Perovskite / crystalline silicon laminated cell
By introducing buffer layer and double-layer design into perovskite/crystalline silicon stacked batteries, the parasitic absorption problem of top battery functional layer is solved, the battery efficiency and stability are improved, and the industry of perovskite stacked solar cells is promoted. change.
Patent Information
- Application Number
- CN202323616235.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2033-12-28
AI Technical Summary
In existing perovskite/crystalline silicon stacked solar cells, there are problems such as severe parasitic absorption of the top cell functional layer and difficult deposition process, resulting in low device efficiency.
The buffer layer is used to protect the perovskite absorber layer while improving the airtightness of the cell, and optimize the energy level matching between the film layers through a double-layer design, including the arrangement between the inorganic hole transport layer and the organic molecule self-assembly layer. Organic molecules self-assemble layers to reduce parasitic absorption and optimize process flow to reduce open circuit voltage loss.
The efficiency and stability of perovskite/crystalline silicon stacked batteries have been significantly improved, the industrialization of perovskite stacked solar cells has been promoted, and the production cost and process complexity have been reduced.
Smart Images

Figure CN222073786U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the field of solar cells, and in particular relates to a perovskite / crystalline silicon stacked cell. Background Art
[0002] In recent years, environmental pollution and energy shortage have become the focus of world attention. Solar energy, with its high reserves, wide distribution, renewable and pollution-free characteristics, is considered to be the key to solving the problems of energy shortage and environmental pollution. As an effective way to utilize solar energy, the basic principle of solar cells is to use the photovoltaic effect to directly convert solar radiation energy into electrical energy. Perovskite solar cells (PSCs) are a new type of solar cells with significant advantages such as low manufacturing cost and high photoelectric conversion efficiency. Perovskite solar cells have attracted widespread attention due to their constantly refreshing conversion efficiency, and research on industrialization is also constantly advancing.
[0003] At present, perovskite crystalline silicon / tandem cells are developing rapidly, and the highest device efficiency can reach 33.7%. However, most perovskite crystalline silicon / tandem solar cells are inverted pin structures. The inverted pin structure of PVK / TOPCon tandem cells requires the change of the production process of crystalline silicon bottom cells, which is not conducive to the existing process production. At present, the efficiency of formal perovskite crystalline silicon tandem cells is much lower than that of inverted tandem cell structures due to the serious parasitic absorption of the top cell functional layer.
[0004] Therefore, it is urgent to solve the problems of severe parasitic absorption in formal perovskite / crystalline silicon tandem cells and difficult perovskite top cell deposition process. Utility Model Content
[0005] In view of the shortcomings of the prior art, the purpose of the utility model is to provide a perovskite / crystalline silicon tandem cell. The utility model improves the air tightness of the cell while protecting the perovskite light-absorbing layer with the help of a buffer layer, optimizes the energy level matching between the film layers, reduces the loss of open-circuit voltage, improves the efficiency and stability of the tandem cell, and significantly improves the optical management of the perovskite / crystalline silicon tandem cell, which is conducive to promoting the industrialization of perovskite tandem solar cells.
[0006] In order to achieve the purpose of this utility model, the utility model adopts the following technical solutions:
[0007] In a first aspect, the utility model provides a perovskite / crystalline silicon stacked cell, wherein the perovskite / crystalline silicon stacked cell comprises a silicon substrate, a tunneling layer, a first semiconductor layer, a perovskite light absorbing layer, a buffer layer, a second semiconductor layer and an electrode stacked in sequence.
[0008] The utility model improves the air tightness of the battery while protecting the perovskite light-absorbing layer with the help of a buffer layer, optimizes the energy level matching between film layers, reduces the loss of open-circuit voltage, improves the efficiency and stability of the tandem battery, and significantly improves the optical management of the perovskite / crystalline silicon tandem battery, which is conducive to promoting the industrialization of perovskite tandem solar cells.
[0009] As a preferred technical solution of the present invention, the material of the buffer layer includes aluminum oxide.
[0010] As a preferred technical solution of the present invention, the thickness of the buffer layer is 1-5 nm, for example, 1 nm, 2 nm, 3 nm, 4 nm or 5 nm.
[0011] As a preferred technical solution of the utility model, the material of the inorganic hole transport layer includes nickel oxide and / or cuprous thiocyanate.
[0012] As a preferred technical solution of the utility model, an organic molecular self-assembly layer is arranged between the second semiconductor layer and the electrode.
[0013] In the utility model, the parasitic absorption of the second semiconductor layer is greatly reduced through the double-layer design of the second semiconductor layer and the organic molecule self-assembly layer, and the energy level matching between the film layers is optimized.
[0014] As a preferred technical solution of the utility model, the material of the organic molecular self-assembly layer includes any one of Me-4PACz, MeO-2PACz or 2PACz, or a combination of at least two of them.
[0015] As a preferred technical solution of the utility model, the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is (5-15):(2-8), wherein the thickness selection range of the inorganic hole transport layer "5-15" can be, for example, 5nm, 8nm, 9nm, 10nm, 11nm, 12nm or 15nm, and the thickness selection range of the organic molecular self-assembly layer "2-8" can be, for example, 2nm, 3nm, 4nm, 5nm or 8nm.
[0016] In the present invention, if the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is too small, that is, the organic molecular self-assembly layer is too thick, the synergistic effect of the double hole transport layer is poor, resulting in that the performance of the battery cannot be effectively improved; if the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is too large, that is, the organic molecular self-assembly layer is too thin, the synergistic effect of the double hole transport layer is poor, resulting in that the performance of the battery cannot be effectively improved.
[0017] As a preferred technical solution of the present invention, the first semiconductor layer is an electron transport layer.
[0018] Preferably, the material of the electron transport layer includes C 60 .
[0019] Preferably, the thickness of the electron transport layer is 10-20 nm, for example, 10 nm, 12 nm, 14 nm, 16 nm, 18 nm or 20 nm.
[0020] As a preferred technical solution of the utility model, the tunneling layer includes an ITO composite layer.
[0021] Preferably, the thickness of the tunneling layer is 15-25 nm, for example, 15 nm, 20 nm or 25 nm.
[0022] As a preferred technical solution of the utility model, an ITO film is further provided between the organic molecular self-assembly layer and the electrode, and the thickness of the ITO film is 100-140nm, for example, 100nm, 110nm, 120nm, 1330nm or 140nm.
[0023] Preferably, the material of the electrode includes Au or Ag.
[0024] Preferably, the thickness of the electrode is 800-1000 nm, for example, 800 nm, 900 nm or 1000 nm.
[0025] As a preferred technical solution of the utility model, the silicon substrate is a formal nip crystalline silicon cell, and the first semiconductor layer is arranged on the P-face polycrystalline silicon of the formal nip crystalline silicon cell.
[0026] In a second aspect, the utility model provides a method for preparing the perovskite / crystalline silicon tandem battery as described in the first aspect, the preparation method comprising the following steps:
[0027] A tunneling layer, a first semiconductor layer, a perovskite light-absorbing layer, a buffer layer, a second semiconductor layer, an organic molecule self-assembly layer and an electrode are sequentially prepared on the surface of a silicon substrate to obtain the perovskite / crystalline silicon stacked cell.
[0028] The preparation method provided by the utility model has high production efficiency and low cost, can optimize the energy level matching between film layers and reduce the opening voltage loss; by preparing a buffer layer between the perovskite light absorption layer and the functional layer, the damage to the perovskite light absorption layer caused by the subsequent sputtering process can be reduced; the design of the second semiconductor layer and the organic molecular self-assembly layer can reduce the parasitic absorption of the transmission layer and improve the device efficiency.
[0029] The preparation method of the perovskite / crystalline silicon tandem battery provided by the utility model has a wide range of applications, and is applicable to both planar crystalline silicon and velvet crystalline silicon. In addition, compared with the preparation method of the traditional formal perovskite / crystalline silicon tandem battery, the production cycle is faster and the material cost is lower.
[0030] As a preferred technical solution of the utility model, the preparation method of the buffer layer includes atomic layer deposition.
[0031] Preferably, the method for preparing the organic molecular self-assembled layer comprises the following steps:
[0032] The organic molecule self-assembly layer precursor solution is spin-coated on the second semiconductor layer, and the organic molecule self-assembly layer is obtained after annealing.
[0033] As a preferred technical solution of the utility model, the concentration of the organic molecular self-assembled layer precursor solution is 0.5-1.5mmol / L, for example, it can be 0.5mmol / L, 0.7mmol / L, 0.9mmol / L, 1.1mmol / L, 1.3mmol / L or 1.5mmol / L.
[0034] Preferably, the spin coating rate is 2000-4000 rpm, for example, it can be 2000 rpm, 2500 rpm, 3000 rpm, 3500 rpm or 4000 rpm.
[0035] Preferably, the annealing temperature is 80-120°C, for example, 80°C, 90°C, 100°C, 110°C or 120°C, and the annealing time is 8-12 min, for example, 8 min, 9 min, 10 min, 11 min or 12 min.
[0036] As a preferred technical solution of the utility model, the preparation method comprises the following steps:
[0037] (1) Depositing a 15-25 nm thick ITO composite layer on the P-side polysilicon of the formal nip crystalline silicon cell as a tunneling layer;
[0038] (1) using a vacuum evaporation method to deposit an electron transport layer with a thickness of 10-20 nm on the tunneling layer;
[0039] (2) A two-step method is used to prepare a perovskite light absorbing layer on the electron transport layer. The specific steps include:
[0040] A lead halide film with a thickness of 150-250 nm is deposited on the electron transport layer by vacuum evaporation, and then an organic ammonium salt solution is spin-coated on the lead halide film by spin coating, and a perovskite light absorption layer is formed after annealing;
[0041] (3) using atomic layer deposition to deposit a buffer layer with a thickness of 1-5 nm on the perovskite light absorbing layer;
[0042] (4) sputtering an inorganic hole transport layer with a thickness of 8-12 nm on the buffer layer by magnetron sputtering;
[0043] (5) spin coating an organic molecular self-assembled layer precursor solution with a concentration of 0.5-1.5 mmol / L on the inorganic hole transport layer at a rate of 2000-4000 rpm, and then annealing at 80-120° C. for 8-12 min to obtain an organic molecular self-assembled layer;
[0044] (6) An ITO film with a thickness of 100-140 nm is prepared on the organic molecular self-assembled layer, and an Ag metal electrode with a thickness of 800-1000 nm is evaporated on the ITO film by a vacuum evaporation method.
[0045] It should be noted that the present invention does not specifically limit the type of lead halide, and illustratively, it may be lead iodide, etc.
[0046] In the present invention, the thickness of the lead halide film is 150-250nm, for example, 150nm, 200nm or 250nm, etc. The thickness of the ITO film is 100-140nm, for example, 100nm, 110nm, 120nm, 130nm or 140nm, etc.
[0047] As a preferred technical solution of the utility model, the organic ammonium salt solution comprises an organic ammonium salt and a solvent, the organic ammonium salt comprises any one or a combination of at least two of FAI, FABr or MACl, and the solvent comprises isopropanol.
[0048] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0049] Compared with the prior art, the utility model has the following beneficial effects:
[0050] The utility model improves the air tightness of the battery while protecting the perovskite light-absorbing layer with the help of a buffer layer, optimizes the energy level matching between film layers, reduces the loss of open-circuit voltage, improves the efficiency and stability of the tandem battery, and significantly improves the optical management of the perovskite / crystalline silicon tandem battery, which is conducive to promoting the industrialization of perovskite tandem solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1This is a schematic diagram of the structure of the perovskite / crystalline silicon tandem battery prepared in Example 1 of the present utility model.
[0052] Among them, 1-formal nip crystalline silicon bottom cell; 2-ITO layer; 3-electron transport layer; 4-perovskite light absorption layer; 5-buffer layer; 6-inorganic hole transport layer; 7-organic molecular self-assembly layer; 8-ITO film; 9-metal back electrode; 10-metal electrode. DETAILED DESCRIPTION
[0053] The technical solution of the present invention is further described below by specific implementation methods. Those skilled in the art should understand that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0054] Example 1
[0055] This embodiment provides a perovskite / crystalline silicon stacked cell. The structural schematic diagram of the perovskite / crystalline silicon stacked cell is shown in FIG. Figure 1 As shown, the perovskite / crystalline silicon stacked cell includes a formal nip crystalline silicon bottom cell 1 and a perovskite cell stacked in sequence;
[0056] The perovskite cell comprises an ITO layer 2, an electron transport layer 3, a perovskite light absorption layer 4, a buffer layer 5, an inorganic hole transport layer 6, an organic molecule self-assembly layer 7 and a metal back electrode 9 which are stacked in sequence. The ITO layer 2 of the perovskite cell is attached to the p-side polysilicon of the formal nip crystalline silicon bottom cell 1;
[0057] The thickness ratio of the inorganic hole transport layer 6 to the organic molecular self-assembly layer 7 is 10:3, the thickness of the electron transport layer 3 is 15 nm, and the thickness of the buffer layer 5 is 2 nm.
[0058] This embodiment also provides a method for preparing the above-mentioned perovskite / crystalline silicon tandem cell, the preparation method comprising the following steps:
[0059] (1) Depositing an ITO layer 2 with a thickness of 20 nm on the P-side polysilicon of the formal nip crystalline silicon bottom cell 1 as a tunneling layer;
[0060] (2) using a vacuum evaporation method to deposit an electron transport layer 3 with a thickness of 15 nm on the ITO layer 2;
[0061] Among them, the electron transport layer 3 is C 60 layer;
[0062] (3) A two-step method is used to prepare a perovskite light absorbing layer 4 on the electron transport layer 3. The specific steps include:
[0063] A lead iodide film with a thickness of 200 nm is deposited on the electron transport layer 3 by vacuum evaporation, and then an organic ammonium salt solution is spin-coated on the lead iodide film by spin coating, and a perovskite light absorption layer 4 is formed after annealing;
[0064] The organic ammonium salt solution includes 0.55 mol / L FAI, 0.1 mol / L FABr, 0.15 mol / L MACl and solvent isopropanol;
[0065] (4) depositing a buffer layer 5 with a thickness of 2 nm on the perovskite light absorbing layer 4 by atomic layer deposition;
[0066] Wherein, the buffer layer 5 is an aluminum oxide film;
[0067] (5) sputtering an inorganic hole transport layer 6 with a thickness of 10 nm on the buffer layer 5 by magnetron sputtering;
[0068] Wherein, the inorganic hole transport layer 6 is a nickel oxide thin film;
[0069] (6) spin coating an organic molecular self-assembled layer precursor solution with a concentration of 1 mmol / L on the inorganic hole transport layer 6 at a rate of 3000 rpm, and then annealing at 100° C. for 10 min to obtain an organic molecular self-assembled layer 7 with a thickness of 3 nm;
[0070] Wherein, the solvent of the precursor solution is ethanol, and the organic molecular self-assembled layer 7 is a ME-4PACZ molecular self-assembled layer;
[0071] (7) preparing an ITO film 8 with a thickness of 120 nm on the organic molecular self-assembled layer 7, and vapor-depositing an Ag metal back electrode 9 with a thickness of 900 nm on the ITO film 8 by vacuum evaporation;
[0072] (8) A layer of Ag metal electrode 10 with a thickness of 900 nm is deposited on the N side of the formal nip crystalline silicon bottom cell 1 by vacuum evaporation.
[0073] Example 2
[0074] This embodiment provides a perovskite / crystalline silicon stacked cell, wherein the perovskite / crystalline silicon stacked cell comprises a formal nip crystalline silicon bottom cell and a perovskite cell stacked in sequence;
[0075] The perovskite cell comprises an ITO layer, an electron transport layer, a perovskite light absorption layer, a buffer layer, an inorganic hole transport layer, an organic molecule self-assembly layer and a metal back electrode stacked in sequence, and the ITO layer of the perovskite cell is attached to the p-side polysilicon of the formal nip crystalline silicon bottom cell.
[0076] Among them, the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is 8:2, the thickness of the electron transport layer is 10nm, and the thickness of the buffer layer is 1nm.
[0077] This embodiment also provides a method for preparing the above-mentioned perovskite / crystalline silicon tandem cell, the preparation method comprising the following steps:
[0078] (1) Depositing an ITO layer with a thickness of 20 nm on the P-side polysilicon of the formal nip crystalline silicon bottom cell as a tunneling layer;
[0079] (2) using a vacuum evaporation method to deposit an electron transport layer with a thickness of 10 nm on the ITO layer;
[0080] The electron transport layer is C 60 layer;
[0081] (3) A two-step method is used to prepare a perovskite light absorbing layer on the electron transport layer, and the specific steps include:
[0082] A lead iodide film with a thickness of 150 nm is deposited on the electron transport layer by vacuum evaporation, and then an organic ammonium salt solution is spin-coated on the lead iodide film by spin coating, and a perovskite light absorption layer is formed after annealing;
[0083] The organic ammonium salt solution includes 0.55 mol / L FAI, 0.1 mol / L FABr, 0.15 mol / L MACl and solvent isopropanol;
[0084] (4) using atomic layer deposition to deposit a buffer layer with a thickness of 1 nm on the perovskite light absorbing layer;
[0085] Wherein, the buffer layer is an aluminum oxide film;
[0086] (5) sputtering an inorganic hole transport layer with a thickness of 8 nm on the buffer layer by magnetron sputtering;
[0087] Wherein, the inorganic hole transport layer is a nickel oxide film;
[0088] (6) spin coating an organic molecular self-assembled layer precursor solution with a concentration of 0.5 mmol / L on the inorganic hole transport layer at a rate of 2000 rpm, and then annealing at 80° C. for 12 min to obtain an organic molecular self-assembled layer with a thickness of 2 nm;
[0089] The solvent of the precursor solution is ethanol, and the organic molecular self-assembled layer is a ME-4PACZ molecular self-assembled layer;
[0090] (7) preparing an ITO film with a thickness of 100 nm on the organic molecular self-assembled layer, and using a vacuum evaporation method to evaporate an Ag metal back electrode with a thickness of 800 nm on the ITO film;
[0091] (8) A 2 nm thick Ag metal electrode is deposited on the N side of the formal nip crystalline silicon bottom cell using vacuum evaporation.
[0092] Example 3
[0093] This embodiment provides a perovskite / crystalline silicon stacked cell, wherein the perovskite / crystalline silicon stacked cell comprises a formal nip crystalline silicon bottom cell and a perovskite cell stacked in sequence;
[0094] The perovskite cell comprises an ITO layer, an electron transport layer, a perovskite light absorption layer, a buffer layer, an inorganic hole transport layer, an organic molecule self-assembly layer and a metal back electrode stacked in sequence, and the ITO layer of the perovskite cell is attached to the p-side polysilicon of the formal nip crystalline silicon bottom cell.
[0095] Among them, the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is 12:5, the thickness of the electron transport layer is 20nm, and the thickness of the buffer layer is 5nm.
[0096] This embodiment also provides a method for preparing the above-mentioned perovskite / crystalline silicon tandem cell, the preparation method comprising the following steps:
[0097] (1) Depositing an ITO layer with a thickness of 20 nm on the P-side polysilicon of the formal nip crystalline silicon bottom cell as a tunneling layer;
[0098] (2) using a vacuum evaporation method to deposit a 20 nm thick electron transport layer on the ITO layer;
[0099] The electron transport layer is C 60 layer;
[0100] (3) A two-step method is used to prepare a perovskite light absorbing layer on the electron transport layer, and the specific steps include:
[0101] A lead iodide film with a thickness of 250 nm is deposited on the electron transport layer by vacuum evaporation, and then an organic ammonium salt solution is spin-coated on the lead iodide film by spin coating, and a perovskite light absorption layer is formed after annealing;
[0102] The organic ammonium salt solution includes 0.55 mol / L FAI, 0.1 mol / L FABr, 0.15 mol / L MACl and solvent isopropanol;
[0103] (4) using atomic layer deposition to deposit a buffer layer with a thickness of 5 nm on the perovskite light absorbing layer;
[0104] Wherein, the buffer layer is an aluminum oxide film;
[0105] (5) sputtering an inorganic hole transport layer with a thickness of 12 nm on the buffer layer by magnetron sputtering;
[0106] Wherein, the inorganic hole transport layer is a nickel oxide film;
[0107] (6) spin coating an organic molecular self-assembled layer precursor solution with a concentration of 1.5 mmol / L on the inorganic hole transport layer at a rate of 4000 rpm, and then annealing at 120° C. for 8 min to obtain an organic molecular self-assembled layer with a thickness of 5 nm;
[0108] The solvent of the precursor solution is ethanol, and the organic molecular self-assembled layer is a ME-4PACZ molecular self-assembled layer;
[0109] (7) An ITO film with a thickness of 140 nm was prepared on the organic molecular self-assembled layer, and a Ag metal back electrode with a thickness of 1000 nm was evaporated on the ITO film by vacuum evaporation.
[0110] (8) A layer of Ag metal electrode with a thickness of 1000 nm is deposited on the N side of the formal nip crystalline silicon bottom cell using vacuum evaporation.
[0111] Example 4
[0112] The difference between this embodiment and embodiment 1 is that the concentration of the organic molecular self-assembled layer precursor solution in step (5) is 5 mmol / L.
[0113] The rest of the preparation methods and parameters were the same as those in Example 1.
[0114] Example 5
[0115] The difference between this embodiment and embodiment 1 is that the thickness of the inorganic hole transport layer in step (4) is 15 nm.
[0116] The rest of the preparation methods and parameters were the same as those in Example 1.
[0117] Example 6
[0118] The difference between this embodiment and embodiment 1 is that the thickness of the buffer layer in step (3) is 10 nm.
[0119] The rest of the preparation methods and parameters were the same as those in Example 1.
[0120] Example 7
[0121] The difference between this embodiment and embodiment 1 is that the spin coating rate of the organic molecular self-assembled layer precursor solution in step (5) is adjusted so that the thickness ratio of the inorganic hole transport layer to the organic molecular self-assembled layer is 10:16.
[0122] The rest of the preparation methods and parameters were the same as those in Example 1.
[0123] Example 8
[0124] The difference between this embodiment and embodiment 1 is that the spin coating rate of the organic molecular self-assembled layer precursor solution in step (5) is adjusted so that the thickness ratio of the inorganic hole transport layer to the organic molecular self-assembled layer is 15:1.
[0125] The rest of the preparation methods and parameters were the same as those in Example 1.
[0126] Comparative Example 1
[0127] The difference between this comparative example and Example 1 is that the buffer layer, the inorganic hole transport layer and the organic molecular self-assembly layer are replaced by a Spiro-OMeTAD hole transport layer.
[0128] The rest of the preparation methods and parameters were the same as those in Example 1.
[0129] Comparative Example 2
[0130] The difference between this comparative example and Example 1 is that no buffer layer is provided.
[0131] The rest of the preparation methods and parameters were the same as those in Example 1.
[0132] Comparative Example 3
[0133] The difference between this comparative example and Example 1 is that no organic molecular self-assembly layer is provided.
[0134] The rest of the preparation methods and parameters were the same as those in Example 1.
[0135] Performance Testing
[0136] The photovoltaic performance test was carried out on the perovskite / crystalline silicon tandem cells prepared in the above application examples and application comparison examples.
[0137] Test conditions: AM1.5, 1000W / m 2 , 25±2℃.
[0138] The test results are shown in Table 1.
[0139] Table 1
[0140]
[0141] analyze:
[0142] It can be seen from the above table that the utility model improves the airtightness of the battery while protecting the perovskite light-absorbing layer with the help of the buffer layer. At the same time, the design of the double hole transport layer greatly reduces the parasitic absorption of the hole transport layer, optimizes the energy level matching between the film layers, reduces the loss of open circuit voltage, and improves the battery efficiency and stability. Based on this, the optical management of the formal perovskite / crystalline silicon tandem battery can be significantly improved, the efficiency of the overall device can be improved, and it is conducive to promoting the industrialization of perovskite tandem solar cells.
[0143] It can be seen from the data results of Examples 1, 4 and 5 that the thickness of the hole transport layer is very important for the photoelectric management and efficiency of the stacked device. The appropriate thickness of the inorganic hole transport layer and the concentration of the organic molecular self-assembly layer precursor solution help to obtain excellent device efficiency.
[0144] It can be seen from the data results of Example 1 and Example 6 that if the buffer layer is too thick, the transmission of carriers will be hindered, resulting in a decrease in device efficiency.
[0145] It can be seen from the data results of Example 1 and Examples 7-8 that if the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is too small, the synergistic effect of the double hole transport layer is poor, resulting in the battery performance cannot be effectively improved; if the thickness ratio of the inorganic hole transport layer and the organic molecular self-assembly layer is too large, the synergistic effect of the double hole transport layer is poor, resulting in the battery performance cannot be effectively improved.
[0146] It can be seen from the data results of Example 1 and Comparative Example 1 that the opening voltage and filling of the nickel oxide + ME-4PACZ double hole transport layer in Example 1 are better than those of the Spiro-OMETAD layer in Comparative Example 1. This is because the nickel oxide + ME-4PACZ double hole transport layer can reduce parasitic absorption in the formal perovskite silicon stack and thus improve the overall device efficiency.
[0147] It can be seen from the data results of Example 1 and Comparative Example 2 that providing an aluminum oxide buffer layer between the perovskite light absorbing layer and the sputtered hole transport layer can effectively reduce the damage to the perovskite layer caused by subsequent sputtering and improve the device efficiency.
[0148] It can be seen from the data results of Example 1 and Comparative Example 3 that if an organic molecular self-assembly layer is not provided on the inorganic hole transport layer, the device efficiency cannot be significantly improved.
[0149] The applicant declares that the utility model illustrates the process method of the utility model through the above-mentioned embodiments, but the utility model is not limited to the above-mentioned process steps, that is, it does not mean that the utility model must rely on the above-mentioned process steps to be implemented. The technicians in the relevant technical field should understand that any improvement of the utility model, the equivalent replacement of the raw materials selected by the utility model, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the utility model.
Claims
1. A perovskite / crystalline silicon tandem cell, characterized in that: The perovskite / crystalline silicon stacked cell comprises a silicon substrate, a tunneling layer, a first semiconductor layer, a perovskite light-absorbing layer, a buffer layer, a second semiconductor layer and electrodes which are stacked in sequence.
2. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The buffer layer includes an aluminum oxide layer; The thickness of the buffer layer is 1-15 nm.
3. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The second semiconductor layer is an inorganic hole transport layer; The inorganic hole transport layer includes a nickel oxide layer and / or a cuprous thiocyanate layer.
4. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: An organic molecular self-assembly layer is arranged between the second semiconductor layer and the electrode.
5. The perovskite / crystalline silicon tandem cell according to claim 4, characterized in that: The organic molecular self-assembly layer includes any one of a Me-4PACz layer, a MeO-2PACz layer or a 2PACz layer, or a combination of at least two of them.
6. The perovskite / crystalline silicon tandem cell according to claim 4, characterized in that: The thickness ratio of the second semiconductor layer to the organic molecular self-assembly layer is (5-15):(2-8).
7. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The first semiconductor layer is an electron transport layer; The electron transport layer comprises C 60 layer; The thickness of the first semiconductor layer is 10-20 nm.
8. The perovskite / crystalline silicon tandem cell according to claim 1, characterized in that: The tunneling layer includes an ITO composite layer; The thickness of the tunneling layer is 15-25 nm.
9. The perovskite / crystalline silicon tandem cell according to claim 4, characterized in that: An ITO film is also provided between the organic molecular self-assembly layer and the electrode, and the thickness of the ITO film is 100-140 nm; The electrode comprises an Au electrode or an Ag electrode; The thickness of the electrode is 800-1000 nm.