Manufacturing method of composite thermal storage element

By preparing alumina-based waste catalyst powder with a particle size of 30μm or larger and less than 150μm, and combining it with alumina-based binders and auxiliary additives, a composite thermal storage element was manufactured, which solved the problems of efficient removal and thermal storage performance of perfluorinated compounds, and achieved low-temperature decomposition and improved stability.

CN123125445APending Publication Date: 2026-11-17ECOPROHN CO LTD CHEONGJU SI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580028177.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-04-01
Filing Date
2025-04-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, perfluorinated compounds emitted during semiconductor manufacturing processes are difficult to remove effectively, and catalytic decomposition methods suffer from high energy consumption and frequent catalyst replacement.

Method used

A composite thermal storage element with a particle size of 30 μm or larger and less than 150 μm was prepared by grinding alumina-based waste catalyst. This element was then combined with alumina-based binder and auxiliary additives to prepare a composite thermal storage element for decomposing perfluorinated compounds at low temperatures. The composite thermal storage element with thermal storage function was then formed by extrusion molding, drying, and calcination.

Benefits of technology

It achieves high decomposition efficiency and excellent heat storage performance of perfluorinated compounds, extends catalyst life, reduces operating costs, and improves the stability and economy of harmful gas removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125445A_ABST
    Figure CN123125445A_ABST
Patent Text Reader

Abstract

The method for manufacturing a composite thermal storage element according to an embodiment of the present invention includes the following steps: grinding an alumina-based waste catalyst to prepare powder with a particle size (D90) of 30 μm or more and less than 150 μm; heat-treating the powder; mixing an alumina-based binder with the heat-treated powder to prepare a first mixed solution; mixing the first mixed solution, a solvent, and an acidic solution to prepare a second mixed solution; extruding the second mixed solution to prepare a pre-composite thermal storage element; and drying and calcining the pre-composite thermal storage element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing a composite thermal storage element. Background Technology

[0002] Hazardous emissions from semiconductor manufacturing processes are highly diverse and primarily consist of highly volatile components that are harmful to humans or have a high global warming potential. In particular, perfluorinated compounds (PFCs) emitted during etching and deposition processes are chemically very stable and difficult to remove. PFCs accumulate in the atmosphere due to their high global warming potential and long atmospheric lifetimes, and their emissions from semiconductor manufacturing processes are increasing year by year. Therefore, regulations concerning PFCs are being strengthened globally.

[0003] To date, no alternative gas has been developed that offers higher etching efficiency and superior process performance than carbon tetrafluoride (CF4) used for etching silicon substrates. Therefore, CF4 continues to be used in semiconductor processes.

[0004] Catalytic decomposition is a technique for decomposing perfluorinated compounds; however, because the catalysts used in this method require decomposition reactions at temperatures above 700°C in a reactor, continuous operation costs exceeding predetermined levels can occur, leading to high energy consumption. Furthermore, the cost may increase if specific metals or compounds are used to prepare the catalyst.

[0005] Catalytic decomposition is a technology that uses catalysts and steam to decompose difficult-to-decompose PFCs at low temperatures below 800°C. Conventional devices for decomposing harmful gases such as perfluorinated compounds are constructed by receiving a heat storage element and a catalyst in a chamber, and supplying the harmful gas into the chamber for decomposition. However, the catalyst used to stably remove harmful gases should be replaced at regular intervals, resulting in the disposal of spent catalyst. If the catalyst is not replaced at regular intervals, the efficiency of harmful gas removal decreases.

[0006] Therefore, there is a need to develop a composite thermal storage element that can solve the problems of waste catalyst generation, stable removal of harmful gases, and improvement of the service life of catalysts and devices. Summary of the Invention

[0007] The problem the invention aims to solve

[0008] One object of the present invention is to provide a method for manufacturing a composite thermal storage element that can effectively decompose perfluorinated compounds and has excellent thermal storage performance.

[0009] Solution for solving the problem

[0010] A method for manufacturing a composite thermal storage element according to an exemplary embodiment of the present disclosure includes: grinding an alumina-based waste catalyst to prepare powder with a particle size (D90) of 30 μm or more and less than 150 μm; heat-treating the powder; mixing an alumina-based binder with the heat-treated powder to prepare a first mixed solution; mixing the first mixed solution, a solvent, and an acidic solution to prepare a second mixed solution; extruding the second mixed solution to prepare a pre-composite thermal storage element; and drying and calcining the pre-composite thermal storage element.

[0011] According to an exemplary implementation, the number of channels per square inch (CPSI) of the composite thermal storage element can be 30 to 70.

[0012] According to an exemplary embodiment, the content of alumina-based waste catalyst can be from 50% to 95% by weight, based on the total weight of the first mixed solution.

[0013] According to an exemplary embodiment, the content of the alumina-based binder may be less than 30% by weight, based on the total weight of the first mixed solution.

[0014] According to an exemplary embodiment, the alumina-based binder may include at least one selected from the group consisting of α-alumina (α-Al2O3), β-alumina (β-Al2O3), γ-alumina (γ-Al2O3), δ-alumina (δ-Al2O3), θ-alumina (θ-Al2O3), κ-alumina (κ-Al2O3), and boehmite.

[0015] According to an exemplary embodiment, the first mixed solution may further include auxiliary additives.

[0016] According to an exemplary embodiment, the content of auxiliary additives may be less than 30% by weight, based on the total weight of the first mixed solution.

[0017] According to an exemplary embodiment, the auxiliary additive may include at least one selected from the group consisting of: tungsten-containing compounds, lanthanum-containing compounds, silica, zeolite, cordierite, mullite, silica-alumina, titanium dioxide, magnesium oxide, Fe2O3 / TiO2, Fe2O3 / Al2O3, MgO / TiO2, ZrO2 / Al2O3, ZrO x / TiO2, CeO2 / TiO2, CeO2 / ZrO2 and V2O5 / TiO2.

[0018] According to an exemplary embodiment, the heat treatment temperature in the step of heat treating the powder can be above 200°C.

[0019] According to an exemplary embodiment, the calcination temperature in the step of drying and calcining the prepared composite thermal storage element can be above 600°C.

[0020] The effects of the invention

[0021] The composite thermal storage element manufactured by the method according to an embodiment of the present invention exhibits high decomposition efficiency of perfluorinated compounds and excellent heat capacity and strength. Furthermore, by recycling spent catalyst as the composite thermal storage element, it provides economic and environmental advantages.

[0022] When composite thermal storage elements are applied to hazardous gas removal devices, the perfluorinated compound removal performance is also imparted to the thermal storage stage, which improves catalyst life and the stability of the hazardous gas removal performance. Furthermore, by recovering heat, the energy required to maintain the temperature can be reduced. Attached Figure Description

[0023] Figure 1 This is a schematic flowchart of a method for manufacturing a composite thermal storage element according to an exemplary embodiment.

[0024] Figure 2 and Figure 3 This is a schematic diagram illustrating the honeycomb structure of a composite thermal storage element according to an exemplary embodiment.

[0025] Figure 4 This is a schematic diagram illustrating a reactor including a composite thermal storage element assembly according to an exemplary embodiment.

[0026] Figure 5 This is a photograph showing the evaluation results of the shape stability of a composite thermal storage element according to an exemplary embodiment.

[0027] Figure 6 These are a set of photographs showing the evaluation results of the shape stability of the composite thermal storage element according to Comparative Example 2.

[0028] Figure 7 These are a set of photographs showing the evaluation results of the shape stability of the composite thermal storage element according to Comparative Example 1. Detailed Implementation

[0029] The present disclosure will be described in detail below with reference to the accompanying drawings. However, this is merely illustrative, and the present disclosure is not limited to the specific embodiments described herein.

[0030] An exemplary embodiment of this disclosure provides a method for manufacturing a composite thermal storage element, the method comprising: grinding an alumina-based waste catalyst to prepare powder with a particle size (D90) of 30 μm or more and less than 150 μm; heat-treating the powder; mixing an alumina-based binder with the heat-treated powder to prepare a first mixed solution; mixing the first mixed solution, a solvent, and an acidic solution to prepare a second mixed solution; extruding the second mixed solution to prepare a pre-composite thermal storage element; and drying and calcining the pre-composite thermal storage element.

[0031] The term "alumina-based waste catalyst" can refer to catalysts used in downstream processes of semiconductor manufacturing and subsequently discarded. Specifically, alumina-based waste catalysts can refer to catalysts used to remove perfluorinated compounds generated in semiconductor manufacturing processes used to manufacture memory devices or LCDs, etc.

[0032] Examples of perfluorinated compounds may include fully fluorinated compounds such as CF4, C2F6, C3F8, and C4F6. 10 Hydrofluoric compounds, such as CHF3, CH2F2, C2HF5, C3HF7, and C4HF9; and perfluorooctanoic acid, perfluorosulfonic acid, perfluorobutyric acid, and perfluorononanoic acid. For example, perfluorinated compounds may include compounds generated from etching gases used in etching processes or reactor cleaning gases used in chemical vapor deposition processes. In one embodiment, the perfluorinated compound may include CF4.

[0033] The manufacturing method of composite thermal storage elements can reduce raw material costs by using alumina-based waste catalysts, thus providing an economic advantage and minimizing negative environmental impacts, such as improving greenhouse gas reduction efficiency by reducing waste generation. Furthermore, high thermal stability and heat transfer efficiency can be achieved by using alumina-based waste catalysts.

[0034] Although conventional catalysts for decomposing perfluorinated compounds (PFCs) do not have heat storage capabilities, composite heat storage elements manufactured by the method of manufacturing composite heat storage elements according to exemplary embodiments of the present disclosure have catalytic capabilities that exhibit high decomposition efficiency for perfluorinated compounds (PFCs) and can also have heat storage capabilities in regenerative catalytic systems (RCS).

[0035] Since the decomposition of perfluorinated compounds (PFCs) using catalysts takes place in the reactor at temperatures above 700°C, continuous operating costs are incurred. In contrast, composite thermal storage elements manufactured by a method of manufacturing composite thermal storage elements according to an exemplary embodiment of this disclosure can significantly reduce the operating costs required to maintain the reactor temperature by recovering heat through their thermal storage performance.

[0036] Furthermore, the composite thermal storage element manufactured by the method of manufacturing the composite thermal storage element according to the exemplary embodiment of the present disclosure has excellent decomposition efficiency for perfluorinated compounds, thereby helping to extend the catalyst life and enhance the stability of perfluorinated compound decomposition within the device.

[0037] In one embodiment, in the step of grinding the alumina-based spent catalyst to prepare powder with a particle size (D90) of 30 μm or more and less than 150 μm, a pin mill, ball mill, jet mill, or hammer mill can be used for grinding. The grinding conditions are not particularly limited, as long as it is possible to prepare powder with a particle size (D90) of 30 μm or more and less than 150 μm by grinding the alumina-based spent catalyst.

[0038] In one embodiment, the particle size (D90) can be 30 μm or more, 40 μm or more, 50 μm or more, or less than 150 μm, 145 μm or less, 140 μm or less, 130 μm or less, 120 μm or less, 110 μm or less, or 100 μm or less.

[0039] When the particle size (D90) of the powder meets the above range, the shape stability of the composite thermal storage element can be maintained, and surface cracks can be minimized.

[0040] In one embodiment, the heat treatment temperature in the step of heat treating the powder can be above 200°C.

[0041] For example, the heat treatment temperature can be 200℃.

[0042] When the heat treatment temperature meets the above range, the reactivity and reaction efficiency of the powder can be improved.

[0043] In one embodiment, the heat treatment time in the step of heat-treating the powder can be 4 hours or more. For example, the heat treatment time can be 4 hours.

[0044] When the heat treatment time meets the above range, the reactivity and reaction efficiency of the powder can be improved.

[0045] In one embodiment, the content of alumina-based waste catalyst may be from 50% by weight (“wt%”) to 95 wt% based on the total weight of the first mixed solution.

[0046] For example, based on the total weight of the first mixed solution, the content of alumina-based waste catalyst can be 55 wt% to 90 wt% or 60 wt% to 90 wt%.

[0047] When the content of alumina-based spent catalyst meets the above-mentioned range, the strength of the composite thermal storage element can be improved, as can its perfluorinated compound decomposition performance. For example, when the content of alumina-based spent catalyst is less than 50 wt%, the amount of active material per unit area capable of decomposing perfluorinated compounds decreases, which may reduce the perfluorinated compound decomposition performance of the composite thermal storage element. Conversely, when the content of alumina-based spent catalyst exceeds 90 wt%, the amount of active material per unit area increases, which can improve the perfluorinated compound decomposition performance; however, the bonding strength between the raw materials may be insufficient, thereby reducing the strength of the composite thermal storage element.

[0048] In one embodiment, the content of the alumina-based binder may be less than 30 wt% based on the total weight of the first mixed solution.

[0049] In one embodiment, the content of the alumina-based binder may be more than 5 wt%, more than 10 wt%, or more than 20 wt%, based on the total weight of the first mixed solution.

[0050] When the content of alumina-based binder meets the above range, the strength of the composite thermal storage element can be improved, and the density of the composite thermal storage element can be increased, thereby increasing the heat capacity.

[0051] In one embodiment, the alumina-based binder may include at least one selected from the group consisting of α-alumina (α-Al2O3), β-alumina (β-Al2O3), γ-alumina (γ-Al2O3), δ-alumina (δ-Al2O3), θ-alumina (θ-Al2O3), κ-alumina (κ-Al2O3), and boehmite.

[0052] In one embodiment, the alumina-based binder may include two or more alumina-based compounds with different crystal structures.

[0053] In one embodiment, the alumina-based binder may include at least one of α-alumina (α-Al2O3) and γ-alumina (γ-Al2O3).

[0054] In one embodiment, the alumina-based binder may include α-alumina (α-Al2O3) and γ-alumina (γ-Al2O3).

[0055] In one embodiment, the alumina-based binder may include α-alumina (α-Al2O3).

[0056] In one embodiment, the first mixed solution may also include auxiliary additives.

[0057] For example, auxiliary additives may include compounds selected from tungsten-containing compounds, lanthanum-containing compounds, silica, zeolites, cordierite, mullite, silica-alumina, titanium dioxide, magnesium oxide, Fe2O3 / TiO2, Fe2O3 / Al2O3, MgO / TiO2, ZrO2 / Al2O3, and ZrO2. x At least one of the group consisting of / TiO2, CeO2 / TiO2, CeO2 / ZrO2 and V2O5 / TiO2.

[0058] For example, tungsten-containing compounds can be W2O3, and lanthanum-containing compounds can be La2O3, but are not limited to these.

[0059] In one embodiment, the content of auxiliary additives may be less than 30 wt% based on the total weight of the first mixed solution.

[0060] For example, based on the total weight of the first mixed solution, the content of auxiliary additives can be more than 1 wt%, more than 3 wt%, or more than 5 wt%, and can be less than 25 wt%, less than 20 wt%, or less than 15 wt%.

[0061] When the content of auxiliary additives meets the above range, it can improve the strength of the composite thermal storage element and maintain the shape of the composite thermal storage element in a stable manner during drying and calcination.

[0062] In one embodiment, the second mixed solution may include the first mixed solution, a solvent, and an acidic solution.

[0063] In one implementation, the solvent may be water.

[0064] In one embodiment, the acidic solution may be a sulfuric acid solution.

[0065] In one embodiment, the type of acid is not limited, as long as the pH of the acidic solution is 5. For example, the acidic solution may include nitric acid, hydrochloric acid, or acetic acid.

[0066] In one embodiment, the solvent content may be 30 wt% to 70 wt% or 50 wt% to 60 wt% based on the total weight of the second mixed solution.

[0067] In one embodiment, based on the total weight of the second mixed solution, the content of the acidic solution can be appropriately adjusted to a range of 0.1 wt% to 5 wt%, such that the pH of the second mixed solution is below 5.

[0068] In one embodiment, in the step of manufacturing a preparative composite thermal storage element by extruding a second mixed solution, the extrusion molding conditions can be appropriately adjusted to meet the particle size of the composite thermal storage element and the number of channels per square inch (CPSI) of the composite thermal storage element.

[0069] In one embodiment, the dryer used for drying the preparatory composite thermal storage element can be a microwave dryer, a hot air dryer, a dielectric dryer, a pressure-reducing dryer, or a vacuum dryer, etc.

[0070] In one implementation, the drying temperature and time can be appropriately adjusted to meet the particle size of the composite thermal storage element and the number of channels per square inch (CPSI) of the composite thermal storage element.

[0071] In one embodiment, the steps of drying and calcining the prepared composite thermal storage element may further include degreasing the prepared composite thermal storage element after drying. Degreasing may be carried out at 400°C for 2 hours.

[0072] In one embodiment, the calcination temperature in the drying and calcination steps of preparing the composite thermal storage element can be above 600°C.

[0073] For example, the calcination temperature can be below 1000℃. For example, the calcination temperature can be between 600℃ and 1000℃ or between 700℃ and 900℃.

[0074] For example, the calcination time in the calcination step can be 2 to 5 hours.

[0075] Figure 2 and Figure 3 This is a schematic diagram illustrating the structure of a composite thermal storage element according to an exemplary embodiment. For example, Figure 3 This is a plan view showing the upper surface of a composite thermal storage element according to an exemplary embodiment.

[0076] In this specification, "height direction" can indicate the direction in which the channel is formed. For example, the height direction can indicate the direction in which a gas containing a perfluorinated compound passes. For example, the height direction can indicate a direction perpendicular to... Figure 3 The directions of the x-axis and y-axis.

[0077] refer to Figure 2 The composite thermal storage element 100 may have a honeycomb shape including a plurality of channels 105. For example, the composite thermal storage element 100 (hereinafter also referred to as "catalyst") may include a body 101, a plurality of channels 105 and separators 106 defining the channels 105.

[0078] In one embodiment, when the perfluorinated compound passes through the composite thermal storage element 100, the contact area between the perfluorinated compound and the catalyst 100 through multiple channels 105 can be increased, thereby improving the decomposition efficiency of the perfluorinated compound.

[0079] According to an exemplary embodiment, a plurality of channels 105 can penetrate from one surface of the body to an opposite surface of the body. For example, channel 105 can penetrate from a first surface 110 to a second surface 120.

[0080] According to an exemplary embodiment, channel 105 may be formed in the height direction. For example, the first surface 110 and the second surface 120 may be fluidly connected through channel 150.

[0081] According to an exemplary embodiment, the channel 105 may have a constant cross-sectional shape in the height direction. For example, when the side 150 of the catalyst 100 is cut in a height direction parallel to the first surface 110 and the second surface 120, the cross-sectional shape of the channel 105 may be the same as the cross-sectional shape of the channel at the first surface 110 and / or the cross-sectional shape of the channel at the second surface 120. A gas containing a perfluorinated compound may pass through the plurality of channels 105 of the catalyst 100.

[0082] The cross-sectional shape of channel 105 is not limited to Figure 2 The cross-sectional shape shown. For example, the cross-sectional shape of channel 105 can be triangular, rectangular, square, trapezoidal, rhomboid, hexagonal, elliptical, or circular. Considering the contact area between the gas and the composite thermal storage element 100, the flow rate, the density of the catalyst material contained in the composite thermal storage element 100, and the strength of the composite thermal storage element 100, the cross-section of channel 105 can be formed in the shape of triangle, quadrilateral, or hexagon.

[0083] According to an exemplary embodiment, multiple channels 105 may be defined by separators 106.

[0084] In an exemplary embodiment, the body 101 and the separator 106 may be made of the same material.

[0085] In some implementations, each of the plurality of channels 105 may be spaced apart at regular intervals. For example, the channels 105 may be spaced apart in a direction perpendicular to the height direction by an amount corresponding to the thickness of the separator 106.

[0086] In one embodiment, the cross-section of each of the plurality of channels 105 may be quadrilateral, and the distance between the plurality of channels 105 (e.g., Figure 3 L2 in the text can be the same.

[0087] In an exemplary embodiment, the efficiency of the catalyst 100 in decomposing perfluorinated compounds can be further improved by adjusting the shape and number of channels 105.

[0088] In an exemplary embodiment, the diameter of channel 105 can be measured at the opening of the channel defined by the first surface 110 or the second surface 120. For example, the diameter of the channel can be measured from a cross-section of channel 105 at the first surface 110.

[0089] In one implementation, the number of channels per square inch (CPSI) of the composite thermal storage element can be 30 to 70.

[0090] For example, the number of channels per square inch (CPSI) of a composite thermal storage element can be 30 to 100, 30 to 90, 30 to 80, or 30 to 60.

[0091] When the number of channels per square inch (CPSI) of the composite thermal storage element meets the above-mentioned range, excellent strength can be maintained without pressure loss. Furthermore, the contact area with perfluorinated compounds can be increased, and catalytic activity per unit time can be increased by maintaining gas flow.

[0092] For example, when the number of channels per square inch (CPSI) of a composite thermal storage element is less than 30, the surface area supporting the catalyst layer on top of the composite thermal storage element decreases, which may reduce the strength of the product. When the number of channels per square inch (CPSI) of a composite thermal storage element exceeds 100, the pressure loss within the regeneration catalytic system using the composite thermal storage element increases, which may reduce operating efficiency.

[0093] In this specification, the number of channels per square inch can be a value measured from a cross-section perpendicular to the height of the channels of the composite thermal storage element 100.

[0094] To improve the catalyst's lifespan and decomposition efficiency, the structure of the composite thermal storage element 100 can be adjusted. The structure of the composite thermal storage element 100 can be adjusted within a range that maintains porosity, density, and strength.

[0095] For example, the composite thermal storage element 100 may have a width and length of 10 mm to 30 mm. The width and length may refer to the width and length of the first surface 110 or the second surface 120. For example, the height of the composite thermal storage element 100 may be 10 mm to 25 mm. The above-mentioned length is exemplary, and the size of the composite thermal storage element 100 is not limited thereto.

[0096] In an exemplary embodiment, the composite thermal storage element 100 may include a catalyst material containing a metal oxide having catalytic activity for decomposing perfluorinated compounds.

[0097] According to an exemplary embodiment, catalyst 100 may include a catalyst material with catalytic activity.

[0098] In some implementations, the composite thermal storage element 100 may be an integrally formed structure.

[0099] In an exemplary embodiment, multiple composite thermal storage elements 100 may be stacked to form a composite thermal storage element assembly 200 (hereinafter also referred to as a “catalyst assembly”).

[0100] Figure 4 This is a schematic diagram illustrating a reactor including a composite thermal storage element assembly 200 according to an exemplary embodiment.

[0101] refer to Figure 4 The reactor 200 may include a chamber 210 and a composite thermal storage element assembly 200 disposed within the chamber 210. The composite thermal storage element assembly 200, comprising multiple catalysts stacked therein, may be disposed within the reactor 200. Figure 4 In this description, each composite thermal storage element 100 is shown individually, but multiple composite thermal storage elements 100 may be in direct contact with each other.

[0102] According to an exemplary embodiment, in a catalyst comprising a plurality of composite thermal storage elements 100, channels can be connected to each other to allow fluid to pass through.

[0103] For example, multiple composite thermal storage elements 100 may each include channels with the same diameter, and the catalyst assembly 200 may be formed by stacking composite thermal storage elements such that the second surface 120 of one composite thermal storage element 100 and the first surface 110 of another composite thermal storage element 100 face and contact each other, thereby connecting the channels.

[0104] For example, the sides 150 of multiple identical composite thermal storage elements 100 can be joined to form a composite thermal storage element assembly 200.

[0105] The number of composite thermal storage elements 100 included in the composite thermal storage element assembly 200 is not limited, but can be determined by taking into account the volume of the reactor.

[0106] A gas containing perfluorinated compounds can be injected into one end of the reactor. For example, the gas containing perfluorinated compounds can flow along... Figure 4 The direction of the middle arrow is in contact with the catalyst assembly 200, and the gas containing the decomposition products of perfluorinated compounds can be discharged from the other end of the reactor.

[0107] The composite thermal storage element assembly 200, including the catalyst according to the above embodiments, can exhibit improved perfluorinated compound removal efficiency. Furthermore, the composite thermal storage element assembly 200 can be used continuously and repeatedly.

[0108] According to an exemplary embodiment, the perfluorinated compound removal efficiency of the composite thermal storage element assembly 200 can be 49% or more, 55% or more, 58% or more, or 62% or more. For example, the perfluorinated compound removal efficiency can be less than 90%, less than 80%, or less than 70%.

[0109] When a gas containing 300 ppm to 700 ppm of perfluorinated compounds is injected into the composite thermal storage element assembly 200 for 1 hour to form a cycle, the initial perfluorinated compound removal efficiency can represent the perfluorinated compound removal efficiency within the first 50 cycles, and the long-term perfluorinated compound removal efficiency can represent the perfluorinated compound removal efficiency during 200 to 500 cycles.

[0110] For example, the perfluorinated compound removal efficiency can be calculated according to the following formula 5.

[0111] [Formula 5]

[0112] Perfluorinated compound removal efficiency (%) = {1-(C E / C I )}×100]

[0113] In Equation 5, C E This indicates the concentration of perfluorinated compounds at the outlet of reactor 200, and C I This indicates the concentration of perfluorinated compounds at the inlet of reactor 200.

[0114] Unless a separate reaction temperature is specified, the removal efficiency of perfluorinated compounds can be expressed as the removal efficiency measured at reaction temperatures above 650°C or 700°C. Typically, high conversion rates of perfluorinated compounds can be achieved above 700°C. However, when a catalyst according to the above embodiments is included, high conversion rates can be achieved even at relatively lower temperatures due to improved gas flowability, the increased surface area of ​​the composite heat storage element 100, and / or increased heat transfer efficiency.

[0115] According to an exemplary embodiment of the present invention, a method for decomposing perfluorinated compounds using the above-described composite thermal storage element or composite thermal storage element assembly is provided.

[0116] According to an exemplary embodiment, a catalyst assembly 200 for decomposing perfluorinated compounds can be prepared. The composite thermal storage element assembly 200 can be, for example, an assembly of the composite thermal storage element 100 described above.

[0117] According to an exemplary embodiment, a gas containing perfluorinated compounds can be injected into one side of a catalyst assembly for decomposing perfluorinated compounds.

[0118] For example, perfluorinated compounds can be decomposed by contacting a gas containing the perfluorinated compound with the catalyst or catalyst assembly described above within a predetermined reaction temperature range.

[0119] According to an exemplary embodiment, the perfluorinated compound can decompose at temperatures above 650°C, between 650°C and 800°C, or between 650°C and 750°C.

[0120] According to an exemplary embodiment, the content of perfluorinated compounds in the gas containing perfluorinated compounds can be from 100 ppm to 1,000 ppm, from 200 ppm to 900 ppm, from 250 ppm to 850 ppm, or from 300 ppm to 800 ppm.

[0121] According to an exemplary embodiment, the gas containing the perfluorinated compound may include water vapor (H2O). For example, the aforementioned pressure difference can be calculated by calculating the partial pressure of the water vapor.

[0122] According to an exemplary embodiment, the water vapor content in the gas containing the perfluorinated compound can be from 1 volume% to 20 volume%, from 3 volume% to 17 volume%, from 5 volume% to 15 volume%, or from 6 volume% to 12 volume%.

[0123] Gases containing perfluorinated compounds may include the remainder of air.

[0124] In the following description, embodiments of the invention will be further described with reference to specific experimental examples. However, the following embodiments and comparative examples included in the experimental examples are merely provided for illustrative purposes, and those skilled in the art will clearly understand that various changes and modifications can be made within the scope and spirit of the invention. Such changes and modifications will be considered to fall within the scope of the appended claims.

[0125] [Implementation Scheme of the Invention]

[0126] Examples and Comparative Examples

[0127] Example 1

[0128] (1) Grinding of spent catalyst

[0129] Powder was prepared by grinding alumina-based waste catalyst to a particle size of 50 μm in a needle mill. The term "particle size" refers to the D90 particle size of the powder obtained by grinding the alumina-based waste catalyst.

[0130] (2) Heat treatment

[0131] The powder was heat-treated at 200°C for 4 hours.

[0132] (3) Preparation of the first mixed solution

[0133] A first mixed solution of 100 parts by weight was prepared by mixing 60 parts by weight of heat-treated powder, 30 parts by weight of γ-alumina and 10 parts by weight of silica using a mixer.

[0134] (4) Preparation of the second mixed solution

[0135] A second mixed solution of 100 parts by weight was prepared by mixing the first mixed solution with 70 parts by weight of water and 2 parts by weight of sulfuric acid solution using a mixer.

[0136] (5) Preparation of composite thermal storage elements

[0137] The second mixed solution is extruded to prepare a preliminary composite thermal storage element. Specifically, the preliminary composite thermal storage element with a honeycomb shape, comprising channels having a quadrilateral cross-sectional shape, is prepared by extruding the second mixed solution in an extruder to a CPSI of 50.

[0138] (6) Drying and calcination

[0139] The prepared composite thermal storage element was dried and degreased at 400°C for 2 hours. Subsequently, a honeycomb composite thermal storage element was prepared by calcining the prepared composite thermal storage element at a temperature of approximately 800°C for 2 hours.

[0140] Examples 2-12 and Comparative Examples 1-4

[0141] Except for controlling the structure of the honeycomb composite thermal storage element by adjusting the powder particle size, waste catalyst content, alumina-based binder content, auxiliary additive content and calcination temperature as shown in Table 1 below, and changing the channel density (CPSI) of the honeycomb composite thermal storage element to the values ​​shown in Table 1 below, the composite thermal storage element was prepared according to the same method as in Example 1.

[0142] [Table 1]

[0143]

[0144] Experimental Example

[0145] (1) Evaluation of the shape stability of composite thermal storage elements

[0146] The shape stability of the composite thermal storage elements prepared in the examples and comparative examples was visually evaluated according to the following criteria, and the results are listed in Table 2 below. Figures 5 to 7 The photos show the specific evaluation criteria.

[0147] ○: Shape retention ( Figure 5 )

[0148] △: Crack ( Figure 6 )

[0149] X: Broken ( Figure 7 )

[0150] (2) Evaluation of pressure loss

[0151] The pressure loss of the composite thermal storage element prepared in the examples and comparative examples was measured. Specifically, when gas was injected into the composite thermal storage element in one direction, a pressure gauge was used to measure the pressure loss at 90 cm / m. 2 The pressure loss per unit area was measured at the baseline flow rate. The measurement results are shown in Table 2 below.

[0152] (3) Evaluation of the removal efficiency of perfluorinated compounds (F- gas)

[0153] The composite thermal storage elements according to the examples and comparative examples were each processed into 3-inch cylindrical samples with a volume of 0.343 L and placed in 3-inch Inconel reaction tubes. The reaction temperature was controlled at 600°C using an external heater, and a gas containing 500 ppm of perfluorinated compounds (tetrafluoromethane (CF4)) was passed through the Inconel reaction tube for 1 hour. The reactants were analyzed using Fourier transform infrared (FT-IR) spectroscopy, and the removal efficiency of the perfluorinated compounds was calculated. The specific reaction conditions and removal efficiencies of the perfluorinated compounds are as follows, and the experimental results are shown in Table 2 below.

[0154] [Reaction Conditions]

[0155] i) Airflow rate: 38.9 L / min

[0156] ii) Distilled water flow rate: 0.88 mL / min

[0157] iii) Airspeed: 7,000 / hr

[0158] [Formula for calculating perfluorinated compound removal efficiency]

[0159] Removal efficiency (%) = {1 - (C)} E / C I )}×100

[0160] In the formula used to calculate the removal efficiency of perfluorinated compounds, C E This indicates the concentration of perfluorinated compounds at the outlet of the reaction tube, and C I This indicates the concentration of perfluorinated compounds at the inlet of the reaction tube.

[0161] (4) Evaluation of heat capacity

[0162] The thermal capacity of the composite thermal storage elements according to the examples and comparative examples was evaluated, and the results are shown in Table 2 below. Specifically, the measurements were performed using a Netzsch DSC 404 F1 instrument according to the ASTM E793 test method.

[0163] [Table 2]

[0164]

[0165] Based on Table 1 above, it can be confirmed that, compared with the composite thermal storage element according to the comparative example, the composite thermal storage element according to the embodiment exhibits excellent shape stability, and also exhibits higher perfluorinated compound removal efficiency or higher heat capacity.

[0166] Specifically, composite thermal storage elements of Examples 1 to 3 were prepared using powder with a particle size (D90) of 30 μm or larger and less than 150 μm obtained by grinding alumina-based waste catalyst. The results demonstrated that, compared with Comparative Examples 1 to 4, the composite thermal storage elements exhibited superior shape stability, higher perfluorinated compound removal efficiency, and superior thermal capacity.

[0167] It was confirmed that Example 2 exhibited superior operating efficiency and lower pressure loss compared to Example 8, which had a CPSI of 70, because the number of channels per square inch (CPSI) of the composite thermal storage element met the range of 30 to 60.

[0168] Furthermore, Examples 4 and 5 were found to exhibit excellent perfluorinated compound removal efficiency because the content of alumina-based waste catalyst was higher than that of Example 9.

[0169] A comparison of Examples 2, 4, 10, and 11 shows that the heat capacity improves with increasing alumina-based binder content.

[0170] Furthermore, a comparison of Examples 2, 6, 7, and 12 shows that while the removal efficiency of perfluorinated compounds generally decreases with increasing calcination temperature, the heat capacity increases.

Claims

1. A method for manufacturing a composite thermal storage element, comprising: Grinding alumina-based waste catalyst to prepare powder with a particle size (D90) of 30 μm or more and less than 150 μm; The powder is then subjected to heat treatment; An alumina-based binder is mixed with the heat-treated powder to prepare a first mixed solution; The first mixed solution, solvent, and acidic solution are mixed to prepare the second mixed solution; The second mixed solution is extruded to form a preparative composite thermal storage element; as well as The prepared composite thermal storage element is dried and calcined.

2. The method for manufacturing the composite thermal storage element according to claim 1, wherein, The composite thermal storage element has 30 to 70 channels per square inch (CPSI).

3. The method for manufacturing the composite thermal storage element according to claim 1, wherein the content of the alumina-based waste catalyst is 50% to 95% by weight based on the total weight of the first mixed solution.

4. The method for manufacturing the composite thermal storage element according to claim 1, wherein, Based on the total weight of the first mixed solution, the content of the alumina-based binder is less than 30% by weight.

5. The method for manufacturing the composite thermal storage element according to claim 1, wherein, The alumina-based binder comprises at least one selected from the group consisting of α-alumina (α-Al2O3), β-alumina (β-Al2O3), γ-alumina (γ-Al2O3), δ-alumina (δ-Al2O3), θ-alumina (θ-Al2O3), κ-alumina (κ-Al2O3), and boehmite.

6. The method for manufacturing the composite thermal storage element according to claim 1, wherein, The first mixed solution also includes auxiliary additives.

7. The method for manufacturing the composite thermal storage element according to claim 6, wherein the content of the auxiliary additive is less than 30% by weight based on the total weight of the first mixed solution.

8. The method for manufacturing the composite thermal storage element according to claim 6, wherein the auxiliary additives include those selected from tungsten-containing compounds, lanthanum-containing compounds, silicon dioxide, zeolite, cordierite, mullite, silicon dioxide-alumina, titanium dioxide, magnesium oxide, Fe2O3 / TiO2, Fe2O3 / Al2O3, MgO / TiO2, ZrO2 / Al2O3, ZrO x At least one of the group consisting of / TiO2, CeO2 / TiO2, CeO2 / ZrO2 and V2O5 / TiO2.

9. The method for manufacturing the composite thermal storage element according to claim 1, wherein, The heat treatment temperature in the step of heat treating the powder is above 200°C.