Gas sensor and method for manufacturing it

DE102009020841B4Active Publication Date: 2024-12-05NITERRA CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
DE102009020841
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2009-03-24
Filing Date
2009-05-12
Publication Date
2024-12-05
Estimated Expiration
2029-05-12

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Gas sensor with a gas sensor element extending in a longitudinal direction thereof, the gas sensor element comprising: a first measuring chamber, which is placed between two solid electrolyte layers stacked with a gap between them, and into which a gas to be measured is introduced from outside the gas sensor; a first pump cell with a first inner pump electrode facing the first measuring chamber and a first counterpart electrode for the first inner pump electrode, wherein the first inner pump electrode is designed to control oxygen partial pressure in the first measuring chamber; a second measuring chamber in reciprocal connection with the first measuring chamber, which is separated from the environment and into which the gas to be measured is introduced from the first measuring chamber at the controlled oxygen partial pressure; and a second pump cell with a second inner pump electrode arranged in the second measuring chamber and a second counterpart electrode for the second inner pump electrode, wherein the second pump cell is designed to detect a specific gas component in the gas to be measured in the second measuring chamber, characterized by the fact that the second inner pump electrode consists of an assembly that contains Pt as its main component, which consists of several Pt particles, in a cross-sectional plane of the gas sensor element along its stacking direction when viewing a reflection electron image that includes an interface between the second inner pump electrode and a solid electrolyte layer in contact with the second inner pump electrode, a surface of the Pt particles forming the outermost surface of the second inner pump electrode is defined as the surface to be measured, maximum and minimum heights between the surface to be measured of individual Pt particles and the interface are determined from a direct distance perpendicular to the interface, and the relationships T1-T2 ≥ 5 µm and T2 / T1≤0.75 are satisfied, where T1 (µm) is a mean of the three largest values ​​of the maximum heights arranged in a descending order from the largest value, and T2 (µm) is a mean of the three smallest values ​​of the minimum heights arranged in an ascending order from the smallest value.
Need to check novelty before this filing date? Find Prior Art

Description

Background of the invention 1. Field of the invention

[0001] The present invention relates to a gas sensor with a gas sensor element that detects the concentration of a specific gas, for example NOx, contained in a combustion gas or exhaust gas, for example from a burner, engine or the like, and to a method for manufacturing the gas sensor. 2. Description of the state of the art

[0002] There is a need to further reduce the amount of nitrogen oxide (NOx) contained in exhaust gases, as regulations regarding engine emissions, for example from motor vehicles, have become stricter. In this regard, a NOx sensor has been developed that can directly measure the NOx concentration.

[0003] The NOx sensor comprises a gas sensing element with one or more cells, each containing a pair of electrodes formed on the surface of an oxygen-ion-conducting solid electrolyte layer, such as zirconium oxide. A first pump cell pumps oxygen out of a first measuring chamber while remaining in reciprocal contact with a second chamber for receiving the gas to be measured. Furthermore, an oxygen concentration detection cell measures the oxygen concentration in the first measuring chamber and controls the first pump cell to achieve a predetermined oxygen concentration in the first measuring chamber. The gas to be measured flows from the first measuring chamber into the second measuring chamber at a controlled oxygen concentration. NOx contained in the gas to be measured is decomposed into N₂ and O₂ by applying a predetermined electrical voltage to the second pump cell.A second pump current flowing between a pair of electrodes of the second pump cell is measured, thereby detecting the NOx concentration in the gas to be measured.

[0004] In such a NOx sensor, an inner second pump electrode of the second pump cell is provided in the second measuring chamber and has the primary function of pumping the O2 component resulting from the decomposition of a trace amount of NOx contained in the gas to be measured. To improve the durability of the inner second pump electrode, a technique was developed that uses cermet, consisting of a Pt-Rh alloy and ceramic, as the electrode material (see patent specification 1). A technique was also developed for using a mixture consisting of Pt-Rh powder and zirconium oxide powder as the material for the inner second pump electrode (see patent specification 2).

[0005] Further generic embodiments are also known from patent specifications 3 to 6. [Patent specification 1]: JP H11 - 183 434 A [Patent 2]: JP 2005 - 283 240 A [Patent specification 3]: US 2007 / 0 151 849 A1 [Patent specification 4]: US 2002 / 0011 410 A1 [Patent specification 5]: DE 198 54 889 A1 [Patent specification 6]: DE 101 09 676 A1 3. Problems to be solved by the invention

[0006] The primary function of the second pump cell is to pump O2, which originates from the decomposition of a trace amount of NOx gas. The concentration of NOx gas to be pumped corresponds to several microamperes with respect to the second pump current. Therefore, even if the pumping power of the second pump cell is low, it is sufficient to decompose the trace amount of NOx gas by the time the NOx concentration is measured.

[0007] Meanwhile, when the NOx sensor is heated to activate the solid electrolytes of the sensor element so that they can transport oxygen, a high concentration of O2 present in the second measuring chamber must be forcibly pumped out. In this respect, the pumping capacity of the second pump cell becomes insufficient. Consequently, a problem arises, as the so-called start-up time increases—that is, the duration from the start of the sensor's activation until the O2 concentration in the second measuring chamber (the second pump current) is reduced to a predetermined value by pumping. Summary of the invention

[0008] Accordingly, one object of the present invention is to provide a gas sensor that can shorten the start-up time by improving the pumping performance of the second pump cell, and a method for manufacturing the gas sensor.

[0009] According to a possible non-inventive embodiment, a gas sensor can be provided comprising a gas sensor element extending in a longitudinal direction, wherein the gas sensor element comprises: a first measuring chamber placed between two solid electrolyte layers stacked with a gap between them, into which a gas to be measured is introduced from outside the sensor; a first pump cell with a first inner pump electrode facing the first measuring chamber and a first counterpart electrode for the first inner pump electrode, wherein the first pump cell is designed to control the oxygen partial pressure in the first measuring chamber; a second measuring chamber in reciprocal communication with the first measuring chamber, which is separated from the environment and into which a gas to be measured with a controlled oxygen partial pressure is introduced from the first measuring chamber;and a second pump cell with a second inner pump electrode arranged in the second measuring chamber, and a second counterpart electrode for the second inner pump electrode, wherein the second pump cell is designed to detect a specific gas component in the gas to be measured in the second measuring chamber, wherein the second inner pump electrode consists of a material comprising as its main component two types of Pt particles having different particle sizes and whose particle size ratio, measured by sedimentation particle size distribution, ranges from 1.75 to 14.2, and has a mixing ratio of large Pt particles to small Pt particles with a mass ratio of 10 / 90 to 50 / 50 (large Pt particles / small Pt particles); and has a 10 kHz–1 Hz resistance value across the second pump cell at 600°C of 150 Ω or less.

[0010] In such a configuration, the large Pt particles contained in the second inner pump electrode can prevent fracture in the second inner pump electrode, which can otherwise occur due to the growth and coagulation of the small Pt particles. Furthermore, the small Pt particles form a coarsely structured electrode over the surface of the solid electrolyte layer, thereby improving the triple-layer interface ratio and electrode activity.

[0011] In a preferred embodiment of the foregoing non-inventive configuration, the second inner pump electrode has an average thickness of 15 µm or less, and the second inner pump electrode has a minimum thickness ranging from 4 µm to 11 µm.

[0012] According to a first embodiment, the problem according to the invention is solved by providing a gas sensor comprising a gas sensor element extending in a longitudinal direction, wherein the gas sensor element comprises: a first measuring chamber placed between two solid electrolyte layers stacked with a gap between them, into which a gas to be measured is introduced from outside the sensor; a first pump cell with a first inner pump electrode facing the first measuring chamber and a first counterpart electrode for the first inner pump electrode, wherein the first inner pump electrode is configured to control the oxygen partial pressure in the first measuring chamber; a second measuring chamber in reciprocal communication with the first measuring chamber, which is separated from the environment and into which a gas to be measured with a controlled oxygen partial pressure is introduced from the first measuring chamber;and a second pump cell with a second inner pump electrode arranged in the second measuring chamber, and a second counterpart electrode for the second inner pump electrode, wherein the second pump cell is designed to detect a specific gas component in the gas to be measured in the second measuring chamber, wherein the second inner pump electrode consists of an aggregate containing Pt as its main component, which consists of several Pt particles comprising larger Pt particles and smaller Pt particles; wherein, in a cross-sectional plane of the gas sensor element along its stacking direction, when viewing a reflection electron image comprising an interface between the second inner pump electrode and a solid electrolyte layer in contact with the second inner pump electrode, a surface of the Pt particle comprising the outermost surface of the second inner pump electrode is defined on the reflection electron image as the surface to be measured;wherein the maximum and minimum heights between the surface to be measured of individual PT particles and the interface are determined from a direct distance perpendicular to the interface; and wherein the relationships T1-T2≥5 and T2 / T1≤0.75 are satisfied, where T1 (µm) is an average of the three largest values ​​of the maximum heights, arranged in descending order from the largest value, and T2 (µm) is an average of the three smallest values ​​of the minimum heights, arranged in ascending order from the smallest value.

[0013] In such a configuration, the larger Pt particles contained in the second inner pump electrode can prevent fracture in the second inner pump electrode, which can otherwise occur due to the growth and coagulation of the smaller Pt particles. Furthermore, the smaller Pt particles form a coarsely structured electrode over the surface of the solid electrolyte layer, thereby improving the triple-layer interface ratio and electrode activity. If either T1-T2 < 5 or T2 / T1 > 0.75 occurs, the surface areas of the respective exposed Pt particles decrease, thus reducing the triple-layer interface ratio.

[0014] The expression “an interface between the second inner pump electrode and a solid electrolyte layer in contact with the second inner pump electrode” means a straight line connecting the Pt particle closest to the solid electrolyte layer and the Pt particle second closest to the solid electrolyte layer from among the Pt particles contained in the second inner pump electrode on the reflection electron image.

[0015] In a preferred embodiment of the foregoing first configuration, the second inner pump electrode contains 10 to 23 wt.% zirconium oxide.

[0016] According to a second embodiment, the present invention provides a method for manufacturing a gas sensor comprising a gas sensor element according to the preceding first embodiment, wherein the method comprises: applying a paste to an electrolyte layer of the gas sensor element, the paste containing as its main component two types of Pt particles having different particle sizes and whose particle size ratio, measured by sedimentation particle size distribution, ranges from 1.75 to 14.2, and wherein the paste has a mixing ratio of large Pt particles to small Pt particles with a mass ratio of 50 / 50 to 10 / 90 (large Pt particles / small Pt particles), and sintering the paste to form the second inner pump electrode.

[0017] In a preferred embodiment of the aforementioned second configuration, the second inner pump electrode, based on a total mass of the two types of Pt particles, contains 10 to 28 mass percent zirconium oxide.

[0018] The present invention makes it possible to shorten the start-up time by improving the pumping performance of the second pump cell. Brief description of the drawings

[0019] Illustrative embodiments of the invention are described in more detail with reference to the following figures. These show: Fig. 1 a cross-sectional view of a NOx sensor of an embodiment according to the invention along its longitudinal direction; Fig. 2 a cross-sectional view of the NOx sensor element along its longitudinal direction; Fig. 3 a view showing a method for measuring a start-up time; Fig.4 a view showing a relationship between a 10kHz-1 Hz resistance value achieved across a second pump cell and the start-up time; Fig. 5 a view showing a relationship between a particle size ratio of Pt particles used in a second inner pump electrode and the start-up time; Fig. 6 a view showing a relationship between a particle size ratio of Pt particles used in the second inner pump electrode and the 10kHz-1Hz resistance value achieved across the second pump cell; Fig. 7. A clear illustration of how to calculate T1 and T2 from a reflection electron image; Fig. 8 a reflection electron image of a sample of the tenth embodiment of the invention; and Fig. 9 a reflection electron image of a sample from the sixth comparison example. Detailed description of preferred embodiments

[0020] Next, an embodiment of the invention will be described with reference to the drawings. However, the present invention should not be limited to this embodiment.

[0021] Fig.Figure 1 is a cross-sectional view of a gas sensor (NOx sensor) 200 of an embodiment according to the invention along its longitudinal direction. The NOx sensor 200 comprises: a cylindrical metal casing 138 with an outer surface on which a thread 139 is formed for attachment to an exhaust pipe; an NOx sensor element (a gas sensor element) 10, which takes the form of a plate extending in an axial direction (the longitudinal direction of the NOx sensor 200: the vertical direction in the drawing); a cylindrical ceramic shell 106, which is arranged so that it surrounds a radial circumference of the NOx sensor element 10; an insulating contact element 166, which is arranged such that an inner wall surface, which defines an axially extending contact insertion hole 168, surrounds a circumference of a rear end of the NOx sensor element; and six terminals 110, which are located between the NOx sensor element 10 and the insulating contact element 166 (two of which are in Fig.1 are shown) are set.

[0022] The metal sheath 138 is formed into a substantially cylindrical shape with an axially extending through-bore 154 and a shoulder 152 that projects inwards with respect to a radial direction of the through-bore 154. The metal sheath 138 also accommodates the NOx sensor element 10 in the through-bore 154. A front end of the NOx sensor element 10 projects from a front end of the through-bore 154, while electrode terminals 220 and 221 are located outside the rear end of the through-bore 154. Furthermore, the shoulder 152 has an inwardly directed tapered surface that is inclined with respect to a plane perpendicular to the axial direction.

[0023] An annular ceramic holder 151, layers of pressed powder 153 and 156 (hereinafter also referred to as talc rings 153 and 156), and the protruding ceramic shell 106 are stacked in this order from the front end to the rear end of the through-hole 154 of the metal jacket 138 to surround the radial circumference of the NOx sensor element 10. A crimp packing 157 is placed between the ceramic shell 106 and a rear end 140 of the metal jacket 138. A metal holder 158, which holds the talc ring 153 and the ceramic holder 151 and maintains hermeticity, is placed between the ceramic holder 151 and the shoulder 152 of the metal jacket 138. The rear end 140 of the metal jacket 138 is crimped to press the ceramic shell 106 toward the front end by means of the crimp packing 157.

[0024] However, as in Fig.Figure 1 shows a double guard covering a prominent part of the NOx sensor element 10, which has several holes, is made of metal (e.g., stainless steel or the like), and consists of an outer guard 142 and an inner guard 143, on an outer circumference of the front end (in Fig. 1 a lower side) of the metal casing 138 attached by welding and the like.

[0025] An outer casing 144 is attached to an outer circumference of the rear end of the metal sheath 138. A grommet 150 with conductor wire entry holes 161, into which six conductor wires 146 (in Fig. (1 only five of them are shown) are inserted to be electrically connected to the electrode terminals 220 and 221 of the NOx sensor element 10, and is placed in an opening at the rear end of the outer housing 144 (in Fig. 1 (an upper position).

[0026] An insulating contact element 166 is located at a rear end (one in Fig. The insulating contact element 166 is positioned (as shown in the upper part of Figure 1) of the NOx sensor element 10, which projects from the rear end 140 of the metal casing 138. The insulating contact element 166 is arranged around the electrode terminals 220 and 221, which are formed on the surface of the rear end of the NOx sensor element 10. The insulating contact element 166 is cylindrical with an axially extending contact insertion hole 168. The insulating contact element 166 has a flange 167 that projects radially outward from an outer surface. The insulating contact element 166 is positioned within the outer casing 144 by means of a retaining element 169 via the flange 167.

[0027] Now, a structure of the NOx sensor element 10 is shown with reference to a cross-sectional view of Fig. 2 described along a longitudinal direction of the sensor element.

[0028] In Fig.2 The NOx sensor element 10 has a structure consisting of a first solid electrolyte layer 11a, an insulating layer 14a, a second solid electrolyte layer 12a, an insulating layer 14b, a third solid electrolyte layer 13a, and insulating layers 14c and 14d, all stacked in this order. The first measuring chamber 16 is formed between the first solid electrolyte layer 11a and the second solid electrolyte layer 12a, and a gas GM to be measured is introduced from outside by means of a first diffusion resistance element 15a, which is arranged at the left end (an inlet) of the first measuring chamber 16.

[0029] A second diffusion resistance element 15b is arranged at one end of the first measuring chamber 16 opposite the inlet. A second measuring chamber 18, which remains in reciprocal communication with the first measuring chamber 16, is formed on the right side of the first measuring chamber 16 by means of the second diffusion resistance element 15b. The second measuring chamber 18 is formed between the first solid electrolyte layer 11a and the third solid electrolyte layer 13a by penetrating the second solid electrolyte layer 12a.

[0030] A heating element 50 in the form of an elongated plate, extending along one longitudinal direction of the NOx sensor element 10 (a direction in which the solid electrolyte layers 11a to 13a are stacked), is embedded between the insulating layers 14c and 14d. The heating element 50 is used to raise the temperature of the gas sensor to an active temperature and to improve the conductivity of oxygen ions in the solid electrolyte layers. In this way, the operation of the sensor element is stabilized.

[0031] The insulating layers 14a to 14d consist primarily of aluminum oxide, and the first diffusion resistance element 15a and the second diffusion resistance element 15b consist of a porous substance, for example, aluminum oxide. Furthermore, the heating element 50 consists of platinum and the like.

[0032] The first pump cell 11 has the first solid electrolyte layer 11a, which consists mainly of zirconium oxide exhibiting oxygen conductivity, and a first inner pump electrode 11c and a first counterpart electrode (a first outer pump electrode) 11b, which pairs with the first inner pump electrode 11c, the first solid electrolyte layer 11a being sandwiched between the first inner pump electrode 11c and the first counterpart electrode 11a. The first inner pump electrode 11c faces the first measuring chamber 16. Both the first inner pump electrode 11c and the first outer pump electrode 11b consist mainly of platinum, and the surfaces of the respective electrodes are coated with protective layers 11e and 11d, which consist of a porous substance.

[0033] An oxygen concentration detection cell 12 comprises a second solid electrolyte layer 12a, consisting primarily of zirconium oxide, and a detection electrode 12b and a reference electrode 12d, arranged such that the second solid electrolyte layer 12a is sandwiched between them. The detection electrode 12b is located downstream of the first inner pump electrode 11c and faces the first measuring chamber 16.

[0034] Both the detection electrode 12b and the reference electrode 12c consist primarily of platinum.

[0035] The insulating layer 14b is notched such that the reference electrode 12c, which contacts the second solid electrolyte layer 12a, is embedded in the insulating layer 14b, and the cutout is filled with a porous substance to create a reference oxygen chamber 17. During operation, an extremely small electric current of a predetermined value is first introduced into the oxygen concentration detection cell 12, thereby supplying oxygen from the first measuring chamber 16 to the reference oxygen chamber 17 and establishing an oxygen reference concentration.

[0036] The second pump cell 13 has a third solid electrolyte layer 13a, consisting primarily of zirconium oxide, and a second inner pump electrode 13b, as well as a second counterpart electrode (a second counterpart pump electrode 13c) paired with the second inner pump electrode 13b, which are arranged on regions of the surface of the third solid electrolyte layer 13a facing the second measuring chamber 18. Both the second inner pump electrode 13b and the second counterpart pump electrode 13c consist primarily of platinum.

[0037] The second counterpart pump electrode 13c is arranged in the cutout of the insulating layer 14b, which is located above the third solid electrolyte layer 13a; it is opposite the reference electrode 12c and faces the reference oxygen chamber 17.

[0038] An exemplary operation of the NOx sensor element 10 is now described. When power is initially supplied from an external power supply by starting the engine, the heating element 50 operates via a predetermined control circuit, thereby heating the first pump cell 11, the oxygen concentration detection cell 12, and the second pump cell 13 to an activation temperature. Once the respective cells 11 to 13 have reached the activation temperature, the first pump cell 11 pumps excess oxygen from the first inner pump electrode 11c to the first counterpart electrode 11b in the gas GM (an exhaust gas) to be measured, which has been introduced into the first measuring chamber 16.

[0039] At this point, the oxygen concentration in the first measuring chamber 16 corresponds to an electrical voltage Vs (a voltage from terminal to terminal) across the electrodes of the oxygen concentration detection cell 12. Therefore, a voltage from electrode to electrode (a voltage from terminal to terminal) Vp1 of the first pump cell 11 is controlled such that the voltage from electrode to electrode Vs reaches a constant voltage V1 (e.g. 425 mV), thereby adjusting the oxygen concentration in the first measuring chamber 16 to such an extent that NOx is not decomposed.

[0040] The gas GN to be measured, with an adjusted oxygen concentration, flows towards the second measuring chamber 18. A predetermined electrical voltage Vp2 (a voltage higher than a control voltage for the oxygen concentration detection cell 12, for example, 450 mV), at which NOx gas in the gas GN to be measured decomposes into oxygen and N2 gas, is applied as an electrode-to-electrode voltage (a terminal-to-terminal voltage) Vp2 to the second pumping cell 13, whereupon NOx decomposes into nitrogen and oxygen. A second pumping current Ip2 flows through the second pumping cell 13 such that the oxygen resulting from the decomposition of NOx is pumped out of the second measuring chamber 18. Since there is a linear relationship between the second pumping current Ip2 and the NOx concentration at this point in time, the NOx concentration in the gas to be measured can be detected by detecting Ip2.

[0041] The second inner pump electrode 13b is now described. The second inner pump electrode 13b consists primarily of two types of Pt particles of different sizes, with a particle size ratio, measured with respect to a sedimentation particle size distribution, ranging from 1.75 to 14.2. Furthermore, the mixing ratio between large and small Pt particles, with respect to mass, ranges from 10 / 90 to 50 / 50 (large Pt particles / small Pt particles). The second inner pump electrode 13b is manufactured by applying a mixture of these Pt particles in paste form, together with a binder, a component of the solid electrolyte layer, a solvent, and the like, and sintering the mixture at a temperature of approximately 800°C or higher. However, the manufacturing process is not limited to the above.

[0042] If the second inner pump electrode 13b consists of a mixture of such Pt particles, the resistance value of the second pump cell 13, ranging from 10 kHz to 1 Hz, becomes 150 Ω or less, thus reducing the start-up time. This is because the small Pt particles form a coarsely structured electrode over the surface of the solid electrolyte layer, thereby improving the triple-layer interface ratio and increasing the electrode activity. Furthermore, the mixing of large Pt particles prevents fracture in the second inner pump electrode 13b, which would otherwise be due to the growth and coagulation of the small Pt particles.

[0043] The particle size ratio between the two types of Pt particles with different particle sizes of this invention ranges from 1.75 to 14.2. If the particle size ratio is below 1.75, the start-up time is not reduced. One possible reason for this is that, due to the small difference in particle size between the two types of Pt particles, the larger Pt particles cannot inhibit the growth of the smaller Pt particles, which in turn causes a fracture in the second inner pump electrode 13b. Conversely, even if the particle size ratio exceeds 14.2, the start-up time is not reduced. One possible reason for this is that, due to the large difference in particle size between the two types of Pt particles, the growth and coagulation of the smaller Pt particles are accelerated, which in turn makes the electrode prone to fracture.

[0044] The particle size measured with respect to a sedimentation particle size distribution represents an average particle size determined by utilizing a phenomenon where the observed sedimentation rate depends on particle size as fine particles settle in a stationary fluid. The sedimentation particle size distribution can be measured using, for example, a centrifugal sedimentation particle size distribution measuring device (SA-CP3) manufactured by Shimadzu Corporation.

[0045] The mixing ratio of Pt particles contained in the second inner pump electrode 13b ranges from 10 / 90 to 50 / 50 (large Pt particles / small Pt particles) with respect to mass ratio. If the mass ratio is below 10 / 90, the large Pt particles become less numerous, and the growth and coagulation of the small Pt particles can lead to a fracture in the second inner pump electrode 13b. Conversely, if the mass ratio exceeds 50 / 50, the small Pt particles become more numerous. This makes it difficult to form a coarsely structured electrode above the surface of the solid electrolyte layer, which in turn does not improve the triple-layer interface ratio or the electrode activity.

[0046] The Pt particles grow from a powder after the formation of the second inner pump electrode 13b. Even when considering the electrode, it is difficult to detect a difference in particle size among the Pt particles. However, if the second inner pump electrode consists of the aforementioned Pt particles, the sensor element exhibits a resistance value of 150 Ω or less across the second pump cell 13 at 600°C in the 10 kHz to 1 Hz range.

[0047] The present inventors have experimentally determined that the response time is reduced by half or more than that of a prior art NOx sensor by setting the 10 kHz–1 Hz resistance value across the second pump cell 13 to 150 Ω or less. The 10 kHz–1 Hz resistance value is obtained by measuring an AC impedance between a pair of electrodes of the second pump cell 13 at a single frequency ranging from 0 to 100 kHz and by plotting a measurement result using a Cole-Cole diagram (representing a measurement result on a complex impedance plane).

[0048] The start-up time is the period from which the sensor's start-up control begins, until the O2 concentration in the second measuring chamber (the second pump flow) is reduced to a predetermined value by means of pumping. Several methods are available for measuring the start-up time. For example, a Fig.The procedure shown in section 3 is described. First, a gas sensor is placed in the atmosphere at room temperature, and the change in the sensor output value with respect to the second pump current, Ip2, is measured over time since the heating element was switched on. An Ip2 value reached after 30 minutes following the heating element switch-on is considered the saturated value, Is, and a time tL at which Ip2 reaches a value of Is ± 10 ppm is considered the start-up time. Ip2 typically reaches a large value at the time the heating element is switched on. A time at which Ip2 reaches a value 10 ppm greater than Is is used as tL.

[0049] A region of the second inner pump electrode 13b, which is exposed in the second measuring chamber and acts as an electrode, consists of the aforementioned Pt particles. It is preferred to use an ordinary Pt material for the other conduction part.

[0050] If the second inner pump electrode 13b, based on a total mass of Pt particles of two types, contains 10 to 28 wt% zirconium oxide, electrode adhesion to the solid electrolyte is preferentially improved. Zirconium oxide is the main component of the solid electrolyte layer. If the zirconium oxide content is below 10 wt%, the improvement in electrolyte adhesion is small, and the triple-layer interface ratio decreases. If the zirconium oxide content exceeds 28 wt%, electrode adhesion increases. However, electrode fracture may occur, and the triple-layer interface ratio decreases.

[0051] Furthermore, the second inner pump electrode 13b is preferably doped with one or more of Rh, Pd, Ru and Ir as a component to improve the activity of the electrode.

[0052] The mean thickness of the second inner pump electrode 13b is preferably 15 µm or less, and its minimum thickness is preferably 11 µm or less. This is because, in a situation where a triple-layer interface is generated, oxygen can migrate to the solid electrode layer immediately after decomposition at the electrode, since the second inner pump electrode 13b is thinner, thus improving the pumping efficiency. A preferred minimum thickness of the second inner pump electrode 13b is 4 µm or more. This allows sufficient oxygen to be pumped out of the second measuring chamber 18 without causing the second inner pump electrode 13b to break.

[0053] When measuring the mean thickness and minimum thickness of the second inner pump electrode, a surface roughness measuring instrument specified in JIS B0651 (2007 version) (a 3.2-inch contact surface roughness measuring instrument) is used to measure along, for example, a longitudinal direction of Fig. 2 to carry out a sweeping operation from the third solid electrolyte layer 13a (exposed on the left side) beyond the second inner pump electrode 13b in order to reach the third solid electrolyte layer 13a (exposed on the right side) by crossing the second inner pump electrode 13b, thereby determining the shape of the inner second pump electrode.

[0054] The mean thickness of the second inner pump electrode can be determined by Rz(total) - Rc(one electrode). Rz(total) denotes the maximum height achieved over the entire swept area, and Rc(one electrode) denotes a mean height achieved within the area over which the second inner pump electrode 13b is swept. The minimum thickness of the second inner pump electrode can be determined by Rz(total) to Rz(one electrode). Rz(one electrode) denotes the maximum height achieved in the area over which the second inner pump electrode 13b is swept.

[0055] Of the Pt particles forming the second inner pump electrode 13b, the outermost surface of the second inner pump electrode 13b is defined as the area to be measured. The areas to be measured of the respective Pt particles, as well as the maximum and minimum heights located at an interface between the second inner pump electrode 13b and the third solid electrolyte layer 13a, are determined with reference to a direct distance N obtained in a direction perpendicular to the interface. If an average of three of the three largest values ​​of the maximum heights thus determined is taken as T1 (µm), and if an average of the three minimum values ​​of the minimum heights is taken as T2 (µm), it is preferred to achieve a relationship of T1-T2 ≥ 5 and T2 / T1 ≤ 0.75.By adopting such a configuration, large Pt particles from the Pt particles contained in the second inner pump electrode 13b prevent electrode fracture, which can otherwise occur due to growth and coagulation of the small Pt particles. Furthermore, the small Pt particles form a coarsely structured electrode over the surface of the third solid electrolyte layer 13a, thereby improving the triple-layer interface ratio and electrode activity.

[0056] T1 and T2 can be specified by viewing from the section planes obtained by cutting the gas sensor element 10 in a stacking direction, a reflection electron microscopy (SEM) image that includes the second inner pump electrode 13b and the interface L between the second inner pump electrode 13b and the third solid electrolyte layer 13a.

[0057] Specifically, the interface L is first defined in the reflection electron picture, as shown in Fig. Figure 7 shows the interface L being specified as a straight line connecting the Pt particle (K1) closest to the third solid electrolyte layer 13a with the Pt particle (K2) second closest to the third solid electrolyte layer 13a from the Pt particles in the second inner pump electrode 13b.

[0058] The outermost surfaces of the Pt particles forming the second inner pump electrode 13b are defined as the areas M to be measured. The maximum and minimum heights reached between the area M to be measured of each Pt particle and the interface L are determined with reference to a direct distance achieved in a direction perpendicular to the interface L. Fig.Figure 7 shows only the maximum heights D1, D2, D3 and D4 as well as the minimum heights E1, E2, E3 and E4; however, other maximum heights and minimum heights can also be determined.

[0059] An average of three values ​​(D2, D3 and D4 in Fig. 7), which are in descending order from the highest value of the maximum heights, is taken as T1. An average of three values ​​(E1, E2 and E3 in Fig. 7), which are in ascending order from the smallest value of the minimum heights, are taken as T2.

[0060] T1 and T2 are measured by examining a cross-sectional plane encompassing the interface between the second inner pump electrode 13b and the third solid electrolyte layer 13a, and cut along the stacking direction of the gas sensor, using the reflected electron image from a scanning electron microscope (SEM). The required measurement range for the reflected electron image is a magnification of 1000x or higher. The reflected electron image can typically be viewed in a field of view of approximately 70 × 50 µm.

[0061] Furthermore, the reason for obtaining a relationship of T1-T2≥5 (µm) is that when the difference between T1 and T2 reaches an absolute value of 5 µm or more, the large Pt particles are closer to the surface of the second inner pump electrode 13b than the small Pt particles, and irregularities of the outermost surface become larger.

[0062] Furthermore, if T2 / T1≤0.75 is reached, T1 far exceeds a quarter of the length of T2, and the irregularities of the outermost surface of the second inner pump electrode 13b become large.

[0063] It is considered that the larger irregularities show the extent to which the large Pt particles are strongly distributed outside the second inner pump electrode 13b, and that, furthermore, the small Pt particles are correspondingly strongly distributed over the surface of the third solid electrolyte layer 13a.

[0064] Normally, in the gas sensor, the pumping power of the second pump cell 13 is low, and the electric current flowing through the first pump cell 11 is 20 times or more greater than the electric current flowing through the second pump cell 13.

[0065] If the lower limit of the oxygen concentration in the first measuring chamber 16 is 1%, the minimum value of the first pump current Ip1 is 0.125 mA (= 125 µA). If the upper limit of the NOx concentration in the second measuring chamber 18 is 2000 ppm, the second pump current Ip2 at this time is on the order of 6 µA.

[0066] If, as in Fig. Figure 2 shows that if the second inner pump electrode 13b and the second counterpart pump electrode 13c of the second pump cell 13 are located on the same surface side of the third solid electrolyte layer 13a (i.e., in the drawing, a top surface), the cell resistance is higher than it is when the inner pump electrode 13b and the second counterpart electrode 13c are opposite each other, which reduces the pumping performance. Thus, the present invention is effective.

[0067] The present invention is specifically described with reference to the following examples. Of course, the present invention is not limited to these examples.

[0068] The one in connection with the in Fig. 1 and Fig. The NOx sensor described in the embodiment shown in Figure 2 was manufactured according to a prior art method. The second inner pump electrode 13a was formed by applying one of the Pt pastes described below over the third solid electrolyte layer 13a by means of screen printing, thus stacking the paste layer over another layer, and sintering the structure (e.g. for one hour at 1,500°C).

[0069] Pt pastes were produced by mixing a Pt powder (containing large Pt particles) with a mean particle size of 7.9 µm with a Pt powder (containing small Pt particles) with a mean particle size of 4.5 µm at the ratios shown in Table 1. Zirconium oxide and an organic binder were also added to all the Pt powders at the ratios shown in Table 1, and a solvent and a plasticizer were added to the mixtures as needed to produce the Pt pastes.

[0070] The impedance between the second inner pump electrode 13b and the second counterpart pump electrode 13c in the second pump cell 13 of the NOx sensor thus obtained was measured using an impedance analyzer (model 1260, manufactured by Solartron Co., Ltd.). The sensor was controlled to a temperature of 600°C by means of the heating element at the time of measurement. An applied electrical voltage was set to an alternating voltage (AC) of 200 mV, and a sweep was performed at a measurement frequency domain of 10 kΩ to 1 Hz.

[0071] As with reference to Fig.As described in section 3 regarding the start-up time, the gas sensor was placed in a normal temperature atmosphere, and hourly changes in the sensor output value, specifically the second pump current Ip2, were measured starting from the activation of the heating element. The current Ip2 reached after 30 minutes following the activation of the heating element is considered the saturated value Is, and a time tL at which Ip2 reaches a value of Is ≤ 10 ppm was taken as the start-up time. The heating element was controlled so that the sensor temperature reached 680°C. Table 1 Paste component used to manufacture the second inner pump electrode Thickness of the second inner pump electrode assessment Large Pt particles (wt%) (average particle size 7.9 µm) Pt particles with small particle sizes (wt%) (average particle size 4.5 µm) Zirconium oxide (wt% based on total amount of Pt) Organic binder (wt% based on total amount of Pt) Minimum thickness (µm) Average thickness (µm) 10kHz to -1Hz Resistance (Ω) Start-up time Adhere fracture Comparative example 1 0 100 10 14 3 11 158 45 - - Comparative example 2 0 100 28 14 3 12 170 48 - - Comparative example 3 0 100 28 5 2 11 210 51 - - First example of the invention 10 90 7 14 5 12 35 37 △ ◯ Second example of the invention 50 50 7 14 11 15 145 39 △ ◯ Third example of the invention 10 90 10 14 5 12 8 37 ◯ ◯ Fourth example of the invention 10 90 28 14 4 11 20 38 ◯ ◯ Fifth example of the invention 10 90 28 5 7 12 24 37 ◯ ◯ Sixth example of the invention 26 74 10 14 9 12 50 36 ◯ ◯ Seventh example of the invention 26 74 28 14 11 13 80 39 ◯ ◯ Eighth example of the invention 26 74 28 5 9 13 84 38 ◯ ◯ Ninth example of the invention 50 50 10 14 11 15 115 37 ◯ ◯ Tenth example of the invention 50 50 14 10 11 15 120 38 ◯ ◯ Eleventh example of the invention 50 50 28 14 11 14 132 39 ◯ ◯ Twelfth example of the invention 50 50 28 5 10 15 150 38 ◯ ◯ Thirteenth example of the invention 50 50 32 14 11 15 145 39 ◯ △ Fourteenth example of the invention 10 90 32 14 4 11 37 37 ◯ △ Comparative example 4 74 26 10 14 12 15 230 60 - - Comparative example 5 74 26 28 14 13 16 250 63 - - Comparative example 6 74 26 22 7 12 15 330 81 - - Comparative example 7 74 26 28 5 11 17 360 88 - - Comparative example 8 100 0 10 14 13 18 480 125 - - Comparative example 9 100 0 28 14 14 19 500 140 - - Comparative example 10 100 0 28 5 12 18 650 220 - -

[0072] The results obtained in this way are shown in Table 1 and Fig.4 shown. In the first to fourteenth examples of the invention, where the mass ratio falls in a range of 10 / 90 to 50 / 50 (large Pt particles / small Pt particles), the start-up time was in all cases 40 seconds or less, and the 10kHz-1hZ resistance value achieved across the second pump cell was 150 Ω or less.

[0073] In contrast, in the first three comparison examples, where only small Pt particles were used, and in the fourth through tenth comparison examples, where the proportion of large Pt particles exceeded 50 percent by mass, the start-up time was over 40 seconds. The resistance value across the second pump cell at 10 kHz–1 Hz exceeded 150 Ω this time.

[0074] Thus, according to the invention, the mixing ratio between the Pt particles is set to 10 / 90 to 50 / 50, and the 10 kHz–1 Hz resistance value achieved across the second pump cell is set to 150 Ω or less. In the first example, the particle size ratio between the Pt particles was 1.75.

[0075] In a reflection electron microscopy (SEM) image considered in conjunction with the tenth example of the invention (see Fig. 8), T1-T2=8.9 and T2 / T1=0.586 were obtained. In contrast, a reflection electron micrograph (SEM), which was used in conjunction with the sixth comparative example (see Fig. 9) was obtained, T1-T2=2.4 and T2 / T1=0.879 were obtained.

[0076] The adhesion and breakage of the second inner pump electrode were assessed as follows in connection with the first to fourteenth examples of the invention.

[0077] Electrode adhesion was assessed in accordance with JIS H8504 (2007 version). First, a 10 mm² strip of adhesive tape, which was not to be affixed, was applied to a possible flat surface of the second inner pump electrode 13b. The tape was continuously pressed firmly with a finger for approximately 10 seconds, taking care to prevent the formation of bubbles. Next, a portion of the tape that remained untacked was pulled firmly so that it became perpendicular to the electrode surface. The tape was then temporarily removed, and the adhesion of the surface was visually assessed. If adhesion of the electrode material to the surface cannot be visually determined, the adhesion is determined to be excellent (O). If adhesion of the electrode material can be visually determined, the adhesion is determined to be somewhat deficient (Δ).Even if the assessment reveals that the electrode is somewhat (Δ) defective, this does not pose a practical problem.

[0078] At room temperature, a four-terminal tester is used to determine whether or not a fracture is present in an electrode. If one or more (10% or more) out of ten sensor samples are fractured, the electrode(s) are determined to have a fracture (Δ). Even if the assessment reveals that the electrode is slightly (Δ) defective, this does not pose a practical problem.

[0079] In the first and second examples of the invention, the proportion of zirconium oxide based on the total Pt content in the second inner pump electrode 13b was less than 10% by mass, and the electrode adhesion was worse than in the other examples of the invention. In the thirteenth and fourteenth examples of the invention, however, the proportion of zirconium oxide based on the total Pt content in the second inner pump electrode 13b exceeded 28% by mass, and the electrode fractured. Example 2

[0080] NOx sensors were produced using methods characteristic of Example 1. The second inner pump electrode 13b was produced by applying the respective Pt pastes shown in Table 2 over the third solid electrolyte layer 13a by screen printing, thus stacking the electrolyte layer over another layer, and by sintering the structure (e.g. for one hour at 1,500°C).

[0081] In example 2, Pt particles were mixed at a constant mass ratio of 50 / 50 (large Pt particles A / small Pt particles B). Table 2 To make the second inner pump. electrode paste component used assessment Pt particles A with a large particle size (average particle size, µm) Pt particles B with a small particle size (average particle size, µm) Particle size ratio (Pt particles AlPt particles B) Zirconium oxide (wt% based on the total amount of Pt) Organic binder (wt% based on the total amount of Pt) 10kHz to 1 Hz resistance (Ω) Start-up time Comparative example 11 12,8 0,6 21,30 28% 5% 235 62 Twenty-first example of the invention 12,8 0,9 14,20 28% 5% 145 38 Twenty-second example of the invention 7,9 0, 8,78 28% 5% 125 37 Twenty-third example of the invention 12,8 4,5 2,84 28% 5% 130 39 Twenty-fourth example of the invention 7,9 4,5 1,75 28% 5% 150 38 Comparative example 12 7,9 7,9 1,00 28% 5% 265 68

[0082] The results obtained in this way are shown in Table 2, Fig. 5 and Fig. Figure 6 shows that in the twenty-first to twenty-fourth examples of the invention, where the particle size ratio of the Pt particles ranged from 1.75 to 14.2, the start-up time was 40 seconds or less in all cases. The 10 kHz to 1 Hz resistance value achieved across the second pump cell was this time 150 Ω or less.

[0083] In contrast, in the eleventh comparison example, where the particle size ratio of the Pt particles exceeded 14.2, and in the twelfth comparison example, where the particle size ratio of the Pt particles was below 1.75, the start-up time was over 40 seconds in both cases. The 10 kHz to 1 Hz resistance value across the second pump cell exceeded 150 Ω this time.

[0084] Based on the foregoing, according to the invention a particle size ratio for the Pt particles is set to 1.75 to 14.2 and the 10kHz-1 Hz resistance value achieved over the second pump cell is set to 150 Ω or less.

[0085] The present invention is not limited to the foregoing embodiment and naturally includes various modifications and equivalents that fall within the nature and scope of the appended claims. For example, the planar shape of the heating element is not limited to the one mentioned above.

[0086] In this embodiment, the solid electrolyte layer forming the NOx sensor element is configured as a triple layer; however, the solid electrolyte layer can also be embodied as a double layer. The structure of an NOx sensor element with a double solid electrolyte layer is described, for example, in JP 2004 - 354 400 A ( Fig. 3) described.

[0087] The present invention can be applied to a gas sensor for detecting the concentration of NOx gas in the exhaust gas of a motor vehicle or of various engines, or the concentration of NOx gas in the combustion gas of a steam boiler or the like, as well as to an oxygen sensor, for example, a broadband fuel / air ratio sensor. However, the present invention is not limited to these applications. For example, the present invention can also be applied to a gas sensor with a gas sensor element for measuring the concentration of a gas other than NOx gas (e.g., COx, H2O, HC, and the like).

[0088] According to a first illustrative embodiment of the exemplary design, the second inner pump electrode consists of a material which contains as its main component two types of Pt particles, which have different particle sizes and whose particle size ratio, measured by a sedimentation particle size distribution, ranges from 1.75 to 14.2, and which has a mixing ratio of large Pt particles to small Pt particles, which assumes a mass ratio of 10 / 90 to 50 / 60 (large Pt particles / small Pt particles); and a resistance value of 10 kHz to 1 Hz achieved across the second pump cell is 150 Ω or less at 600°C.

[0089] In this configuration, the large Pt particles contained in the second inner pump electrode prevent electrode fracture, which could otherwise occur due to the growth and coagulation of the smaller Pt particles. Furthermore, the small Pt particles form a coarsely structured electrode over the surface of the solid electrolyte layer, thereby improving the triple-layer interface ratio and electrode activity. Consequently, a resistance value of 150 Ω or less is achieved across the second pump cell at 10 kHz to 1 Hz, and the response time is reduced compared to that achieved by a state-of-the-art NOx sensor.

[0090] According to another illustrative embodiment of the exemplary design, the mean thickness of the second inner pump electrode is 15 µm or less, and its minimum thickness ranges from 4 µm to 11 µm.

[0091] In such a configuration, oxygen can migrate to the solid electrolyte layer immediately after decomposition at the electrode, provided the second inner pump electrode is thin and no electrode fracture occurs in the situation where a triple-layer interface is created. This improves pumping efficiency.

[0092] According to yet another illustrative embodiment of the exemplary design, the second inner pump electrode consists of an aggregate containing Pt as its main component, comprising several Pt particles including larger and smaller Pt particles, in a cross-sectional plane of the gas sensor element along its stacking direction, when a reflection electron image is considered that includes an interface between the second inner pump electrode and a solid electrolyte layer in contact with the second inner pump electrode, a surface of the Pt particle forming the outermost surface of the second inner pump electrode is defined on the reflection electron image as the area to be measured, the maximum and minimum heights between the surface to be measured of individual Pt particles and the interface are determined from a direct distance perpendicular to the interface, and the relationships T1-T2≥5 and T2 / T1≤0.75 are satisfied.where T1 (µm) is an average of the three largest values ​​of the maximum heights, arranged in descending order from the largest value, and T1 (µm) is an average of the three smallest values ​​of the minimum heights, arranged in ascending order from the smallest value.

[0093] In this configuration, the large Pt particles contained in the second inner pump electrode prevent electrode fracture, which can otherwise occur due to the growth and coagulation of the small Pt particles. Furthermore, the small Pt particles form a coarsely structured electrode over the surface of the solid electrolyte layer, thereby improving the triple-layer interface ratio and electrode activity. If either T1-T2 < 5 or T2 / T1 > 0.75, the surface areas of the exposed Pt particles decrease, thus reducing the triple-layer interface ratio.

[0094] According to yet another illustrative embodiment of the exemplary design, the second inner pump electrode contains 10 to 28 wt.% zirconium oxide.

[0095] In such a configuration, the zirconium oxide, which is the main component of the solid electrolyte layer, simultaneously provides an improved triple-layer interface ratio at the electrode and improved electrode adhesion. Preferably, zirconium oxide partially stabilized by yttrium oxide or the like is used. As a result of using such partially stabilized zirconium oxide, it becomes less likely that zirconium oxide will become embedded in a space within the electrode. The triple-layer interface thus exposed in this space can function adequately, thereby improving electrode activity. The use of zirconium oxide with a particle size ranging from 0.2 to 2 µm is also preferred. This makes it less likely that zirconium oxide will become embedded in a space within the electrode, and the triple-layer interface exposed in this space can function adequately, thereby improving electrode activity.

[0096] In a further illustrative embodiment of the exemplary design, the second inner pump electrode is manufactured by: applying a paste to an electrolyte layer, the paste containing as its main component two types of Pt particles having different particle sizes and whose particle size ratio, measured by a sedimentation particle size distribution, ranges from 1.75 to 14.2, and wherein the paste has a mixing ratio of large Pt particles to small Pt particles, which assumes a mass ratio of 50 / 50 to 10 / 90 (large Pt particles / small Pt particles), and by sintering the paste.

[0097] The second inner pump electrode preferably contains 10 to 28 mass percent zirconium oxide based on the total mass of the two types of Pt particles.

[0098] In such a configuration, zirconium oxide, which is the main component of the solid electrolyte layer, simultaneously promotes an improved triple-layer interface ratio in the electrode and improved electrode adhesion.

[0099] This application is based on Japanese patent applications No. 2008-124263, filed on May 12, 2008, and No. 2009-071806 (JP 2009 - 300 428 A), filed on March 24, 2009, the disclosures of which are incorporated herein by reference in their entirety.

Claims

[1] A gas sensor having a gas sensor element extending in a longitudinal direction thereof, the gas sensor element comprising: a first measuring chamber which is placed between two solid electrolyte layers stacked with a gap therebetween and into which a gas to be measured is introduced from outside the gas sensor; a first pumping cell having a first inner pumping electrode facing the first measuring chamber and a first counterpart electrode for the first inner pumping electrode, wherein the first inner pumping electrode is configured to control oxygen partial pressure in the first measuring chamber; a second measuring chamber in mutual communication with the first measuring chamber, which is separated from the environment and into which the gas to be measured is introduced with the controlled oxygen partial pressure from the first measuring chamber; and a second pump cell having a second inner pump electrode arranged in the second measuring chamber and a second counterpart electrode for the second inner pump electrode, wherein the second pump cell is designed to detect a specific gas component in the gas to be measured in the second measuring chamber, characterized by , that the second inner pumping electrode consists of an aggregate containing Pt as its main component, which consists of several Pt particles, in a sectional plane of the gas sensor element along its stacking direction when viewing a reflection electron image comprising an interface between the second inner pumping electrode and a solid electrolyte layer in contact with the second inner pumping electrode, a surface of the Pt particles forming the outermost surface of the second inner pumping electrode is defined as the surface to be measured, maximum heights and minimum heights between the surface to be measured of individual Pt particles and the interface are determined from a direct distance perpendicular to the interface, and the relationships T1-T2 ≥ 5 µm and T2 / T1≤0.75 are satisfied, where T1 (µm) is an average of the three largest values ​​of the maximum heights arranged in descending order from the largest value, and T2 (µm) is an average of the three smallest values ​​of the minimum heights arranged in ascending order from the smallest value. [2] Gas sensor according to claim 1, characterized by that the second inner pumping electrode (13b) contains 10 to 28 weight percent zirconium oxide. [3] A method of manufacturing a gas sensor comprising a gas sensor element extending in a longitudinal direction thereof, the gas sensor element comprising: a first measuring chamber which is placed between two solid electrolyte layers stacked with a gap therebetween and into which a gas to be measured is introduced from outside the sensor, a first pumping cell having a first inner pumping electrode facing the first measuring chamber and a first counterpart electrode for the first inner pumping electrode, wherein the first inner pumping electrode is configured to control oxygen partial pressure in the first measuring chamber; a second measuring chamber in mutual communication with the first measuring chamber, which is separated from the environment and into which a gas to be measured with a controlled oxygen partial pressure is introduced from the first measuring chamber; and a second pump cell having a second inner pump electrode arranged in the second measuring chamber and a second counterpart electrode for the second inner pump electrode, wherein the second pump cell is designed to detect a specific gas component in the gas to be measured in the second measuring chamber, the method comprising: applying to a solid electrolyte layer of the gas sensor element a paste containing, as a main component, two kinds of Pt particles having different particle sizes, the particle size ratio of which ranges from 1.75 to 14.2 as measured by sedimentation particle size distribution, and wherein the paste has a mixing ratio of large Pt particles to small Pt particles adopting a mass ratio of 50 / 50 to 10 / 90 (large Pt particles / small Pt particles), and sintering the paste to thereby form the second inner pumping electrode. [4] A method for manufacturing a gas sensor according to claim 3, characterized by that the second inner pumping electrode contains 10 to 28 mass percent of zirconium oxide based on a total mass of the two types of Pt particles.

Citation Information

Patent Citations

  • Flux-film forming apparatus

    JP2008124263A

  • Mobile communication terminal unit

    JP2009071806A

  • Gas sensor and method of manufacturing the same

    JP2009300428A

  • Nitrogen oxides detection device comprises an oxygen pump cell for removing oxygen from measuring gas, and a detection cell for measuring nitrogen oxides contained in the measuring gas from which oxygen is removed

    DE10109676A1

  • Sensor for determining nitrogen oxides in vehicle exhaust gas

    DE19854889A1