A low dielectric loss high purity quartz glass fiber material prepared by sol-gel method and a preparation method thereof

CN122853688APending Publication Date: 2026-10-02JIAXING FREBANG NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611017293.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-09
Publication Date
2026-10-02

AI Technical Summary

Technical Problem

但该类方法通常依赖较多有机成纤组分或模板组分来保证纺丝稳定性和孔结构调控,后续热处理过程中容易引入残碳、表面缺陷及开放孔道,导致材料吸湿性增强,进而使介电损耗升高

Benefits of technology

[0044]与现有技术相比,本发明的有益效果为:本发明以硅氧体系为主体构建前驱溶胶和最终骨架,通过硅酸酯低聚体溶液、含氢硅氧烷低聚体溶液与硅化模板分散液,使纺丝前驱体系兼具可纺性与无机网络生长能力,在静电纺丝、预固化和热处理过程中逐步完成由有机辅助成形向无机骨架支撑的转变,减少有机成纤组分依赖,降低有机残留对纤维形貌和电性能的不利影响;通过模板限域成孔、分段加热、表面封孔与脱羟处理的配合,减少表面极性位点和外界水分进入通道,从而降低介电损耗。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122853688A_ABST
    Figure CN122853688A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of high-performance glass fiber preparation, and provides a low-dielectric-loss high-purity quartz glass fiber material prepared by a sol-gel method and a preparation method thereof. First, a silicate oligomer solution, a hydrogen-containing siloxane oligomer solution and a siliconized template dispersion liquid are prepared, and then are compounded with a silicon source and a fiber-forming aid to form a spinning precursor sol, and through electrospinning, pre-curing, segmented heat treatment, sealing and dehydroxy treatment, the high-purity quartz glass fiber material is obtained. Through the synergistic effect of oligomeric siloxane structure regulation, template limited pore formation, surface sealing and dehydroxy, the fiber continuous forming, low-connected-pore construction and impurity control are considered, which is conducive to reducing the dielectric loss and improving the material purity, structural stability and application adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-performance glass fiber preparation technology, and relates to a low dielectric loss high-purity quartz glass fiber material prepared by sol-gel method and its preparation method. Background Technology

[0002] Quartz-based glass fiber materials possess characteristics such as heat resistance, insulation, lightweight, and structural designability, making them promising for applications in electronic packaging, wave-transparent materials, thermal insulation, and high-frequency insulation. Especially in high-frequency electric field environments, materials need to maintain not only a low dielectric constant but also low dielectric loss to reduce energy dissipation and signal attenuation. Furthermore, the purity, hydroxyl content, pore structure morphology, and fiber continuity of the quartz material significantly impact its dielectric properties and service stability.

[0003] Among existing methods for preparing quartz or silica fibers, the sol-gel combined electrospinning route has attracted attention due to its mild forming process and easily tunable structure. However, this type of method typically relies on a large amount of organic fiber-forming components or template components to ensure spinning stability and pore structure control. Subsequent heat treatment can easily introduce residual carbon, surface defects, and open channels, leading to increased hygroscopicity and consequently higher dielectric loss. Simultaneously, catalysts, template agents, impurity ions in the precursor system, and exogenous contamination during preparation can also adversely affect material purity. If strong heat treatment is subsequently used to remove organic residues and surface hydroxyl groups, it can easily cause fiber shrinkage, embrittlement, or even localized crystallization, affecting fiber morphological stability and overall performance. Furthermore, the synergistic control of "dielectric reduction" and "loss reduction" in existing technologies remains insufficient. Simply introducing pores to reduce the dielectric constant often increases pore connectivity and surface active sites, which is detrimental to controlling adsorbed water and hydroxyl residues; simply emphasizing high-temperature purification and densification may weaken the lightweight and porous characteristics required for glass fibers. Summary of the Invention

[0004] To address the shortcomings of existing technologies, the present invention aims to provide a low-dielectric-loss, high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. By constructing a synergistic system of silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, and silicified template dispersion, combined with electrospinning, pre-curing, segmented heat treatment, pore sealing, and dehydroxylation processes, continuous fiber forming, low interconnected pore control, and impurity suppression are achieved, resulting in a quartz glass fiber material with high purity, low dielectric loss, and good structural stability.

[0005] To achieve this objective, the present invention adopts the following technical solution:

[0006] In a first aspect, the present invention provides a method for preparing a low-dielectric-loss, high-purity quartz glass fiber material using a sol-gel method, the method comprising:

[0007] S1, Tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and reacted to obtain silicate ester oligomer solution;

[0008] S2, Triethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and reacted to obtain a solution of hydrogen-containing siloxane oligomers;

[0009] S3, poloxamer 407, ethylene glycol and ethanol aqueous solution are mixed to obtain soft template dispersion, silicate ester oligomer solution is added dropwise to the soft template dispersion to react, tetraethoxysilane is dispersed in anhydrous ethanol and added dropwise to the reaction solution to react, to obtain silanized template dispersion;

[0010] S4, tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and pre-hydrolyzed, and silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, silanized template dispersion and polyethylene oxide are added in sequence to obtain spinning precursor sol.

[0011] S5, electrospinning the spinning precursor sol to obtain a precursor glass fiber membrane, the precursor glass fiber membrane is sequentially pre-cured and heated in segments to obtain a glass fiber membrane, the glass fiber membrane is immersed in a sealing liquid to obtain a sealing glass fiber membrane, the sealing glass fiber membrane is subjected to dehydroxylation treatment to obtain a low dielectric loss high purity quartz glass fiber material.

[0012] Specifically, it includes:

[0013] S1, mix tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution, stir for 50-70 min under ice-water bath conditions, then heat to 40-50℃ for 3-5 h, then heat to 55-65℃ and hold for 1.5-2.5 h, remove solvent under reduced pressure, redissolve in toluene and perform fractional precipitation with n-hexane, take the intermediate fraction and redisperse in anhydrous ethanol to obtain silicate oligomer solution;

[0014] S2, triethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and stirred in an ice-water bath for 50-70 min, then reacted at room temperature for 4-8 h, then heated to 40-55 °C and aged under nitrogen protection for 3-6 h. After removing the solvent under reduced pressure, it is redissolved in toluene and fractionally precipitated with n-hexane. The intermediate fraction is redispersed in anhydrous ethanol to obtain a solution of hydrogen-containing siloxane oligomers.

[0015] S3, poloxamer 407, ethylene glycol and ethanol aqueous solution are mixed and stirred for 1.5-2.5h to obtain a soft template dispersion. A silicate ester oligomer solution is added dropwise to the soft template dispersion, and the reaction is continued at 30-40℃ for 1.0-2.0h. Then, tetraethoxysilane is dispersed in anhydrous ethanol and added dropwise to the reaction solution. The pH is adjusted to 4.5-5.2 with ammonium bicarbonate aqueous solution, and the reaction is continued for 1.5-3.0h. After centrifugation, washing and redispersing in anhydrous ethanol, a silanized template dispersion is obtained.

[0016] S4, mix tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution and pre-hydrolyze at room temperature for 30-50 min, then add silicate ester oligomer solution, hydrogen siloxane oligomer solution, silicified template dispersion and polyethylene oxide in sequence, stir and let stand to degas, to obtain spinning precursor sol.

[0017] S5, electrospinning the precursor sol to obtain a precursor glass fiber membrane, pre-curing the precursor glass fiber membrane in segments to obtain a pre-cured fiber membrane, heating the pre-cured fiber membrane in segments to obtain a glass fiber membrane, immersing the glass fiber membrane in a sealing solution for 3-8 seconds and drying it at 55-65℃ for 20-40 minutes, repeating this process 1-2 times to obtain a sealed glass fiber membrane, and then performing a dehydroxylation treatment on the sealed glass fiber membrane to obtain a low dielectric loss high-purity quartz glass fiber material.

[0018] Tetraethoxysilane undergoes hydrolysis in an acidic alcohol-water system, converting the ethoxy group into a silanol. Subsequently, dehydration condensation occurs between the silanols, and dealcohydride condensation occurs between the silanols and the residual ethoxy group, forming an oligomeric silicate ester dominated by siloxane-silicon bonds. Under acidic conditions, hydrolysis precedes condensation, and the system initially generates oligomers containing silanols and residual ethoxy groups. During aging, these oligomers continue to condense, increasing the segment length and network connectivity. This oligomeric silicate ester then enters the subsequent host system, participating in subsequent condensation and backbone construction using existing siloxane segments, residual silanols, and residual ethoxy groups.

[0019] Triethoxysilane undergoes hydrolysis and condensation in similar acidic alcohol-water systems to generate oligomeric siloxanes containing siloxane-silicon bonds and silane-hydrogen bonds. The silane-hydrogen bonds in this oligomer remain at side group positions and do not serve as the primary reaction sites for conventional sol-condensation, but they do affect segment polarity, intersegmental interactions, and the skeletal rearrangement during heat treatment. After entering the host system, this oligomer undergoes co-condensation with the silanols formed by the hydrolysis of tetraethoxysilane, and the original oligomeric siloxane segments are incorporated into the host siloxane network, forming a continuous inorganic backbone.

[0020] Poloxamer forms aggregates in an ethanol-water system, with polyoxypropylene segments located inside and polyoxyethylene segments on the outer layer. Ethylene glycol forms hydrogen bonds with the polyoxyethylene segments, altering the solvation environment of the template's outer layer. After the addition of silicate oligomers, hydrogen bonds and dipole interactions occur between the silanols and polyether segments, enriching the oligomeric silica components near the template's outer layer. Subsequent addition of tetraethoxysilane further hydrolyzes and condenses in this region, further discontinuing the silica layer around the template. Adjusting the system's pH with ammonium bicarbonate increases the condensation rate, causing newly generated silanols to connect more concentratedly on the template's outer surface, forming a silica layer encapsulating the template.

[0021] The spinning system simultaneously contains incompletely hydrolyzed tetraethoxysilane, pre-formed silanols, silicate oligomers, hydrosiloxane oligomers, composite template particles, and a small amount of polyethylene oxide. Tetraethoxysilanes continuously provide a hydrolyzable silicon source, silicate oligomers provide pre-formed inorganic segments, hydrosiloxane oligomers provide an oligomeric siloxane backbone that can be incorporated into the main network, composite template particles provide local phase separation centers, and polyethylene oxide provides the chain entanglement required for electrospinning. After mixing, silanol formation, siloxane bond growth, physical entanglement between oligomeric segments, and adsorption and embedding of oligomeric siloxane segments onto the template surface occur simultaneously in the system, forming a composite sol that can be continuously stretched under an electric field.

[0022] During electrospinning, the jet is continuously stretched under the traction of an electric field. The polyethylene oxide segments are oriented during axial stretching and maintain the continuity of the jet. The inorganic oligomers concentrate and continue to condense during evaporation, and the sol transforms from a liquid state to a gel state. The composite template particles are fixed inside the forming inorganic continuous phase. Because the solvent preferentially evaporates from the outer surface, the fiber surface first forms a shell with a higher degree of condensation, and the inner layer forms a skeleton later. This creates a radial structural difference where the outer layer solidifies first and the inner layer solidifies later. This difference makes it easier to retain the internal pores after the template is removed.

[0023] During the pre-curing stage, residual ethoxy groups continue to hydrolyze, and silanols continue to condense. The morphological support of the fibers gradually shifts from polyethylene oxide chain entanglement to a silicon-oxygen network connection. The surface layer undergoes more complete condensation due to faster early evaporation, while the inner layer retains more incomplete condensation sites due to slower evaporation and diffusion. During subsequent organic matter removal, the outer framework initially provides support. After the removal of the inner template and fiber-forming agent, the corresponding space is restricted by the outer inorganic framework, forming low-connectivity pores. During segmented heating, polyethylene oxide, poloxamer, and ethylene glycol are oxidized and removed sequentially. After polyethylene oxide removal, the continuous fiber morphology is maintained by the silicon-oxygen network; after the removal of the poloxamer core, cavities remain in situ on the template; after the removal of ethylene glycol, the organic phase around the template is further reduced. Since a silicon-oxygen layer has already formed on the outside of the template, template removal manifests as cavity retention. During heating, the hydrogen-containing siloxane oligomers continue to incorporate into the silica network, residual organic side groups are eliminated, and the network gradually transforms into an inorganic framework dominated by silicon-oxygen-silicon bonds.

[0024] In the sealing solution, tetraethoxysilane undergoes further hydrolysis in an acidic alcohol-water system to generate silanol. During impregnation, the sealing solution preferentially enters the open pores and pore opening regions on the surface. During drying, the silanol entering the pore opening region undergoes local condensation, forming a new silica layer. Due to the controlled impregnation time, the newly added silica layer is mainly distributed near the pore openings and surface open pores, altering the connectivity between the pores and the outside environment and reducing the channels for external moisture to enter the internal pores. During the dehydroxylation treatment stage, the silanol on the fiber surface and pore walls continues to condense, while adsorbed water and hydrogen-bonded water desorb, reducing the number of surface polar sites. Silanol and adsorbed water can undergo orientation polarization and relaxation in an alternating electric field, thus increasing dielectric loss. Sealing reduces the pathway for moisture entry, and dehydroxylation reduces the polar sites on the pore walls and surface. After dehydroxylation, the air phase formed by the template remains inside the fiber, and the open channels and polar sites on the surface and pore openings are reduced. The final framework consists of a silicon-oxygen network formed by tetraethoxysilane, silicon-oxygen units incorporated by hydrogen-containing siloxane oligomers, and a newly added surface silicon-oxygen layer during the sealing process. The main components remain within the silicon-oxygen system. The template agent and fiber-forming aids are removed during heat treatment and do not exist as components of the final framework. The air phase in the material is left after the template occupies the sites, the continuous silicon-oxygen phase is established by sol condensation and heat treatment, the open channels are weakened by sealing, and the surface polar sites are reduced by dehydroxylation, ultimately forming a high-purity quartz glass fiber structure with low dielectric loss.

[0025] As a preferred embodiment of the present invention, in S1, the mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution is (40-45):(20-25):(5-6), for example, it can be (40, 40.5, 41, 41.5, 42, 42.5, 43, 43.5, 44, 44.5 or 45):(20, 20.5, 21, 21.5, 22, 22.5, 23, 23.5, 24, 24.5 or 25):(5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9 or 6.0), but it is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0026] In some alternative embodiments, the hydrochloric acid solution has a mass fraction of 0.5-1 wt.%, for example, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, or 1.0%, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0027] In some optional embodiments, the solid content of the silicate oligomer solution is 20-25 wt.%, for example, it can be 20 wt.%, 20.5 wt.%, 21 wt.%, 21.5 wt.%, 22 wt.%, 22.5 wt.%, 23 wt.%, 23.5 wt.%, 24 wt.%, 24.5 wt.%, or 25 wt.%, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0028] As a preferred embodiment of the present invention, in S2, the mass ratio of triethoxysilane, anhydrous ethanol, and hydrochloric acid solution is (22-26):(34-38):(2.5-3.5), for example, it can be (22, 22.4, 22.8, 23.2, 23.6, 24, 24.4, 24.8, 25.2, 25.6 or 26):(34, 34.4, 34.8, 35.2, 35.6, 36, 36.4, 36.8, 37.2, 37.6 or 38):(2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4 or 3.5), but it is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0029] In some optional embodiments, the hydrochloric acid solution has a mass fraction of 1-3 wt.%, for example, it may be 1.0 wt.%, 1.2 wt.%, 1.4 wt.%, 1.6 wt.%, 1.8 wt.%, 2.0 wt.%, 2.2 wt.%, 2.4 wt.%, 2.6 wt.%, 2.8 wt.%, or 3.0 wt.%, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0030] In some optional embodiments, the solid content of the hydrogen-containing siloxane oligomer solution is 18-22 wt.%, for example, it can be 18 wt.%, 18.4 wt.%, 18.8 wt.%, 19.2 wt.%, 19.6 wt.%, 20.0 wt.%, 20.4 wt.%, 20.8 wt.%, 21.2 wt.%, 21.6 wt.%, or 22 wt.%, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0031] As a preferred embodiment of the present invention, in S3, the mass ratio of poloxamer 407, ethylene glycol, aqueous ethanol solution, silicate ester oligomer solution, tetraethoxysilane, and anhydrous ethanol is (1.8-2.2):(2.5-3.5):(27-33):(5-7):(1.6-2.2):(8-12), for example, it can be (1.8, 1.84, 1.88, 1.92, 1.96, 2.0, 2.04, 2.08, 2.12, 2.16, or 2.2):(2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, or 3.5):(27, 2 7.6, 28.2, 28.8, 29.4, 30, 30.6, 31.2, 31.8, 32.4 or 33: (5.0, 5.2, 5.4, 5.6, 5.8, 6.0, 6.2, 6.4, 6.6, 6.8 or 7.0): (1.6, 1.66, 1.72, 1.78, 1.84, 1.9, 1.96, 2.02, 2.08, 2.14 or 2.2): (8, 8.4, 8.8, 9.2, 9.6, 10.0, 10.4, 10.8, 11.2, 11.6 or 12), but not limited to the listed values; other unlisted values ​​within this range also apply.

[0032] In some optional embodiments, the mass ratio of anhydrous ethanol to deionized water in the aqueous ethanol solution is 4:1.

[0033] In some optional embodiments, the concentration of the ammonium bicarbonate aqueous solution is 0.01-0.03 mol / L, for example, it can be 0.01 mol / L, 0.012 mol / L, 0.014 mol / L, 0.016 mol / L, 0.018 mol / L, 0.02 mol / L, 0.022 mol / L, 0.024 mol / L, 0.026 mol / L, 0.028 mol / L or 0.03 mol / L, but is not limited to the listed values, other unlisted values ​​within this range are also applicable.

[0034] In some optional embodiments, the solid content of the silanized template dispersion is 12-16 wt.%, for example, it can be 12 wt.%, 12.4 wt.%, 12.8 wt.%, 13.2 wt.%, 13.6 wt.%, 14.0 wt.%, 14.4 wt.%, 14.8 wt.%, 15.2 wt.%, 15.6 wt.%, or 16 wt.%, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0035] As a preferred embodiment of the present invention, in S4, the mass ratio of tetraethoxysilane, anhydrous ethanol, hydrochloric acid solution, silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, silanized template dispersion, and polyethylene oxide is (28-32):(22-26):(6-7):(5-7):(12-15):(14-18):(0.25-0.4), for example, it can be (28, 28.4, 28.8, 29.2, 29.6, 30.0, 30.4, 30.8, 31.2, 31.6 or 32):(22, 22.4, 22.8, 23.2, 23.6, 24, 24.4, 24.8, 25.2, 25.6 or 26):(6.0, 6.1, 6.2, 6.3, 6.4, 6.5, ... 6.6, 6.7, 6.8, 6.9, or 7.0: (5.0, 5.2, 5.4, 5.6, 5.8, 6.0, 6.2, 6.4, 6.6, 6.8, or 7.0): (12, 12.3, 12.6, 12.9, 13.2, 13.5, 13.8, 14.1, 14.4, 14.7, or 15): (14, 14.4, 14.8) 15.2, 15.6, 16.0, 16.4, 16.8, 17.2, 17.6 or 18: (0.25, 0.265, 0.28, 0.295, 0.31, 0.325, 0.34, 0.355, 0.37, 0.385 or 0.4), but not limited to the listed values; other unlisted values ​​within this range also apply.

[0036] In some alternative embodiments, the hydrochloric acid solution has a mass fraction of 0.5-1 wt.%, for example, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, or 1.0%, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0037] In some optional embodiments, the molecular weight of the polyethylene oxide is 600,000-1,000,000, for example, 600,000, 640,000, 680,000, 720,000, 760,000, 800,000, 840,000, 880,000, 920,000, 960,000 or 1,000,000, but is not limited to the listed values, and other unlisted values ​​within this range are also applicable.

[0038] As a preferred embodiment of the present invention, in step S5, the parameters of the electrospinning are: spinning voltage of 18-24 kV, feed rate of 0.6-0.8 mL / h, distance from needle tip to receiver of 16-20 cm, ambient temperature of 22-26 °C, and relative humidity not exceeding 20%. For example, the parameters could be: spinning voltage of (18, 18.6, 19.2, 19.8, 20.4, 21, 21.6, 22.2, 22.8, 23.4, or 24) kV, feed rate of (0.6, 0.62, 0.64, 0.66, 0.68, 0.7, 0.72, 0.74, 0.76, 0.78, or 0.8) mL / h, and distance from needle tip to receiver of (16, 16.4, 24, 23.4, 2 ... The values ​​are: 16.8, 17.2, 17.6, 18, 18.4, 18.8, 19.2, 19.6 or 20 cm; ambient temperature is (22, 22.4, 22.8, 23.2, 23.6, 24, 24.4, 24.8, 25.2, 25.6 or 26) °C; and relative humidity is not higher than 20%, but are not limited to the listed values. Other unlisted values ​​within this range also apply.

[0039] In some optional embodiments, the parameters for segmented pre-curing are as follows: sequentially heat preservation at 35-45℃ for 1.5-2.5h, at 75-85℃ for 3-5h, at 110-130℃ for 1.5-2.5h, and at 170-190℃ for 0.5-1.5h. For example, it could be: holding at (35, 36, 37, 38, 39, 40, 41, 42, 43, 44 or 45)℃ for (1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5) hours, holding at (75, 76, 77, 78, 79, 80, 81, 82, 83, 84 or 85)℃ for (3.0, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8 or 5.0) hours, holding at (110, 112, 114, 116, 118, 1 The temperature shall be maintained at (20, 122, 124, 126, 128 or 130)℃ for (1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5) h, or at (170, 172, 174, 176, 178, 180, 182, 184, 186, 188 or 190)℃ for (0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4 or 1.5) h, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0040] In some optional embodiments, the parameters for the segmented heating are as follows: the segmented heating is carried out in flowing dry air, with the temperature increased to 280-320℃ at a rate of 0.3-0.6℃ / min and held for 1-2 hours, then increased to 380-400℃ at a rate of 1-2℃ / min and held for 0.5-1 hours, then increased to 430-470℃ at a rate of 0.5-1℃ / min and held for 1.5-2.5 hours, and then increased to 580-620℃ at a rate of 0.5-1℃ / min and held for 1.5-3.0 hours. For example, it could be: heating at (0.3, 0.33, 0.36, 0.39, 0.42, 0.45, 0.48, 0.51, 0.54, 0.57, or 0.6) °C / min to (280, 284, 288, 292, 296, 300, 304, 308, 312, 316, or 320) °C and holding at that temperature for (1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0) h, then... Increase the temperature at (1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2.0) °C / min to (380, 382, ​​384, 386, 388, 390, 392, 394, 396, 398 or 400) °C and hold for (0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95 or 1.0) h, then increase the temperature at (0.5, 0.55, 0) °C / min to (380, 382, ​​384, 386, 388, 390, 392, 394, 396, 398 or 400) °C for (0.5, 0.55, 0) h. Increase the temperature by (0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, or 1.0)℃ / min to (430, 434, 438, 442, 446, 450, 454, 458, 462, 466, or 470)℃ and hold for (1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, or 2.5) h, then increase the temperature by (0.5, 0.55, 0.6, 0.65, 0.7, ...)℃ / min to (430, 434, 438, 442, 446, 450, 454, 458, 462, 466, or 470) h, then ...0.65, 0.7, ...)℃ / min to (430, 434, 438, 442, 446, 450, 454, 458, 462, 4 Increase the temperature by 0.75, 0.8, 0.85, 0.9, 0.95 or 1.0)℃ / min to (580, 584, 588, 592, 596, 600, 604, 608, 612, 616 or 620)℃ and hold for (1.5, 1.65, 1.8, 1.95, 2.1, 2.25, 2.4, 2.55, 2.7, 2.85 or 3.0)h, but is not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0041] In some optional embodiments, the sealing solution is prepared by mixing tetraethoxysilane, anhydrous ethanol, and 1-2 wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for 1-3 hours to obtain the sealing solution, wherein the mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution is (1.5-2.5):(18-24):(2-4). For example, it can be prepared by mixing tetraethoxysilane, anhydrous ethanol, and (1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0) wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for (1.0, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, or 3.0) hours to obtain the sealing solution, wherein the mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution is (1.5, 1.6, 1.7, 1.8, 1.9, 1.9, or 2.0) wt.% hydrochloric acid solution. 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5: (18, 18.6, 19.2, 19.8, 20.4, 21, 21.6, 22.2, 22.8, 23.4 or 24): (2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8 or 4.0), but not limited to the listed values; other unlisted values ​​within this range also apply.

[0042] In some optional embodiments, the parameters for the dehydroxylation treatment are: nitrogen atmosphere, holding at 760-820°C for 20-40 min, then raising the temperature to 880-920°C and holding for 5-10 min. For example, it could be: a nitrogen atmosphere, held at (760, 766, 772, 778, 784, 790, 796, 802, 808, 814 or 820)℃ for (20, 22, 24, 26, 28, 30, 32, 34, 36, 38 or 40) min, then heated to (880, 884, 888, 892, 896, 900, 904, 908, 912, 916 or 920)℃ and held for (5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5 or 10) min, but not limited to the listed values; other unlisted values ​​within this range are also applicable.

[0043] In a second aspect, the present invention provides a low dielectric loss high-purity quartz glass fiber material prepared by the preparation method described in the first aspect.

[0044] Compared with the prior art, the beneficial effects of the present invention are as follows: The present invention constructs the precursor sol and the final skeleton mainly based on the silicon-oxygen system. Through the silicate ester oligomer solution, the hydrogen-containing siloxane oligomer solution and the siliconized template dispersion, the spinning precursor system has both spinnability and inorganic network growth capability. During the electrospinning, pre-curing and heat treatment processes, the transformation from organic-assisted forming to inorganic skeleton support is gradually completed, reducing the dependence on organic fiber-forming components and reducing the adverse effects of organic residues on fiber morphology and electrical properties. Through the combination of template confined pore formation, segmented heating, surface sealing and dehydroxylation treatment, the surface polar sites and external moisture ingress channels are reduced, thereby reducing dielectric loss. Attached Figure Description

[0045] Figure 1 This is a SEM image of the low dielectric loss high-purity quartz glass fiber material provided in Embodiment 1 of the present invention. Detailed Implementation

[0046] The technical solutions of the present invention will be described in detail below with reference to specific embodiments and accompanying drawings. The embodiments described herein are specific implementations of the present invention, used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary, and should not be construed as limiting the implementation methods or the scope of protection of the present invention. In addition to the embodiments described herein, those skilled in the art can employ other obvious technical solutions based on the content disclosed in the claims and specification of this application. These technical solutions include those that make any obvious substitutions and modifications to the embodiments described herein.

[0047] The chemical reagents used in the embodiments and comparative examples of this invention are all commercially available products and have not undergone any further purification treatment.

[0048] Example 1

[0049] This embodiment provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The preparation method specifically includes the following steps:

[0050] S1, Tetraethoxysilane, anhydrous ethanol and 0.5 wt.% hydrochloric acid solution are mixed, the mass ratio of tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution is 40:25:5, stirred for 70 min under ice-water bath conditions, then heated to 40℃ for 5 h for aging, then heated to 55℃ and held for 2.5 h, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a silicate oligomer solution with a solid content of 20 wt.%;

[0051] S2, Triethoxysilane, anhydrous ethanol and 1 wt.% hydrochloric acid solution are mixed, the mass ratio of triethoxysilane, anhydrous ethanol and hydrochloric acid solution is 22:38:2.5, stirred for 70 min under ice-water bath conditions, then reacted at room temperature for 4 h, then heated to 55 °C, aged for 3 h under nitrogen protection, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a hydrogen-containing siloxane oligomer solution with a solid content of 22 wt.%;

[0052] S3, poloxamer 407, ethylene glycol, and an aqueous ethanol solution were mixed and stirred for 2.5 h to obtain a soft template dispersion. The mass ratio of anhydrous ethanol to deionized water in the aqueous ethanol solution was 4:1. A silicate ester oligomer solution was added dropwise to the soft template dispersion, and the reaction was continued at 30 °C for 2.0 h. Then, tetraethoxysilane was dispersed in anhydrous ethanol and added dropwise to the reaction solution. The mass ratio of poloxamer 407, ethylene glycol, aqueous ethanol solution, silicate ester oligomer solution, tetraethoxysilane, and anhydrous ethanol was 2.2:2.5:33:5:2.2:8. The pH was adjusted to 4.5 using a 0.01 mol / L ammonium bicarbonate aqueous solution, and the reaction was continued for 3.0 h. After centrifugation, washing, and redispersing in anhydrous ethanol, a silanized template dispersion with a solid content of 12 wt.% was obtained.

[0053] S4, tetraethoxysilane, anhydrous ethanol, and 0.5 wt.% hydrochloric acid solution are mixed and pre-hydrolyzed at room temperature for 50 min. Then, silicate ester oligomer solution, hydrosiloxane oligomer solution, silanized template dispersion, and polyethylene oxide with a molecular weight of 1,000,000 are added sequentially. The mass ratio of tetraethoxysilane, anhydrous ethanol, hydrochloric acid solution, silicate ester oligomer solution, hydrosiloxane oligomer solution, silanized template dispersion, and polyethylene oxide is 28:26:6:5:15:14:0.25. The mixture is stirred and allowed to stand to remove bubbles, thus obtaining a spinning precursor sol.

[0054] S5. Electrospinning the precursor sol to obtain a precursor glass fiber membrane. The electrospinning parameters are: spinning voltage of 18kV, feed rate of 0.8mL / h, needle tip to receiver distance of 16cm, ambient temperature of 22℃, and relative humidity not exceeding 20%. The precursor glass fiber membrane is then pre-cured in segments to obtain a pre-cured fiber membrane. The segmental pre-curing parameters are: sequentially holding at 35℃ for 2.5h, at 75℃ for 5h, at 130℃ for 1.5h, and at 170℃ for 1.5h. The pre-cured fiber membrane is then heated in segments to obtain a glass fiber membrane. The segmental heating parameters are: segmental heating is carried out in flowing dry air, increasing the temperature to 280℃ at a rate of 0.6℃ / min and holding for 2h, then increasing the temperature at a rate of 2℃ / min. The temperature was raised to 380℃ and held for 1 hour, then increased to 470℃ at a rate of 0.5℃ / min and held for 1.5 hours, then increased to 580℃ at a rate of 1℃ / min and held for 3.0 hours. The glass fiber membrane was then immersed in the sealing solution for 8 seconds and dried at 55℃ for 40 minutes. This process was repeated twice to obtain the sealed glass fiber membrane. The sealing solution was prepared by mixing tetraethoxysilane, anhydrous ethanol, and 1 wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for 1 hour to obtain the sealing solution. The mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution was 1.5:24:2. The sealed glass fiber membrane was then subjected to a dehydroxylation treatment. The parameters for the dehydroxylation treatment were: nitrogen atmosphere, holding at 760℃ for 40 minutes, then raising the temperature to 880℃ and holding for 10 minutes to obtain a low dielectric loss high-purity quartz glass fiber material.

[0055] Figure 1 The image shows a SEM image of the low dielectric loss high-purity quartz glass fiber material provided in this embodiment. The fibers are of uniform thickness and have no obvious nodules.

[0056] Example 2

[0057] This embodiment provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The preparation method specifically includes the following steps:

[0058] S1, Tetraethoxysilane, anhydrous ethanol and 1 wt.% hydrochloric acid solution are mixed, the mass ratio of tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution is 45:20:6, stirred for 50 min under ice water bath conditions, then heated to 50℃ for 3 h for aging, then heated to 65℃ and kept at that temperature for 1.5 h, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a silicate oligomer solution with a solid content of 25 wt.%;

[0059] S2, triethoxysilane, anhydrous ethanol and 3 wt.% hydrochloric acid solution are mixed, the mass ratio of triethoxysilane, anhydrous ethanol and hydrochloric acid solution is 26:34:3.5, stirred for 50 min under ice-water bath conditions, then reacted at room temperature for 8 h, then heated to 40 °C, aged for 6 h under nitrogen protection, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a hydrogen-containing siloxane oligomer solution with a solid content of 18 wt.%;

[0060] S3, poloxamer 407, ethylene glycol, and an aqueous ethanol solution were mixed and stirred for 1.5 h to obtain a soft template dispersion. The mass ratio of anhydrous ethanol to deionized water in the aqueous ethanol solution was 4:1. A silicate ester oligomer solution was added dropwise to the soft template dispersion, and the reaction was continued at 40 °C for 1.0 h. Then, tetraethoxysilane was dispersed in anhydrous ethanol and added dropwise to the reaction solution. The mass ratio of poloxamer 407, ethylene glycol, aqueous ethanol solution, silicate ester oligomer solution, tetraethoxysilane, and anhydrous ethanol was 1.8:3.5:27:7:1.6:12. The pH was adjusted to 5.2 with 0.03 mol / L ammonium bicarbonate aqueous solution, and the reaction was continued for 1.5 h. After centrifugation, washing, and redispersing in anhydrous ethanol, a silanized template dispersion with a solid content of 16 wt.% was obtained.

[0061] S4, tetraethoxysilane, anhydrous ethanol and 1 wt.% hydrochloric acid solution are mixed and pre-hydrolyzed at room temperature for 30 min. Then, silicate ester oligomer solution, hydrosiloxane oligomer solution, silanized template dispersion and polyethylene oxide with a molecular weight of 600,000 are added sequentially. The mass ratio of tetraethoxysilane, anhydrous ethanol, hydrochloric acid solution, silicate ester oligomer solution, hydrosiloxane oligomer solution, silanized template dispersion and polyethylene oxide is 32:22:7:7:12:18:0.4. The mixture is stirred and allowed to stand to remove bubbles to obtain a spinning precursor sol.

[0062] S5. Electrospinning the precursor sol to obtain a precursor glass fiber membrane. The electrospinning parameters are: spinning voltage of 24kV, feed rate of 0.6mL / h, needle tip to receiver distance of 20cm, ambient temperature of 26℃, and relative humidity not exceeding 20%. The precursor glass fiber membrane is then pre-cured in segments to obtain a pre-cured fiber membrane. The segmental pre-curing parameters are: sequentially holding at 45℃ for 1.5h, at 85℃ for 3h, at 110℃ for 2.5h, and at 190℃ for 0.5h. The pre-cured fiber membrane is then heated in segments to obtain a glass fiber membrane. The segmental heating parameters are: segmental heating is carried out in flowing dry air, with the temperature increased to 320℃ at a rate of 0.3℃ / min and held for 1h, followed by a further increase in temperature at a rate of 1℃ / min. The temperature was raised to 400℃ and held for 0.5 h, then increased to 430℃ at 1℃ / min and held for 2.5 h, then increased to 620℃ at 0.5℃ / min and held for 1.5 h. The glass fiber membrane was then immersed in the sealing solution for 3 s and dried at 65℃ for 20 min. This process was repeated once to obtain the sealed glass fiber membrane. The sealing solution was prepared by mixing tetraethoxysilane, anhydrous ethanol, and 2 wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for 3 h to obtain the sealing solution. The mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution was 2.5:18:4. The sealed glass fiber membrane was then subjected to a dehydroxylation treatment. The parameters for the dehydroxylation treatment were: nitrogen atmosphere, holding at 820℃ for 20 min, then increasing to 920℃ and holding for 5 min to obtain a low dielectric loss high-purity quartz glass fiber material.

[0063] Example 3

[0064] This embodiment provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The preparation method specifically includes the following steps:

[0065] S1, Tetraethoxysilane, anhydrous ethanol and 0.8 wt.% hydrochloric acid solution are mixed, the mass ratio of tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution is 42:22:5.5, stirred for 60 min under ice-water bath conditions, then heated to 45℃ for 4 h for aging, then heated to 60℃ and held for 2.0 h, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a silicate oligomer solution with a solid content of 22 wt.%;

[0066] S2, Triethoxysilane, anhydrous ethanol and 2 wt.% hydrochloric acid solution are mixed, the mass ratio of triethoxysilane, anhydrous ethanol and hydrochloric acid solution is 24:36:3.0, stirred for 60 min under ice-water bath conditions, then reacted at room temperature for 6 h, then heated to 48 °C, aged for 4.5 h under nitrogen protection, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a hydrogen-containing siloxane oligomer solution with a solid content of 20 wt.%;

[0067] S3, poloxamer 407, ethylene glycol, and an aqueous ethanol solution were mixed and stirred for 2.0 h to obtain a soft template dispersion. The mass ratio of anhydrous ethanol to deionized water in the aqueous ethanol solution was 4:1. A silicate ester oligomer solution was added dropwise to the soft template dispersion, and the reaction was continued at 35 °C for 1.5 h. Then, tetraethoxysilane was dispersed in anhydrous ethanol and added dropwise to the reaction solution. The mass ratio of poloxamer 407, ethylene glycol, aqueous ethanol solution, silicate ester oligomer solution, tetraethoxysilane, and anhydrous ethanol was 2.0:3.0:30:6:1.9:10. The pH was adjusted to 4.8 using a 0.02 mol / L ammonium bicarbonate aqueous solution, and the reaction was continued for 2.2 h. The mixture was centrifuged, washed, and redispersed in anhydrous ethanol to obtain a silanized template dispersion with a solid content of 14 wt.%.

[0068] S4, tetraethoxysilane, anhydrous ethanol, and 0.8 wt.% hydrochloric acid solution are mixed and pre-hydrolyzed at room temperature for 40 min. Then, silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, silanized template dispersion, and polyethylene oxide with a molecular weight of 800,000 are added sequentially. The mass ratio of tetraethoxysilane, anhydrous ethanol, hydrochloric acid solution, silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, silanized template dispersion, and polyethylene oxide is 30:24:6.5:6:13:16:0.32. The mixture is stirred and allowed to stand to remove bubbles, thus obtaining a spinning precursor sol.

[0069] S5. Electrospinning the precursor sol to obtain a precursor glass fiber membrane. The electrospinning parameters are: spinning voltage of 21kV, feed rate of 0.7mL / h, needle tip to receiver distance of 18cm, ambient temperature of 24℃, and relative humidity not exceeding 20%. The precursor glass fiber membrane is then pre-cured in segments to obtain a pre-cured fiber membrane. The segmental pre-curing parameters are: sequentially holding at 40℃ for 2.0h, at 80℃ for 4h, at 120℃ for 2.0h, and at 180℃ for 1.0h. The pre-cured fiber membrane is then heated in segments to obtain a glass fiber membrane. The segmental heating parameters are: segmental heating is carried out in flowing dry air, with the temperature increased to 300℃ at a rate of 0.45℃ / min and held for 1.5h, followed by further heating at a rate of 1.5℃ / min. The temperature was raised to 390℃ and held for 0.8 h, then increased to 450℃ at 0.8℃ / min and held for 2.0 h, then increased to 600℃ at 0.8℃ / min and held for 2.2 h. The glass fiber membrane was then immersed in the sealing solution for 5 s and dried at 60℃ for 30 min. This process was repeated once to obtain a sealed glass fiber membrane. The sealing solution was prepared by mixing tetraethoxysilane, anhydrous ethanol, and 1.5 wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for 2 h to obtain the sealing solution. The mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution was 2.0:21:3. The sealed glass fiber membrane was then subjected to a dehydroxylation treatment. The parameters for the dehydroxylation treatment were: nitrogen atmosphere, holding at 790℃ for 30 min, then raising the temperature to 900℃ and holding for 8 min to obtain a low dielectric loss high-purity quartz glass fiber material.

[0070] Example 4

[0071] This embodiment provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The preparation method specifically includes the following steps:

[0072] S1, Tetraethoxysilane, anhydrous ethanol and 0.6 wt.% hydrochloric acid solution are mixed, the mass ratio of tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution is 43:23:5.8, stirred for 65 min under ice-water bath conditions, then heated to 48℃ for 4.5 h for aging, then heated to 62℃ and held for 2.2 h, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a silicate oligomer solution with a solid content of 23 wt.%;

[0073] S2, Triethoxysilane, anhydrous ethanol and 2.5 wt.% hydrochloric acid solution are mixed, the mass ratio of triethoxysilane, anhydrous ethanol and hydrochloric acid solution is 25:35:3.2, stirred for 65 min under ice-water bath conditions, then reacted at room temperature for 7 h, then heated to 50 °C, aged for 5 h under nitrogen protection, after removing the solvent under reduced pressure, redissolved in toluene and fractionally precipitated with n-hexane, the intermediate fraction is redispersed in anhydrous ethanol to obtain a hydrogen-containing siloxane oligomer solution with a solid content of 19 wt.%;

[0074] S3, poloxamer 407, ethylene glycol, and an aqueous ethanol solution were mixed and stirred for 2.2 h to obtain a soft template dispersion. The mass ratio of anhydrous ethanol to deionized water in the aqueous ethanol solution was 4:1. A silicate ester oligomer solution was added dropwise to the soft template dispersion, and the reaction was continued at 38 °C for 1.8 h. Then, tetraethoxysilane was dispersed in anhydrous ethanol and added dropwise to the reaction solution. The mass ratio of poloxamer 407, ethylene glycol, aqueous ethanol solution, silicate ester oligomer solution, tetraethoxysilane, and anhydrous ethanol was 1.9:3.2:31:6.5:2.0:11. The pH was adjusted to 5.0 with 0.025 mol / L ammonium bicarbonate aqueous solution, and the reaction was continued for 2.5 h. After centrifugation, washing, and redispersing in anhydrous ethanol, a silanized template dispersion with a solid content of 15 wt.% was obtained.

[0075] S4, tetraethoxysilane, anhydrous ethanol, and 0.6 wt.% hydrochloric acid solution are mixed and pre-hydrolyzed at room temperature for 45 min. Then, silicate ester oligomer solution, hydrosiloxane oligomer solution, silanized template dispersion, and polyethylene oxide with a molecular weight of 900,000 are added sequentially. The mass ratio of tetraethoxysilane, anhydrous ethanol, hydrochloric acid solution, silicate ester oligomer solution, hydrosiloxane oligomer solution, silanized template dispersion, and polyethylene oxide is 31:25:6.8:6.5:14:15:0.35. The mixture is stirred and allowed to stand to remove bubbles, thus obtaining a spinning precursor sol.

[0076] S5. Electrospinning the precursor sol to obtain a precursor glass fiber membrane. The electrospinning parameters are: spinning voltage of 22kV, feed rate of 0.65mL / h, needle tip to receiver distance of 19cm, ambient temperature of 25℃, and relative humidity not exceeding 20%. The precursor glass fiber membrane is then pre-cured in segments to obtain a pre-cured fiber membrane. The segmental pre-curing parameters are: sequentially holding at 42℃ for 2.2h, at 82℃ for 4.5h, at 125℃ for 2.2h, and at 185℃ for 1.2h. The pre-cured fiber membrane is then subjected to segmental heating to obtain a glass fiber membrane. The segmental heating parameters are: segmental heating is carried out in flowing dry air, with the temperature increased to 310℃ at a rate of 0.5℃ / min and held for 1.8h, followed by a further increase in temperature at a rate of 1.8℃ / min. The temperature was raised to 395℃ and held for 0.6 h, then increased to 460℃ at 0.6℃ / min and held for 2.2 h, then increased to 610℃ at 0.6℃ / min and held for 2.5 h. The glass fiber membrane was then immersed in the sealing solution for 6 s and dried at 62℃ for 35 min. This process was repeated twice to obtain the sealed glass fiber membrane. The sealing solution was prepared by mixing tetraethoxysilane, anhydrous ethanol, and 1.8 wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for 2.5 h to obtain the sealing solution. The mass ratio of tetraethoxysilane, anhydrous ethanol, and hydrochloric acid solution was 2.2:22:3.5. The sealed glass fiber membrane was then subjected to a dehydroxylation treatment. The parameters for the dehydroxylation treatment were: nitrogen atmosphere, holding at 800℃ for 35 min, then increasing to 910℃ and holding for 6 min to obtain a low dielectric loss high-purity quartz glass fiber material.

[0077] Comparative Example 1

[0078] This comparative example provides a low dielectric loss high purity quartz glass fiber material prepared by sol-gel method and its preparation method. The difference between this example and Example 1 is that no silicified template dispersion is added in S4, and an equal mass of anhydrous ethanol is used to replace the silicified template dispersion in Example 1. Other process parameters and operating conditions are exactly the same as in Example 1.

[0079] Comparative Example 2

[0080] This comparative example provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The difference between this and Example 1 is that in S3, after mixing poloxamer, ethylene glycol and ethanol aqueous solution to obtain a soft template dispersion, the silicate ester oligomer solution is not added dropwise, nor is tetraethoxysilane added dropwise for silanization reaction. Instead, the soft template dispersion is directly added to S4 as a silanization template dispersion. Other process parameters and operating conditions are exactly the same as in Example 1.

[0081] Comparative Example 3

[0082] This comparative example provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The difference between this example and Example 1 is that no hydrogen-containing siloxane oligomer solution is added in S4, and an equal mass of anhydrous ethanol is used to replace the hydrogen-containing siloxane oligomer solution in Example 1. Other process parameters and operating conditions are exactly the same as in Example 1.

[0083] Comparative Example 4

[0084] This comparative example provides a low dielectric loss high-purity quartz glass fiber material prepared by the sol-gel method and its preparation method. The difference between this and Example 1 is that the sealing treatment step is omitted. That is, after obtaining the glass fiber membrane, the sealing solution is not impregnated and dried, but the dehydroxylation treatment is carried out directly. Other process parameters and operating conditions are exactly the same as those in Example 1.

[0085] The dielectric constant (Dk) and dielectric loss factor (Df) were tested at 1 MHz using the parallel plate method according to ASTM D150-22, and the sample thickness was determined according to ASTM D374 / D374M-23.

[0086] The dielectric constant (Dk) and dielectric loss factor (Df) were tested at 10 GHz using the split-pillar dielectric resonator method according to IPC-TM-6502.5.5.15.

[0087] The test results for dielectric constant and dielectric loss factor are shown in Table 1.

[0088] Table 1 Test results of quartz glass fiber materials in Examples 1-4 and Comparative Examples 1-4

[0089]

[0090] As shown in Table 1, compared to Example 1, the dielectric constants and dielectric loss factors of Comparative Examples 1-4 all increased. This is because Comparative Example 1 did not include a silanized template dispersion, resulting in a lack of stable pore-forming units within the fiber. After heat treatment, the proportion of the air phase decreased, leading to an increase in the dielectric constant. Simultaneously, the pore structure regulation weakened, and uneven local shrinkage increased interfacial polarization, resulting in an increase in the dielectric loss factor. In Comparative Example 2, when a non-silanized template was used, open pores and non-uniform channels were easily formed after subsequent heating to remove the template. Although the air phase could retain some dielectric-lowering effect, the increased number of open channels enhanced the influence of adsorbed water and surface polar sites, thus increasing losses. In Comparative Example 3, without the addition of a hydrogen-containing siloxane oligomer solution, the number of inorganic oligomer segments that could be incorporated into the main network in the precursor sol decreased. The structural uniformity of the skeleton established during spinning and heat treatment decreased, leading to a decrease in pore wall continuity. Consequently, both the dielectric constant and dielectric loss factor were higher than in Example 1. In Comparative Example 4, after the sealing treatment was removed, the surface open pores and pore channels were not weakened by the secondary silica layer, making it easier for external moisture to enter the fiber interior. The polarization loss caused by silanol and adsorbed water on the pore wall was enhanced, and the dielectric loss factor increased.

[0091] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A method for preparing low-dielectric-loss, high-purity quartz glass fiber material using a sol-gel method, characterized in that, The preparation method includes: S1, tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and reacted to obtain silicate ester oligomer solution; S2, triethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and reacted to obtain a solution of hydrogen-containing siloxane oligomers; S3, poloxamer 407, ethylene glycol and ethanol aqueous solution are mixed to obtain a soft template dispersion. A silicate ester oligomer solution is added dropwise to the soft template dispersion to react. Tetraethoxysilane is dispersed in anhydrous ethanol and added dropwise to the reaction solution to react, to obtain a silanized template dispersion. S4, tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution are mixed and pre-hydrolyzed, and silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, silanized template dispersion and polyethylene oxide are added in sequence to obtain spinning precursor sol; S5, electrospinning the spinning precursor sol to obtain a precursor glass fiber membrane, the precursor glass fiber membrane is sequentially pre-cured and heated in segments to obtain a glass fiber membrane, the glass fiber membrane is immersed in a sealing liquid to obtain a sealing glass fiber membrane, the sealing glass fiber membrane is subjected to dehydroxylation treatment to obtain a low dielectric loss high purity quartz glass fiber material.

2. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S1: The mass ratio of the tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution is (40-45):(20-25):(5-6).

3. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S2: The mass ratio of the triethoxysilane, anhydrous ethanol and hydrochloric acid solution is (22-26):(34-38):(2.5-3.5).

4. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S3: The mass ratio of poloxamer 407, ethylene glycol, aqueous ethanol solution, silicate oligomer solution, tetraethoxysilane and anhydrous ethanol is (1.8-2.2):(2.5-3.5):(27-33):(5-7):(1.6-2.2):(8-12).

5. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S4: The mass ratio of tetraethoxysilane, anhydrous ethanol, hydrochloric acid solution, silicate ester oligomer solution, hydrogen-containing siloxane oligomer solution, silicified template dispersion to polyethylene oxide is (28-32):(22-26):(6-7):(5-7):(12-15):(14-18):(0.25-0.4).

6. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S5: The parameters for electrospinning are as follows: spinning voltage of 18-24kV, feed rate of 0.6-0.8mL / h, distance from needle tip to receiver of 16-20cm, ambient temperature of 22-26℃, and relative humidity not exceeding 20%.

7. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S5: The parameters for segmented pre-curing are as follows: heat preservation at 35-45℃ for 1.5-2.5h, heat preservation at 75-85℃ for 3-5h, heat preservation at 110-130℃ for 1.5-2.5h, and heat preservation at 170-190℃ for 0.5-1.5h.

8. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S5: The parameters for the segmented heating are as follows: the segmented heating is carried out in flowing dry air, with the temperature increased to 280-320℃ at a rate of 0.3-0.6℃ / min and held for 1-2 hours, then increased to 380-400℃ at a rate of 1-2℃ / min and held for 0.5-1 hours, then increased to 430-470℃ at a rate of 0.5-1℃ / min and held for 1.5-2.5 hours, and then increased to 580-620℃ at a rate of 0.5-1℃ / min and held for 1.5-3.0 hours.

9. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S5: The sealing solution is prepared by mixing tetraethoxysilane, anhydrous ethanol and 1-2 wt.% hydrochloric acid solution, and stirring and hydrolyzing at room temperature for 1-3 h to obtain the sealing solution, wherein the mass ratio of tetraethoxysilane, anhydrous ethanol and hydrochloric acid solution is (1.5-2.5):(18-24):(2-4).

10. The method for preparing low-dielectric-loss high-purity quartz glass fiber material by sol-gel method according to claim 1, characterized in that, In S5: The parameters for the dehydroxylation treatment are: nitrogen atmosphere, holding at 760-820℃ for 20-40 min, then raising the temperature to 880-920℃ and holding for 5-10 min.

11. A low-dielectric-loss, high-purity quartz glass fiber material prepared by a sol-gel method, characterized in that, It is prepared by the preparation method according to any one of claims 1-10.