Imaging lens and electronic device
By adopting the design of multi-layer silica film stack and aluminum oxide nanostructure layer in the imaging lens, the problem of reduced anti-reflective performance in harsh environments is solved, and the stable performance and anti-reflection of the lens in high temperature and high humidity environments are achieved. Reflection performance improved.
Patent Information
- Application Number
- CN202420377947.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-30
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2034-02-28
AI Technical Summary
The anti-reflective performance of existing imaging lenses decreases in harsh environments, and the integrity of the ridge-shaped convex structure is affected, resulting in lens performance degradation.
Using an interlayer stacked with multiple layers of silicon dioxide films, combined with the ridge-shaped protrusion design of the aluminum oxide nanostructure layer, the weather resistance and anti-reflective performance of the lens are improved by adjusting the equivalent refractive index and light interference of the interface.
In an environment with a temperature of 85°C and a relative humidity of 85%, the imaging lens can maintain normal performance, with the average reflectance only doubling after 1,000 hours of placement, and light interference and stray light are reduced.
Smart Images

Figure CN221860734U_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an imaging lens, and particularly to an imaging lens applied to a portable electronic device. Background Art
[0002] In recent years, portable electronic devices have developed rapidly, such as smart electronic devices, tablet computers, etc., which have flooded into modern people's lives. The imaging lenses mounted on portable electronic devices have also developed vigorously. However, as technology advances, users' requirements for the quality of imaging lenses are getting higher and higher.
[0003] Specifically, the optical elements in the prior art are configured with a relatively thin intermediate layer. After the optical elements are placed in a harsh environment for a long time, the structural integrity of the ridge-like protrusions is affected, resulting in a decrease in the anti-reflection performance. Further, the situation where the structural integrity of the ridge-like protrusions is affected, such as: the structure collapses, the boundary line between the bottom of the structure and the intermediate layer becomes blurred, or other structural changes that cause the anti-reflection performance to decrease. Therefore, developing an imaging lens that can still maintain normal performance in a harsh environment has become an important and urgent problem in the industry. Summary of the Utility Model
[0004] The present disclosure provides an imaging lens and an electronic device. By using a stack of multiple silicon dioxide thin films as the intermediate layer, it can still maintain normal performance in a harsh environment and helps to avoid light interference while the intermediate layer is thickened.
[0005] According to an embodiment of the present disclosure, an imaging lens is provided, which includes an optical element. The optical element includes a substrate, a nanostructure layer, and an intermediate layer. The substrate is a light-transmitting substrate. The nanostructure layer is disposed on a surface of the substrate. The nanostructure layer is an aluminum oxide nanostructure layer, and the nanostructure layer has a plurality of ridge-like protrusions extending non-directionally. The bottom of each ridge-like protrusion is closer to the substrate than the top, and each ridge-like protrusion tapers from the bottom to the top. The intermediate layer is disposed between the substrate and the nanostructure layer, and the intermediate layer includes a first thin film and a plurality of second thin films. The first thin film is a first silicon dioxide thin film, each second thin film is a second silicon dioxide thin film, and the second thin films are stacked with the first thin film. The thickness of the first thin film is Tf1, the thickness of each second thin film is Tf2, and the thickness of the intermediate layer is Ti, which satisfy the following conditions: Tf2 < Tf1; 45 nm < Tf1 < 180 nm; and 101 nm < Ti < 45 nm.
[0006] For the imaging lens according to the above-described embodiment, the thickness of the first thin film is Tf1, which can satisfy the following conditions: 50 nm < Tf1 < 120 nm.
[0007] According to the imaging lens of the embodiment described in the previous paragraph, the thickness of the first film is Tf1, and the thickness of each second film is Tf2, which can meet the following conditions: 1.3 <Tf1 / Tf2<55。
[0008] According to the imaging lens of the embodiment described in the previous paragraph, the thickness of the intermediate layer is Ti, which can meet the following conditions: 110nm <Ti<330nm。
[0009] According to the imaging lens of the embodiment described in the previous paragraph, the average reflectivity R0 of the optical element corresponding to light wavelengths of 450nm to 600nm can meet the following condition: R0<0.65%.
[0010] According to the imaging lens of the embodiment described in the preceding paragraph, wherein the average reflectivity of the optical element corresponding to the wavelength of light from 450nm to 600nm is R0, after the optical element is placed in an environment with a temperature of 85°C and a relative humidity of 85% for 1000 hours, the average reflectivity of the optical element corresponding to the wavelength of light from 450nm to 600nm is R1000, which can meet the following conditions: 1.05 <R1000 / R0<15。
[0011] According to the imaging lens of the embodiment described in the previous paragraph, the bottom of each ridge-shaped protrusion may be in physical contact with the interposer.
[0012] In the imaging lens according to the embodiment described in the preceding paragraph, a portion of a top portion of the intermediate layer may be in contact with air.
[0013] According to the imaging lens of the embodiment described in the preceding paragraph, the average height of the nanostructure layer is Havg, which can meet the following conditions: 70nm <Havg<350nm。
[0014] According to the imaging lens of the embodiment described in the previous paragraph, the optical element may be a lens element. The imaging lens may further include a lens group, and the optical element is closer to an object side or an image side than the lens group.
[0015] The imaging lens according to the embodiment described in the preceding paragraph may further include an optical path inflection element, wherein the optical element is closer to the optical path inflection element than the lens assembly.
[0016] In the imaging lens according to the embodiment described in the preceding paragraph, the substrate of the optical element may include an optically active portion and a peripheral portion. The optically active portion has light refractive power, and the peripheral portion is disposed around the optically active portion. The thickness of the intermediary layer corresponding to the optically active portion is greater than the thickness of the intermediary layer corresponding to the peripheral portion.
[0017] According to one embodiment of the present disclosure, an imaging lens is provided, which includes an optical element. The optical element includes a substrate, a nanostructure layer and an intermediate layer. The substrate is a light-transmitting substrate. The nanostructure layer is disposed on a surface of the substrate, and the nanostructure layer is an aluminum oxide nanostructure layer, wherein the nanostructure layer has a plurality of ridge-like protrusions extending in a non-directional direction, a bottom of each ridge-like protrusion is closer to the substrate than a top, and each ridge-like protrusion tapers from the bottom to the top. The intermediate layer is disposed between the substrate and the nanostructure layer, and includes a plurality of thin films, wherein each thin film is a silicon dioxide thin film, and the thin films are stacked adjacent to each other. The thickness of the intermediate layer is Ti, which satisfies the following conditions: 101nm <Ti<450nm。
[0018] According to the imaging lens of the embodiment described in the previous paragraph, the average reflectivity R0 of the optical element corresponding to light wavelengths of 450nm to 600nm can meet the following condition: R0<0.65%.
[0019] According to the imaging lens of the embodiment described in the previous paragraph, the thickness of the intermediate layer is Ti, which can meet the following conditions: 110nm <Ti<330nm。
[0020] According to the imaging lens of the embodiment described in the preceding paragraph, wherein the average reflectivity of the optical element corresponding to the wavelength of light from 450nm to 600nm is R0, after the optical element is placed in an environment with a temperature of 85°C and a relative humidity of 85% for 1000 hours, the average reflectivity of the optical element corresponding to the wavelength of light from 450nm to 600nm is R1000, which can meet the following conditions: 1.05 <R1000 / R0<15。
[0021] According to the imaging lens of the embodiment described in the previous paragraph, the bottom of each ridge-shaped protrusion may be in physical contact with the interposer.
[0022] In the imaging lens according to the embodiment described in the preceding paragraph, a portion of a top portion of the intermediate layer may be in contact with air.
[0023] According to the imaging lens of the embodiment described in the preceding paragraph, the average height of the nanostructure layer is Havg, which can meet the following conditions: 70nm <Havg<350nm。
[0024] According to the imaging lens of the embodiment described in the preceding paragraph, the optical element may be a lens element, and the imaging lens may further include a lens group. The optical element is closer to an object side or an image side than the lens group.
[0025] The imaging lens according to the embodiment described in the preceding paragraph may further include an optical path inflection element, wherein the optical element is closer to the optical path inflection element than the lens assembly.
[0026] In the imaging lens according to the embodiment described in the preceding paragraph, the substrate of the optical element may include an optically active portion and a peripheral portion. The optically active portion has light refractive power. The peripheral portion surrounds the optically active portion. The thickness of the intermediary layer corresponding to the optically active portion may be greater than the thickness of the intermediary layer corresponding to the peripheral portion.
[0027] According to one embodiment of the present disclosure, an electronic device is provided, comprising the imaging lens according to the aforementioned embodiment. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1A A schematic diagram illustrating an imaging lens according to a first embodiment of the present disclosure is shown;
[0029] Figure 1B Drawing in accordance with Figure 1A A schematic diagram of an optical element in the first embodiment;
[0030] Figure 1C Drawing in accordance with Figure 1A A cross-sectional view of the optical element in the first embodiment;
[0031] Figure 1D Drawing in accordance with Figure 1C A partial enlarged view of the optical element in the first embodiment;
[0032] Figure 1E Drawing in accordance with Figure 1C Another partial enlarged view of the optical element in the first embodiment;
[0033] Figure 1F Drawing in accordance with Figure 1A A graph showing the reflectivity of the optical element in the first embodiment in an environment with a temperature of 85°C and a relative humidity of 85%;
[0034] Figure 2 FIG2 is a schematic diagram illustrating an optical element according to a second embodiment of the present disclosure;
[0035] Figure 3A A schematic diagram illustrating an imaging lens according to a third embodiment of the present disclosure is shown;
[0036] Figure 3B Drawing in accordance with Figure 3A A schematic diagram of an optical element in a third embodiment;
[0037] Figure 3C Drawing in accordance with Figure 3A A partial enlarged view of the optical element in the third embodiment;
[0038] Figure 4A A schematic diagram illustrating an imaging lens according to a fourth embodiment of the present disclosure is shown;
[0039] Figure 4B Drawing in accordance with Figure 4A A schematic diagram of an optical element in a fourth embodiment;
[0040] Figure 5A A schematic diagram illustrating an electronic device according to a fifth embodiment of the present disclosure is shown;
[0041] Figure 5B Drawing in accordance with Figure 5A Another schematic diagram of the electronic device in the fifth embodiment;
[0042] Figure 5C Drawing in accordance with Figure 5A A schematic diagram of an image captured by an electronic device in the fifth embodiment;
[0043] Figure 5D Drawing in accordance with Figure 5A A schematic diagram of another image captured by the electronic device in the fifth embodiment;
[0044] Figure 5E Drawing in accordance with Figure 5A A schematic diagram of another image captured by the electronic device in the fifth embodiment;
[0045] Figure 6 A schematic diagram illustrating an electronic device according to a sixth embodiment of the present disclosure is shown;
[0046] Figure 7A A schematic diagram illustrating a vehicle tool according to a seventh embodiment of the present disclosure is shown;
[0047] Figure 7B Drawing in accordance with Figure 7A Another schematic diagram of the vehicle tool in the seventh embodiment; and
[0048] Figure 7C Drawing in accordance with Figure 7A Another schematic diagram of the vehicle tool in the seventh embodiment.
[0049]
Explanation of symbols
[0050] 10,30,40,710: Imaging lenses
[0051] 11,31,41: lens group
[0052] 12,32,42: lens barrel
[0053] 13: Optical path turning element
[0054] 14,34,44: Electronic photosensitive elements
[0055] 100, 200, 300, 400: Optical components
[0056] 110,210,310,410:Substrate
[0057] 111: Optically effective portion
[0058] 112: Peripheral Department
[0059] 120, 220, 320, 420: nanostructured layer
[0060] 121,321: ridge-like protrusions
[0061] 130, 230, 330, 430: Intermediary layer
[0062] 131,231,331,431:First film
[0063] 132,132a,132b,132c,132d,232,332,332a,332b,332c,332d,432: Second film
[0064] 433:Titanium oxide film
[0065] 50,60: Electronic devices
[0066] 521: User Interface
[0067] 522,611,612: Ultra-wide-angle imaging lens
[0068] 523: High-pixel imaging lens
[0069] 524,615,616,617,618: Telephoto lenses
[0070] 525: Imaging signal processing element
[0071] 526,620: Flash module
[0072] 613,614: Wide-angle imaging lens
[0073] 619:TOF module
[0074] 70: Vehicle Tools
[0075] IMG: Imaging surface
[0076] X: Optical axis
[0077] L: Optical path
[0078] LF: Virtual Line
[0079] I1, I2, I3, I4: External space information
[0080] Ti: thickness of the interposer
[0081] Tf1: thickness of the first film
[0082] Tf2: Thickness of each second thin film
[0083] H: Vertical height of the ridge protrusion
[0084] θ: Viewing angle Detailed implementation manners
[0085] The present disclosure provides an imaging lens, which includes an optical element. The optical element includes a substrate, a nanostructure layer, and an intermediate layer. The substrate is a light-transmissive substrate. The nanostructure layer is disposed on a surface of the substrate. The nanostructure layer is an aluminum oxide nanostructure layer, and the nanostructure layer has a plurality of ridge protrusions extending non-directionally. A bottom of each ridge protrusion is closer to the substrate than a top, and each ridge protrusion tapers from the bottom to the top. The intermediate layer is disposed between the substrate and the nanostructure layer, and the intermediate layer includes a plurality of thin films. Each thin film is a silicon dioxide (SiO2) thin film, and the thin films are stacked adjacent to each other. The thickness of the intermediate layer is Ti, which satisfies the following condition: 101 nm < Ti < 450 nm. Thus, in response to the increasing demand for weather resistance, the optical element can still maintain normal performance under harsh environments (such as a temperature of 85°C and a relative humidity of 85%). When the thickness of the intermediate layer satisfies the above condition, it helps to improve the weather resistance of the nanostructure layer. When the intermediate layer is formed by stacking multiple silicon dioxide thin films, it helps to avoid light interference while increasing the thickness of the intermediate layer.
[0086] Furthermore, the optical element can be a lens element or an optical path turning element, and the material of the substrate can be plastic, glass, or molded glass, but is not limited thereto. Moreover, the main component of the nanostructure layer is aluminum oxide, and the main component of each thin film is silicon dioxide. The main component means that the content of the above components is greater than 50%.
[0087] Specifically, the ridge protrusion has a shape of a wide bottom and a narrow top like a mountain ridge. Through the mountain-ridge-like structure, the equivalent refractive index of the nanostructure layer can gradually decrease from the bottom (the foot of the mountain) to the top (the top of the mountain), thereby avoiding total internal reflection of light at the interface. Moreover, the film structure can be measured by SEM (scanning electron microscope) or TEM (transmission electron microscope) according to the situation, but is not limited thereto.
[0088] The thin film can be a first thin film and multiple second thin films. The first thin film and each second thin film are respectively a first silicon dioxide thin film and a second silicon dioxide thin film, and the second thin films are stacked on the first thin film. The thickness of the first thin film is Tf1, and the thickness of each second thin film is Tf2, which can satisfy the following conditions: Tf2 < Tf1; and 45nm < Tf1 < 180nm. By arranging a relatively thick first thin film and relatively thin second thin films, it helps to reduce the coating process and can reduce the impact on the visible light transmittance. Furthermore, the main component of the first thin film and the main component of each second thin film are both silicon dioxide.
[0089] The bottom of each ridge protrusion can be in physical contact with the intermediate layer, and the main component of the ridge protrusion can be different from the main component of the intermediate layer. Thereby, it helps to adjust the equivalent refractive index of the interface. Furthermore, other material thin films, such as titanium dioxide (TiO2) thin films, can be added to the intermediate layer as needed, but it is not limited thereto.
[0090] A partial area of the top of the intermediate layer can be in contact with air. Specifically, the ridge protrusion has micro holes, enabling a partial area of the top of the intermediate layer to be in contact with air, which helps to adjust the equivalent refractive index of the nanostructure layer.
[0091] The optical element can be a lens element, and the imaging lens can further include a lens group, where the optical element is closer to the object side end or the image side end than the lens group. Thereby, it can prevent the optical quality from being affected by environmental conditions. Specifically, the optical element closer to the outside requires better weather resistance.
[0092] The imaging lens can further include an optical path turning element, where the optical element is closer to the optical path turning element than the lens group. The nanostructure layer can reduce stray light generated between the optical path turning element and the optical element.
[0093] The substrate of the optical element can include an optically effective part and a peripheral part. The optically effective part has a light refraction force, the peripheral part is arranged around the optically effective part, and the thickness of the intermediate layer corresponding to the optically effective part is greater than the thickness of the intermediate layer corresponding to the peripheral part. By arranging a relatively thick first thin film on the optically effective part, it helps to reduce the production time. Specifically, the optically effective part has higher requirements for reflectivity and requires a relatively thick intermediate layer to protect the nanostructure layer. Furthermore, by only arranging a relatively thick thin film on the optically effective part, it helps to improve the production efficiency.
[0094] The thickness of the first thin film is Tf1, which can satisfy the following conditions: 50nm < Tf1 < 120nm. Thereby, it helps the optical element to maintain the stability of the nanostructure layer under harsh environmental conditions.
[0095] The thickness of the first thin film is Tf1, and the thickness of each second thin film is Tf2, which can satisfy the following conditions: 1.3 < Tf1 / Tf2 < 55. Thereby, thin film interference can be avoided.
[0096] The thickness of the intermediate layer is Ti, which can satisfy the following conditions: 110 nm < Ti < 330 nm.
[0097] The average reflectivity of the optical element corresponding to the light wavelength from 450 nm to 600 nm is R0, which can satisfy the following conditions: R0 < 0.65%. Thereby, it helps to avoid stray light generated by the imaging lens.
[0098] The average reflectivity of the optical element corresponding to the light wavelength from 450 nm to 600 nm is R0. After the optical element is placed in an environment with a temperature of 85 °C and a relative humidity of 85% for 1000 hours, the average reflectivity of the optical element corresponding to the light wavelength from 450 nm to 600 nm is R1000, which can satisfy the following conditions: 1.05 < R1000 / R0 < 15. Accordingly, the optical element can still maintain a certain degree of functional operation after experiencing a harsh environment.
[0099] The average structural height of the nanostructure layer is Havg, which can satisfy the following conditions: 70 nm < Havg < 350 nm. Specifically, in the field of view of an electron microscope for the nanostructure layer, at least three or more ridge-like protrusions are taken to calculate the average structural height. The structural height of the ridge-like protrusions can be measured destructively. When observed from the cross-section, the vertical height of each ridge-like protrusion is from the absolute bottom (the foot of the mountain part) to the top (the top of the mountain part) of each ridge-like protrusion.
[0100] Each technical feature in the imaging lens of the above disclosure can be combined and configured to achieve the corresponding effects.
[0101] The present disclosure provides an electronic device, wherein the electronic device includes the aforementioned imaging lens.
[0102] According to the above embodiments, specific examples are presented below and will be described in detail with reference to the accompanying drawings.
[0103] <First Embodiment>
[0104] Please refer to Figure 1A , which shows a schematic diagram of the imaging lens 10 in the first embodiment according to the present disclosure. From Figure 1AAs can be seen, the imaging lens 10 includes an optical element 100, a lens assembly 11, a lens barrel 12, an optical path deflection element 13, and an electronic photosensitive element 14. The lens barrel 12 is used to accommodate the optical element 100 and the lens assembly 11. The optical path deflection element 13 is disposed on the image side of the optical element 100. The optical element 100 may be closer to the optical path deflection element 13 than the lens assembly 11. The optical path deflection element 13 is used to deflect the optical path L. The electronic photosensitive element 14 is disposed on an imaging surface IMG of the imaging lens 10. In the first embodiment, the imaging lens 10 is a telephoto imaging lens, and the optical element 100 is a lens element.
[0105] Furthermore, the optical element 100 can be closer to an image side end than the lens assembly 11 to prevent the optical quality from being affected by environmental conditions. Specifically, the optical element 100 closer to the outside needs better weather resistance.
[0106] Please refer to Figures 1B to 1E ,in Figure 1B Drawing in accordance with Figure 1A A schematic diagram of the optical element 100 in the first embodiment, Figure 1C Drawing in accordance with Figure 1A A cross-sectional view of the optical element 100 in the first embodiment, Figure 1D Drawing in accordance with Figure 1C A partial enlarged view of the optical element 100 in the first embodiment, Figure 1E Drawing in accordance with Figure 1C Another partially enlarged view of the optical element 100 in the first embodiment. Figures 1B to 1E As can be seen, the optical element 100 includes a substrate 110, a nanostructured layer 120, and an intermediary layer 130. The substrate 110 is a transparent substrate, wherein the material of the substrate 110 can be plastic, glass, or molded glass, but is not limited thereto. The nanostructured layer 120 is disposed on a surface of the substrate 110. The nanostructured layer 120 is an aluminum oxide nanostructured layer, wherein the nanostructured layer 120 has a plurality of ridges 121 extending in a non-directional direction, wherein a bottom portion of each ridge 121 is closer to the substrate 110 than a top portion thereof, and each ridge 121 tapers from the bottom portion to the top portion. The intermediary layer 130 is disposed between the substrate 110 and the nanostructured layer 120 and comprises a plurality of thin films, wherein each thin film is a silicon dioxide thin film, and the thin films are stacked adjacent to each other. The primary component of the nanostructured layer 120 is aluminum oxide, and the primary component of each thin film is silicon dioxide, wherein the primary component represents a content of the aforementioned component greater than 50%. In response to the increasing demand for weather resistance, the optical element 100 can maintain normal performance in harsh environments (such as temperature 85° C. and relative humidity 85%). Furthermore, the nanostructure layer 120 can reduce stray light between the optical path turning element 13 and the optical element 100.
[0107] Specifically, when the intermediary layer 130 is formed by stacking multiple layers of silicon dioxide films, it helps to avoid light interference caused by increasing the thickness of the intermediary layer 130 .
[0108] Depend on Figure 1B 、 Figure 1D and Figure 1E It can be seen that the thin film can be a first thin film 131 and a second thin film 132, wherein the first thin film 131 and each second thin film 132 are respectively a first silicon dioxide thin film and a second silicon dioxide thin film, and the second thin film 132 and the first thin film 131 are stacked. Figure 1B The second film 132 in FIG. 1 is a schematic diagram of the whole film. Figure 1D and Figure 1E The second films 132 are shown as four second films 132a, 132b, 132c, and 132d. Furthermore, the main component of the first film and the main component of each second film are silicon dioxide.
[0109] Depend on Figure 1D It can be seen that the bottom of each ridge-shaped protrusion 121 is in physical contact with the intermediate layer 130 , and the main component of the ridge-shaped protrusion 121 is different from the main component of the intermediate layer 130 , thereby helping to adjust the equivalent refractive index of the interface.
[0110] Depend on Figure 1D It can be seen that a portion of the top of the intermediary layer 130 is in contact with air. Specifically, the ridge-like protrusions 121 have tiny holes, which allow a portion of the top of the intermediary layer 130 to be in contact with air, helping to adjust the equivalent refractive index of the interface. In detail, each ridge-like protrusion 121 has a shape that is wide at the bottom and narrow at the top, like a ridge. This ridge-like structure can gradually reduce the equivalent refractive index of the nanostructured layer 120 from the bottom (the foot of the mountain) to the top (the top of the mountain), thereby preventing total internal reflection of light at the interface. Furthermore, the film structure can be measured using an SEM or a TEM, depending on the situation, but is not limited to this.
[0111] Depend on Figure 1B and Figure 1C As can be seen, the substrate 110 of the optical element 100 includes an optically effective portion 111 and a peripheral portion 112. The optically effective portion 111 has light-refracting properties, while the peripheral portion 112 surrounds the optically effective portion 111. Furthermore, the thickness of the intermediary layer 130 corresponding to the optically effective portion 111 is greater than the thickness of the intermediary layer 130 corresponding to the peripheral portion 112, thereby reducing production time. Specifically, the optically effective portion 111 has a higher reflectivity requirement, necessitating a thicker intermediary layer 130 to protect the nanostructured layer 120.
[0112] Depend on Figure 1B 、 Figure 1C and Figure 1EIt can be seen that an optical effective portion 111 and a peripheral portion 112 of a substrate 110 are separated by a virtual line LF, and Figure 1E It can be seen that the first thin film 131 can be disposed only on the optical effective portion 111, thereby improving production efficiency.
[0113] From Figure 1D It can be seen that the thickness of the first thin film 131 is Tf1, the thicknesses of the second thin films 132a, 132b, 132c, and 132d are Tf2, the thickness of the intermediate layer 130 is Ti, and the vertical height of the ridge protrusion 121 is H. The parameters satisfy the conditions in Table 1 below.
[0114]
[0115] <00003
[0123]
[0124]
[0125]
[0126]
[0127]
[0128]
[0129]
[0130]
[0131]
[0132]
[0133]
[0134]
[0135] Table 3 shows that the average reflectivity of the optical element 100 for light with a wavelength of 450 nm to 600 nm is R0 (i.e., the value at 0 hrs). After the optical element 100 is placed in an environment at a temperature of 85°C and a relative humidity of 85% for 1000 hours, the average reflectivity of the optical element 100 for light with a wavelength of 450 nm to 600 nm is R1000 (i.e., the value at 1000 hrs), and R1000 / R0 is 3.977. Furthermore, after the optical element 100 is placed in an environment at a temperature of 85°C and a relative humidity of 85% for 120 hours, 250 hours, and 500 hours, the average reflectivity of the optical element 100 for light with a wavelength of 450 nm to 600 nm is the same as the values for 120 hrs, 250 hrs, and 500 hrs, respectively.
[0136] It must be pointed out that Figure 1B and Figure 1C The range of the peripheral portion 112 is indicated by the mesh bottom, so as to distinguish the optically effective portion 111 from the peripheral portion 112. Figure 1B Different line segments are used to represent the arrangement relationship of the nanostructure layer 120, the first film 131 and the second film 132, and Figure 1D The film thickness is not drawn according to the actual film ratio, and is only used to illustrate the configuration of the film.
[0137] <Second embodiment>
[0138] Please refer to Figure 2, which is a schematic diagram of an optical element 200 according to the second embodiment of the present disclosure. Figure 2 As can be seen, the optical element 200 includes a substrate 210, a nanostructured layer 220, and an intermediary layer 230. The substrate 210 is a transparent substrate. The nanostructured layer 220 is disposed on a surface of the substrate 210. The nanostructured layer 220 is an aluminum oxide nanostructured layer. The nanostructured layer 220 has a plurality of ridges (not shown) extending in a non-directional direction. The bottom of each ridge is closer to the substrate 210 than the top, and each ridge tapers from the bottom to the top. The intermediary layer 230 is disposed between the substrate 210 and the nanostructured layer 220 and includes a first thin film 231 and a plurality of second thin films 232. The first thin film 231 and each second thin film 232 are a first silicon dioxide thin film and a second silicon dioxide thin film, respectively. The second thin films 232 are stacked on the first thin film 231.
[0139] Furthermore, the optical element 200 of the second embodiment is a light path bending element for bending a light path, and the optical element 200 can be applied to the imaging lens 10 of the first embodiment.
[0140] It must be pointed out that Figure 2 Different line segments are used to represent the disposition relationship among the nanostructure layer 220 , the first film 231 and the second film 232 , and the second film 232 is shown as a whole. The number of the second films 232 may be four.
[0141] In addition, the structures and configurations of the remaining components of the second embodiment are the same as those of the first embodiment, and will not be further described here.
[0142] <Third embodiment>
[0143] Please refer to Figure 3A , which illustrates a schematic diagram of an imaging lens 30 according to a third embodiment of the present disclosure. Figure 3A As can be seen, the imaging lens 30 has an optical axis X and includes an optical element 300, a lens assembly 31, a lens barrel 32, and an electronic photosensitive element 34. The lens barrel 32 is used to accommodate the optical element 300 and the lens assembly 31, and the electronic photosensitive element 34 is disposed on an imaging surface IMG of the imaging lens 30. In the third embodiment, the imaging lens 30 is a wide-angle imaging lens, and the optical element 300 is a lens element. The optical element 300 may be closer to an object side than the lens assembly 31.
[0144] Please refer to Figure 3B and Figure 3C ,in Figure 3B Drawing in accordance with Figure 3A A schematic diagram of an optical element 300 in the third embodiment, Figure 3C Drawing in accordance with Figure 3AA partial enlarged view of the optical element 300 in the third embodiment. Figure 3B and Figure 3C As can be seen, the optical element 300 includes a substrate 310, a nanostructured layer 320, and an intermediary layer 330. The substrate 310 is a transparent substrate. The nanostructured layer 320 is disposed on a surface of the substrate 310. The nanostructured layer 320 is an aluminum oxide nanostructured layer. The nanostructured layer 320 has a plurality of ridges 321 extending in a non-directional direction. The bottom of each ridge 321 is closer to the substrate 310 than the top, and each ridge 321 tapers from the bottom to the top. The intermediary layer 330 is disposed between the substrate 310 and the nanostructured layer 320 and comprises a plurality of thin films, each of which is a silicon dioxide thin film, stacked adjacently.
[0145] Furthermore, the thin films may be a first thin film 331 and a second thin film 332, wherein the first thin film 331 and each second thin film 332 are respectively a first silicon dioxide thin film and a second silicon dioxide thin film, and the second thin film 332 and the first thin film 331 are stacked. Figure 3B The second film 332 is a schematic diagram of the whole, Figure 3C The second films 332 are shown as four second films 332a, 332b, 332c, and 332d, and the first film 331 is disposed between the second films 332b and 332c.
[0146] Depend on Figure 3C It can be seen that the bottom of each ridge protrusion 321 is in physical contact with the intermediary layer 330 , the main component of the ridge protrusion 321 is different from the main component of the intermediary layer 330 , and a portion of a top area of the intermediary layer 330 is in contact with air.
[0147] In the third embodiment, the thickness of the first film 331 is Tf1, the thickness of each second film 332a, 332b, 332c, 332d is Tf2, the thickness of the intermediate layer 330 is Ti, and the vertical height of the ridge protrusion 321 is H. The parameters meet the conditions in Table 4 below.
[0148]
[0149]
[0150] Furthermore, the average height of the structure of the nanostructure layer 320 is Havg, which can meet the following conditions: 70nm <Havg<350nm。
[0151] It must be pointed out that Figure 3B Different line segments are used to represent the arrangement relationship of the nanostructure layer 320, the first film 331 and the second film 332, and Figure 3CThe film thickness is not drawn according to the actual film ratio, which is only used to illustrate the configuration of the film, and the film configuration can be adjusted according to the situation.
[0152] <Fourth embodiment>
[0153] Please refer to Figure 4A , which illustrates a schematic diagram of an imaging lens 40 according to a fourth embodiment of the present disclosure. Figure 4A As can be seen, the imaging lens 40 has an optical axis X and includes an optical element 400, a lens assembly 41, a lens barrel 42, and an electronic photosensitive element 44. The lens barrel 42 is used to accommodate the optical element 400 and the lens assembly 41, and the electronic photosensitive element 44 is disposed on an imaging surface IMG of the imaging lens 40. In the fourth embodiment, the imaging lens 40 is an ultra-wide-angle imaging lens, and the optical element 400 is a lens element. The optical element 400 may be closer to an object side than the lens assembly 41.
[0154] Please refer to Figure 4B , which is drawn according to Figure 4A Schematic diagram of the optical element 400 in the fourth embodiment. Figure 4B As can be seen, optical element 400 includes a substrate 410, a nanostructured layer 420, and an intermediary layer 430. Substrate 410 is a transparent substrate. Nanostructured layer 420 is disposed on a surface of substrate 410. Nanostructured layer 420 is an aluminum oxide nanostructured layer, and has a plurality of ridges (not shown) extending in a non-directional manner. The bottom of each ridge is closer to substrate 410 than the top, and each ridge tapers from the bottom to the top. Intermediary layer 430 is disposed between substrate 410 and nanostructured layer 420 and comprises a plurality of thin films, each of which is a silicon dioxide thin film, stacked adjacently.
[0155] Specifically, the thin film may be a first thin film 431 and a second thin film 432, wherein the first thin film 431 and each second thin film 432 are a first silicon dioxide thin film and a second silicon dioxide thin film, respectively, and the second thin film 432 and the first thin film 431 are stacked. Figure 4B The second film 432 in FIG. 4 is shown as a whole, and the number of the second films 432 is three.
[0156] Furthermore, according to different situations, the intermediate layer 430 may further include a titanium oxide film 433 , wherein the titanium oxide film 433 is disposed between the nanostructure layer 420 and the second film 432 .
[0157] In the fourth embodiment, the thickness of the first film 431 is Tf1, the thickness of each second film 432 is Tf2, the thickness of the intermediate layer 430 is Ti, the vertical height of the ridge protrusion is H, and the thickness of the titanium oxide film 433 is Tt. The parameters meet the conditions of Table 5 below. The parameter markings of the fourth embodiment can be referred to Figure 1D and Figure 3C In Table 5, the second film 432 corresponds to the upper, middle, and lower parts, respectively, to represent the second film 432 in contact with the titanium oxide film 433, the second film 432 disposed in the middle, and the second film 432 in contact with the first film 431.
[0158]
[0159] It must be pointed out that Figure 4B Different line segments are used to represent the disposition relationship among the nanostructure layer 420 , the first thin film 431 , the second thin film 432 , and the titanium oxide thin film 433 .
[0160] <Fifth embodiment>
[0161] Please refer to Figure 5A and Figure 5B ,in Figure 5A FIG. 1 is a schematic diagram illustrating an electronic device 50 according to a fifth embodiment of the present disclosure. Figure 5B Drawing in accordance with Figure 5A Another schematic diagram of the electronic device 50 in the fifth embodiment. Figure 5A and Figure 5B As can be seen, electronic device 50 is a smartphone and includes an imaging lens and a user interface 521. Specifically, the imaging lenses are an ultra-wide-angle imaging lens 522, a high-pixel imaging lens 523, and a telephoto imaging lens 524, and user interface 521 is a touch screen, but this is not a limitation. Specifically, the imaging lens can be any of the imaging lenses described in the first through fourth embodiments, but this disclosure is not limited thereto.
[0162] The user interface 521 has a touch function, and the user can enter the shooting mode through the user interface 521. The user interface 521 is used to display the image and can be used to manually adjust the shooting angle to switch between different imaging lenses. In this case, the imaging lens focuses the imaging light onto an electronic photosensitive element (not shown) of the imaging lens and outputs an electronic signal related to the image to the image signal processing element (ISP) 525.
[0163] Depend on Figure 5BIt can be seen that, depending on the camera specifications of the electronic device 50, the electronic device 50 may further include an optical image stabilization component (not shown). Furthermore, the electronic device 50 may further include at least one focus assist module (not shown) and at least one sensor element (not shown). The focus assist module may be a flash module 526 that compensates for color temperature, an infrared ranging element, a laser focus module, etc. The sensor element may have the function of sensing physical momentum and actuation energy, such as an accelerometer, a gyroscope, or a Hall Effect Element, to sense shaking and vibration imposed by the user's hand or the external environment. This, in turn, facilitates the autofocus function and optical image stabilization component configured in the imaging lens of the electronic device 50 to achieve good image quality. This helps the electronic device 50 according to the present disclosure to have multiple shooting modes, such as optimized selfies, low-light HDR (High Dynamic Range) imaging, and high-resolution 4K video recording. In addition, the user can directly view the camera's shooting image through the user interface 521 and manually control the framing range on the user interface 521 to achieve a what-you-see-is-what-you-get auto-focus function.
[0164] Furthermore, the imaging lens, optical image stabilization assembly, sensor components, and focus assist module can be disposed on a flexible printed circuit board (FPC) (not shown) and electrically connected to the imaging signal processing component 525 and other related components via a connector (not shown) to execute the shooting process. Current electronic devices, such as smartphones, are trending towards being thinner and lighter. Configuring the imaging lens and related components on a flexible printed circuit board and then integrating the circuits onto the electronic device's mainboard via a connector can meet the structural design and circuit layout requirements within the limited space within the electronic device and provide greater margin. This also allows for more flexible control of the imaging lens' autofocus function via the electronic device's touch screen. In a fifth embodiment, the electronic device 50 can include multiple sensor components and multiple focus assist modules. The sensor components and focus assist modules are disposed on the flexible printed circuit board and at least one additional flexible printed circuit board (not shown), and are electrically connected to the imaging signal processing component 525 and other related components via corresponding connectors to execute the shooting process. In other embodiments (not shown), the sensor element and the auxiliary optical element may also be disposed on a mainboard or other types of carrier boards of the electronic device according to the requirements of the mechanical design and circuit layout.
[0165] In addition, the electronic device 50 may further include but is not limited to a display unit (Display), a control unit (Control Unit), a storage unit (Storage Unit), a random access memory (RAM), a read-only memory unit (ROM) or a combination thereof.
[0166] Figure 5C Drawing in accordance with Figure 5A Schematic diagram of an image captured by the electronic device 50 in the fifth embodiment. Figure 5C It can be seen that the ultra-wide-angle imaging lens 522 can capture images in a wider range and has the function of accommodating more scenery.
[0167] Figure 5D Drawing in accordance with Figure 5A Another image diagram captured by the electronic device 50 in the fifth embodiment. Figure 5D It can be seen that the high-pixel imaging lens 523 can capture images within a certain range and have high pixels, and has the functions of high resolution and low distortion.
[0168] Figure 5E Drawing in accordance with Figure 5A Another image diagram captured by the electronic device 50 in the fifth embodiment. Figure 5E It can be seen that the telephoto imaging lens 524 has a high magnification function, which can capture distant images and magnify them to a high magnification.
[0169] Depend on Figures 5C to 5E It can be seen that by framing with imaging lenses having different focal lengths and combining them with image processing technology, the zoom function can be implemented in the electronic device 50 .
[0170] <Sixth embodiment>
[0171] Please refer to Figure 6 , which illustrates a schematic diagram of an electronic device 60 according to a sixth embodiment of the present disclosure. Figure 6 As can be seen, electronic device 60 is a smartphone and includes an imaging lens. Specifically, the imaging lens comprises ultra-wide-angle imaging lenses 611, 612, wide-angle imaging lenses 613, 614, telephoto imaging lenses 615, 616, 617, 618, and a Time-of-Flight (TOF) module 619. The TOF module 619 can also be another type of imaging lens and is not limited to this configuration. Specifically, the imaging lens can be any of the imaging lenses described in the first to fourth embodiments, but the present disclosure is not limited thereto.
[0172] Furthermore, the telephoto imaging lenses 617 and 618 are used to bend the light path, but the present disclosure is not limited thereto.
[0173] Depending on the camera specifications of the electronic device 60, the electronic device 60 may further include an optical image stabilization component (not shown). Furthermore, the electronic device 60 may further include at least one focus assist module (not shown) and at least one sensor element (not shown). The focus assist module may be a flash module 620 that compensates for color temperature, an infrared rangefinder, a laser focus module, or the like. The sensor element may be capable of sensing physical momentum and actuation energy, such as an accelerometer, a gyroscope, or a Hall Effect Element, to detect movement and jitter imposed by the user's hand or the external environment. This facilitates the autofocus function and optical image stabilization component configured in the imaging lens of the electronic device 60, thereby achieving good image quality. This helps the electronic device 60 according to the present disclosure to have multiple shooting modes, such as optimized selfies, low-light HDR (High Dynamic Range) imaging, and high-resolution 4K video recording.
[0174] In addition, the structures and configurations of the remaining components of the sixth embodiment are the same as those of the fifth embodiment, and will not be further elaborated here.
[0175] <Seventh embodiment>
[0176] Please refer to 7A to 7C ,in Figure 7A A schematic diagram of a vehicle tool 70 according to a seventh embodiment of the present disclosure is shown. Figure 7B Drawing in accordance with Figure 7A Another schematic diagram of the vehicle tool 70 in the seventh embodiment, Figure 7C Drawing in accordance with Figure 7A Another schematic diagram of the vehicle tool 70 in the seventh embodiment. 7A to 7C As can be seen, an electronic device (not shown) is applied to a vehicle tool 70, and the electronic device includes a plurality of imaging lenses 710. In the seventh embodiment, the number of imaging lenses 710 is six, and the imaging lens can be any of the imaging lenses described in the first to fourth embodiments, but the present disclosure is not limited thereto.
[0177] Depend on Figure 7A and Figure 7B As can be seen, imaging lens 710 is a vehicle-use imaging lens. Two imaging lenses 710 are located below the left and right rearview mirrors, respectively, and are used to capture image information within a viewing angle θ. Specifically, viewing angle θ can satisfy the following condition: 40 degrees < θ < 90 degrees. This allows image information to be captured within the left and right lanes.
[0178] Depend on Figure 7BAs can be seen, the other two imaging lenses 710 can be installed in the space inside the vehicle tool 70. Specifically, the two imaging lenses 710 are respectively installed near the interior rearview mirror and the rear window. Furthermore, the imaging lenses 710 can also be installed on the non-mirror surface of the left and right rearview mirrors of the vehicle tool 70, but this is not limited to this.
[0179] Depend on Figure 7C As can be seen, two of the imaging lenses 710 can be positioned at the front and rear ends of the vehicle tool 70. The placement of the imaging lenses 710 at the front and rear ends of the vehicle tool 70 and below the left and right rearview mirrors helps the driver obtain information about the external space outside the cockpit, such as, but not limited to, external space information I1, I2, I3, and I4. This provides more viewing angles, reduces blind spots, and thus helps improve driving safety. Furthermore, the placement of the imaging lenses 710 around the vehicle tool 70 facilitates the identification of road conditions outside the vehicle tool 70, thereby facilitating automated assisted driving.
[0180] Although the present invention has been disclosed above by way of implementation methods and examples, they are not intended to limit the present invention. Anyone with ordinary knowledge in the technical field may make slight changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims.
Claims
1. An imaging lens, characterized in that: Comprising: An optical element, comprising: A substrate, which is a light-transmitting substrate; A nanostructure layer disposed on one surface of the substrate, the nanostructure layer being an aluminum oxide nanostructure layer, wherein the nanostructure layer has a plurality of ridge-like protrusions extending non-directionally, a bottom of each ridge-like protrusion being closer to the substrate than a top thereof, and each ridge-like protrusion tapering from the bottom to the top; and An intermediate layer disposed between the substrate and the nanostructure layer, and the intermediate layer comprises: A first thin film, the first thin film being a first silicon dioxide thin film; and A plurality of second thin films, each second thin film being a second silicon dioxide thin film, and the plurality of second thin films being stacked with the first thin film; Wherein, the thickness of the first thin film is Tf1, the thickness of each second thin film is Tf2, and the thickness of the intermediate layer is Ti, which satisfy the following conditions: Tf2 < Tf1; 45 nm < Tf1 < 180 nm; and 101 nm < Ti < 450 nm.
2. The imaging lens according to claim 1, wherein: The thickness of the first thin film is Tf1, which satisfies the following conditions: 50 nm < Tf1 < 120 nm.
3. The imaging lens according to claim 1, wherein: The thickness of the first thin film is Tf1, and the thickness of each second thin film is Tf2, which satisfy the following conditions: 1.3 < Tf1 / Tf2 < 55.
4. The imaging lens according to claim 1, wherein: The thickness of the intermediate layer is Ti, which satisfies the following conditions: 110 nm < Ti < 330 nm.
5. The imaging lens according to claim 1, wherein: The average reflectivity of the optical element corresponding to the light wavelength from 450 nm to 600 nm is R0, which satisfies the following conditions: R0<0.65%。 6. The imaging lens according to claim 5, wherein: The average reflectivity of the optical element corresponding to the light wavelength from 450 nm to 600 nm is R0. After the optical element is placed in an environment of 85°C and 85% relative humidity for 1000 hours, the average reflectivity of the optical element corresponding to the light wavelength from 450 nm to 600 nm is R1000, which satisfies the following conditions: 1.05 < R1000 / R0 < 15.
7. The imaging lens according to claim 1, wherein: The bottom of each ridge-like protrusion is in physical contact with the intermediate layer.
8. The imaging lens according to claim 7, wherein: A partial area of the top of the intermediate layer is in contact with air.
9. The imaging lens according to claim 1, wherein: The structural average height of the nanostructure layer is Havg, which satisfies the following conditions: 70 nm < Havg < 350 nm.
10. The imaging lens according to claim 1, wherein: The optical element is a lens element, and the imaging lens further comprises: A lens group, the optical element being closer to the object side end or the image side end than the lens group.
11. The imaging lens according to claim 10, wherein: Further comprising: An optical path turning element, the optical element being closer to the optical path turning element than the lens group.
12. The imaging lens according to claim 10, wherein: The substrate of the optical element comprises: An optically effective part, having light refraction power; and A peripheral part, disposed around the optically effective part; Wherein, the thickness of the intermediate layer corresponding to the optically effective part is greater than the thickness of the intermediate layer corresponding to the peripheral part.
13. An imaging lens, characterized in that: Comprising: An optical element, comprising: A substrate, which is a light-transmitting substrate; A nanostructure layer disposed on one surface of the substrate, the nanostructure layer being an aluminum oxide nanostructure layer, wherein the nanostructure layer has a plurality of ridge-like protrusions extending non-directionally, a bottom of each ridge-like protrusion being closer to the substrate than a top thereof, and each ridge-like protrusion tapering from the bottom to the top; and An intermediate layer disposed between the substrate and the nanostructure layer, and comprising: A plurality of thin films, each of which is a silicon dioxide thin film, and the plurality of thin films are stacked adjacent to each other; Wherein, the thickness of the interposer is Ti, which satisfies the following conditions: 101nm <Ti<450nm。 14. The imaging lens according to claim 13, wherein: The average reflectivity of the optical element corresponding to the light wavelength of 450nm to 600nm is R0, which meets the following conditions: R0<0.65%。 15. The imaging lens according to claim 13, wherein: The thickness of the interposer is Ti, which satisfies the following conditions: 110nm <Ti<330nm。 16. The imaging lens according to claim 14, wherein: The average reflectivity of the optical element corresponding to the wavelength of light from 450nm to 600nm is R0. After the optical element is placed in an environment with a temperature of 85°C and a relative humidity of 85% for 1000 hours, the average reflectivity of the optical element corresponding to the wavelength of light from 450nm to 600nm is R1000, which meets the following conditions: 1.05 <R1000 / R0<15。 17. The imaging lens according to claim 13, wherein: The bottom of each of the ridge-shaped protrusions is in physical contact with the interposer.
18. The imaging lens according to claim 17, wherein: A partial area of a top portion of the intermediate layer is in contact with air.
19. The imaging lens according to claim 13, wherein: The average structural height of the nanostructure layer is Havg, which satisfies the following conditions: 70nm <Havg<350nm。 20. The imaging lens according to claim 13, wherein: The optical element is a lens element, and the imaging lens further comprises: A lens group, the optical element is closer to an object side end or an image side end than the lens group.
21. The imaging lens according to claim 20, wherein: Also includes: A light path turning element, the optical element is closer to the light path turning element than the lens group.
22. The imaging lens according to claim 20, wherein: The substrate of the optical element comprises: an optically effective portion having light refraction power; and a peripheral portion disposed around the optically effective portion; The thickness of the intermediate layer corresponding to the optically effective portion is greater than the thickness of the intermediate layer corresponding to the peripheral portion.
23. An electronic device, characterized in that: Include: The imaging lens according to claim 1 or 13.