Semiconductor substrate and semiconductor device
By arranging a composite buffer layer structure with reverse stress on both sides of the silicon substrate, the lattice constant temperature and thermal mismatch problems between the silicon substrate and gallium nitride are solved, and uneven stress distribution and warping of the epitaxial layer are avoided. Qu, improving the performance and consistency of semiconductor devices.
Patent Information
- Application Number
- CN202420233928.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-31
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2034-01-31
Smart Images

Figure CN221827892U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of semiconductors, in particular to a semiconductor substrate and a semiconductor device. Background Art
[0002] At present, due to the lack of high-quality, large-size commercial GaN substrates, GaN-based devices are generally grown on sapphire, silicon carbide, silicon and other substrates through heteroepitaxial methods. As an important GaN heteroepitaxial substrate, silicon substrate has the advantages of high crystal quality, large wafer size, high thermal conductivity (about 3 times that of sapphire), low price, and substrate conductivity can be controlled by doping, so it has attracted more and more attention from the industry.
[0003] The huge lattice constant and thermal mismatch between the silicon substrate and gallium nitride will produce dislocations. These dislocations will appear as non-radiative recombination centers when the device is working, affecting the efficiency of the device. At the same time, they will cause the leakage current to increase, causing the device to age rapidly, affecting the working efficiency and life of the device. Therefore, the prior art usually sets a buffer layer between the silicon substrate and gallium nitride to shield the defect charges on the surface of the silicon substrate. However, the preparation of a buffer layer on the surface of the silicon substrate will increase the stress on the surface of the silicon substrate, resulting in warping problems, which will become more serious as the substrate size increases, affecting the optical and electrical properties of the device and reducing the consistency of product performance. Utility Model Content
[0004] In order to solve the above technical problems, the utility model provides a semiconductor substrate and a semiconductor device.
[0005] A semiconductor substrate, comprising:
[0006] A silicon substrate, the silicon substrate having a first surface for epitaxial growth and a second surface for non-epitaxial growth, wherein the roughness of the first surface is smaller than the roughness of the second surface;
[0007] A first composite buffer layer, the first composite buffer layer is disposed on the first surface, the first composite buffer layer comprises a first cycle structure, and the first cycle structure is a periodic cycle of a first sublayer and a second sublayer;
[0008] A second composite buffer layer, the second composite buffer layer is disposed on the second surface, the second composite buffer layer comprises a second cyclic structure, and the second cyclic structure is a periodic cycle of the third sublayer and the fourth sublayer;
[0009] Among them, the first sublayer and the third sublayer are made of the same material, and the second sublayer and the fourth sublayer are made of the same material, so that the first composite buffer layer provides stress opposite to the second composite buffer layer; the cycle period of the second cycle structure is greater than the cycle period of the first cycle structure, and the thickness of the second composite buffer layer is 2-4 times the thickness of the first composite buffer layer.
[0010] Preferably, the roughness of the first surface is in the range of 0-0.5 nm, and the roughness of the second surface is in the range of 0.5-10 nm.
[0011] Preferably, the first composite buffer layer further includes a first buffer structure, and the second composite buffer layer further includes a second buffer structure, and the first buffer structure and the second buffer structure are made of the same material.
[0012] Preferably, the first sublayer and the third sublayer are SiO 2 layer, the second sublayer and the fourth sublayer are SiN layers; the first buffer structure and the second buffer structure are AlN layers, and the first buffer structure and the second buffer structure are respectively arranged on the first circulation structure and the second circulation structure.
[0013] Preferably, the first sublayer and the third sublayer are Al 2 O 3 The second sublayer and the fourth sublayer are SiN layers; the first buffer structure and the second buffer structure are SiO 2 layer, the first buffer structure is arranged between the first circulation structure and the silicon substrate, and the second buffer structure is arranged between the second circulation structure and the silicon substrate.
[0014] Preferably, the thickness of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer is 5-100 nm, the thickness of the third sublayer is smaller than the thickness of the first sublayer, and the thickness of the fourth sublayer is smaller than the thickness of the second sublayer.
[0015] A semiconductor device, which is a light-emitting device, comprising:
[0016] The semiconductor substrate as above, and the layers sequentially grown on the first composite buffer layer
[0017] Al 2 O 3 layer, thickness is 10-50nm;
[0018] Nitride buffer layer, thickness 1-5 μm;
[0019] N-type nitride layer, thickness 1-10 μm, dopant is Si, doping concentration is 1×10 18 cm -3 -8×10 18 cm -3 ;
[0020] A nitride light-emitting layer, comprising a nitride quantum well layer and a nitride quantum barrier layer that are grown in a periodic overlapping manner, wherein the cycle period is 2-10, the thickness of the nitride quantum well layer is 1-6 nm, and the thickness of the nitride quantum barrier layer is 6-25 nm;
[0021] P-type nitride layer, thickness is 20-300nm, dopant is Mg, doping concentration is 1×10 19 cm -3 -1×10 21 cm -3 .
[0022] A semiconductor device, comprising:
[0023] The semiconductor substrate as above; and sequentially grown on the first composite buffer layer
[0024] Nitride buffer layer, the nitride buffer layer is GaN, and has a thickness of 1-5 μm;
[0025] A nitride channel layer, the nitride channel layer is GaN, and has a thickness of 100-1000 nm;
[0026] A nitride barrier layer, wherein the nitride barrier layer is AlGaN, the Al component is 0.2-0.5, and the thickness is 5-30 nm;
[0027] The drain, source and gate, the source and drain are located on the nitride barrier layer, and form ohmic contacts with the nitride barrier layer respectively, and the gate is located on the nitride barrier layer, and forms a Schottky contact with the nitride barrier layer. The above technical solution of the utility model has the following advantages compared with the prior art:
[0028] The utility model sets a first composite buffer layer and a second composite buffer layer on both sides of the silicon substrate respectively, and the layer structure material in the first composite buffer layer is the same as the layer structure material in the second composite buffer layer, so that the second composite buffer layer located on the second surface provides stress opposite to the first composite buffer layer located on the first surface. During the epitaxial process, since the roughness of the first surface is less than that of the second surface, the second surface has a larger stress distribution than the surface of the first surface. Therefore, the utility model sets the thickness of the second composite buffer layer to be 2-4 times the thickness of the first composite buffer layer. On the one hand, it can ensure that the second composite buffer layer has the effect of releasing the stress of the second surface, especially when the substrate size is relatively large, it can avoid defects such as cracks on the surface of the epitaxial layer due to large tensile stress; on the other hand, it can provide a suitable stress modulation effect to avoid problems such as large warping of the epitaxial layer and poor uniformity of stress distribution on the epitaxial layer film, thereby improving the performance of semiconductor devices and product consistency. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to make the content of the utility model more clearly understood, the utility model is further described in detail below based on specific embodiments of the utility model in combination with the accompanying drawings.
[0030] Figure 1 It is a schematic diagram of a semiconductor substrate of the utility model.
[0031] Figure 2 This is the optical microscope surface morphology of sample A of the present invention.
[0032] Figure 3 This is the optical microscope surface morphology of sample C of the present invention.
[0033] Figure 4 This is the optical microscope surface morphology of sample F of the present invention.
[0034] Figure 5 , 6 It is a schematic diagram of a specific embodiment of the semiconductor substrate buffer layer of the utility model.
[0035] Figure 7 The utility model is a flow chart of a method for processing a semiconductor substrate.
[0036] Figure 8 It is a schematic diagram of a semiconductor light emitting device of the utility model.
[0037] Fig. 9 It is a schematic diagram of a semiconductor transistor device of the utility model.
[0038] Description of the accompanying drawings: 1. silicon substrate; 11. first surface; 12. second surface; 2. first composite buffer layer; 21. first circulation structure; 211. first sublayer; 212. second sublayer; 22. first buffer structure; 3. second composite buffer layer; 31. second circulation structure; 311. third sublayer; 312. fourth sublayer; 32. second buffer structure; 41. Al 2 O 3 layer; 42, nitride buffer layer; 43, N-type nitride layer; 44, nitride light-emitting layer; 45, P-type nitride layer; 51, nitride buffer layer; 52, nitride channel layer; 53, nitride barrier layer; 54, drain; 55, source; 56, gate. DETAILED DESCRIPTION
[0039] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0040] like Figure 1 As shown, the utility model provides a semiconductor substrate, comprising:
[0041] A silicon substrate 1, wherein the silicon substrate 1 has a first surface 11 for epitaxial growth and a second surface 12 for non-epitaxial growth, wherein the roughness of the first surface 11 is less than that of the second surface 12; specifically, the roughness of the first surface 11 is in a range of 0-0.5 nm, and the roughness of the second surface 12 is in a range of 0.5-10 nm; setting a relatively large roughness on the second surface 12 can reduce the requirements for the precision of the silicon substrate grinding process, and the relatively rough surface can release the internal stress of the silicon substrate and reduce the phenomenon of substrate fragmentation;
[0042] A first composite buffer layer 2, wherein the first composite buffer layer 2 is disposed on the first surface 11, and the first composite buffer layer 2 comprises a first cycle structure 21, wherein the first cycle structure 21 is a periodic cycle of a first sub-layer 211 and a second sub-layer 212;
[0043] A second composite buffer layer 3, the second composite buffer layer 3 is disposed on the second surface 12, the second composite buffer layer 3 comprises a second cycle structure 31, the second cycle structure 31 is a periodic cycle of a third sublayer 311 and a fourth sublayer 312;
[0044] Among them, the first sublayer 211 and the third sublayer 311 are made of the same material, and the second sublayer 212 and the fourth sublayer 312 are made of the same material, so that the first composite buffer layer 2 provides stress opposite to the second composite buffer layer 3; the cycle period of the second cycle structure 31 is greater than the cycle period of the first cycle structure 21, and the thickness of the second composite buffer layer 3 is 2-4 times the thickness of the first composite buffer layer 2.
[0045] In the utility model, the first composite buffer layer as a passivation layer needs to have a certain thickness to ensure that it can play the role of passivating the surface defects of the substrate. Since the cycle period of the first composite buffer layer is smaller than that of the second composite buffer layer, and during the epitaxial process, the stress in the thickness direction of the substrate extends along the direction from the second surface to the first surface, the stress inside the substrate close to the second surface is higher than the stress close to the first surface, that is, the second surface has a larger stress distribution than the surface of the first surface. In this way, during the epitaxial process, a relatively thick buffer layer thickness is required for the second surface. At the same time, the thickness of the second composite buffer layer located on the second surface will increase with the increase of the thickness of the third sublayer and the fourth sublayer due to the difference in lattice constant. Therefore, setting the thickness of the third sublayer to be smaller than the thickness of the first sublayer and the thickness of the fourth sublayer to be smaller than the thickness of the second sublayer can make the lattice constant compromised during the periodic cycle, release the stress layer by layer, improve the uniformity of stress distribution inside the substrate, and thus improve the uniformity of the epitaxial wafer.
[0046] In order to avoid warping problems in subsequent processes, the utility model respectively arranges a first composite buffer layer 2 and a second composite buffer layer 3 on both sides of the silicon substrate 1, wherein the first composite buffer layer 2 includes a first cycle structure 21, which is a periodic cycle of a first sublayer 211 and a second sublayer 212, and the second composite buffer layer 3 includes a second cycle structure 31, which is a periodic cycle of a third sublayer 311 and a fourth sublayer 312. The first sublayer 211 and the third sublayer 311 are made of the same material, and the second sublayer 212 and the fourth sublayer 312 are made of the same material, so that the second composite buffer layer 3 located on the second surface 12 provides stress opposite to the first composite buffer layer 2 located on the first surface 11. During the epitaxial growth process, since the roughness of the first surface 11 is less than the roughness of the second surface 12, the stress direction in the thickness direction of the silicon substrate 1 is the direction in which the second surface 12 extends toward the first surface 11. The stress inside the substrate near the second surface 12 is higher than the stress near the first surface 11, that is, the second surface 12 has a larger stress distribution than the surface of the first surface 11. Therefore, the thickness of the second composite buffer layer 3 set in the utility model is 2-4 times the thickness of the first composite buffer layer 2. On the one hand, it can ensure that the second composite buffer layer 3 can release the stress of the second surface 12, especially when the substrate size is relatively large, it can avoid defects such as cracks on the surface of the epitaxial layer due to large tensile stress; on the other hand, it can provide a suitable stress modulation effect to avoid problems such as large warping of the epitaxial layer and poor uniformity of stress distribution on the epitaxial layer film, thereby improving the performance of semiconductor devices and product consistency.
[0047] The utility model provides three samples made of the thickness relationship between the second composite buffer layer and the first composite buffer layer, and explores its influence on the epitaxial layer stress, thickness uniformity, surface roughness and surface defect density. Among them, the thickness of the second composite buffer layer of sample A is 1 times the thickness of the first composite buffer layer, the thickness of the second composite buffer layer of sample B is 2 times the thickness of the first composite buffer layer, the thickness of the second composite buffer layer of sample C is 3 times the thickness of the first composite buffer layer, the thickness of the second composite buffer layer of samples D and E is 4 times the thickness of the first composite buffer layer, and the thickness of the second composite buffer layer of sample F is 5 times the thickness of the first composite buffer layer. The third sublayer and the fourth sublayer of samples A, B, C, D, and F are the same as the thickness of the first sublayer and the second sublayer, respectively. The thickness of the third sublayer and the fourth sublayer of sample E is reduced by 10% compared with the first sublayer and the second sublayer, respectively. The results are shown in the following table:
[0048] Sample No. Epitaxial layer stress / Gpa Thickness uniformity / % Surface roughness / nm <![CDATA[Surface defect density / 10 8 cm -2 > A 1.09 3.82 4.95 9.9 B 0.45 1.33 0.30 5.1 C 0.38 1.08 0.25 4.8 D 0.33 1.21 0.23 4.3 E 0.18 1.08 0.20 1.9 F 0.94 2.54 3.97 7.1
[0049] It can be seen from the above table that when the thickness of the second composite buffer layer 3 is 2-4 times the thickness of the first composite buffer layer 2, the obtained epitaxial layer is optimal in terms of epitaxial layer stress, thickness uniformity, surface roughness and surface defect density. Figure 2-4The optical microscope surface morphologies of samples A, C, and E are shown in Figure 2. Figure 2-4 It can be clearly seen from the comparison in the above table that when the thickness of the second composite buffer layer 3 is 2-4 times the thickness of the first composite buffer layer 2, the surface of the obtained epitaxial layer is smoother. When the thickness of the second composite buffer layer is less than 2 times the thickness of the first composite buffer layer, the stress release of the second composite buffer layer on the second surface will not work because the stress of the second surface of the substrate is greater than the stress of the first surface. Especially when the substrate size is relatively large, the surface of the epitaxial layer will still have defects such as cracks due to large tensile stress; when the thickness of the second composite buffer layer is greater than 4 times the thickness of the first composite buffer layer, the surface of the epitaxial layer is modulated by the stress of the second composite buffer layer, which can avoid the crack phenomenon of the epitaxial layer, but it often brings about excessive compressive stress modulation, resulting in large warping of the epitaxial layer and poor uniformity of stress distribution of the epitaxial layer film.
[0050] Since the lattice constants of the layers in the composite buffer layer are different, stress will be generated. The utility model can compromise the lattice constant by setting a periodic cycle of the layer structure so that the stress is released layer by layer, thereby improving the uniformity of stress distribution inside the substrate, thereby improving the uniformity of stress inside the epitaxial layer and ensuring the uniformity of the thickness of the epitaxial wafer.
[0051] The first composite buffer layer 2 further includes a first buffer structure 22 , and the second composite buffer layer 3 further includes a second buffer structure 32 . The first buffer structure 22 and the second buffer structure 32 are made of the same material.
[0052] In a preferred embodiment, the thickness of the third sublayer 311 and the fourth sublayer 312 is 5-100 nm. In a single cycle, the stress between the third sublayer 311 and the fourth sublayer 312 increases as their thickness increases, because the smaller the thickness of a single sublayer in a cycle, the smaller the thickness of the third sublayer 311 and the fourth sublayer 312 in the cycle is, and the smaller the stress between the third sublayer 311 and the fourth sublayer 312 in the cycle, the smaller the stress between the third sublayer 311 and the fourth sublayer 312 in the cycle, which can ensure that the stress can be better released in each cycle, avoid concentrated release in the form of defects in a local area inside the buffer layer, and ensure the crystal quality and uniformity of the buffer layer in the cycle, and then provide a low-stress growth template for epitaxial layer growth.
[0053] Furthermore, in order to reduce the internal stress of the first cycle structure 21, the thickness of the first sublayer 211 and the second sublayer 212 is 5-100 nm.
[0054] like Figure 5 As shown, in an optional embodiment, the first sublayer 211 and the third sublayer 311 are SiO 2 The second sublayer 212 and the fourth sublayer 312 are SiN layers; wherein SiO2 The layer shields the defect charges on the surface of the silicon substrate 1 and plays a role in passivating the surface of the silicon substrate 1; the SiN layer itself has a nanoporous film structure, which strengthens the lateral epitaxy of the nitride buffer layer, interrupts the extension of dislocations to the top of the nitride buffer layer, improves the crystal quality of the nitride buffer, reduces the electron diffusion in the buffer layer, and improves the leakage performance of the epitaxial wafer. If used in light-emitting devices, the nanoporous structure of the SiN layer can also be used to change the direction of light emitted from the nitride light-emitting layer to the surface of the nanoporous structure, improve the forward light emission of the epitaxial wafer, and thus improve the brightness of the epitaxial wafer.
[0055] The first buffer structure 22 and the second buffer structure 32 are AlN layers, which are respectively arranged on the first cyclic structure 21 and the second cyclic structure 31. On the one hand, the AlN layer can play a role in filling the SiN pore structure; on the other hand, the AlN filling is arranged inside the SiN nanostructure and can serve as the nucleation center of the subsequent nitride epitaxial layer, so as to avoid the formation of nitride on the SiO 2 The problem of difficulty in nucleation and growth of nitride epitaxial layer.
[0056] like Figure 6 As shown, in another optional embodiment, the first sublayer 211 and the third sublayer 311 are Al 2 O 3 The second sublayer 212 and the fourth sublayer 312 are SiN layers; the SiN layer itself has a nanoporous film structure, which strengthens the lateral epitaxy of the nitride buffer layer, interrupts the extension of dislocations to the top of the nitride buffer layer, improves the crystal quality of the nitride buffer, reduces the electron diffusion in the buffer layer, and improves the leakage performance of the epitaxial wafer. 2 O 3 There are a lot of negative charges in the Al layer and a lot of positive charges in the SiN layer. The positive and negative charges form a PN junction. If used in transistor devices, when the source-drain voltage is applied, the Al 2 O 3 The cyclic structure of the SiN layer and the SiN layer can ensure that there are multiple PN junction reverse biases on the leakage path, reduce the leakage current of the nitride buffer layer, and improve the breakdown voltage of the semiconductor transistor device.
[0057] The first buffer structure 22 and the second buffer structure 32 are SiO 2 The first buffer structure 22 is arranged between the first loop structure 21 and the silicon substrate 1, and the second buffer structure 32 is arranged between the second loop structure 31 and the silicon substrate 1. Since the surface of the silicon substrate 1 contains a large number of unbonded dangling bonds, by arranging SiO 2The layer can make the Si-O valence bonds match, which effectively saturates the dangling bonds on the surface of the silicon substrate 1, thereby reducing the defect density and surface charge on the surface of the silicon substrate 1; at the same time, the SiO 2 The layer has strong adhesion on the silicon substrate 1, which can play a good role in surface protection and passivation, avoiding Al 2 O 3 Directly contacting with the silicon substrate 1, a SiAl mixed solution is formed at the interface, which affects the morphology, structure and stability of the substrate surface.
[0058] like Figure 7 As shown, the utility model provides a method for processing a semiconductor substrate, which is used to prepare the semiconductor substrate as above, comprising the following steps:
[0059] Providing a silicon substrate, the silicon substrate having a first surface for epitaxial growth and a second surface for non-epitaxial growth, the roughness of the first surface being smaller than the roughness of the second surface;
[0060] Placing the silicon substrate into a deposition device with the second surface facing the deposition direction, for preparing a second composite buffer layer on the second surface, wherein the second composite buffer layer includes a second cycle structure, and the second cycle structure is a periodic cycle of the third sublayer and the fourth sublayer;
[0061] Putting the silicon substrate into a deposition device with the first surface facing the deposition direction, for preparing a first composite buffer layer on the first surface, wherein the first composite buffer layer includes a first cycle structure, and the first cycle structure is a periodic cycle of a first sublayer and a second sublayer;
[0062] Among them, the first sublayer and the third sublayer are made of the same material, and the second sublayer and the fourth sublayer are made of the same material, so that the first composite buffer layer provides stress opposite to the second composite buffer layer; the cycle period of the second cycle structure is greater than the cycle period of the first cycle structure, and the thickness of the second composite buffer layer is 2-4 times the thickness of the first composite buffer layer.
[0063] Preferably, the growth temperature of the third sublayer is higher than that of the first sublayer, and the growth temperature of the fourth sublayer is higher than that of the second sublayer. Under relatively high temperature conditions, the third and fourth sublayers in the second composite buffer layer can improve the migration ability of internal atoms within the plane, which is beneficial to improving the uniformity of stress distribution in the second composite buffer layer; while the first and second sublayers in the first composite buffer layer can reduce the stress of the first composite buffer layer under relatively low temperature conditions, greatly reducing the warping between the first composite buffer layer and the silicon substrate caused by high temperature, thereby obtaining a high-quality, uniform first composite buffer layer.
[0064] Because the first surface is the direction of epitaxial layer growth, in the semiconductor substrate processing method of the present invention, a second composite buffer layer is first prepared on the second surface, which can increase the surface stress of the first surface during the preparation of the first surface and increase the internal stress of the composite buffer layer on the first surface, thereby improving the uniformity of the epitaxial layer.
[0065] In an optional embodiment, preparing the second composite buffer layer further includes preparing a second buffer structure on the second circulation structure; preparing the first composite buffer layer further includes preparing a first buffer structure on the first circulation structure.
[0066] In another optional embodiment, before preparing the second circulation structure, the method further includes preparing a second buffer structure on the silicon substrate; before preparing the first circulation structure, the method further includes preparing a first buffer structure on the silicon substrate.
[0067] like Figure 8 As shown, the utility model provides a semiconductor device, which is a light-emitting device, comprising:
[0068] As the semiconductor substrate above,
[0069] And sequentially grown on the first composite buffer layer 2:
[0070] Al 2 O 3 Layer 41, thickness 10-50 nm;
[0071] A nitride buffer layer 42 having a thickness of 1-5 μm;
[0072] The N-type nitride layer 43 has a thickness of 1-10 μm, a dopant of Si, and a doping concentration of 1×10 18 cm -3 -8×10 18 cm -3 ;
[0073] The nitride light emitting layer 44 comprises a nitride quantum well layer and a nitride quantum barrier layer which are grown in a periodic overlapping manner, wherein the cycle period is 2-10, the thickness of the nitride quantum well layer is 1-6 nm, and the thickness of the nitride quantum barrier layer is 6-25 nm;
[0074] The P-type nitride layer 45 has a thickness of 20-300 nm and is doped with Mg at a doping concentration of 1×10 19 cm -3 -1×10 21 cm -3 .
[0075] like Fig. 9 As shown, the utility model provides a semiconductor device, which is a transistor, comprising:
[0076] The semiconductor substrate as above; and sequentially grown on the first composite buffer layer 2
[0077] A nitride buffer layer 51, wherein the nitride buffer layer 51 is GaN and has a thickness of 1-5 μm;
[0078] A nitride channel layer 52, wherein the nitride channel layer 52 is GaN and has a thickness of 100-1000 nm;
[0079] A nitride barrier layer 53, wherein the nitride barrier layer 53 is AlGaN, wherein the Al component is 0.2-0.5 and the thickness is 5-30 nm;
[0080] The drain 54 , the source 55 and the gate 56 , the source 55 and the drain 54 are located on the nitride barrier layer 53 and form ohmic contacts with the nitride barrier layer 53 respectively, and the gate 56 is located on the nitride barrier layer 53 and forms a Schottky contact with the nitride barrier layer 53 .
[0081] Obviously, the above embodiments are merely examples for the purpose of clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention of the utility model.
Claims
1. A semiconductor substrate, characterized in that: The semiconductor substrate comprises: A silicon substrate, the silicon substrate having a first surface for epitaxial growth and a second surface for non-epitaxial growth, wherein the roughness of the first surface is smaller than the roughness of the second surface; A first composite buffer layer, wherein the first composite buffer layer is disposed on the first surface, and the first composite buffer layer comprises a first cycle structure, wherein the first cycle structure is a periodic cycle of a first sublayer and a second sublayer; A second composite buffer layer, the second composite buffer layer is disposed on the second surface, the second composite buffer layer comprises a second cyclic structure, and the second cyclic structure is a periodic cycle of the third sublayer and the fourth sublayer; Among them, the first sublayer and the third sublayer are made of the same material, and the second sublayer and the fourth sublayer are made of the same material, so that the first composite buffer layer provides stress opposite to the second composite buffer layer; the cycle period of the second cycle structure is greater than the cycle period of the first cycle structure, and the thickness of the second composite buffer layer is 2-4 times the thickness of the first composite buffer layer.
2. The semiconductor substrate according to claim 1, characterized in that The roughness of the first surface is in the range of 0-0.5 nm, and the roughness of the second surface is in the range of 0.5-10 nm.
3. The semiconductor substrate according to claim 1, characterized in that The first composite buffer layer further includes a first buffer structure, and the second composite buffer layer further includes a second buffer structure. The first buffer structure and the second buffer structure are made of the same material.
4. The semiconductor substrate according to claim 3, characterized in that The first sublayer and the third sublayer are SiO2 layers, the second sublayer and the fourth sublayer are SiN layers; the first buffer structure and the second buffer structure are AlN layers, and the first buffer structure and the second buffer structure are respectively arranged on the first circulation structure and the second circulation structure.
5. The semiconductor substrate according to claim 3, characterized in that The first sublayer and the third sublayer are Al2O3 layers, and the second sublayer and the fourth sublayer are SiN layers; the first buffer structure and the second buffer structure are SiO2 layers, the first buffer structure is arranged between the first circulation structure and the silicon substrate, and the second buffer structure is arranged between the second circulation structure and the silicon substrate.
6. The semiconductor substrate according to any one of claims 1 to 5, characterized in that: The thicknesses of the first sublayer, the second sublayer, the third sublayer and the fourth sublayer are 5-100 nm, the thickness of the third sublayer is smaller than the thickness of the first sublayer, and the thickness of the fourth sublayer is smaller than the thickness of the second sublayer.
7. A semiconductor device, characterized in that: The semiconductor device is a light emitting device, comprising: The semiconductor substrate according to any one of claims 1 to 6, and an Al2O3 layer sequentially grown on the first composite buffer layer, with a thickness of 10-50 nm; Nitride buffer layer, thickness 1-5 μm; N-type nitride layer, with a thickness of 1-10 μm and doped with Si; A nitride light-emitting layer, comprising a nitride quantum well layer and a nitride quantum barrier layer that are grown in a periodic overlapping manner, wherein the cycle period is 2-10, the thickness of the nitride quantum well layer is 1-6 nm, and the thickness of the nitride quantum barrier layer is 6-25 nm; P-type nitride layer, thickness is 20-300nm, dopant is Mg.
8. A semiconductor device, characterized in that: include: The semiconductor substrate according to any one of claims 1 to 6; and A nitride buffer layer, wherein the nitride buffer layer is GaN and has a thickness of 1-5 μm; A nitride channel layer, wherein the nitride channel layer is GaN and has a thickness of 100-1000 nm; A nitride barrier layer, wherein the nitride barrier layer is AlGaN and has a thickness of 5-30 nm; A drain, a source and a gate, wherein the source and the drain are located on the nitride barrier layer and form ohmic contacts with the nitride barrier layer respectively, and the gate is located on the nitride barrier layer and forms a Schottky contact with the nitride barrier layer.