Optical laminate

By using molecular binder layers, especially amino-based and epoxy-based silane coupling agents, in optical laminates, color shift and transmittance changes in holograms are suppressed, solving the problem of insufficient color shift in existing technologies and achieving high color quality and good interlayer adhesion.

CN123125550APending Publication Date: 2026-11-17NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202580029045.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-23
Filing Date
2025-04-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the color shift suppression effect of holograms is insufficient, which cannot meet the requirements for high color quality of holograms in recent years.

Method used

A molecular adhesive layer is used between the photopolymer layer containing the hologram and other layers to suppress color shift through chemical and physical actions. The molecular adhesive layer is composed of amino-based silane coupling agents and epoxy-based silane coupling agents, and is thin and uniformly coated.

Benefits of technology

It effectively suppresses color shift in holograms, with wavelength variation of less than 20nm and transmittance variation of less than 30%, and maintains excellent interlayer adhesion at high temperatures, making it suitable for small display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123125550A_ABST
    Figure CN123125550A_ABST
Patent Text Reader

Abstract

The optical laminate of the present application has a first layer which is a photopolymer layer containing a hologram, a second layer laminated to the first layer, and a molecular adhesive layer interposed between the first layer and the second layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to optical laminates. Background Technology

[0002] Patent Document 1 discloses an optical laminate comprising: a photopolymer layer on which a hologram is recorded by exposure; an adhesive layer bonded to the photopolymer layer; and further bonded other layers such as a substrate. In the configuration of Patent Document 1, pressure-sensitive adhesives or hot-melt adhesives such as polyolefin adhesives or urethane adhesives are used as the adhesive layer.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Publication No. 2015-510526 Summary of the Invention

[0006] The problem the invention aims to solve

[0007] According to Patent Document 1, the disclosed configuration can suppress color shift in holograms, that is, it can suppress the color change of the hologram in the bonded laminate relative to the color of the hologram in the standalone state of the photopolymer layer before bonding. However, in the configuration including the aforementioned adhesive layer, the suppression of color shift is insufficient, and sometimes fails to meet the high requirements for high color quality of holograms in recent years.

[0008] The purpose of this disclosure is to suppress color shift of the hologram before and after bonding in an optical laminate consisting of a photopolymer layer containing a hologram bonded to other layers.

[0009] Problem Solving Methods

[0010] One aspect of this disclosure is an optical laminate having: a first layer, a second layer stacked on the first layer, and a molecular adhesive layer between the first layer and the second layer, wherein the first layer is a photopolymer layer containing a hologram.

[0011] The effects of the invention

[0012] According to this disclosure, in an optical laminate formed by bonding a photopolymer layer containing a hologram to other layers, it is possible to suppress color shift of the hologram before and after bonding. Attached Figure Description

[0013] Figure 1 This is a schematic diagram illustrating an optical laminate according to one embodiment of the present disclosure.

[0014] Figure 2 This is a schematic diagram showing the optical laminate of the first embodiment.

[0015] Figure 3 This is a schematic diagram showing the optical laminate of the second embodiment.

[0016] Figure 4 This is a schematic diagram of the layer structure of a representative embodiment and a comparative example.

[0017] Figure 5 This is the transmittance spectrum of the optical laminate of Example 1-1.

[0018] Figure 6 This is the transmittance spectrum of the optical laminate of Comparative Example 1.

[0019] Symbol Explanation

[0020] 1. First layer (photopolymer layer)

[0021] 2 Second layer

[0022] 2A Second layer (substrate)

[0023] 2B Second layer (photopolymer layer)

[0024] 3. Molecular adhesive layer

[0025] 10, 10A, 10B Optical Laminates Detailed Implementation

[0026] Hereinafter, specific embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. It should be noted that in this specification and the accompanying drawings, for constituent elements having substantially the same functional configuration, repeated descriptions are sometimes omitted by using the same symbols.

[0027] (Optical laminate)

[0028] Figure 1 An optical laminate 10 according to one embodiment of the present disclosure is shown. The optical laminate 10 has: a first layer 1, a second layer 2 laminated on the first layer 1, and a molecular adhesive layer 3 between the first layer 1 and the second layer 2, wherein the first layer 1 is a photopolymer layer containing a hologram. In this specification, an optical laminate refers to a structure having optical functions formed by stacking multiple layers.

[0029] In this disclosure, the first layer 1 is a photopolymer layer containing a hologram, and the second layer 2 is not particularly limited. The second layer 2 may be, for example, a substrate for supporting or reinforcing the first layer 1, or it may be a photopolymer layer containing a hologram, similar to the first layer 1. In addition, the second layer 2 may be a material layer used in the optical field other than the substrate and the photopolymer layer, and may be a layer having given optical properties, such as a given refractive index, a given transmittance, etc.

[0030] In this embodiment, by bonding the first layer 1 and the second layer 2 together via a molecular adhesive layer 3, it is possible to suppress color changes (also known as color shifts) in the hologram contained in the first layer 1. In this specification, suppression of hologram color changes refers to color changes that may occur due to interlayer bonding. More specifically, by comparing the state before bonding the first layer 1 and the second layer 2 with the state after bonding the first layer 1 and the second layer 2, the color changes in the hologram contained in the optical laminate are reduced or eliminated.

[0031] When holograms exhibit significant color variations due to interlayer adhesion, it becomes impossible to display the hologram in the desired color, especially in multicolor holograms, where a proper holographic image sometimes cannot be displayed. To address this, the inventors have discovered that by using a molecular adhesive layer 3 to bond the first layer 1 and the second layer 2, color variations in the hologram can be effectively suppressed. This enables the achievement of high color quality in the hologram. This is attributed to the minimal chemical and / or physical effects of the molecular adhesive layer 3 on the contact layer in contact with it. Furthermore, this is attributed to the fact that the thickness of the molecular adhesive layer 3 is thinner than that of adhesive layers formed without a molecular adhesive, thus minimizing the impact on the optical properties of the optical laminate even when light enters the molecular adhesive layer 3.

[0032] The color change of the hologram described above can be evaluated by measuring the transmittance spectrum of the hologram using a spectrophotometer or similar instrument, and by comparing the shape of the spectrum before and after bonding the first layer 1 and the second layer 2. For example, the degree to which the wavelength of the apex of a given peak in the transmittance spectrum shifts before and after bonding (the amount of wavelength change) can be determined, i.e., the difference between the wavelength (nm) of the apex of a given peak in the spectrum before bonding and the wavelength (nm) of the apex of a given peak in the spectrum after bonding can be determined, thereby enabling evaluation. According to the optical laminate 10 of this disclosure, such a wavelength change can be suppressed to 20 nm or less, 15 nm or less, 10 nm or less, or 5 nm or less.

[0033] Furthermore, the perceived color of a hologram can change due to its transmittance; therefore, the color change of the hologram can also be evaluated by calculating the change in transmittance before and after bonding. To calculate the change in transmittance, the transmittance spectrum of the hologram is measured using a spectrophotometer or similar instrument, similar to the method described above, and the spectra are compared before and after bonding the first layer 1 and the second layer 2. Then, for example, the degree to which the transmittance (%) of the apex of the maximum peak in the transmittance spectrum changed before and after bonding (the amount of transmittance change) is calculated; that is, the difference (%pt) between the transmittance (%) of the apex of the maximum peak in the spectrum before bonding and the transmittance (%) of the apex of the maximum peak in the spectrum after bonding is calculated, thereby enabling evaluation. According to the optical laminate 10 of this disclosure, such a change in transmittance can be suppressed to 30% or less, 20% or less, 10% or less, or 5% or less.

[0034] It should be noted that, when suppressing color changes in the hologram is the top priority, it is also possible to avoid placing the adhesive layer between the first layer 1 and the second layer 2, and instead directly overlap the first layer 1 and the second layer 2 to form a laminate. However, in this case, due to insufficient interlayer adhesion, the strength is low, and a laminate suitable for use as an optical laminate cannot be obtained. Therefore, more specifically, the optical laminate of this embodiment, as described above, suppresses color changes while possessing sufficient interlayer adhesion to function as an optical laminate.

[0035] Furthermore, the optical laminate 10 of this embodiment exhibits excellent resistance to a given environment, particularly high-temperature resistance. Here, high-temperature resistance refers to the excellent color change and interlayer adhesion of the hologram after high-temperature storage. High-temperature resistance can be evaluated, for example, by storing the optical laminate 10 at a high temperature, specifically 60°C or higher, preferably 80°C or higher, for a given period of time.

[0036] (Photopolymer layer)

[0037] The first layer 1 is the layer on which the hologram is recorded in the photopolymer layer. In this embodiment, the photopolymer layer used is not particularly limited as long as it is composed of a photopolymer capable of recording holograms. The photopolymer layer may, for example, contain a photopolymerizable monomer, a photopolymerization initiator, and a binder. Alternatively, the photopolymer layer may not contain a binder, but may contain a matrix polymer, a writing monomer as a photopolymerizable monomer, and a photoinitiator. In this case, the matrix polymer may be an amorphous thermoplastic resin. Examples of matrix polymers include: homopolymers or copolymers containing one or more monomers such as acrylic polymers, (meth)acrylic acid, (meth)acrylates, and their derivatives; polybutyl acrylate; polyvinyl acetate; polyvinyl butyrate; gelatin; cellulose esters; cellulose ethers; silicone copolymers; polyurethane; polybutadiene; polyisoprene; polyethylene oxide; epoxy resin polyamide; polycarbonate, etc.

[0038] As the photopolymer layer, a photopolymer film for holographic recording, known in the art, can be used, for example. Commercially available photopolymer films for holographic recording include the Bayfol (registered trademark) HX series manufactured by Covestro AG, such as Bayfol HX200. It should be noted that commercially available products including this Bayfol series can be provided with the photopolymer layer sandwiched between a cover film and a substrate film. In this configuration, during the manufacturing of the optical laminate 10 of this embodiment, the cover film can be peeled off and bonded to the second layer 2 during lamination. At this time, the manufacturing process can be performed while the substrate film is bonded to and retained within the photopolymer layer. Alternatively, the optical laminate 10 can also be configured to include a substrate film.

[0039] The thickness of the photopolymer layer can be, for example, 1 μm or more, preferably 5 μm or more. It should be noted that the thickness of the layers in the optical laminate 10 of this disclosure (including the thickness of the molecular adhesive layer 3) can be measured by an optical interferometer or the like.

[0040] (Molecular adhesive layer)

[0041] The molecular adhesive layer 3 is a layer that bonds the first layer 1 and the second layer 2 together. The molecular adhesive layer 3 is formed by placing a molecular adhesive between the first layer 1 and the second layer 2 and then curing it. That is, the molecular adhesive layer 3 can be considered a cured product of the molecular adhesive. Here, the molecular adhesive refers to an adhesive containing a compound having two or more reactive functional groups. When the molecular adhesive is placed between the first layer 1 and the second layer 2, the two or more reactive functional groups in the compound contained in the molecular adhesive chemically react with the functional groups on the surfaces of the first layer 1 and the second layer 2, which are the adhered objects, thereby forming covalent bonds between the first layer 1 and the second layer 2 via the aforementioned compound.

[0042] There are no particular limitations on the molecular adhesive used to form the molecular adhesive layer 3; silane coupling agents, triazine molecular adhesives, etc., can be used.

[0043] Examples of silane coupling agents include: amino-based silane coupling agents, epoxy-based silane coupling agents, vinyl-based silane coupling agents, acrylic-based silane coupling agents, methacrylic-based silane coupling agents, mercapto-based silane coupling agents, urea-based silane coupling agents, isocyanate-based silane coupling agents, and combinations thereof, with a combination of amino-based and epoxy-based silane coupling agents being preferred.

[0044] Specific examples of amino-based silane coupling agents include: N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldiethoxysilane, N-2-(aminoethyl)-3-aminopropyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyldiethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyldimethylmethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, or their hydrochlorides.

[0045] Commercially available amino-based silane coupling agents include: KBM-602, KBM-603, KBM-903, KBE-603, and KBE-903 manufactured by Shin-Etsu Chemical Co., Ltd.; Z-6011, Z-6020, Z-6026, Z-6032, Z-6094, and Z-6610 manufactured by Toray Dow Corning Co., Ltd.; and A-1100, A-1110, A-1120, A-2120, and Y-9669 manufactured by Momentive Performance Materials Japan LLC.

[0046] Specific examples of epoxy silane coupling agents include: 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-epoxypropoxypropylmethyldimethoxysilane, 3-epoxypropoxypropylmethyldiethoxysilane, 3-epoxypropoxypropyltrimethoxysilane, 3-epoxypropoxypropyltriethoxysilane, etc.

[0047] Commercially available epoxy silane coupling agents include: KBM-303, KBM-402, KBM-403, KBE-402, KBE-403 manufactured by Shin-Etsu Chemical Co., Ltd.; SH6040, Z-6040, Z-6042, Z-6043, Z-6044 manufactured by Toray Dow Corning Co., Ltd.; and A-186, A-187, A-1871 manufactured by Momentive Performance Materials Japan LLC.

[0048] The aforementioned amino-based silane coupling agents and epoxy-based silane coupling agents can each be used individually or in combination of two or more. Furthermore, the molecular adhesive may contain silane coupling agents other than amino-based and epoxy-based silane coupling agents, or it may contain molecular adhesives other than silane coupling agents, such as the aforementioned triazine molecular adhesives.

[0049] Triazine-based molecular adhesives can be, for example, triazine ring-containing compounds having at least a reactive group A and a reactive group B (reactive group A is amino, azide, diazomethyl, diazirine, mercapto, isocyanate, urea, or epoxy; reactive group B is at least one functional group selected from silanol or a group that can generate silanol through hydrolysis). Specific examples of triazine-based molecular adhesives include: 6-(3-triethoxysilylpropyl)amino-1,3,5-triazine-2,4-diazide, N,N'-bis(2-aminoethyl)-6-(3-trihydroxysilylpropyl)amino-1,3,5-triazine-2,4-diamine, etc.

[0050] Among the aforementioned molecular adhesives, from the perspective of effectively improving the interlayer tightness between the first layer 1 and the second layer 2, which are photopolymer layers, while suppressing possible color changes in the hologram due to adhesion, the molecular adhesive is preferably a silane coupling agent, and more preferably composed of an amino-based silane coupling agent and an epoxy-based silane coupling agent.

[0051] When the molecular adhesive used to form the molecular adhesive layer 3 contains both an amino-based silane coupling agent and an epoxy-based silane coupling agent, the mass ratio of the amino-based silane coupling agent to the epoxy-based silane coupling agent is preferably 20:80 to 80:20, more preferably 30:70 to 70:30, and even more preferably 60:40 to 40:60. By using the amino-based silane coupling agent and the epoxy-based silane coupling agent in the above ratio, a molecular adhesive layer 3 that improves the interlayer adhesion or bonding can be obtained. Therefore, an optical laminate that suppresses color changes in the hologram that may occur due to interlayer adhesion and has high adhesion between the first layer 1 and the second layer 2 can be obtained. It should be noted that when manufacturing the optical laminate, the molecular adhesive is preferably used in the form of a solution of the aforementioned silane coupling agent (described later).

[0052] The thickness of the molecular adhesive layer 3 is thinner than that of conventional adhesive layers formed using pressure-sensitive adhesives, hot-melt adhesives, etc. Therefore, the effects caused by the thickness of the adhesive layer between the first layer 1 and the second layer 2 can be suppressed. Furthermore, because the molecular adhesive layer 3 is thin, the optical laminate 10 can be constructed with a relatively thin overall thickness, making it suitable for various applications. The thickness of the molecular adhesive layer 3 can be less than 1 μm, less than 500 nm, less than 100 nm, or less than 50 nm.

[0053] The hologram contained in the first layer 1, which is the photopolymer layer, is preferably a volume hologram, and can be either a reflective hologram or a transmissive hologram. The hologram can be formed, for example, by exposing the interference pattern to ultraviolet light by irradiating the precursor of the first layer 1, i.e., the hologram recording medium material layer.

[0054] The optical laminate 10 of this embodiment can be constructed to be thin and small, and therefore can be suitably used in small display devices. For example, it can be particularly suitable for use in augmented reality (AR) devices, such as AR glasses like smart glasses, head-mounted displays (HMDs), etc.

[0055] Next, more specific embodiments of this disclosure will be described.

[0056] (First Implementation)

[0057] Figure 2 A schematic diagram of the optical laminate 10A according to the first embodiment is shown. In the first embodiment, the second layer 2 is used as a substrate to support the first layer 1, which is a photopolymer layer. That is, the laminate 10A of the first embodiment includes: a first layer 1 as a photopolymer layer containing a hologram, a second layer 2A as a substrate laminated on the first layer 1, and a molecular adhesive layer 3 between the first layer 1 and the second layer 2A.

[0058] The second layer is substrate 2A, which strengthens the first layer 1 and prevents damage to it, thereby improving the overall mechanical strength or robustness of the optical laminate 10A. Substrate 2A is preferably a transparent substrate. Alternatively, substrate 2A can be one or more substrates comprising glass and resin, preferably a substrate made of glass or resin. When substrate 2A is a resin, it can be a thermosetting resin or a thermoplastic resin, such as poly(meth)acrylate resin, polycarbonate resin, polyurethane resin, epoxy resin, polyamide resin, polyimide resin, polyolefin resin, (meth)acrylate resin, cyclic polyolefin resin (norbornene resin), polyarylate resin, polystyrene resin, polyvinyl alcohol resin, cellulose resins such as cellulose triacetate resin films, polyester resin, polyethersulfone resin, and polysulfone resin.

[0059] The thickness of the substrate 2A can be 1 μm or more, preferably 5 μm or more.

[0060] According to this embodiment, it is possible to suppress the color change of the hologram contained in the first layer 1 before and after it is bonded to the substrate 2A.

[0061] (Second Implementation)

[0062] Figure 3 The image shows an optical laminate 10B according to a second embodiment. In the optical laminate 10B, the first layer 1 is a photopolymer layer containing a hologram, and the second layer 2 is also a photopolymer layer containing a hologram. That is, the laminate 10B of the second embodiment includes: a first layer 1 as a photopolymer layer containing a hologram, a second layer 2B as a photopolymer layer containing a hologram stacked on the first layer 1, and a molecular adhesive layer 3 between the first layer 1 and the second layer 2B. In other words, the optical laminate 10B has a configuration consisting of two photopolymer layers containing holograms stacked together.

[0063] Here, the photopolymer layer used in the first layer 1 can be the same as or different from the photopolymer layer used in the second layer 2B. That is, the composition and thickness of the photopolymer layer in the second layer 2B can be the same as or different from the composition and thickness of the photopolymer layer in the first layer 1. For example, the same commercially available photopolymer film for holographic recording as described above can be used for both the first layer 1 and the second layer 2B.

[0064] It should be noted that, Figure 3The optical laminate 10B shown may further include an optical polymer layer containing a hologram. Therefore, the number of optical polymer layers containing holograms included in the optical laminate 10B can be 3 or more and 100 or less. When the optical laminate 10B has the additional optical polymer layer containing a hologram, the additional optical polymer layer can be bonded to the first layer 1 or the second layer 2 via an additional molecular adhesive layer.

[0065] Thus, for a structure consisting of multiple photopolymer layers containing holograms, it is possible to separate and guide light of different wavelengths according to various colors in each photopolymer layer to display a color image.

[0066] (Other implementation methods)

[0067] Furthermore, unlike the first and second embodiments, the second layer 2 ( Figure 1 The second layer 2 is a functional layer other than the substrate and the photopolymer layer containing the hologram. For example, the second layer 2 can be a layer with specific optical properties. The specific optical properties can be specific refractive index, transmittance, reflectance, etc., preferably a layer with a specific refractive index, and more preferably a low refractive index layer.

[0068] When the second layer 2 is a low-refractive-index layer, one embodiment of this disclosure is an optical laminate comprising: a first layer as a photopolymer layer containing a hologram, a second layer as a low-refractive-index layer laminated on the first layer, and a molecular adhesive layer between the first layer and the second layer. In this embodiment, color changes of the hologram before and after bonding between the layers can be suppressed, enabling display with appropriate colors, and the function of the low-refractive-index layer, i.e., the low refractive index, is not compromised. When the second layer 2 is a low-refractive-index layer, the refractive index of the second layer 2 is preferably 1.05 or higher and 1.25 or lower, more preferably 1.08 or higher and 1.20 or lower, and even more preferably 1.10 or higher and 1.18 or lower. As the material constituting the low-refractive-index layer, materials described in, for example, those disclosed in International Publication No. 2004 / 113966, Japanese Patent Application Publication No. 2013-254183, and Japanese Patent Application Publication No. 2012-189802 can be used. Specific examples of materials constituting the low-refractive-index layer include silicon compounds, organic polymers, polymerizable monomers, and curable resins. These can be used alone or in combination of two or more. Preferably, the material constituting the low-refractive-index layer contains a silicon compound.

[0069] (Manufacturing method of optical laminates)

[0070] The manufacturing method of the aforementioned optical laminate 10 (including optical laminates 10A and 10B) may include, for example, preparing a first layer as a photopolymer layer recording a hologram (S1); applying a molecular adhesive to one side of the first layer (S2); laminating a second layer 2 on the side coated with the molecular adhesive (S3); and curing (S4).

[0071] In the step (S2) of coating one side of the first layer with a molecular adhesive, the molecular adhesive can be used in the form of a solution, preferably an aqueous solution. By dissolving the molecular adhesive in a solvent to prepare a solution, a coating liquid with low viscosity can be obtained, thus allowing the molecular adhesive layer 3 to exist as uniformly and seamlessly as possible between the first layer 1 and the second layer 2. Furthermore, the thickness of the molecular adhesive layer 3 in the resulting optical laminate 10 can also be reduced. When preparing a solution of the molecular adhesive, the concentration of the solution is preferably 0.01% by mass or more and 30% by mass or less, more preferably 0.05% by mass or more and 20% by mass or less, and even more preferably 0.1% by mass or more and 10% by mass or less. For coating the molecular adhesive or the solution of the molecular adhesive, a reverse coating machine, a gravure coating machine (direct, reverse, offset), a reverse bar coating machine, a roller coating machine, a die coating machine, a wire-wound bar coating machine, a bar coating machine, a spin coating machine, a spray coating machine, etc., can be used.

[0072] It should be noted that when the photopolymer layer is obtained by sandwiching a cover film and a substrate film, in the process of coating the molecular adhesive (S2), the cover film is peeled off to expose one side of the photopolymer layer, and the molecular adhesive is coated on the exposed side.

[0073] It should be noted that, for at least one of the first and second layers, the surface to be in contact with the molecular adhesive may be surface-treated before contact with the molecular adhesive, preferably with a hydrophilic treatment or a wettability-enhancing treatment. Such surface treatment can be corona treatment, plasma treatment, etc.

[0074] The curing process (S4) can be performed immediately after the lamination process (S3), or pressure can be applied in the thickness direction (lamination direction) to the laminate formed by laminating the first and second layers with a molecular adhesive. For example, a roller such as a manual roller can be used. By applying pressure, the molecular adhesive can be distributed seamlessly between the layers, thereby improving interlayer adhesion.

[0075] The curing process (S4) is a process used to promote the reaction between the molecular binder and the materials of the first layer 1 and the second layer 2 by means of heat, light, etc. For example, the curing process (S4) can be a heating process of 60°C or higher and 120°C or lower.

[0076] It should be noted that the step (S1) of preparing the first layer of the photopolymer layer on which the hologram is recorded may include a hologram recording step (S1a) of recording the hologram on the first layer of the photopolymer. In the hologram recording step (S1a), known methods can be used to record the hologram on the photopolymer layer. For example, the hologram can be recorded by irradiating a laser of a given wavelength using a known hologram recording laser device, thereby forming an interference pattern on the photopolymer layer. When there are two or more photopolymer layers, for example, when both the first and second layers are photopolymer layers, holograms are recorded on each layer separately. The hologram can be a volume hologram, a reflection hologram, or a transmission hologram. Furthermore, the hologram can be a monochromatic hologram or a multicolor hologram.

[0077] In addition, the holographic recording process (S1a) may not include the process of preparing the first layer (S1), and may be performed after the curing process (S4) or before the curing process (S4).

[0078] Example

[0079] The present disclosure will now be described based on embodiments.

[0080] <Materials used in sample preparation>

[0081] • Holographic recording medium material (photosensitive material): Covestro AG's "Bayfol (registered trademark) HX200", a three-layer structure consisting of a polyethylene capping layer, a photopolymer layer, and a cellulose triacetate (TAC) layer.

[0082] • Glass substrate: Made by Corning Inc. "EAGLEXG (registered trademark)"

[0083] The following substances were prepared as adhesives.

[0084] • Molecular binder A: A molecular binder solution was prepared by adding an amino-based silane coupling agent (Shin-Etsu Chemical Co., Ltd. "KBM-903", 3-aminopropyltriethoxysilane, molecular weight 179.3) and an epoxy-based silane coupling agent (Shin-Etsu Chemical Co., Ltd. "KBM-403", 3-epoxypropoxypropyltrimethoxysilane, molecular weight 236.3) to distilled water at a mass ratio of 50:50 to achieve a given concentration of all silane coupling agents (also referred to as silane coupling agent concentration). It should be noted that molecular binder solutions with silane coupling agent concentrations of 0.1%, 1%, and 10% by mass were prepared respectively.

[0085] • Molecular binder B: A molecular binder solution was prepared by adding an amino-based silane coupling agent (Shin-Etsu Chemical Co., Ltd. "KBM-603", N-2-(aminoethyl)-3-aminopropyltriethoxysilane, molecular weight 222.4) and an epoxy-based silane coupling agent (Shin-Etsu Chemical Co., Ltd. "KBM-403", 3-epoxypropoxypropyltrimethoxysilane, molecular weight 236.3) to distilled water at a mass ratio of 50:50 to achieve a given concentration of all silane coupling agents (also referred to as silane coupling agent concentration). It should be noted that molecular binder solutions with silane coupling agent concentrations of 0.1%, 1%, and 10% by mass were prepared respectively.

[0086] • Molecular binder C: A molecular binder solution was prepared by adding an amino-based silane coupling agent (Shin-Etsu Chemical Co., Ltd. "X-12-972F") and an epoxy-based silane coupling agent (Shin-Etsu Chemical Co., Ltd. "KBM-403", 3-epoxypropoxypropyltrimethoxysilane, molecular weight 236.3) to distilled water at a mass ratio of 50:50 to achieve a given concentration of all silane coupling agents (also referred to as silane coupling agent concentration). It should be noted that molecular binder solutions with silane coupling agent concentrations of 0.1%, 1%, and 10% by mass were prepared respectively.

[0087] • Adhesive a: Nitto Denko Corporation, Optical Transparent Adhesive Sheet "LUCIACS CS986 UAS (Thickness 25μm)"

[0088] <Creating Layered Objects>

[0089] The following laminated bodies were fabricated using the materials described above. It should be noted that the laminated bodies fabricated in Examples 1-1 and 2-1, as well as Comparative Examples 1 and 2, exhibit differences in... Figure 4 A schematic diagram is shown in the figure.

[0090] (Example 1-1)

[0091] A hologram (holographic diffraction grating) was recorded onto the photopolymer layer from the cellulose triacetate (TAC) layer side of the holographic recording medium material using a semiconductor laser (Coherent, Verdi G series, peak wavelength 532 nm) via two-beam interferometry. Next, light from a xenon lamp source was applied to the glass substrate side to fade it. The polyethylene capping layer was then peeled off from the material containing the hologram, exposing the photopolymer layer (first layer). The exposed surface of the photopolymer layer was subjected to corona treatment (treatment conditions: 1000 W·min / m). 2 In addition, one side of the aforementioned glass substrate (second layer) was also subjected to corona treatment (treatment conditions: 1000 W·min / m).2 Then, a 10% by mass aqueous solution of molecular adhesive A is applied to the entire treated surface. Next, a photopolymer layer is laminated such that the corona-treated surface of the photopolymer layer is in contact with the aqueous solution of molecular adhesive A, resulting in a laminate. Further, pressure is applied to the entire laminate using a hand roller. This causes the molecular adhesive in the middle to spread, ensuring that the molecular adhesive is distributed throughout the entire surface between the photopolymer layer and the glass substrate. Subsequently, heating in an oven at 90°C for 5 minutes promotes the reaction of the molecular adhesive. This yields an optical laminate with dimensions of 50mm × 50mm, which has a structure in which a photopolymer layer containing a cellulose triacetate (TAC) layer and a glass substrate are bonded together via the molecular adhesive layer.

[0092] (Examples 1-2)

[0093] An optical laminate was obtained in the same manner as in Example 1-1, except that a 1.0% by mass aqueous solution of molecular binder B was used instead of a 10% by mass aqueous solution of molecular binder A used in Example 1-1.

[0094] (Examples 1-3)

[0095] An optical laminate was obtained in the same manner as in Example 1-1, except that a 0.1% by mass aqueous solution of molecular binder C was used instead of a 10% by mass aqueous solution of molecular binder A used in Example 1-1.

[0096] (Example 2-1)

[0097] Using the aforementioned holographic recording medium material instead of a glass substrate as the second layer, a laminate was obtained in the same manner as in Example 1-1. Specifically, a laminate consisting of two photopolymer layers bonded together by a molecular adhesive was fabricated. More specifically, holograms were recorded on the two holographic recording medium materials in the same manner as in Example 1-1, and then decolorized. The polyethylene capping layer was then peeled off from each holographic-recorded medium material, exposing the photopolymer layer. The exposed surfaces of the photopolymer layers were subjected to the same corona treatment as that performed on the photopolymer layers in Example 1-1. A 10% by mass aqueous solution of molecular adhesive A was applied to the corona-treated surface of one photopolymer layer, and the other photopolymer layer was laminated in contact with the corona-treated surface of that photopolymer layer. Furthermore, after applying an adhesive (Optical Clear Adhesive (OCA) tape, 25 μm thick) to the triacetate cellulose layer of one photopolymer layer, the corona-treated glass substrate used in Example 1-1 was laminated. Under the same conditions as in Examples 1-1, the resulting laminate was subjected to pressure and heated. This resulted in an optical laminate measuring 50 mm × 50 mm, having a structure in which two photopolymer layers, each containing a cellulose triacetate (TAC) layer, are bonded together via a molecular adhesive layer.

[0098] (Example 2-2)

[0099] A 0.1% by mass aqueous solution of molecular binder B was used instead of the 10% by mass aqueous solution of molecular binder A used in Example 2-1. Otherwise, the laminate was fabricated in the same manner as in Example 2-1, and a hologram was recorded to obtain an optical laminate.

[0100] (Examples 2-3)

[0101] A 10% by mass aqueous solution of molecular binder C was used instead of the 10% by mass aqueous solution of molecular binder A used in Example 2-1. Otherwise, the laminate was fabricated in the same manner as in Example 2-1, and a hologram was recorded to obtain an optical laminate.

[0102] (Comparative Example 1)

[0103] An adhesive a was used instead of an aqueous solution of molecular adhesive A, and otherwise, a laminate containing a hologram was obtained in the same manner as in Examples 1-1. More specifically, after adhering adhesive a (adhesive tape) to the corona-treated surface of a glass substrate, a photopolymer layer was laminated such that the corona-treated exposed surface of the photopolymer layer was in contact with adhesive a, thus obtaining an optical laminate.

[0104] (Comparative Example 2)

[0105] Without using adhesives or binders, the corona-treated surface of the photopolymer layer was directly contacted with the corona-treated surface of the glass substrate, and the glass substrate and the photopolymer layer were laminated. Otherwise, a laminate was obtained in the same manner as in Example 1-1.

[0106] <Evaluation>

[0107] The optical properties and interlayer adhesion of the obtained laminated specimens were evaluated as follows.

[0108] (Optical properties)

[0109] The optical properties were evaluated by determining (i) the change in diffraction wavelength before and after bonding, (ii) the change in transmittance before and after bonding, (iii) after high-temperature storage (i), and (iv) after high-temperature storage (ii).

[0110] (i) Change in diffraction wavelength

[0111] For the laminates obtained as described above, i.e., laminates containing photopolymer layers with recorded holograms (bonded samples), the transmittance spectra were measured according to the method of JIS Z 8791:2011. More specifically, transmittance spectra in the range of 400 nm to 700 nm were obtained using a spectrophotometer (Hitachi High-Tech Science UH4150). The wavelength (nm) at the apex of the transmittance peak was then recorded as the diffraction wavelength of the sample. On the other hand, in each example, a laminate (unbonded sample) was fabricated by directly laminating the photopolymer layer and the second layer (glass substrate or photopolymer layer) without an adhesive, with a hologram recorded on the photopolymer layer. The transmittance spectrum was measured in the same manner as above, and the diffraction wavelength was recorded in the same manner. The diffraction wavelength of the unbonded sample was set as λn (nm), and the diffraction wavelength of the bonded sample was set as λa (nm). The change in diffraction wavelength was λa-λn (nm). It should be noted that the unbonded laminates in Examples 1-1 and 2-1 to 2-9, where the second layer is a glass substrate, are equivalent to the laminates prepared in Comparative Example 4.

[0112] (ii) Change in transmittance

[0113] The transmittance (%) at the apex of the peak in the transmittance spectrum obtained as described above is recorded as the transmittance of the sample. The transmittance of the unbonded sample is set as Tn (%), and the diffraction wavelength of the bonded sample is set as Ta (%). Ta-Tn (%pt) is used as the change in transmittance.

[0114] (iii) Change in diffraction wavelength after high-temperature storage

[0115] For the bonded samples described above, after being stored at 80°C for 240 hours, the diffraction wavelength was determined using the same method as described in "(i) Change in diffraction wavelength". The diffraction wavelength of the unbonded sample is denoted as λn, and the diffraction wavelength of the bonded sample after high-temperature storage is denoted as λa. H , will λa H -λn(nm) represents the change in diffraction wavelength after high-temperature storage.

[0116] (iv) Change in transmittance after high-temperature storage

[0117] For the bonded samples described above, after being stored at 80°C for 240 hours, the transmittance was determined using the same method as described in "(ii) Change in transmittance". The transmittance of the unbonded sample is denoted as Tn, and the diffraction wavelength of the bonded sample after high-temperature storage is denoted as Ta. H , will Ta H -Tn(%pt) represents the change in transmittance after high-temperature storage.

[0118] (Interlayer tightness)

[0119] The interlayer adhesion of the hologram-containing laminates obtained in each example was evaluated using a cross-cut test based on JIS K 5400-8.5:1999. More specifically, 11 longitudinal and 11 transverse cuts were made at 1 mm intervals on the triacetyl cellulose (TAC) layer side of the obtained laminate, forming a total of 100 squares. Cellulose tape was applied approximately 50 mm over the cut surfaces, and the tape was rubbed with an eraser to achieve adhesion. After 1–2 minutes, the end of the cellulose tape was held and lifted at a right angle relative to the surface, then instantly peeled off. The number of squares adhering to the cellulose tape that were not removed was counted. The number of unremoved squares relative to 100 was recorded. For example, if the number of unremoved squares is 10, it is recorded as 10 / 100.

[0120] The results are shown in Table 1.

[0121]

[0122] in addition, Figure 5 The diagram shows the changes in the transmittance spectrum of the optical laminate of Example 1-1 before bonding, after bonding, and after high-temperature storage following bonding. Similarly, Figure 6 The diagram shows the changes in the transmittance spectrum of the optical laminate of Comparative Example 1 before bonding, after bonding, and after high-temperature storage following bonding.

[0123] According to Table 1 and Figure 5 It is evident that in optical laminates formed by bonding a holographic photopolymer layer and a substrate via a molecular adhesive layer (Examples 1-1 to 1-3), and in optical laminates formed by bonding holographic photopolymer layers to each other via a molecular adhesive layer (Examples 2-1 to 2-3), changes in wavelength and transmittance before and after bonding are suppressed, and color shift is suppressed (resulting in excellent optical properties). Furthermore, these optical laminates also exhibit high interlayer adhesion.

[0124] On the other hand, the optical properties of the optical laminates (Comparative Examples 1-3) that include an adhesive layer that is not a molecular adhesive layer are lower than those of Examples 1-1-1-3. In addition, in the case of manufacturing without the use of an adhesive, although the optical properties are the same as those of Examples 1-1-1-3, the interlayer adhesion is poor and it cannot withstand the general use of the optical laminate.

[0125] Furthermore, the manner of this disclosure is as follows, for example.

[0126] <1> An optical laminate comprising: a first layer, a second layer stacked on the first layer, and a molecular adhesive layer between the first layer and the second layer, wherein the first layer is a photopolymer layer containing a hologram.

[0127] <2> according to <1> The optical laminate, wherein the second layer is a substrate comprising at least one of glass and resin.

[0128] <3> according to <1> The optical laminate, wherein the second layer is a photopolymer layer containing a hologram.

[0129] <4> according to <1> ~ <3> The optical laminate of any one of the above, wherein the molecular adhesive layer comprises a cured product of the molecular adhesive, and the molecular adhesive comprises a silane coupling agent.

[0130] <5> according to <4> The optical laminate, wherein the molecular binder comprises amino-based silane coupling agents and epoxy-based silane coupling agents.

[0131] <6> according to <5> In the optical laminate, the ratio of the amino-based silane coupling agent to the epoxy-based silane coupling agent is 20:80 to 80:20 by mass.

[0132] <7> A method for manufacturing an optical laminate, the method comprising: preparing a first layer as a photopolymer layer recording a hologram, applying a molecular adhesive to one side of the first layer, laminating a second layer on the side coated with the molecular adhesive, and curing.

[0133] <8> according to <7> The method for manufacturing the optical laminate, wherein the molecular binder comprises a silane coupling agent.

[0134] <9> according to <7> or <8> The method for manufacturing the optical laminate includes applying the molecular binder as a solution of 0.01% by mass or more and 30% by mass or less.

[0135] This application claims priority based on Japanese Patent Application No. 2024-069481, filed on April 23, 2024, the entire contents of which are incorporated herein by reference.

Claims

1. An optical laminate, comprising: First layer The second layer stacked on top of the first layer, and A molecular adhesive layer located between the first layer and the second layer, The first layer is a photopolymer layer containing a hologram.

2. The optical laminate according to claim 1, wherein, The second layer is a substrate comprising at least one of glass and resin.

3. The optical laminate according to claim 1, wherein, The second layer is a photopolymer layer containing a hologram.

4. The optical laminate according to claim 1 or 2, wherein, The molecular adhesive layer comprises a cured product of the molecular adhesive, wherein the molecular adhesive comprises a silane coupling agent.

5. The optical laminate according to claim 4, wherein, The molecular adhesive comprises amino-based silane coupling agents and epoxy-based silane coupling agents.

6. The optical laminate according to claim 5, wherein, The ratio of the amino-based silane coupling agent to the epoxy-based silane coupling agent is 20:80 to 80:20 by mass.

Citation Information

Patent Citations

  • Antireflection film, polarizer and display device

    JP2012189802A

  • Antireflection film, manufacturing method thereof, polarizer, and image display device

    JP2013254183A

  • Layered composite material comprising a photosensitive polymer film and an adhesive layer

    JP2015510526A

  • Novel immune enhancer and vaccine composition comprising the same

    JP2024069481A