Oil-water separation membrane, oil-water separation assembly and oil-water separation equipment
By using a sandwich structure with graphene oxide layer and polymer support layer in the oil-water separation membrane, the technical problem of difficulty in separation of emulsified oil is solved, and efficient oil-water separation effect and low-cost treatment process are achieved.
Patent Information
- Application Number
- CN202221862350.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-19
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2032-07-19
AI Technical Summary
Emulsified oil is difficult to effectively separate and treat. The existing membrane separation technology needs to adjust the pH value and pretreat when treating emulsified oil wastewater, and the operating cost is high.
The oil-water separation membrane of sandwich structure consisting of graphene oxide layer and polymer support layer is used. The graphene oxide layer is located between the polymer support layer, with a layer spacing of less than 10 nanometers, and the surface hydrophilic angle of the graphene oxide layer is between 10°-90. °, the polymer support layer is a hydrophilic porous membrane material, used to achieve oil-water separation of emulsified oil.
The separation purity of water in the emulsified oil is achieved between 99% and 99.9%, without adjusting the pH value and pretreatment, reducing operating costs, and simple manufacturing methods and low manufacturing costs.
Smart Images

Figure CN221955863U_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sewage treatment, and in particular to an oil-water separation membrane, an oil-water separation component and an oil-water separation device for treating sewage containing emulsified oil. Background Art
[0002] Normally, water and oil are immiscible, for example, there is a clear boundary between diesel and water. Figure 2 As shown in the left container, due to its low density, diesel will float on the surface of water. Even if it is mechanically stirred and mixed, it will still return to the oil-water separation state after standing for a period of time. Emulsified oil is generally a surfactant added to oil or water, which can make the oil dispersed and suspended in the water phase in the form of small oil droplets to form an oil-water mixture. For example, Figure 3 As shown in the figure, the surfactant sodium dodecyl sulfate has a hydrophilic head at one end and a hydrophobic tail at the other end. The hydrophobic tail will connect with the oil molecule, and the hydrophilic head will connect with the water molecule. After the oil-water mixed solution is externally mechanically stirred and mixed, an oil-in-water emulsion (or emulsified oil) with small oil droplets dispersed and suspended inside will be formed. Figure 2 As shown in the container on the right of the emulsified oil, it is difficult to effectively separate and process it because the emulsified oil is relatively stable.
[0003] Membrane separation technology is used to treat emulsified oil wastewater, which has unique technical advantages: by selecting appropriate membrane materials and component forms, there is no need to adjust the pH value and pretreatment; there is no need to destroy the emulsion, which reduces the operating cost. Therefore, in order to achieve a better oil-water separation effect when treating emulsified oil, it is necessary to provide an oil-water separation membrane, oil-water separation component and oil-water separation equipment. Utility Model Content
[0004] One of the embodiments of the present specification provides an oil-water separation membrane, comprising: a graphene oxide layer; and two polymer support layers; wherein the graphene oxide layer is located between the two polymer support layers to form a sandwich structure; the graphene oxide layer comprises at least two graphene oxide sheets, and the interlayer spacing between two adjacent graphene oxide sheets in the at least two graphene oxide sheets is within a range of less than 10 nanometers.
[0005] In some embodiments, the graphene oxide layer has a thickness in the range of 100 nanometers to 10 micrometers.
[0006] In some embodiments, a diameter of any one of the at least two graphene oxide sheets is in the range of 100 nanometers to 10 micrometers.
[0007] In some embodiments, the surface hydrophilicity angle of the graphene oxide layer is in the range of 10°-90°.
[0008] In some embodiments, the polymer support layer has a thickness in the range of 1 micrometer to 100 micrometers.
[0009] In some embodiments, the polymer support layer is a hydrophilic porous membrane material, the surface hydrophilic angle of the polymer support layer is in the range of 20°-90°, and the pore size of the polymer support layer is in the range of 10 nanometers-100 micrometers.
[0010] In some embodiments, the material of the polymer support layer is one or more of polypropylene, polysulfone, polyethersulfone, polyethylene, polyvinylidene fluoride, polyaniline, and the like.
[0011] In some embodiments, the oil-water separation membrane has a separation purity of water in the emulsified oil in the range of 99%-99.9%.
[0012] One of the embodiments of the present specification also provides an oil-water separation component, comprising the oil-water separation membrane as described in any embodiment of the present specification.
[0013] One of the embodiments of the present specification also provides an oil-water separation device, including an oil-water separation membrane or an oil-water separation component as described in any embodiment of the present specification. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] This specification will be further described in the form of exemplary embodiments, which will be described in detail by the accompanying drawings. These embodiments are not restrictive, and in these embodiments, the same number represents the same structure, wherein:
[0015] Figure 1 is an exemplary cross-sectional view of an oil-water separation membrane according to some embodiments of the present specification;
[0016] Figure 2 is an exemplary schematic diagram of an oil-water obvious boundary state and an emulsified oil state according to some embodiments of the present specification;
[0017] Figure 3 is a molecular structure diagram of a surfactant according to some embodiments of this specification;
[0018] Figure 4 is an exemplary cross-sectional view of an oil-water separation process according to some embodiments of the present specification;
[0019] Figure 5 It is a statistical diagram of oil droplet size observed by a dynamic light scattering spectrophotometer according to some embodiments of this specification;
[0020] Fig. 6A is an optical microscope photograph of the emulsified oil shown in some embodiments of this specification;
[0021] Figure 6B is an optical microscope photograph of the filtered clean water shown in some embodiments of this specification;
[0022] Fig. 7A It is a photograph of the experimental process of the oil-water separation process shown in some embodiments of this specification;
[0023] Figure 7B It is a UV spectrometer data diagram of various substances shown in some embodiments of this specification. DETAILED DESCRIPTION
[0024] In order to more clearly illustrate the technical solutions of the embodiments of this specification, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some examples or embodiments of this specification. For ordinary technicians in this field, this specification can also be applied to other similar scenarios based on these drawings without creative work. Unless it is obvious from the language environment or otherwise explained, the same reference numerals in the figures represent the same structure or operation.
[0025] It should be understood that the "system", "device", "unit" and / or "module" used herein are a method for distinguishing different components, elements, parts, portions or assemblies at different levels. However, if other words can achieve the same purpose, the words can be replaced by other expressions.
[0026] As shown in this specification and claims, unless the context clearly indicates an exception, the words "a", "an", "an" and / or "the" do not refer to the singular and may also include the plural. Generally speaking, the terms "comprise" and "include" only indicate the inclusion of the steps and elements that have been clearly identified, and these steps and elements do not constitute an exclusive list. The method or device may also include other steps or elements.
[0027] Flowcharts are used in this specification to illustrate the operations performed by the system according to the embodiments of this specification. It should be understood that the preceding or following operations are not necessarily performed precisely in order. Instead, the steps may be processed in reverse order or simultaneously. At the same time, other operations may also be added to these processes, or one or more operations may be removed from these processes.
[0028] Figure 1 is an exemplary cross-sectional view of an oil-water separation membrane according to some embodiments of the present specification.
[0029] like Figure 1As shown, the oil-water separation membrane 100 may include a graphene oxide layer 110 and two polymer support layers 120. In some embodiments, the graphene oxide layer 110 may be located between two polymer support layers 120 to form a sandwich-like structure of "polymer support layer-graphene oxide layer-polymer support layer".
[0030] In some embodiments, the graphene oxide layer 110 may include at least two graphene oxide sheets, for example, 200, 500, 1000, 2000, 3000, etc. In some embodiments, as shown in Figure 1, at least two graphene oxide sheets may completely overlap. In some embodiments, at least two graphene oxide sheets may partially overlap.
[0031] In some embodiments, the interlayer spacing (in Figure 4 In the direction indicated by the dashed arrow P shown, the distance between two adjacent graphene oxide sheets) can be in the range of less than 10 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 9 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 8 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 7 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 6 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 5 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 4 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 3 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in at least two graphene oxide sheets can be in the range of less than 2 nanometers. In some embodiments, the interlayer spacing between two adjacent graphene oxide sheets in the at least two graphene oxide sheets may be in a range of less than 1 nanometer.
[0032] In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 100 nanometers to 10 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 200 nanometers to 9.5 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 300 nanometers to 9.0 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 400 nanometers to 8.5 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 500 nanometers to 8.0 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 600 nanometers to 7.5 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 800 nanometers to 7.0 micrometers. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 900 nanometers to 6.5 microns. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 1.0 microns to 6.0 microns. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 1.5 microns to 5.5 microns. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 2.0 microns to 5.0 microns. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 2.5 microns to 4.5 microns. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 3.0 microns to 4.0 microns. In some embodiments, the diameter of any one of the at least two graphene oxide sheets may be in the range of 3.5 microns to 3.8 microns. In some embodiments, the diameter of the graphene oxide sheet may be understood as an equivalent diameter.
[0033] In some embodiments, the thickness of the graphene oxide layer 110 (in the direction in which small molecules such as water molecules pass through the graphene oxide layer) Figure 4In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 200 nanometers to 9.5 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 300 nanometers to 9.0 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 400 nanometers to 8.5 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 500 nanometers to 8.0 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 600 nanometers to 7.5 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 700 nanometers to 7.0 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 800 nanometers to 6.5 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 900 nanometers to 6.0 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 1.0 micrometers to 5.5 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 1.5 micrometers to 5.0 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 2.0 micrometers to 4.5 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 2.5 micrometers to 4.0 micrometers. In some embodiments, the thickness of the graphene oxide layer 110 may be in the range of 3.0 micrometers to 3.5 micrometers.
[0034] In some embodiments, the surface hydrophilicity angle of the graphene oxide layer 110 is in the range of 10°-90°. In some embodiments, the surface hydrophilicity angle of the graphene oxide layer 110 is in the range of 20°-80°. In some embodiments, the surface hydrophilicity angle of the graphene oxide layer 110 is in the range of 30°-70°. In some embodiments, the surface hydrophilicity angle of the graphene oxide layer 110 is in the range of 40°-60°. In some embodiments, the surface hydrophilicity angle of the graphene oxide layer 110 is in the range of 50°-55°.
[0035] In some embodiments, the thickness of the polymer support layer 120 may be in the range of 1 micron to 100 microns. In some embodiments, the thickness of the polymer support layer 120 may be in the range of 10 microns to 90 microns. In some embodiments, the thickness of the polymer support layer 120 may be in the range of 20 microns to 80 microns. In some embodiments, the thickness of the polymer support layer 120 may be in the range of 30 microns to 70 microns. In some embodiments, the thickness of the polymer support layer 120 may be in the range of 40 microns to 60 microns. In some embodiments, the thickness of the polymer support layer 120 may be in the range of 50 microns to 55 microns.
[0036] In some embodiments, the polymer support layer 120 may be a hydrophilic porous membrane material. In some embodiments, the surface hydrophilic angle of the polymer support layer 120 may be in the range of 20°-90°. In some embodiments, the surface hydrophilic angle of the polymer support layer 120 may be in the range of 30°-80°. In some embodiments, the surface hydrophilic angle of the polymer support layer 120 may be in the range of 40°-70°. In some embodiments, the surface hydrophilic angle of the polymer support layer 120 may be in the range of 50°-60°.
[0037] In some embodiments, the pore size of the polymer support layer 120 is in the range of 10 nanometers to 100 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 50 nanometers to 95 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 100 nanometers to 90 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 200 nanometers to 85 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 300 nanometers to 80 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 400 nanometers to 75 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 500 nanometers to 70 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 600 nanometers to 65 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 700 nanometers to 60 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 800 nanometers to 55 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 900 nanometers to 50 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 1 micron to 45 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 5 microns to 40 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 10 microns to 35 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 15 microns to 30 microns. In some embodiments, the pore size of the polymer support layer 120 is in the range of 20 microns to 25 microns.
[0038] In some embodiments, the material of the polymer support layer 120 may be one or more of polypropylene, polysulfone, polyethersulfone, polyethylene, polyvinylidene fluoride, polyaniline, and the like.
[0039] By attaching two polymer support layers 120 to the upper and lower surfaces of the graphene oxide layer 110 to form a sandwich-like structure of "polymer support layer-graphene oxide layer-polymer support layer", the polymer support layer 120 can protect the middle graphene oxide layer 110 from physical damage, making it easier to separate the oil and water in the emulsified oil, thereby improving the quality of the oil-water separation membrane, and the manufacturing method is simple and the manufacturing cost is low.
[0040] In the embodiments of this specification, the method for preparing the oil-water separation membrane may include the following steps.
[0041] Step (1) Preparation of graphene oxide water-based dispersion:
[0042] In some embodiments, the preparation of the graphene oxide water-based dispersion may include: adding 1 kg of graphite powder, 4-6 kg of potassium permanganate powder and 40-60 L of concentrated sulfuric acid with a concentration of more than 94% to a reactor, and stirring thoroughly; heating the reactor to 40-50° C. and maintaining this temperature for continuous stirring for 4-8 hours; then cooling the reactor to below 10° C., adding 40-60 kg of ice cubes made of pure water and continuing to stir until the ice cubes are completely melted; continuing to stir, and slowly adding 2-3 L of hydrogen peroxide to obtain a first reaction solution; filtering the first reaction solution through a filter press to separate a first filter solid; mixing the first filter solid with 40-60 L of 5%- The invention discloses a method for preparing a graphene oxide solid. The method comprises the steps of: adding a 10% hydrochloric acid solution to a reactor and stirring to obtain a second reaction solution; then filtering the second reaction solution through a filter press to separate and obtain a second filtered solid; drying the second filtered solid to obtain a graphene oxide solid; taking 200-500 g of the graphene oxide solid, adding it to 200 L of pure water, and stirring; after stirring, ultrasonically treating the solution to uniformly disperse the graphene oxide sheets, and obtaining a 1-10 wt % graphene oxide water-based dispersion.
[0043] In some embodiments, the particle size of the graphite powder may be in the range of 100 mesh to 10000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 200 mesh to 8000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 400 mesh to 6000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 800 mesh to 5000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 900 mesh to 4000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 1100 mesh to 3000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 1300 mesh to 2000 mesh. In some embodiments, the particle size of the graphite powder may be in the range of 1600 mesh to 1800 mesh.
[0044] In some embodiments, the mass ratio of graphene oxide solid to water may be in the range of (0.2-0.5): 100. In some embodiments, the mass ratio of graphene oxide solid to water may be in the range of (0.25-0.45): 100. In some embodiments, the mass ratio of graphene oxide solid to water may be in the range of (0.3-0.4): 100. In some embodiments, the mass ratio of graphene oxide solid to water may be in the range of (0.34-0.36): 100.
[0045] Step (2) Preparation of graphene oxide layer:
[0046] The graphene oxide water-based dispersion was poured on a 1m 2The surface of the microfiltration membrane support layer is coated with a scraper or negative pressure filter to remove the aqueous solution in the graphene oxide water-based dispersion solution, and the water flows through the microfiltration membrane support layer and flows away from the bottom. Then, a low-temperature drying treatment is performed under normal pressure to form a layer of graphene oxide with a thickness of 100 nanometers to 10 microns on the surface of the microfiltration membrane.
[0047] In some embodiments, the volume of the graphene oxide water-based dispersion may be 2 L to 6 L. In some embodiments, the volume of the graphene oxide water-based dispersion may be 3 L to 5 L. In some embodiments, the volume of the graphene oxide water-based dispersion may be 4 L to 4.5 L.
[0048] In some embodiments, the thickness of the graphene oxide layer may be in the range of 100 nanometers to 10 microns (i.e., 0.1 micron to 10 microns). In some embodiments, the thickness of the graphene oxide layer may be in the range of 0.5 microns to 9.5 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 1.0 micron to 9.0 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 1.5 microns to 8.5 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 2.0 microns to 8.0 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 2.5 microns to 7.5 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 3.0 microns to 7.0 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 3.5 microns to 6.5 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 4.0 microns to 6.0 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 4.5 microns to 5.5 microns. In some embodiments, the thickness of the graphene oxide layer may be in the range of 5.0 microns to 5.3 microns.
[0049] Step (3) Preparation of a polymer support layer-graphene oxide layer-polymer support layer sandwich structure:
[0050] In some embodiments, the polymer support layer can be attached to the upper and lower surfaces of the graphene oxide layer using a melt-blowing method, an electrostatic spinning method, or a phase change method. In some embodiments, the material of the polymer support layer can be one or more of polypropylene, polysulfone, polyethersulfone, polyethylene, polyvinylidene fluoride, polyaniline, etc.
[0051] In some embodiments, the phase change method is used as an example to describe the preparation of a sandwich structure of polymer support layer-graphene oxide layer-polymer support layer.
[0052] In some embodiments, a polysulfone or polyethersulfone organic solution is added to an organic solvent such as dimethylacetamide, dimethylacetamide or methyl pyrrolidone to obtain a mixed solution; the mixed solution is heated to 70° C. and stirred for 12 hours, then degassed under negative pressure and cooled to room temperature to obtain a polysulfone solution or polyethersulfone solution with a weight percentage of 5-8wt%.
[0053] In some embodiments, a polysulfone solution or a polyethersulfone solution is scraped on the surface of the graphene oxide layer, and the entire membrane (a microfiltration membrane having a graphene oxide layer deposited on the surface and a polysulfone solution or a polyethersulfone solution on the surface of the graphene oxide layer) is immersed in a 20-70°C water bath for 12 hours; then the entire membrane is taken out of the water bath and dried at normal pressure, and an external force is used to separate the microfiltration membrane support layer from the entire membrane to obtain a graphene oxide layer having a polysulfone or polyethersulfone on the surface.
[0054] In some embodiments, a polysulfone solution or a polyethersulfone solution is scraped onto the other surface of the graphene oxide layer, and the entire membrane is immersed in a 20-70°C water bath for 12 hours; then the entire membrane is taken out of the water bath, dried at normal pressure, and packaged into an oil-water separation component.
[0055] Figure 4 is an exemplary cross-sectional view of an oil-water separation process according to some embodiments of this specification. Figure 4 As shown, 410 may represent a graphene oxide sheet, 420 may represent a small oil droplet, and 430 may represent a large oil droplet.
[0056] The oil-water separation membrane shown in some embodiments of this specification utilizes the synergistic effect of the two principles of size exclusion and affinity of the base liquid to perform the oil-water separation process of the emulsified oil.
[0057] Graphene oxide sheets have hydrophilic functional groups at the edges and surface defects, and superhydrophobic surfaces on other lattice surfaces. Figure 4 As shown, the graphene oxide layer composed of graphene oxide sheets 410 has a small interlayer spacing (less than 10 nanometers). When the emulsified oil contacts the surface of the graphene oxide layer, the water dispersed between the small oil droplets will enter the graphene oxide layer through the edge or surface defects of the graphene oxide sheet 410 and pass through the graphene oxide layer. The size of the small oil droplets is much larger than the interlayer spacing between the graphene oxide sheets 410, and the surface repulsion between the hydrophilic functional groups of the surfactant and the hydrophilic functional groups of the graphene oxide sheet 410 makes it difficult for the small oil droplets to enter and pass through the graphene oxide layer. As the oil-water separation process proceeds, the water between the small oil droplets decreases, causing the distance between the small oil droplets to be greatly reduced. The small oil droplets will condense into large oil droplets, and finally form a continuous oil liquid containing a surfactant, while the water that passes through the graphene oxide layer becomes clear water without oil, and finally completes the oil-water separation process of the emulsified oil.
[0058] In some embodiments, the separation purity of water in the emulsified oil by the oil-water separation membrane 100 may be in the range of 99%-99.9%. In some embodiments, the separation purity of water in the emulsified oil by the oil-water separation membrane 100 may be in the range of 99.1%-99.8%. In some embodiments, the separation purity of water in the emulsified oil by the oil-water separation membrane 100 may be in the range of 99.2%-99.7%. In some embodiments, the separation purity of water in the emulsified oil by the oil-water separation membrane 100 may be in the range of 99.3%-99.6%. In some embodiments, the separation purity of water in the emulsified oil by the oil-water separation membrane 100 may be in the range of 99.4%-99.5%.
[0059] Example
[0060] 1. Preparation of graphene oxide water-based dispersion:
[0061] 1 kg of graphite powder with a particle size of 500 mesh, 4 kg of potassium permanganate powder and 40 liters of concentrated sulfuric acid with a concentration of more than 94% are added to the reactor and stirred thoroughly. Then the reactor is heated to 40-50°C and stirred for 6 hours at a temperature of 40-50°C. Then the reactor is cooled to below 10°C and 40 kg of ice cubes made of pure water are added. Stirring is continued until all the ice cubes melt. Continue stirring and slowly add 2 liters of hydrogen peroxide to obtain a first reaction solution. The first reaction solution is then filtered through a filter press to separate the first filter press solid. The first filter press solid is added to a reactor together with 40 liters of 5% hydrochloric acid solution and stirred to obtain a second reaction solution. Then the second reaction solution is filtered through a filter press to separate the second filter press solid, and the second filter press solid is dried to obtain graphene oxide solid. Take 200 grams of graphene oxide solid, add it to 100 liters of pure water, and stir. The stirred aqueous solution is subjected to ultrasonic treatment to uniformly disperse the graphene oxide sheets to obtain a graphene oxide water-based dispersion.
[0062] 2. Preparation of graphene oxide layer:
[0063] 5 liters of graphene oxide water-based dispersion was poured on the surface of 1 square meter of microfiltration membrane support layer, and vacuum was drawn on the other side of the microfiltration membrane support layer, so that water flowed through the microfiltration membrane support layer from the bottom surface, and a 2 micron thick graphene oxide layer was deposited on one side of the microfiltration membrane support layer. Then the microfiltration membrane with the graphene oxide layer deposited on the surface was dried at room temperature and pressure.
[0064] 3. Preparation of polymer support layer-graphene oxide layer-polymer support layer sandwich structure:
[0065] 600 g of polysulfone was added into 10 liters of dimethylacetamide solvent to obtain a mixed solution; the mixed solution was heated to 60° C. and stirred for 12 hours, then degassed under negative pressure and cooled to room temperature to obtain a polysulfone solution.
[0066] A 50-micron-thick polysulfone solution is scraped on the surface of one side of the graphene oxide layer, and the entire membrane (a microfiltration membrane with a graphene oxide layer deposited on the surface and a polysulfone solution on the surface of the graphene oxide layer) is immersed in a 40°C water bath for 12 hours; then the entire membrane is taken out of the water bath, and then dried at normal pressure, and the microfiltration membrane support layer is separated from the entire membrane with auxiliary external force to obtain a graphene oxide layer with polysulfone on the surface.
[0067] A 50-micron-thick polysulfone solution is scraped on the other side of the graphene oxide layer, and the graphene oxide layer with polysulfone on the surface is immersed in a 40°C water bath for 12 hours; then the graphene oxide layer with polysulfone on the surface is taken out of the water bath, dried under normal pressure, and packaged into an oil-water separation component.
[0068] 4. Emulsified oil and water separation experiment:
[0069] Mix 1 liter of toluene solution, 1 liter of pure water and 20 grams of sodium dodecyl sulfate and stir for 12 hours to prepare an emulsified oil. Figure 5 As shown in Figure 2, the diameter of the toluene droplets in the emulsified oil ranges from a few hundred nanometers to a few hundred micrometers. Fig. 6A As shown, small toluene droplets dispersed in the emulsified oil can be clearly seen under a microscope.
[0070] like Fig. 7A As shown, the emulsified oil is poured into the glass tube above the oil-water separation membrane. The emulsified oil is white and turbid. A vacuum pump is used to create negative pressure below the oil-water separation membrane. The water in the emulsified oil passes through the oil-water separation membrane and flows into the conical flask below the membrane. The filtered clear water in the conical flask (or called filtered clear water) is transparent and clear. The oil in the emulsified oil remains in the glass tube above the oil-water separation membrane. The filtered clear water in the conical flask is observed under an optical microscope. Figure 6B As shown, no dispersed oil droplets were observed.
[0071] Use UV spectrometer data to analyze oil (toluene), clean water (or original clean water), emulsified oil and filtered clean water, such as Figure 7B As shown, it can be seen that under the same absorbance, the light wavelength of oil (toluene) is the largest, the light wavelength of clean water is the lowest, the light wavelength of emulsified oil is between clean water and oil (toluene), and the light wavelength of filtered clean water is exactly the same as that of original clean water, which proves that the clean water in the emulsified oil has been completely separated.
[0072] The oil-water separation membrane prepared by the above method was tested to have a total thickness of about 100 microns, of which the graphene oxide layer was about 2 microns; when separating the emulsified oil of toluene and water, the water flux was 50L / m 2 / h, the purity of separated water is in the range of 99%-99.9%.
[0073] Some embodiments of this specification also provide an oil-water separation component, which includes the oil-water separation membrane described in this specification. For more technical details about the oil-water separation membrane, please refer to Figure 1 The relevant description will not be repeated here.
[0074] Some embodiments of this specification also provide an oil-water separation device, which includes the oil-water separation membrane or oil-water separation component described in this specification. For more technical details about the oil-water separation membrane, please refer to Figure 1 The relevant description will not be repeated here.
[0075] The beneficial effects that may be brought about by the embodiments of this specification include but are not limited to: (1) by preparing a sandwich structure of a polymer support layer-graphene oxide layer-polymer support layer, the polymer support layer can protect the middle graphene oxide layer from physical damage, so that the quality of the oil-water separation membrane is better, and the manufacturing method is simple and the manufacturing cost is low; (2) because the graphene oxide layer has hydrophilic functional groups at the edges and surface defects, and the interlayer spacing between two adjacent graphene oxide sheets is less than 10 nanometers, the water dispersed between the small oil droplets will enter the graphene oxide layer through the edges or surface defects of the graphene oxide sheets and pass through the graphene oxide layer, and has a good blocking effect on the small oil droplets in the emulsified oil, and can better filter the water in the emulsified oil. The purity of the separated water is in the range of 99%-99.9%, and it has the advantages of good oil-water separation effect (low water content in the separated oil, low oil content in the separated water) and fast separation speed. It should be noted that different embodiments may produce different beneficial effects. In different embodiments, the beneficial effects that may be produced may be any one or a combination of the above, or any other beneficial effects that may be obtained.
[0076] The basic concepts have been described above. Obviously, for those skilled in the art, the above detailed disclosure is only for example and does not constitute a limitation of this specification. Although not explicitly stated here, those skilled in the art may make various modifications, improvements and corrections to this specification. Such modifications, improvements and corrections are suggested in this specification, so such modifications, improvements and corrections still belong to the spirit and scope of the exemplary embodiments of this specification.
[0077] At the same time, this specification uses specific words to describe the embodiments of this specification. For example, "one embodiment", "an embodiment", and / or "some embodiments" refer to a certain feature, structure or characteristic related to at least one embodiment of this specification. Therefore, it should be emphasized and noted that "one embodiment" or "an embodiment" or "an alternative embodiment" mentioned twice or more in different positions in this specification does not necessarily refer to the same embodiment. In addition, certain features, structures or characteristics in one or more embodiments of this specification can be appropriately combined.
[0078] In addition, unless explicitly stated in the claims, the order of the processing elements and sequences described in this specification, the use of alphanumeric characters, or the use of other names are not intended to limit the order of the processes and methods of this specification. Although the above disclosure discusses some currently considered useful utility model embodiments through various examples, it should be understood that such details are only for illustrative purposes, and the attached claims are not limited to the disclosed embodiments. On the contrary, the claims are intended to cover all modifications and equivalent combinations that are consistent with the essence and scope of the embodiments of this specification. For example, although the system components described above can be implemented by hardware devices, they can also be implemented only by software solutions, such as installing the described system on an existing server or mobile device.
[0079] Similarly, it should be noted that in order to simplify the description disclosed in this specification and thus help understand one or more utility model embodiments, in the above description of the embodiments of this specification, multiple features are sometimes combined into one embodiment, figure or description thereof. However, this disclosure method does not mean that the features required by the object of this specification are more than the features mentioned in the claims. In fact, the features of the embodiments are less than all the features of the single embodiment disclosed above.
[0080] In some embodiments, numbers describing the number of components and attributes are used. It should be understood that such numbers used in the description of the embodiments are modified by the modifiers "about", "approximately" or "substantially" in some examples. Unless otherwise specified, "about", "approximately" or "substantially" indicate that the numbers are allowed to vary by ±20%. Accordingly, in some embodiments, the numerical parameters used in the specification and claims are approximate values, which may change according to the required features of individual embodiments. In some embodiments, the numerical parameters should take into account the specified significant digits and adopt the general method of retaining digits. Although the numerical domains and parameters used to confirm the breadth of their range in some embodiments of this specification are approximate values, in specific embodiments, the setting of such numerical values is as accurate as possible within the feasible range.
[0081] Each patent, patent application, patent application publication, and other materials, such as articles, books, specifications, publications, documents, etc., cited in this specification are hereby incorporated by reference in their entirety. Except for application history documents that are inconsistent with or conflicting with the contents of this specification, documents that limit the broadest scope of the claims of this specification (currently or later attached to this specification) are also excluded. It should be noted that if the descriptions, definitions, and / or use of terms in the materials attached to this specification are inconsistent or conflicting with the contents described in this specification, the descriptions, definitions, and / or use of terms in this specification shall prevail.
[0082] Finally, it should be understood that the embodiments described in this specification are only used to illustrate the principles of the embodiments of this specification. Other variations may also fall within the scope of this specification. Therefore, as an example and not a limitation, alternative configurations of the embodiments of this specification may be considered consistent with the teachings of this specification. Accordingly, the embodiments of this specification are not limited to the embodiments explicitly introduced and described in this specification.
Claims
1. An oil-water separation membrane, characterized in that: include: Graphene oxide layer; as well as Two polymer support layers; wherein, The graphene oxide layer is located between the two polymer support layers to form a sandwich structure; The graphene oxide layer comprises at least two graphene oxide sheets, The interlayer spacing between two adjacent graphene oxide sheets in the at least two graphene oxide sheets is less than 10 nanometers.
2. The oil-water separation membrane according to claim 1, characterized in that: The thickness of the graphene oxide layer is in the range of 100 nanometers to 10 micrometers.
3. The oil-water separation membrane according to claim 1, characterized in that: The diameter of any one of the at least two graphene oxide sheets is in the range of 100 nanometers to 10 micrometers.
4. The oil-water separation membrane according to claim 1, characterized in that: The surface hydrophilicity angle of the graphene oxide layer is in the range of 10°-90°.
5. The oil-water separation membrane according to claim 1, characterized in that: The thickness of the polymer support layer is in the range of 1 micron to 100 microns.
6. The oil-water separation membrane according to claim 1, characterized in that: The polymer support layer is a hydrophilic porous membrane material, the surface hydrophilic angle of the polymer support layer is in the range of 20°-90°, and the pore size of the polymer support layer is in the range of 10 nanometers-100 micrometers.
7. The oil-water separation membrane according to claim 1, characterized in that: The material of the polymer support layer is polypropylene, polysulfone, polyethersulfone, polyethylene, polyvinylidene fluoride or polyaniline.
8. The oil-water separation membrane according to claim 1, characterized in that: The separation purity of water in emulsified oil by the oil-water separation membrane is in the range of 99%-99.9%.
9. An oil-water separation component, characterized in that: It comprises the oil-water separation membrane as described in any one of claims 1 to 8.
10. An oil-water separation device, characterized in that: It comprises the oil-water separation membrane according to any one of claims 1 to 8 or the oil-water separation component according to claim 9.