weight was added to the end of the sample not adhered to the stainless steel plate, and the sample was placed in a 180-degree direction. After 24 hours, the displacement of the adhesion position (in mm) was measured. Additionally, in the case where the sample completely shifted from the adhered object and fell, the time until it fell to the ground was measured.

[0306] The evaluation criteria for retention force are as follows.

[0307] S: Offset less than 0.1 mm

[0308] A: 0.1 mm or more and less than 1.0 mm

[0309] B: Offset greater than 1.0 mm and less than 5.0 mm

[0310] C: Falling after 180 minutes

[0311] D: Falling within 180 minutes

[0312] The smaller the offset, the less likely it is to shift or peel off during grinding, thus firmly fixing the grinding pad and making it suitable for various grinding processes. S is the best, A is suitable, B is generally usable, C has limited applications, and D is unusable.

[0313] <Grounding area ratio of adhesive layer A>

[0314] On the peeling surface of the peeling sheet FB, which is cut into 4 cm squares, Pt-Pd is vapor-deposited using a vacuum vapor deposition apparatus (JEOL Ltd.) to form a vapor-deposited film.

[0315] The release sheet FA of the adhesive sheet, which is cut into 3 cm squares, is peeled off to expose the adhesive layer A. The adhesive layer A is then bonded to the vapor-deposited film of the release sheet FB, which is cut into 4 cm squares, using a hand roller. The 2 kg roller is then pressed back and forth once to prepare the test sample.

[0316] The interface between the adhesive layer A and the 4 cm square exfoliated slide FB was examined using a digital microscope (Keyence) through the 4 cm square exfoliated slide FB, with a coaxial light source and 20x magnification (field of view approximately 1.0 cm²). 2 Observe and take 3 photos. For the 3 photos, use image processing software (GNU Image Manipulation Program (GIMP)) to perform monochrome and binarization, calculate the area ratio of the part of the vapor-deposited film (represented by black) that is in close contact with the adhesive layer A and the part that is not in close contact, and calculate the arithmetic mean as the grounding area ratio (%).

[0317] <Evaluation of batch variation in grinding>

[0318] Peel off the release tab FB from the adhesive sheet used to fix the abrasive pad with the release tab. On the exposed adhesive layer B, overlap the non-abrasive surface of the abrasive pad (CMP cloth manufactured by Musashino-Denshi, Φ200 mm, standard type). The abrasive pad with the adhesive sheet is made by bonding under the conditions of roller temperature: 80°C, pressure: 0.1 MPa, and speed: 1.0 m / min.

[0319] Using the MA-200 manufactured by Musashino-Denshi as a polishing device, the release liner FA was peeled off from the prepared polishing pad with adhesive pads, and the exposed adhesive layer A was attached to the aluminum plate. Polishing was performed under the following conditions.

[0320] (condition)

[0321] Table speed: 100 rpm

[0322] Head speed: 105 rpm

[0323] Polishing object: A test piece made by cutting a 200 mm wafer (75 μm thick) with a polycrystalline silicon layer (500 nm) on its surface into 3 cm square pieces.

[0324] Grinding pressure: 10.0 kPa

[0325] Grinding time: 15 min

[0326] Polishing slurry: Colloidal silica polishing slurry #80 manufactured by Musashino-Denshi Co., Ltd.

[0327] The ground test piece was washed with water, and air was blown onto the surface to remove water droplets. Then, the thickness of a point in the center of the test piece was measured using an Otsuka Electronics FE-300 film thickness measuring instrument.

[0328] Without changing the grinding pad, only 10 grinding objects were replaced and grinding was carried out under the same conditions. The thickness of the 10 test pieces after grinding was measured, and the difference between the maximum and minimum film thickness was calculated. The evaluation was carried out according to the following criteria.

[0329] S: less than 40 nm

[0330] A: Above 40 nm and below 60 nm

[0331] B: 60 nm or higher and less than 80 nm

[0332] C: 80 nm or higher and less than 100 nm

[0333] In the repeated use of polishing pads for CMP polishing requiring precision, case S is the best, case A is suitable, case B is generally usable, and case C is unusable.

[0334] [Table 1]

[0335]

[0336] In addition, this disclosure also discloses the manufacturing method of the adhesive sheet for fixing the abrasive pad described below

[13] to

[15] .

[0337]

[13] A method for manufacturing an adhesive sheet for fixing an abrasive pad with release tabs FA and FB, comprising a release tab FA, an adhesive layer A, a sheet substrate, an adhesive layer B, and a release tab FB, wherein the method comprises an adhesive sheet for fixing an abrasive pad with release tabs FA and FB.

[0338] The manufacturing method comprises the following steps (1) to (4):

[0339] (1) A process of applying adhesive a to the surface of a release sheet FA, which has a regular and fixed shape when viewed from above and has an average height Rc of 5 μm to 25 μm of the surface after the release treatment, to form an adhesive layer A.

[0340] (2) The process of overlapping sheet substrates on the surface of the adhesive layer A that is not in contact with the release sheet FA.

[0341] (3) The process of applying adhesive b to the peeled surface of the release sheet FB to form an adhesive layer B.

[0342] (4) The process of overlapping the surface of the adhesive layer B, which is not in contact with the adhesive layer A, with the surface of the adhesive layer B, which is not in contact with the release sheet FB.

[0343] The surface of adhesive layer A that is not in contact with the sheet substrate has unevenness. In the Beck smoothness test...

[0344] The smoothness of the surface determined under the following condition 1 is 0.1 seconds to 30 seconds.

[0345] The smoothness of the surface determined under the following condition 2 is 1 second to 500 seconds.

[0346] Condition 1: The time it takes for the pressure to change from -50.7 kPa to -48.0 kPa.

[0347] Condition 2: The time it takes for the pressure to change from -50.7 kPa to -29.3 kPa.

[0348]

[14] : A method for manufacturing an adhesive sheet for fixing an abrasive pad with release tabs FA and FB, comprising a release tab FA, an adhesive layer A, a sheet-like substrate, an adhesive layer B, and a release tab FB, wherein the adhesive sheet for fixing an abrasive pad with release tabs FA and FB is manufactured.

[0349] The manufacturing method comprises the following steps (5) to (8):

[0350] (5) The process of applying adhesive a to one side of a sheet substrate to form an adhesive layer A.

[0351] (6) The process of the surface of the release sheet FA, which is not in contact with the adhesive layer A and has a regular and well-defined shape when viewed from above, and whose average height Rc of the uneven surface after peeling is 5 μm to 25 μm.

[0352] (7) The process of applying adhesive b to the peeled surface of the release sheet FB to form an adhesive layer B.

[0353] (8) The process of overlapping the surface of the adhesive layer B, which is not in contact with the adhesive layer A, with the surface of the adhesive layer B, which is not in contact with the release sheet FB.

[0354] The surface of adhesive layer A that is not in contact with the sheet substrate has unevenness. In the Beck smoothness test...

[0355] The smoothness of the surface determined under the following condition 1 is 0.1 seconds to 30 seconds.

[0356] The smoothness of the surface determined under the following condition 2 is 1 second to 500 seconds.

[0357] Condition 1: The time it takes for the pressure to change from -50.7 kPa to -48.0 kPa.

[0358] Condition 2: The time it takes for the pressure to change from -50.7 kPa to -29.3 kPa.

[0359]

[15] : A method for manufacturing an adhesive sheet for fixing an abrasive pad with release tabs FA and FB, comprising a release tab FA, an adhesive layer A, a sheet substrate, an adhesive layer B, and a release tab FB, wherein the manufacturing method comprises the following steps (9) to (12).

[0360] (9) The process of applying adhesive b to the peeled surface of the release sheet FB to form an adhesive layer B.

[0361] (10) A process of overlapping sheet substrates on the surface of the adhesive layer B that is not in contact with the release sheet FB.

[0362] (11) A process of applying adhesive a to the surface of a release sheet FA, which has a regular and fixed shape when viewed from above in the concave part of the surface and has an average height Rc of 5 μm to 25 μm of the surface after the release treatment, to form an adhesive layer A.

[0363] (12) The process of overlapping the surface of the adhesive layer A that is not in contact with the release sheet FA on the surface of the sheet substrate that is not in contact with the adhesive layer B.

[0364] The surface of adhesive layer A that is not in contact with the sheet substrate has unevenness. In the Beck smoothness test...

[0365] The smoothness of the surface determined under the following condition 1 is 0.1 seconds to 30 seconds.

[0366] The smoothness of the surface determined under the following condition 2 is 1 second to 500 seconds.

[0367] Condition 1: The time it takes for the pressure to change from -50.7 kPa to -48.0 kPa.

[0368] Condition 2: The time it takes for the pressure to change from -50.7 kPa to -29.3 kPa.

[0369] This application claims priority based on Japanese Patent Application No. 2025-067225, filed on April 16, 2025, the entire contents of which are incorporated herein by reference.

[0370] Explanation of icon numbers

[0371] 1: Adhesive pad for fixing abrasive pads with release tabs FA

[0372] 2: Adhesive pads for fixing abrasive pads with release tabs FA and FB

[0373] 3: Abrasive pad with release plate FA

[0374] 4: Abrasive pad with adhesive pad for fixing abrasive pad

[0375] 5: Adhesive sheet for fixing grinding pad

[0376] A: Adhesive layer A

[0377] FA: Release sheet covering the surface of adhesive layer A

[0378] FA': Pre-peeling sheet

[0379] B: Adhesive layer B

[0380] FB: Release sheet covering the surface of adhesive layer B

[0381] F: Sheet substrate

[0382] PP: Abrasive pad

[0383] R1: Metal roller

[0384] R2: Rubber roller

[0385] SP: Platform

[0386] E: Rubber pressing plate

[0387] G: Glass components

[0388] H: Pressure plate

[0389] PET: PET film

Claims

1. An adhesive sheet for fixing an abrasive pad with a release tab FA, comprising an adhesive layer A on one side of a sheet-like substrate and an adhesive layer B on the other side of the sheet-like substrate, wherein the surface of the adhesive layer A that is not in contact with the sheet-like substrate is in contact with the release tab FA. The adhesive sheet for fixing the abrasive pad with the release tab FA is characterized in that: The protrusions on the outer surface of the peeling strip FA have a regular and well-defined shape when viewed from above. The average height Rc of the unevenness on the outer surface of the release tab FA is 5 μm to 25 μm, and the outer surface of the release tab FA has the same shape as the inner surface of the release tab FA after being reversed. The release tab FA is made of plastic. The outer surface of the release tab FA, which is not in contact with the adhesive layer A, has irregularities. In the Beck smoothness test, The smoothness of the outer surface of the release tab FA, determined under the following condition 1, is 0.1 seconds to 30 seconds. The smoothness of the outer surface of the release detachment FA, determined under the following condition 2, is between 1 second and 500 seconds. Condition 1: The time it takes for the pressure to change from -50.7 kPa to -48.0 kPa. Condition 2: The time it takes for the pressure to change from -50.7 kPa to -29.3 kPa.

2. The adhesive sheet for fixing the abrasive pad with a tape-separation sheet FA according to claim 1, characterized in that, The thickness of the release strip FA is 25 μm to 100 μm.

3. The adhesive sheet for fixing the abrasive pad with a tape peel sheet FA according to claim 1, characterized in that, The average height Rc of the unevenness on the outer surface of the release strip FA is 5 μm to 25 μm, and the average height Rc of the unevenness on the inner surface of the release strip FA is 5 μm to 25 μm.

4. The adhesive sheet for fixing the abrasive pad with a dicing sheet FA according to claim 1, characterized in that, The cutting level difference Rδc of the uneven contour curve of the outer surface of the stripper FA is 1 μm to 10 μm.

5. The adhesive sheet for fixing the abrasive pad with a tape peel sheet FA according to claim 1, characterized in that, The adhesive layer A is an acrylic adhesive layer.

6. The adhesive sheet for fixing the abrasive pad with a release tab FA according to any one of claims 1 to 3, wherein it is wound into a roll and the length of the roll in the width direction is 1000 mm or less.

7. An adhesive sheet for fixing a polishing pad with a tape peeling sheet FA and a peeling sheet FB, characterized by It comprises: an adhesive sheet for fixing an abrasive pad with a release tab FA as described in any one of claims 1 to 3, and a release tab FB. The surfaces of the release tab FB and the adhesive layer B that are not in contact with the sheet-like substrate are in contact. The release tab FB is made of plastic.

8. The adhesive sheet for fixing the abrasive pad with release tabs FA and FB according to claim 7, wherein the sheet is wound into a roll and the length of the roll in the width direction is 1000 mm or less.

9. The adhesive sheet for fixing the abrasive pad with release tabs FA and FB according to claim 7, wherein, The length of the shorter side is less than 1000 mm.

10. An abrasive pad with a release tab FA and an adhesive layer A, comprising an abrasive pad and an adhesive layer for fixing the abrasive pad with a release tab FA as described in any one of claims 1 to 5, wherein, The abrasive pad is in contact with the adhesive layer B.

11. A method for fixing an abrasive pad to a platform via an adhesive sheet, characterized in that: Peel off the release tab FA from the abrasive pad with release tab FA and adhesive layer A as described in claim 10, and attach the adhesive layer A to the platform.

Citation Information

Patent Citations

  • Double-sided adhesive tape for fixing polishing pad

    JP2011122069A

  • Double-sided adhesive tape for polishing cloth fixing, and pad for polishing cloth fixing

    JP2011168714A

  • Double-sided adhesive tape and grinding member

    JP2012057135A

  • Information display device

    JP2025067225A