Battery case and battery

By setting an alloy layer in the battery case and sealing the flame retardant layer inside it, the contradiction between the safety performance and electrochemical performance of lithium-ion batteries is solved, the flame retardant effect when thermal runaway is achieved, and the safety of the battery is improved performance.

CN222088722UActive Publication Date: 2024-11-29JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420279560.4
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-11-29
Estimated Expiration
2034-02-05

AI Technical Summary

Technical Problem

In the context of pursuing higher energy density and ultrafast charging technology, safety issues such as fire and explosion still exist, and the introduction of traditional flame retardants will affect the electrochemical performance of the battery.

Method used

An alloy layer is provided in the battery case, and the flame retardant layer is sealed between the alloy layer and the shell. When the battery is about to or is thermally out of control, the alloy layer melts and releases the flame retardant to improve safety performance.

Benefits of technology

Effectively isolate flame retardants and electrolytes, avoid negative effects on battery performance, and suppress reactions when thermal runaway, improving battery safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222088722U_ABST
    Figure CN222088722U_ABST
Patent Text Reader

Abstract

The utility model provides a battery shell and a battery, the battery shell comprises a shell, an alloy layer is arranged on the inner wall of the shell, and a first flame retardant layer is filled between the alloy layer and the shell. The alloy layer is arranged in the battery shell, so that the flame-retardant material is coated between the alloy layer and the shell, the alloy layer can be molten to release the flame retardant in the thermal runaway process, and the safety performance of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of batteries, in particular to a battery shell and a battery. Background Art

[0002] As an important electrical energy storage device, lithium-ion batteries are widely used in electric vehicles, mobile communication devices, portable electronic products, energy storage systems, etc. due to their high energy density, long cycle life, no memory effect and low self-discharge rate. However, in the context of the continuous pursuit of higher energy density and ultra-fast charging technology, safety issues such as fire and explosion remain a severe challenge facing this technology, limiting the widespread application of lithium-ion batteries.

[0003] In traditional technology, flame retardants are directly added to lithium-ion batteries to improve their safety performance, but this often comes at the expense of the electrochemical performance of the battery. In order to reduce the negative impact of flame retardants on the electrochemical performance of the battery, surface coating and other means are used to prepare microcapsule flame retardants. Microcapsule flame retardants encapsulate flame retardants in micron-sized capsules, so that when the battery is working normally, the flame retardants can be isolated from the internal materials of the battery, thereby reducing the adverse effects of flame retardants on battery performance. However, the introduction of microcapsule flame retardants will still affect the composition of the battery and still have potential adverse effects on battery performance.

[0004] Therefore, there is an urgent need for a flame-retardant battery casing that can provide high safety performance while having little effect on the electrochemical performance of the battery. Utility Model Content

[0005] Based on this, it is necessary to provide a battery casing and a battery. The present application arranges an alloy layer in the battery casing, so that a flame retardant layer is coated between the alloy layer and the casing. When the battery is about to or is experiencing thermal runaway, the alloy layer can be melted, and the flame retardant layer releases the flame retardant, thereby improving the safety performance of the battery.

[0006] The above utility model object can be achieved through the following technical solutions.

[0007] In a first aspect, the present application provides a battery casing, comprising a shell and an alloy layer arranged on a side of the shell adjacent to a battery cell, wherein a first flame retardant layer is filled between the alloy layer and the shell.

[0008] In some embodiments, the melting point of the alloy layer is 80°C to 200°C.

[0009] In some embodiments, the alloy layer has a thickness of 30 μm to 50 μm.

[0010] In some embodiments, the alloy layer includes a tin-bismuth alloy layer, a bismuth-lead alloy layer, a tin-bismuth-thallium alloy layer, a lead-bismuth-silver alloy layer, or an indium-bismuth-tin alloy layer.

[0011] In some embodiments, the first flame retardant layer has a thickness of 10 μm to 30 μm.

[0012] In some embodiments, at least two alloy layers are disposed on a side of the shell adjacent to the battery core, and a second flame retardant layer is filled between two adjacent alloy layers; and the melting points of the alloy layers decrease successively in a direction away from the shell.

[0013] In some embodiments, the material of the first flame retardant layer and the material of the second flame retardant layer independently include a flame retardant or a flame retardant composite material, wherein the flame retardant composite material includes a flame retardant and a coating layer coated on the surface of the flame retardant.

[0014] In some embodiments, the second flame retardant layer has a thickness of 10 μm to 30 μm.

[0015] In some embodiments, a promoter is further filled between two adjacent alloy layers, and the promoter is used to promote the alloy layers to release metal ions.

[0016] In a second aspect, the present application provides a battery, comprising the battery casing as described in the first aspect.

[0017] Compared with the traditional technology, this application has at least the following beneficial effects:

[0018] The present application uses an alloy layer to seal the flame retardant layer in the battery casing, isolates the flame retardant layer from the electrolyte, and prevents the flame retardant layer from directly contacting the electrolyte and affecting the electrical performance of the battery; further, when the battery is about to or is experiencing thermal runaway, the alloy layer can melt and the flame retardant layer releases the flame retardant, thereby blocking the thermal runaway reaction of the battery and improving the safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG. 1 is a schematic structural diagram of a battery housing provided in one embodiment of the present application.

[0020] Among them, 10 is a battery shell; 11 is a first flame retardant layer; 12 is a second flame retardant layer; 13 is a first alloy layer; and 14 is a second alloy layer. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with the accompanying drawings, embodiments and examples. These embodiments and examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. The purpose of providing these embodiments and examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive. It should also be understood that the present invention can be implemented in many different forms and is not limited to the embodiments and examples described herein. Those skilled in the art can make various changes or modifications without violating the connotation of the present invention, and the equivalent forms obtained also fall within the scope of protection of the present invention. In addition, in the description below, a large number of specific details are given in order to provide a more comprehensive understanding of the present invention. It should be understood that the present invention can be implemented without one or more of these details.

[0022] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0023] In the present invention, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "option" is independent.

[0024] In the present utility model, the terms "first", "second", "third", etc. in "the first aspect", "the second aspect", "the third aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0025] In the present utility model, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0026] In the present utility model, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the distribution of optional numerical values ​​within the numerical interval is deemed to be continuous, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints, which is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed in this application should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows for broadly including quantitative intervals such as percentage intervals, ratio intervals, and ratio intervals.

[0027] All documents mentioned in the present utility model are cited as references in the present application, just as each document is cited as a reference separately. Unless they conflict with the utility model purpose and / or technical solution of the present application, the cited documents involved in the present utility model are cited with all contents and all purposes. When the present utility model involves cited documents, the definitions of relevant technical features, terms, nouns, phrases, etc. in the cited documents are also cited. When the present utility model involves cited documents, the examples and preferred methods of the cited relevant technical features can also be incorporated into the present application as references, but are limited to the ability to implement the present utility model. It should be understood that when the cited content conflicts with the description in the present application, the present application shall prevail or be modified adaptively according to the description of the present application.

[0028] In traditional technology, the safety performance of batteries is improved by directly adding flame retardants or microcapsule flame retardants to the electrolyte, but this method often sacrifices the electrochemical performance of the battery. The present application improves the battery casing and uses an alloy layer to seal the flame retardant on the inner wall of the casing, thereby avoiding direct contact between the flame retardant and the battery's electrode materials, electrolyte or diaphragm and other components, and effectively reducing the impact on the electrochemical performance of the battery. At the same time, when the battery is about to or is experiencing thermal runaway, the high temperature causes the alloy layer to melt and release the flame retardant into the battery, promptly suppressing the further occurrence of thermal runaway of the battery.

[0029] In a first aspect, the present application provides a battery casing, comprising a shell and an alloy layer arranged on a side of the shell adjacent to a battery cell, wherein a first flame retardant layer is filled between the alloy layer and the shell.

[0030] The present application uses an alloy layer to seal the flame retardant layer in the battery casing, isolates the flame retardant layer from the electrolyte, and prevents the flame retardant layer from directly contacting the electrolyte and affecting the electrical performance of the battery; further, when the temperature triggering thermal runaway is reached in the battery, the alloy layer can melt and the flame retardant layer releases the flame retardant, thereby inhibiting the thermal runaway reaction of the battery and improving the safety performance of the battery.

[0031] It can be understood that the inner wall of the shell in the present application includes at least one of the side inner wall, the bottom inner wall and the top inner wall of the shell.

[0032] It is understandable that the flame retardant in the present application can be a material that prevents the battery from burning, or it can be a material that can block the battery from burning after the battery burns, so as to achieve the purpose of extinguishing the fire. The flame retardant action mode can be endothermic action, covering action, chain reaction inhibition and non-combustible gas suffocation action. The endothermic action of the flame retardant refers to that the flame retardant can absorb the heat generated in the heat generation stage of thermal runaway and the combustion reaction stage in a short time, thereby preventing the further occurrence of the heat generation reaction and the combustion reaction. The covering effect of the flame retardant refers to that the flame retardant can form a barrier layer at the thermal runaway temperature to isolate the contact between the active material of the battery and oxygen, and has the effects of heat insulation, oxygen isolation and preventing the escape of combustible gases, thereby achieving the purpose of flame retardancy. The chain reaction inhibition effect of the flame retardant refers to that the flame retardant can capture free radicals in the reaction process during the heat generation stage of thermal runaway and the combustion stage, thereby interfering with the heat generation and combustion reactions. For example, the flame retardant can react with the active material or solidify the electrolyte, thereby preventing the heat generation reaction from proceeding. The non-combustible gas asphyxiation effect of flame retardants means that flame retardants decompose non-combustible gases when heated, diluting the concentration of combustible gases decomposed from combustibles to below the lower combustion limit. At the same time, it also dilutes the oxygen concentration in the combustion zone, preventing the continuation of combustion and achieving a flame retardant effect.

[0033] It is understandable that in the production and application of flame retardants, a single flame retardant usually cannot achieve the ideal effect, but multiple flame retardants can be compounded to produce a synergistic inhibition effect, and two or more flame retardants can be compounded to optimize the performance, economic and social benefits, so as to obtain the best compound flame retardant. The compounding of flame retardants can achieve the complementary performance between different flame retardants, improve the inhibition performance, and reduce the dosage, which greatly improves the application scope and effect of flame retardants.

[0034] In some embodiments, the melting point of the alloy layer is 80°C~200°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C.

[0035] In some embodiments, the thickness of the alloy layer is 30 μm to 50 μm, for example, 30 μm, 32 μm, 34 μm, 36 μm, 38 μm, 40 μm, 42 μm, 44 μm, 46 μm, 48 μm or 50 μm.

[0036] In some embodiments, the alloy layer includes a tin-bismuth alloy layer, a bismuth-lead alloy layer, a tin-bismuth-thallium alloy layer, a lead-bismuth-silver alloy layer, or an indium-bismuth-tin alloy layer. For example, when the mass ratio of the tin-bismuth alloy is 58% Sn and 42% Bi, its melting point is 138°C; when the mass ratio of the bismuth-lead alloy is 58% Bi and 42% Pb, its melting point is 125°C; when the mass ratio of the tin-bismuth-indium alloy is 52% Sn, 32% Bi and 16% In, its melting point is 118°C; when the mass ratio of the lead-bismuth-silver alloy is 50% Pb, 25% Bi and 25% Ag, its melting point is 96°C; when the mass ratio of the indium-bismuth-tin alloy is 51% In, 32.5% Bi and 16.5% Sn, its melting point is 60°C.

[0037] In some embodiments, the filling thickness of the first flame retardant layer is 10 μm to 30 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm or 30 μm.

[0038] In some embodiments, at least two alloy layers are disposed on a side of the shell adjacent to the battery core, and a second flame retardant layer is filled between two adjacent alloy layers.

[0039] As shown in Figure 1, the battery shell 10 includes a shell, a first flame retardant layer 11, a second flame retardant layer 12, a first alloy layer 13 and a second alloy layer 14. The first alloy layer 13 and the second alloy layer 14 are sequentially arranged in the shell in a direction away from the inner wall of the shell, wherein the first flame retardant layer 11 is filled between the shell and the first alloy layer 13, and the second flame retardant layer 12 is filled between the first alloy layer 13 and the second alloy layer 14.

[0040] In some embodiments, the melting points of the alloy layers decrease sequentially in a direction away from the shell.

[0041] The present application controls the melting point of the alloy layer, thereby releasing matching flame retardants according to different stages of battery thermal runaway, achieving staged blocking of battery thermal runaway, and avoiding direct thermal failure of the battery or battery failure after the addition of flame retardants.

[0042] Optionally, the first flame retardant and the second flame retardant independently include a flame retardant or a flame retardant composite material, and the flame retardant composite material includes a flame retardant and a coating layer coated on the surface of the flame retardant; further optionally, the flame retardant includes at least one of a phosphorus-based flame retardant, a nitrogen-based flame retardant, a halogen-based flame retardant, a metal compound flame retardant and an electrolyte curing agent.

[0043] In some embodiments, the halogen flame retardant includes one or more of chlorine flame retardants and brominated flame retardants. Chlorine flame retardants include chlorinated polyolefins, chlorinated polyalkanes, chlorinated diphenyl ethers, chlorinated benzenes, etc., specifically including but not limited to the following flame retardants: chlorinated polyethylene (CPE), chlorinated polypropylene (CPP), chlorinated paraffin, decachlorodiphenyl ether, hexachlorobenzene and new high-performance chlorine flame retardants, such as: tetrachlorophthalic anhydride, tetrachlorobisphenol A, hexachlorocyclopentene, bis (hexachlorocyclopentadiene) cyclooctane, perchlorocyclopentane decane, tetrachlorophthalic anhydride and chlorendic acid. Bromine flame retardants can be divided into polybrominated diphenyl ethers, brominated phenols, brominated bisphenol A, brominated phthalic acid, brominated polyols, brominated alkanes, etc. according to their structure. Including but not limited to the following flame retardants, such as: polybrominated diphenyl ethers (PBDEs), 2,4,6-tribromophenol, tetrabromobisphenol A (TBBPA), tetrabromobisphenol A-bis (2,3-dialkylpropyl) ether (TBAB), hexabromocyclododecane (HBCD), brominated polystyrene (BPS), brominated epoxy, decabromodiphenyl ethane, decabromodiphenyl ether, tetrabromobisphenol A, brominated polystyrene, tribromophenol and its derivatives, brominated triazines, brominated epoxy resins, hexabromocyclododecane, tetrabromobisphenol A polycarbonate oligomers, dibromoneopentyl glycol, tetrabromophthalic anhydride, tetrabromophthalic anhydride diol, melamine bromide, potassium perfluorobutyl sulfonate, and declone flame retardants.

[0044] In some embodiments, phosphorus-based flame retardants include red phosphorus flame retardants, ammonium salt flame retardants, phosphate compounds, phosphaphenanthrene compounds, polyphosphazene compounds, hypophosphorous acid and its salt compounds, triazine or piperazine carbon formers. Specific flame retardants include, but are not limited to: red phosphorus, ammonium polyphosphate, melamine phosphate and melamine polyphosphate, melamine cyanurate, bisphenol A bis (diphenyl) phosphate, resorcinol (diphenyl) phosphate, tris (2-chloroethyl) phosphate), tris (1-chloro-2-propyl) phosphate, 10-(2,5-dihydroxyphenyl)-10-hydrogen-9-oxa-10-phosphaphenanthrene-10-oxide (ODOPB), diethyl aluminum hypophosphite, 2-carboxyethyl phenyl hypophosphite, aluminum hypophosphite.

[0045] In some embodiments, the nitrogen-based flame retardant includes one or more of nitrogen-containing polyamide, nitrogen-containing polyurethane, phosphamide, melamine, and ammonium polyphosphate.

[0046] In some embodiments, the metal compound flame retardant includes one or more of magnesium-based flame retardants (magnesium hydroxide), antimony-based flame retardants (antimony oxide, sodium antimonate), aluminum hydroxide, zinc borate, molybdenum oxide, and ammonium molybdate.

[0047] In some embodiments, the electrolyte curing agent refers to an agent that can react with the electrolyte to control the dielectric constant or viscosity of the electrolyte, aiming to suppress Joule heat by destroying the ionic conductivity to force the internal resistance to increase. The curing agent can increase the viscosity of the electrolyte and can convert the liquid electrolyte into a solid substance or gel substance that is not easily conductive. Optionally, the electrolyte curing agent includes one or more of diols and amine compounds. For example, amine curing agents include but are not limited to: 1,3-propylenediamine, benzylamine, dibenzylamine (DBA), 1,2-ethylenediamine (1,2-EDA) and trihexylamine (THA); diol curing agents include but are not limited to: 1,2-ethylene glycol, 1,3-propylene glycol, 1,5-pentanediol.

[0048] In some embodiments, the flame retardant may also be a fire extinguishing agent, which includes one or more of a dry powder fire extinguishing agent and a foam fire extinguishing agent. Dry powder fire extinguishing agents include one or more of ammonium bicarbonate (the decomposition temperature of ammonium bicarbonate is about 60°C, which cannot be used alone and can be mixed with other fire extinguishing agents), ammonium chloride, and ammonium sulfate. The components of foam fire extinguishing agents are mainly composed of substances such as proteins, fluorine compounds, and surfactants. They isolate oxygen and reduce the temperature of the fire source by forming a foam layer. Foam fire extinguishing agents include one or more of protein foam fire extinguishing agents, fluoroprotein foam fire extinguishing agents, synthetic foam fire extinguishing agents, and water-based foam fire extinguishing agents.

[0049] In some embodiments, the material of the coating layer of the flame-retardant composite material can be reasonably selected according to the battery type and thermal runaway requirements.

[0050] Optionally, the rupture temperature of the coating layer in the flame retardant composite material is greater than the melting point of the alloy layer sealing the flame retardant composite material.

[0051] Optionally, the rupture temperature of the coating layer in the flame retardant composite material is 5°C to 150°C greater than the melting point of the alloy layer that seals the flame retardant composite material, for example, it can be 5.0°C, 20°C, 40°C, 60°C, 80°C, 100°C, 120°C, 130°C, 140°C or 150°C, and can further be 5°C to 10°C.

[0052] In the present application, a flame retardant with a core-shell capsule structure can be used. The alloy layer melts before the coating layer of the flame-retardant composite material, so that in the process of thermal runaway, the alloy layer melts to release the flame-retardant composite material, and then the flame-retardant composite material is dispersed into the electrolyte. When the temperature rises further, the flame-retardant capsule ruptures, thereby releasing the flame retardant and blocking the thermal runaway reaction of the battery. In addition, part of the first flame retardant layer or the second flame retardant layer can be replaced with a flame-retardant composite material. When the flame retardant layer releases the flame retardant material, the flame retardant material can be released first to suppress the thermal runaway of the battery, and the flame-retardant composite material with a capsule structure is dispersed into the electrolyte. When it further rises to the rupture temperature of the flame-retardant composite material, it is released to control the thermal runaway of the battery, thereby achieving staged thermal runaway control.

[0053] In some embodiments, the filling thickness of the second flame retardant layer is 10 μm to 30 μm, for example, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 26 μm, 28 μm or 30 μm.

[0054] In some embodiments, the flame retardant includes one or more of a phosphorus flame retardant, a nitrogen flame retardant, a halogen flame retardant, and a metal flame retardant. In particular, the flame retardant may also be a fire extinguishing agent with a fire extinguishing function, a curing agent for curing the electrolyte, and a microcapsule flame retardant with a core-shell structure.

[0055] In some embodiments, the material of the alloy layer farthest from the inner wall of the shell includes tin-lead alloy, tin-bismuth alloy and tin-indium alloy.

[0056] In the present application, the material of the alloy layer is selected, and tin, indium and bismuth release flame retardants after melting, and the flame retardants are transported to the surface of the electrode material along with the electrolyte, blocking the occurrence of the combustion chain reaction between the electrode material and the electrolyte, and avoiding further thermal runaway of the battery, and the reaction products can promote the ionization of tin, indium and bismuth in the electrolyte, and tin, indium and bismuth can be reduced by lithium on the surface of the negative electrode, thereby forming an SEI film containing metal components in situ on the surface of the lithium negative electrode. Moreover, during the cycle, the metal ions in the electrolyte are electrochemically active, which promotes the stability of the metal protective layer on the surface of the lithium negative electrode, and stores lithium by forming an alloy. At the same time, the alloy formed can reduce the diffusion barrier during lithium deposition, promote the rapid migration of lithium ions, and inhibit the growth of lithium dendrites, thereby improving the electrochemical performance of the lithium metal negative electrode.

[0057] The material of the second flame retardant layer includes at least one of pentaerythritol, melamine and a derivative of melamine. For example, the derivative of melamine can be melamine polyphosphate. The present application uses the above materials as flame retardants to promote the precipitation of ions from the alloy layer, thereby improving the reduction effect of the alloy material on the negative electrode surface, and further improving the electrical properties of the negative electrode.

[0058] In some embodiments, the second flame retardant further includes an accelerator, and the accelerator is used to promote the alloy layer to release metal ions.

[0059] Optionally, the promoter includes polyoxometalate. For example, the polyoxometalate includes at least one of isopolymolybdate, isopolytungstate and isopolyvanadate.

[0060] The present application adds a material that can promote the release of metal ions from the alloy layer to the flame retardant that is released first, so that after the inner flame retardant is released, not only can thermal runaway be prevented, but the metal ions generated by the alloy layer can also improve the stability of the negative electrode.

[0061] A second aspect of the present application provides a battery, comprising the battery casing as described in the first aspect.

[0062] In some embodiments, the battery housing is filled with an electrolyte, and the electrolyte contains a promoter. Optionally, the promoter includes polyoxometalate.

[0063] Optionally, the mass proportion of the promoter in the electrolyte is 5% to 10%, for example, it can be 5.0%, 5.5%, 6.0%, 6.5%, 7.0%, 7.5%, 8.0%, 8.5%, 9.0%, 9.5% or 10.0%.

[0064] The present application adds polyoxometalates to the electrolyte, thereby promoting the ionization of the alloy layer when the thermal runaway temperature is reached, and the generated metal ions can improve the stability of the negative electrode.

[0065] Illustratively, the present application provides a method for preparing the above-mentioned battery casing, the preparation method comprising:

[0066] The battery housing is prepared by filling a first flame retardant in the housing and sealing the first flame retardant with a molten alloy material to form the alloy layer.

[0067] In some embodiments, at least two alloy layers are provided on one side of the shell adjacent to the battery core, and a second flame retardant is filled between two adjacent alloy layers. The method for preparing the battery shell further includes:

[0068] A second flame retardant is arranged in the battery housing having the first flame retardant layer and the alloy layer, and the second flame retardant is sealed with a molten alloy material to form a new alloy layer.

[0069] In some embodiments, the liquid flame retardant can be packaged by injection. First, an alloy layer shell is used for packaging, and a liquid injection hole is reserved to inject the liquid flame retardant, and then a second packaging is performed. The packaging material can be an alloy or other packaging material with a higher melting point than the alloy. Alternatively, the liquid flame retardant is microencapsulated to obtain a microcapsule flame retardant, and then the microcapsule flame retardant is packaged.

[0070] The following embodiments of the present invention are described in detail in conjunction with examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are preferably referred to the instructions given in the present invention, and can also be carried out according to the experimental manuals or conventional conditions in the field, or according to the conditions recommended by the manufacturer, or with reference to experimental methods known in the art.

[0071] Example 1

[0072] This embodiment provides a method for preparing a battery shell, comprising:

[0073] A first flame retardant is filled at the bottom of the shell, wherein the first flame retardant includes ammonium polyphosphate and decabromodiphenyl ether in a mass ratio of 1:2, and the first flame retardant is compacted using an indium bismuth tin alloy sheet with a thickness of 50 μm, and the thickness of the first flame retardant layer is 20 μm;

[0074] The lead-bismuth-silver alloy sheet and the inner wall of the shell are sealed with molten lead-bismuth-silver alloy material to form a lead-bismuth-silver alloy layer, and the melting point of the lead-bismuth-silver alloy is 96° C.

[0075] Then, a second flame retardant is filled into the bottom of the shell, wherein the second flame retardant includes melamine polyphosphate, and the second flame retardant is compacted by using an indium bismuth tin alloy sheet with a thickness of 48 μm, and the thickness of the second flame retardant layer is 28 μm;

[0076] An indium-bismuth-tin alloy material is used to seal the lead-bismuth-silver alloy sheet and the inner wall of the shell to form an indium-bismuth-tin alloy layer. The melting point of the indium-bismuth-tin alloy is 60°C.

[0077] This embodiment provides a battery, including the above-mentioned battery casing, electrolyte and battery cell, wherein the battery cell is made by winding an NCM811 positive electrode sheet, a diaphragm, a graphite negative electrode sheet and a diaphragm, and the electrolyte is composed of 1.2 mol / L LiPF6 as a solute and an EC:EMC solvent with a volume ratio of 3:7.

[0078] Example 2

[0079] This embodiment provides a method for preparing a battery shell, comprising:

[0080] Filling the bottom of the battery housing with a first flame retardant, the first flame retardant comprising ammonium polyphosphate, and compacting the first flame retardant with a bismuth-lead alloy sheet having a thickness of 45 μm, the thickness of the first flame retardant layer being 22 μm;

[0081] The bismuth-lead alloy sheet and the inner wall of the shell are sealed with melted bismuth-lead alloy material to form a bismuth-lead alloy layer, and the melting point of the bismuth-lead alloy is 125° C.

[0082] Then, a second flame retardant is filled into the bottom of the shell, wherein the second flame retardant includes at least one of pentaerythritol, melamine and derivatives thereof, and the second flame retardant is compacted by using an indium bismuth tin alloy sheet with a thickness of 44 μm, and the thickness of the second flame retardant layer is 25 μm;

[0083] An indium-bismuth-tin alloy material is used to seal the bismuth-lead alloy sheet and the inner wall of the shell to form an indium-bismuth-tin alloy layer. The melting point of the indium-bismuth-tin alloy is 60°C.

[0084] This embodiment provides a battery, including the above-mentioned battery casing, electrolyte and battery cell, wherein the battery cell is made by winding an NCM811 positive electrode sheet, a diaphragm, a graphite negative electrode sheet and a diaphragm, and the electrolyte is composed of 1.2 mol / L LiPF6 as a solute and an EC:EMC solvent with a volume ratio of 3:7.

[0085] Example 3

[0086] This embodiment provides a method for preparing a battery shell, comprising:

[0087] A first flame retardant is filled at the bottom of the shell, the first flame retardant includes decabromodiphenyl ether, and the first flame retardant is compacted by using an indium bismuth tin alloy sheet with a thickness of 43 μm, and the thickness of the first flame retardant layer is 23 μm;

[0088] The indium bismuth tin alloy sheet and the inner wall of the shell are sealed with melted indium bismuth tin alloy material to form an indium bismuth tin alloy layer. The melting point of the indium bismuth tin alloy is 60°C.

[0089] This embodiment provides a battery, including the above-mentioned battery casing, electrolyte and battery cell, wherein the battery cell is made by winding an NCM811 positive electrode sheet, a diaphragm, a graphite negative electrode sheet and a diaphragm, and the electrolyte is composed of 1.2 mol / L LiPF6 as a solute and an EC:EMC solvent with a volume ratio of 3:7.

[0090] Example 4

[0091] A battery case and a battery were prepared according to the method of Example 1, with the only difference being that the second flame retardant was replaced with triethyl phosphate, which could not increase the ion precipitation of the alloy layer after contacting with the electrolyte.

[0092] Example 5

[0093] The battery case and battery were prepared according to the method of Example 1, except that the second flame retardant was replaced by triethyl phosphate and polyoxometalate in a mass ratio of 1:2, and the polyoxometalate was La 12 W 12 O 36 (H2O) 24 (Nb6O 19 ) 12 .

[0094] Example 6

[0095] A battery case and a battery were prepared according to the method of Example 4, the only difference being that the electrolyte of the battery also contained polyoxometalate, the amount of polyoxometalate added accounted for 6% of the total mass of the electrolyte, and the polyoxometalate was La 12 W 12 O 36 (H2O) 24 (Nb6O 19 ) 12 .

[0096] Example 7

[0097] A battery case and a battery are prepared according to the method of Example 1, with the only difference that a portion of the second flame retardant is replaced by a flame-retardant composite material, the mass proportion of the flame-retardant composite material in the second flame retardant is 50%, the flame-retardant composite material includes ammonium polyphosphate and polymethyl methacrylate coated on the surface of the ammonium polyphosphate, the mass ratio of ammonium polyphosphate to polymethyl methacrylate is 1:1, the average particle size of the flame-retardant composite material is 12 μm, and the release temperature is 200°C.

[0098] Comparative Example 1

[0099] This comparative example provides a battery casing and a battery. Compared with Example 1, the only difference is that a battery casing without an alloy layer and a flame retardant is directly used.

[0100] The battery housings prepared in the above embodiments and comparative examples were subjected to thermal abuse tests and cycle performance tests, and the test methods included:

[0101] The above battery housing is used to assemble a 1Ah NCM811||graphite standard soft pack battery to test the thermal abuse test and cycle performance of the battery;

[0102] The thermal abuse test method includes: The thermal abuse test is carried out in an explosion-proof cabinet. First, the soft-pack battery is placed in the heating device through a heating device with an adjustable nut, and the battery and the heating device are separated by two mica sheets, and a ceramic heating sheet is placed between the mica sheet and the battery on one side. The ceramic sheet is quickly heated to 200°C at the beginning and then stops heating. A K-type thermocouple is fixed between the other side of the battery and another mica sheet to record the temperature changes during the thermal abuse of the battery.

[0103] The test method for cycle performance includes: charging the above 1Ah NCM811||graphite standard soft pack battery to 4.2V and discharging it to 2.75V at a constant current of 0.5 C at 25°C on a Blue Electric charger and discharger (CT3002A), and repeating the test for 400 cycles. The test results are shown in Table 1.

[0104] Table 1

[0105]

[0106] From the above table we can see that:

[0107] (1) Compared with Example 4, it can be seen that the materials of the alloy layer selected in the present application, tin, indium and bismuth release flame retardants after melting, and after the flame retardant and the alloy material react in the electrolyte, the battery is prevented from further thermal runaway, and the reaction products can promote the ionization of tin, indium and bismuth in the electrolyte. Tin, indium and bismuth can be reduced by lithium on the surface of the negative electrode, thereby forming an SEI film containing metal components in situ on the surface of the lithium negative electrode. Moreover, during the cycle, the metal ions in the electrolyte are electrochemically active, which promotes the stability of the metal protective layer on the surface of the lithium negative electrode, and stores lithium by forming an alloy. At the same time, the alloy formed can reduce the diffusion barrier during lithium deposition, promote the rapid migration of lithium ions, and inhibit the growth of lithium dendrites, thereby improving the electrochemical performance of the lithium metal negative electrode.

[0108] (2) Compared with Example 5, it can be seen that the present application adds a material that can promote the release of metal ions from the alloy layer to the flame retardant that is released first, so that after the inner flame retardant is released, not only can the occurrence of thermal runaway be prevented, but the metal ions generated by the alloy layer can also improve the stability of the negative electrode.

[0109] (3) Compared with Example 6, it can be seen that the present application can promote the ionization of the alloy layer when the thermal runaway temperature is reached by adding polyoxometalates to the electrolyte, and the generated metal ions can improve the stability of the negative electrode.

[0110] (4) Compared with Example 7, it can be seen that a flame retardant with a core-shell capsule structure can be used in the present application. The alloy layer melts before the coating layer of the flame-retardant composite material. Therefore, during the thermal runaway process, the alloy layer melts to release the flame-retardant composite material, and then the flame-retardant composite material is dispersed into the electrolyte. When the temperature further increases, the flame-retardant capsule ruptures, thereby releasing the flame retardant and blocking the thermal runaway reaction of the battery.

[0111] (5) Compared with Comparative Example 1, in Example 1, the present application uses an alloy layer to seal the flame retardant layer in the battery casing, isolate the flame retardant layer from the electrolyte, and prevent the flame retardant layer from directly contacting the electrolyte and affecting the electrical performance of the battery; when the thermal runaway temperature is reached in the battery, the alloy layer can melt and release the flame retardant, thereby blocking the thermal runaway reaction of the battery and improving the safety performance of the battery.

[0112] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0113] The above-mentioned embodiments only express several implementation methods of the utility model, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the utility model patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the utility model, which all belong to the protection scope of the utility model. Therefore, the protection scope of the utility model patent shall be based on the attached claims.

Claims

1. A battery casing, characterized in that: The battery casing includes a shell and at least two alloy layers arranged on one side of the shell adjacent to the battery cell, a first flame retardant layer is filled between the alloy layer and the shell; a second flame retardant layer is filled between two adjacent alloy layers; and the melting points of the alloy layers decrease successively in a direction away from the shell.

2. The battery housing according to claim 1, wherein: The melting point of the alloy layer is 80°C to 200°C.

3. The battery housing according to claim 1, characterized in that: The thickness of the alloy layer is 30 μm to 50 μm.

4. The battery housing according to claim 1, wherein: The alloy layer includes a tin-bismuth alloy layer, a bismuth-lead alloy layer, a tin-bismuth-thallium alloy layer, a lead-bismuth-silver alloy layer or an indium-bismuth-tin alloy layer.

5. The battery housing according to claim 1, wherein: The thickness of the first flame retardant layer is 10 μm to 30 μm.

6. The battery housing according to claim 1, wherein: The material of the first flame retardant layer and the material of the second flame retardant layer independently include flame retardants or flame retardant composite materials, wherein the flame retardant composite material includes a flame retardant and a coating layer coated on the surface of the flame retardant.

7. The battery housing according to claim 1, wherein: The thickness of the second flame retardant layer is 10 μm to 30 μm.

8. The battery housing according to claim 1, wherein: A promoter is also filled between two adjacent alloy layers, and the promoter is used to promote the alloy layers to release metal ions.

9. A battery, characterized in that: The battery comprises the battery casing according to any one of claims 1 to 8.