Methods for producing toner products and toner product

A method using a thermoplastic polymer matrix in clay products addresses the energy and time inefficiencies of traditional firing by achieving comparable strength and stability at lower temperatures, reducing costs and logistics.

DE102013111775B4Active Publication Date: 2024-11-14WESTERWALDER BLUMENTOPFFAB SPANG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE102013111775
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2013-10-25
Publication Date
2024-11-14
Estimated Expiration
2033-10-25

AI Technical Summary

Technical Problem

Existing methods for producing clay products, such as vessels, are energy-intensive and time-consuming due to high-temperature firing processes, and alternative plastic products lack mechanical stability and durability.

Method used

A method involving a raw clay mass mixed with a thermoplastic polymer matrix former, shaped into a blank, pre-dried, and coated with a polymer powder, which crosslinks at moderate temperatures below the firing temperature, eliminating the need for ceramic firing.

Benefits of technology

This method achieves dimensional stability and mechanical strength comparable to conventionally fired clay products while reducing energy and time consumption, lowering production costs and eliminating the need for a kiln system.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Method for the manufacture of a clay product, in particular a container or plant pot, comprising the steps of: - Preparation of a mass comprising a raw clay mass, wherein the raw clay mass predominantly comprises unfired clay, and a matrix former, wherein the matrix former is formed from a thermoplastic polymer, wherein the mass ratio of the raw clay mass to the matrix former is between 20:1 and 1:1, - Shaping the mass into a blank, in particular a vessel blank, - Pre-drying the blank at a drying temperature below 100 °C to reduce the water content, - Heating the blank to a process temperature, - Application of a coating by powder coating, in particular by means of a polymer powder, to the heated blank and - Melting of the coating at the process temperature, while simultaneously drying the blank and crosslinking the matrix former at process temperatures below the firing temperature of the raw clay mass.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for producing a clay product, in particular a container or plant pot, and to a clay product, in particular a container, produced by means of the method.

[0002] Clay products, especially containers or plant pots, are known in a wide variety of designs from the prior art and are used in numerous fields of application, for example for the cultivation and storage of plants both in nurseries and by end consumers.

[0003] Although products, especially vessels of the type mentioned above, are generally known and available made from a wide variety of materials, consumers primarily prefer and use vessels made of clay.

[0004] To produce such a product from clay, it is known from the prior art to first form the clay, optionally mixed with additives, into a vessel blank and then to fire it at temperatures of at least 1000 °C for a longer period of time, whereby the vessel blank achieves its final dimensional strength and stability through this ceramic firing.

[0005] Publication GB 544 913 A discloses a hardened but unfired ceramic molded body consisting of a larger proportion of ceramic material containing plastic clay and a smaller proportion of a resin.

[0006] Publication GB 2 139 209 A discloses numerous low-temperature sintered porcelain compositions containing a binder, a thermoplastic resin, additives and, to a large extent, a mixture of a glassy component, aluminum oxide and a clay component (10 - 25 wt% of the mixture).

[0007] The publication DE 38 73 336 T2 refers to ceramic compositions containing light-curing resins as binders for use in dentistry, explicitly intending to fire the ceramic compositions at high temperatures.

[0008] This method, known from the prior art, has numerous disadvantages. Firstly, the firing process is very energy-intensive, and secondly, ceramic firing requires a long firing time followed by a corresponding cooling period, making the production process costly due to both energy consumption and duration.

[0009] Alternatively, it is also known from the prior art to manufacture products, in particular containers, entirely from plastic. However, such containers exhibit significantly lower mechanical stability and a shorter lifespan, especially due to weathering and damage from UV radiation. Furthermore, containers, especially plastic plant pots, and particularly those manufactured in one piece using injection molding, are generally less valued by consumers.

[0010] The invention is therefore based on the objective of providing a method for producing a clay product, in particular a container or plant pot, which can be carried out cost-effectively with low energy and time expenditure and with which clay products can be produced that are comparable to conventionally fired clay products with regard to their mechanical strength and appearance.

[0011] The invention solves the problem by a method for producing a clay product according to claim 1 and with a clay product, in particular a vessel according to claim 16. Advantageous embodiments of the invention are specified in the dependent claims.

[0012] In the inventive process for producing a clay product, in particular a container or plant pot, the first process step involves preparing a mass comprising a raw clay mass, wherein the raw clay mass predominantly comprises unfired clay, and a matrix former, wherein the matrix former is formed from a thermoplastic polymer, wherein the mass ratio of the raw clay mass to the matrix former is between 20:1 and 1:1; shaping the mass into a blank, in particular a container blank; pre-drying the blank at a drying temperature below 100 °C to reduce the water content; heating the blank to a process temperature; and applying a coating by powder coating, in particular by means of a polymer powder.on the heated blank and melting of the coating at the process temperature, as well as simultaneous drying of the blank and crosslinking of the matrix former at process temperatures below a firing temperature of the raw clay mass.

[0013] The manufacturing process for the clay product, and in particular the vessel, according to the invention offers an advantage over prior art methods in that achieving the final dimensional stability of the formed blank made from a clay-containing mass, especially a raw clay mass, no longer requires time-consuming and energy-intensive ceramic firing. Instead, the blank only needs to be heated to a moderate drying temperature at which the matrix former cross-links and thereby imparts the necessary stability to the clay product. The strength of the clay product, and in particular the vessel, dried according to the process is comparable to that achieved by firing a white or colored body at 1000 °C.Furthermore, the inventive method enables further time and cost savings by eliminating the necessary furnace for firing, reduced personnel requirements due to the elimination of the firing process, and simplified logistics during the production of the clay product.

[0014] Furthermore, the invention relates to a clay product, in particular a vessel according to claim 13, which was produced by the method according to claim 1 and / or implements at least one feature of claims 2-12.

[0015] The clay product can be, for example, any decorative or ornamental item such as a statue, frame, picture, bust, or similar object. Alternatively, the clay product can be any type of vessel or building material, such as tiles or slabs.

[0016] The term "vessel" as used in claims 1 and 16 is to be understood comprehensively and includes all products in and on which solid, liquid, or loose objects or masses can be received. In particular, a vessel is understood to be any container suitable for receiving a plant. This can be, on the one hand, a planting container, especially a flowerpot, into which a plant is placed directly. On the other hand, it can also be a cachepot, which serves to hold a planting pot and has the function of preventing water from leaking onto a surface located below the vessel. Furthermore, any three-dimensionally extended container open on at least one side for storing a plant, for example, bowls, plates, and other containers open on multiple sides, are included in the term "vessel."

[0017] The term "plant" is also to be interpreted broadly and includes not only all living plants, especially flowers, shrubs and trees, but also artificially produced plants and similar items, especially for decorative purposes, made from any material, for example plastic, textile and / or wood.

[0018] The processing step is understood to mean any process in which at least two initially separate substances are at least partially mixed and / or comminuted, wherein, in particular, during mixing, one of the substances is at least partially distributed within the other. Preferably, the processing comprises mixing until one substance is substantially homogeneously distributed within another, especially matrix-forming particles within the raw clay mass. Furthermore, the processing or mixing of more than two components is also possible, whereby not all substances necessarily have to be homogeneously mixed into one another, but only one of the substances is distributed within another substance. Preferably, all substances are substantially homogeneously distributed within the resulting mixture after processing.

[0019] The mass is essentially the product of the mixing process. Mass is understood to mean any mixture of substances that can be brought into a different spatial shape by means of at least one forming or shaping process, preferably by pressing or alternatively by casting. Particularly preferably, the mass is a plastically deformable mass that substantially retains its shape after the forming process, especially after shaping by pressing. Furthermore, the plastically deformable mass preferably exhibits highly plastic and only slightly elastic behavior, particularly with regard to elongation and flow.

[0020] In principle, the preparation of the mass can not only directly precede the subsequent process steps, but can also take place at a different production location and essentially independently of the further process in terms of timing. In particular, it is possible to purchase a pre-mixed, preferably plastically formable mass and process it further according to the inventive method.

[0021] The raw clay mass can initially be any substance or mixture of substances comprising a predominant proportion, i.e., more than 50%, preferably more than 75%, and particularly preferably more than 95%, of clay or a clay mixture. Besides naturally occurring clay, the raw clay mass can also be subsequently purified naturally occurring clay or an artificially produced material with clay-like properties. Furthermore, the raw clay mass contains a water content, which can vary considerably depending on the type of clay.

[0022] A matrix former is initially understood to be any substance capable of forming at least a two-dimensional, preferably three-dimensional, network, particularly through a physical transformation or a chemical reaction. This three-dimensional network can, for example, have a sponge-like structure whose pores are preferably filled substantially with raw clay. Preferably, the network-like structure of the matrix former completely permeates the vessel.

[0023] Preferably, the matrix former is a fusible substance that is finely dispersed, particularly as particles, in the plastically deformable mass. The individual particles melt at least partially upon temperature increase and may become fluid, allowing adjacent particles to bond together at their contact points. This process is particularly preferably carried out to such an extent that, after crosslinking of the matrix former, the blank exhibits a single, three-dimensional network structure of the matrix former, at least internally and preferably also on its surface. Furthermore, it is also possible that the substance used as the matrix former bonds with the surface of particles of the plastically deformable mass upon melting in such a way that these particles are spatially fixed relative to one another.

[0024] Furthermore, it is also fundamentally possible to form the clay product from several parts arranged next to each other, shaped separately by forming, in particular by pressing.

[0025] A blank is understood to be a preliminary stage of the finished clay product, particularly as a result of the shaping process, preferably of the forming press, wherein the final shape of the finished clay product, especially a vessel, is already substantially present. The blank preferably exhibits sufficient stability so that it can be transported automatically or manually to the next process step or stored in the interim.

[0026] Drying is generally understood to be any process in which the water content of the raw material is reduced. Preferably, drying is carried out using elevated temperatures and / or a gas stream directed at the raw material. It is also preferably carried out and continued over a prolonged period in such a way that the finished clay product has a lower water content than the raw material, and this is more uniform within the clay product, particularly within the vessel wall.

[0027] The process according to the invention is characterized, among other things, in that the temperature during the drying of the blank and the crosslinking of the matrix former is below the firing temperature of the raw clay. The firing temperature of the raw clay is understood to be the minimum temperature that must be reached to fire the respective raw clay, in particular to achieve sintering and / or ceramic bonding of the raw clay. The temperature required for this is typically in the range between 800 °C (bisque firing for earthenware) and 1300 °C (sinter firing for stoneware).

[0028] After an advantageous further development of the process, the mass is prepared in such a way that it is plastically deformable, and the shaping of the plastically deformable mass can be carried out by forming press.

[0029] Forming press is generally understood as a forming process in which pressure is applied to shape a plastically malleable mass into a blank. Preferably, the plastically malleable mass is placed in a press mold and pressed against it, for which a suitable press ram is particularly preferred. Alternatively, the forming can also be carried out by pressing between several press molds that result in the shape of the blank. Forming press is particularly preferably carried out using a commercially available pot press.

[0030] In a preferred further development of the process, a coating step of the blank is provided, wherein the coating preferably takes place in a single process step together with the drying of the blank. Such a coating enables a particularly simple modification of the properties of the vessel surface, such as its optical appearance, improved water resistance, or reduced susceptibility to dirt.

[0031] In a particularly preferred embodiment of the process, the drying and coating of the blank comprises the following steps: First, the blank is heated for pre-drying, preferably to a temperature below 100 °C, and most preferably to about 90 °C. This reduces the water content of the blank, which can be accompanied by a change in the blank's shape and / or size, known as drying shrinkage. Subsequently, the blank is heated to a drying or process temperature, preferably between 100 °C and 200 °C. A coating is then applied to the heated blank, after which the coating can be melted or dried, particularly at the drying or process temperature. This final process step can also include final drying of the blank.Applying a coating to the heated blank makes it particularly easy to apply and fix a coating at the same time, advantageously without requiring an additional process step.

[0032] In a particularly preferred embodiment of the inventive method, the coating is carried out by powder coating, in particular using a polymer powder, which enables a particularly cost-effective coating. The powder coating material is especially preferably selected such that it can bond with the matrix former during melting, thereby contributing to the stability of the clay product, particularly the vessel. Furthermore, the powder coating can also fulfill decorative functions, i.e., be designed in such a way as to create a desirable overall visual impression of the clay product, for example, with regard to its color and surface texture.

[0033] Furthermore, coating the clay product with clear and / or colored lacquer, particularly by spray application, or by impregnation with a silicone-based preservative is also conceivable. In particular, such coating of the clay product is carried out after the cross-linked blank or container has cooled to room temperature.

[0034] According to an advantageous further development of the inventive method, the temperature during the drying of the blank, in particular the maximum temperature reached during drying, is less than 400 °C, preferably less than 250 °C and is particularly preferably between 100 °C and 200 °C, which significantly reduces the energy expenditure of the drying and the crosslinking of the matrix former, especially compared to the firing processes for clay vessels known from the prior art, leading to significantly reduced manufacturing costs of the clay product.

[0035] Drying can be carried out not only at a constant temperature, but also by means of a temperature program designed over a period of time, in particular a temperature that increases over time.

[0036] According to an advantageous embodiment of the process, the drying temperature of the blank is above the melting and / or reaction temperature of the matrix former, thereby facilitating crosslinking of the matrix former during drying. This ensures that, at the latest after cooling and the associated hardening or solidification of the matrix former, the clay product reaches its final strength. Preferably, the drying temperature of the blank corresponds essentially to the melting and / or reaction temperature of the matrix former. This guarantees crosslinking of the matrix former, minimizes the energy consumption of the process, and also easily prevents potential thermal damage to the matrix former.

[0037] In principle, forming presses can be carried out in any manner. Preferably, for forming presses, the plastically deformable material is first placed into a rigid lower mold and subsequently pressed into a blank using an upper mold. Particularly preferably, the upper mold rotates relative to the lower mold, which allows for a particularly quick and reliable achievement of a consistent shape of the blank. Both the lower and upper molds can be formed as a single component, preferably made of metal, or as an assembly of several components.

[0038] The process according to the invention is characterized in that the raw clay mass consists predominantly of unfired clay, preferably predominantly of unfired ceramic clay, which is particularly cost-effective, especially compared to fired clay, and is particularly easy to process. In principle, the raw clay mass can also be a mixture of several unfired clays, especially ceramic clays.

[0039] According to a further preferred embodiment of the inventive method, the mass, in particular the plastically deformable mass, comprises 5–40%, preferably 10–25% water based on the total mass during preparation, thereby enabling plastic deformation in a particularly simple manner. The water can be partially or completely already contained in the raw clay mass, or it can be added completely or partially up to the desired water content.

[0040] According to a possible further development of the inventive method, the mass comprises 0.1 - 4%, preferably 0.5 - 2%, of at least one rheological auxiliary material, in particular a plasticizing agent, which allows the flow properties to be improved in a simple manner.

[0041] According to a preferred embodiment of the invention, the mass further comprises dyes, in particular color powders, colored clay flours and / or color oxides, whereby the vessel can be colored independently of a surface coating.

[0042] The matrix former is formed from a polymer, preferably a thermoplastic polymer or a polyester, phenolic, or epoxy resin, particularly a heat-curing resin. This allows for simple crosslinking of the matrix former at temperatures close to the drying temperature and results in a low product price for the clay product due to the low material costs. The matrix former can be a single polymer or a mixture of several polymers and / or other substances. Examples of suitable resins include polyester, epoxy, urea-formaldehyde, melamine, or phenolic resins, as well as polyurethane or thermoplastic polymers such as polyethylene, polypropylene, acrylonitrile butadiene styrene (ABS), or polyvinyl chloride (PVC).

[0043] According to a preferred embodiment of the inventive method, the matrix former is homogeneously mixed with the raw clay mass in the form of granules and / or powder, wherein the particle size of the granules is preferably less than 1 mm, particularly preferably less than 500 µm and most particularly preferably less than or equal to 63 µm, thereby achieving a uniform distribution of the matrix former in the mass in a simple manner.

[0044] According to the invention, the mass ratio of the raw clay mass to the matrix former is between 20:1 and 1:1. In a further preferred embodiment of the inventive method, the mass ratio of the raw clay mass to the matrix former is between 9:1 and 2:1, and preferably between 6:1 and 2:1. The high proportion of the particularly cost-effective raw clay mass thus advantageously enables particularly inexpensive production.

[0045] According to a preferred embodiment of the inventive method, drying is carried out until the residual moisture content of the clay product is less than 5%, preferably less than 2%, thereby achieving a particularly high strength of the clay product.

[0046] Preferably, the drying process is carried out in at least two steps. In a first step, drying is achieved by increasing the temperature and / or decreasing the humidity in the dryer, preferably continuing for a period of 4-10 hours, particularly until a residual moisture content of 1-2% is reached. In a second step, the drying and preferably also the crosslinking of the matrix former takes place, with the drying and / or crosslinking being carried out particularly preferably for a period of 20-40 minutes at temperatures up to 200 °C. Both drying steps can be carried out either consecutively and / or in one system or spatially and / or temporally separated from each other in two systems.

[0047] Several embodiments of the invention are explained in more detail below.

[0048] In a first embodiment of the inventive method for manufacturing a plant pot, 85 parts by mass of ready-mixed clay are first prepared with 15 parts by mass of transparent lacquer powder made from heat-curing polyester and epoxy resins. The ready-mixed clay is essentially a mixture of various natural clays. Furthermore, 20% water and 0.5% of the plasticizing agent "Zusoplast P98T" (based on the mass of the resulting mixture) are added and mixed until a homogeneous mixture is obtained.

[0049] Following the preparation, a defined quantity of the plastically malleable mass obtained in this way is placed in a pot press and pressed between a rigid metallic lower mold and a rigid metallic upper mold by bringing the lower mold and the upper mold together in relation to each other to form a vessel blank, which is stable after removal from the mold.

[0050] The container blank is then heated from room temperature to 90 °C for 6 hours to dry, reducing the residual moisture content to less than 2%. It is then heated further to approximately 200 °C for 30 minutes, resulting in final drying. Simultaneously, the lacquer powder contained in the malleable material melts and bonds to the container wall, forming a network-like structure.

[0051] A layer of powder coating is then applied to the container blank, which has been heated during drying. The coating is then briefly reheated to the drying temperature, fusing it to the surface of the container blank. After cooling and the resulting final hardening of the coating powder inside the container, the container reaches its final strength.

[0052] The powder coating applied to the outside of the vessel, which can have an identical composition to the powder coating incorporated into the malleable mass, contributes on the one hand to the final stability of the vessel and on the other hand ensures that the finished vessel is watertight.

[0053] In a second embodiment of the inventive method for manufacturing a flowerpot, Westerwald fat clay is first mixed with transparent lacquer powder in a mass ratio of 7:3, the Westerwald fat clay being characterized by a particularly high plasticity, which is advantageous for the subsequent shaping of the material. Furthermore, during the mixing process, 22% water and 0.8% of the plasticizing agent "Zusoplast P98T" are added, based on the mass of the mixture of clay and lacquer powder.

[0054] The plastically malleable mass thus obtained is then pressed using a pot press similar to the method described in the first embodiment, wherein, unlike the first embodiment, the upper form rotates relative to the lower form during pressing.

[0055] The blank container obtained by pressing is subsequently pre-dried for 8 hours at 90°C and then heated to approximately 200°C for 40 minutes, during which time the lacquer powder melts and forms a three-dimensional lacquer matrix that penetrates the container wall. The resulting container is already watertight and can therefore be used without any further surface coating. Furthermore, a container produced in this way is characterized by gas permeability of the wall, which advantageously ensures ventilation of the potting soil and plant roots within the container.

[0056] According to a third embodiment of the inventive method for producing a planter, 8 mass parts of ready-mixed clay are combined with 2 mass parts of polyethylene microgranules with a particle size of 500 µm or less. Furthermore, 20% water and 0.5% of the plasticizing agent "Zusoplast P98T" (based on the mass of the clay and polymer granule mixture) are added to the mixture to be blended, and all substances are mixed homogeneously.

[0057] The subsequent production of a vessel by pressing into a vessel blank, followed by drying the vessel blank and crosslinking the polyethylene microgranules, is carried out according to the corresponding process steps described in the first embodiment.

Claims

[1] A process for producing a clay product, in particular a container or planter for plants, comprising the steps: - preparing a mass comprising a raw clay mass, wherein the raw clay mass predominantly comprises unfired clay, and a matrix former, wherein the matrix former is formed from a thermoplastic polymer, wherein the mass ratio of the raw clay mass to the matrix former is between 20:1 and 1:1, - shaping the mass into a blank, in particular a vessel blank, - Pre-drying the blank at a drying temperature below 100 °C to reduce the water content, - Heating the blank to a process temperature, - application of a coating by powder coating, in particular by means of a polymer powder, to the heated blank and - Melting of the coating at the process temperature and simultaneous drying of the blank and cross-linking of the matrix former at process temperatures below the firing temperature of the raw clay mass. [2] Method according to claim 1, characterized by that the temperature during drying of the blank is lower than 400 °C. [3] Method according to one of the preceding claims, characterized by that the process temperature during drying of the blank is above a melting and / or reaction temperature of the matrix former or preferably corresponds to a melting and / or reaction temperature of the matrix former. [4] Method according to claim 1, characterized by that the mass obtained by processing is plastically formable and that the forming of the plastically formable mass is carried out by shaping pressing. [5] Method according to one of the preceding claims, characterized bythat for the forming pressing, the plastically formable mass is first introduced into a rigid lower mold and is then pressed into a blank by means of an upper mold, wherein the upper mold preferably rotates relative to the lower mold. [6] Method according to one of the preceding claims, characterized by that the process temperature is between 100 °C and 200 °C. [7] Method according to one of the preceding claims, characterized by that the mass, in particular the plastically formable mass, comprises 5 - 40%, preferably 10 - 25% water based on the total mass during processing. [8] Method according to one of the preceding claims, characterized by that the mass, in particular the plastically formable mass, comprises 0.1 - 4%, preferably 0.5 - 2% of a rheological auxiliary substance, in particular a plasticizer. [9] Method according to one of the preceding claims, characterized bythat the drying temperature is below 90 °C. [10] Method according to one of the preceding claims, characterized by that the matrix former is homogeneously mixed with the raw clay mass during processing as granules and / or powder, wherein the grain size of the granules is preferably less than 1 mm, particularly preferably less than 500 µm and most preferably less than 63 µm. [11] Method according to one of the preceding claims, characterized by that the mass ratio of the raw clay mass to the matrix former is between 9:1 and 2:1 and preferably between 6:1 and 2:

1. [12] Method according to one of the preceding claims, characterized by that the drying is carried out until the residual moisture content of the clay product is less than 5%, preferably less than 2%. [13] Clay product produced by the process according to claim 1, in particular plant pot, comprising - a raw clay mass and - a matrix former, characterized by , that - the raw clay mass is unfired and - the matrix former is cross-linked, having a network-like structure penetrating the clay product and a powder coating on the surface.

Citation Information

Patent Citations

  • CERAMIC COMPOSITIONS AND METHODS FOR THEIR APPLICATION.

    DE3873336T2

  • Low-temperature sintered porcelain composition

    GB2139209A

  • Ceramic bodies and a method of making the same

    GB544913A

  • CERAMIC COMPOSITIONS AND METHODS FOR THEIR APPLICATION.

    DE3873336D1