Manufacturing process for a positive electrode for a secondary battery with non-aqueous electrolyte
A controlled manufacturing method for positive electrodes in nonaqueous electrolyte secondary batteries addresses high viscosity and conductive path issues by optimizing moisture and binder ratios, resulting in electrodes with improved conductivity and durability.
Patent Information
- Application Number
- DE102015103343
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-04-18
- Filing Date
- 2015-03-06
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2035-03-06
AI Technical Summary
Increasing the solid content of the slurry for manufacturing positive electrodes in nonaqueous electrolyte secondary batteries leads to high viscosity, affecting handling and workability, and excessive dispersion of electrically conductive materials can sever conductive paths, reducing electrical conductivity and battery performance.
A manufacturing method involving controlled moisture and binder ratios in kneading steps, using N-methyl-2-pyrrolidone (NMP) with specific moisture and water content, to disperse electrically conductive carbon fine particles and form stable conductive paths, ensuring high productivity and reduced solvent use.
The method produces a positive electrode with superior electrical conductivity, reduced resistance, and enhanced durability, supporting stable battery characteristics over time.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a manufacturing method of a positive electrode for a non-aqueous electrolyte secondary battery. STATE OF THE ART
[0002] Since lithium-ion secondary batteries, among other non-aqueous electrolyte secondary batteries, are lighter in weight and have higher energy density than existing batteries, they are preferred as high-power output power sources for vehicle mounting and as so-called portable power sources and the like.
[0003] Generally, the electrodes of non-aqueous electrolyte secondary batteries are provided with a current collector and an active material layer formed on the current collector. Electrodes of this shape are obtained, for example, by preparing a slurry for forming the active material layer, which is obtained by dissolving or dispersing an active material, binder, and the like in a prescribed liquid medium (also including pastes and inks, and similarly applicable hereinafter), and coating the slurry on the surface of the current collector, followed by drying. Examples of prior patent literature relating to methods for producing an electrode include Patent Literatures 1 and 2. The abstract of Patent Literature 1, for example,describes the preparation of a slurry for forming a positive electrode active material layer by kneading a positive electrode active material, an electrically conductive material, and a polyvinylidene fluoride (PVdF)-based binder in a solvent (N-methyl-2-pyrrolidone), for which the moisture content was reduced to 100 ppm or less. Generic positive electrodes for secondary batteries are known to those skilled in the art from Patent Literatures 3 to 5. LIST OF CITED DOCUMENTSPatent literature [Patent Literature 1] Japanese Patent Application Publication No. JP 2012-186054 A [Patent Literature 2] Japanese Patent Application Publication No. JP 2010-157361 A [Patent Literature 3] Japanese Patent Application, Publication No. JP 2014-49390A [Patent Literature 4] US Patent Application Publication No. US 2010 / 0 248 027 A1 [Patent Literature 5] US Patent Application Publication No. US 2011 / 0 183 173 A1 SUMMARY OF THE INVENTION
[0004] However, in recent years, from the perspective of improving productivity and reducing costs, studies have been conducted to further increase the solid content of the slurry during positive electrode manufacturing. However, if the solid content of the slurry is increased, the slurry viscosity becomes excessively high, and handling and processability during coating may decrease. To address this, a technology exists that reduces the slurry viscosity by highly dispersing an electrically conductive material in the slurry by applying a large amount of energy to the slurry during kneading. However, if the electrically conductive material is excessively dispersed, the network structure of the electrically conductive material will be disrupted, and electrically conductive paths may be shortened.In such a case, the electrical conductivity in the positive electrode (and especially that in the positive electrode active material layer and between the positive electrode active material layer and the positive electrode current collector) decreases and the battery characteristics (and especially the power output characteristics) may decrease.
[0005] In view of the foregoing, an object of the present invention is to provide a method for producing a positive electrode for a nonaqueous electrolyte secondary battery with superior electrical conductivity, both stably and with high productivity. Furthermore, a nonaqueous electrolyte secondary battery provided with this positive electrode is disclosed.
[0006] The inventor of the present invention has conducted extensive studies from various perspectives to solve the above-mentioned problems. As a result, this has led to the completion of the present invention.
[0007] According to the present invention, a method for manufacturing a positive electrode for a non-aqueous electrolyte secondary battery is provided. This manufacturing method comprises the following steps: (1) a first kneading step of kneading electrically conductive carbon fine particles and a hydrophobic binder that gels when contacted with water in N-methyl-2-pyrrolidone (NMP); (2) a second kneading step of adding a positive electrode active material and water to a first kneaded product obtained in the first kneading step, followed by additional kneading; and (3) a step of forming a positive electrode active material layer on the surface of a positive electrode current collector by layering a second kneaded product obtained in the second kneading step on the positive electrode current collector. The first kneaded product includes moisture.In the first kneaded product, the ratio of the mass of moisture to the mass of NMP is 0.002 or less, while in the second kneaded product, water is added at a mass fraction of 0.0022 to 0.0115 based on the mass of NMP. The ratio of the mass of the hydrophobic binder to the mass of NMP in the first kneading step is 0.024 to 0.026; and polyvinylidene fluoride (PVdF) is used as the hydrophobic binder.
[0008] Aggregation of the electrically conductive fine carbon particles can be largely suppressed by ensuring that the moisture content of the first kneaded product is within the above-mentioned range. Furthermore, the hydrophobic binder can be appropriately gelled, and an aggregate comprising the electrically conductive fine carbon particles and the positive electrode active material can be formed by ensuring that the moisture content of the second kneading step is within the above-mentioned range. As a result, a network is formed between the electrically conductive fine carbon particles and the positive electrode active material, and electrically conductive paths can be efficiently formed.Furthermore, since the solid content can be adjusted to a high level during kneading, this manufacturing process simultaneously achieves cost reductions and a reduction in environmental pollution, due to a reduction in the amount of solvent used (NMP), as well as an improvement in productivity resulting from the shortening of the drying step. Consequently, according to the present invention, a positive electrode with superior electrical conductivity can be stably manufactured with high productivity.
[0009] In addition, the moisture content in a kneaded product can be measured using a moisture evaporation Karl Fischer titration method (heating temperature: 120°C, heating time: 30 minutes). Specifically, a measurement sample (first kneaded product) is heated in a dry nitrogen gas atmosphere to evaporate the moisture (water) contained in the measurement sample. The evaporated moisture is then quantified by a Karl Fischer titration (and typically a coulometric titration). As a result, the moisture content in the measurement sample can be determined.
[0010] As a result of limiting the mass ratio of the hydrophobic binder to the mass of NMP in the first kneading step to 0.024 to 0.026, even stronger electrically conductive paths can be formed in the positive electrode and even lower resistance can be achieved. Furthermore, an extremely durable positive electrode can be realized that is resistant to the occurrence of separation and elimination of the positive electrode active material layer.
[0011] Polyvinylidene fluoride (PVdF), which dissolves or disperses in a non-aqueous solvent (typically an organic solvent), is used as the hydrophobic binder. In addition, highly electrically conductive carbon black, such as acetylene black, can be preferentially used as the electrically conductive carbon fine particles.
[0012] A positive electrode obtained by the manufacturing process exhibits low resistance and superior electrical conductivity. Furthermore, it can exhibit high durability, resistant to the occurrence of separation and elimination of the positive electrode active material layer. For example, the 90° peel strength (based on JIS-K6854-1 (1999), similarly applicable hereinafter) of the positive electrode active material layer from the positive electrode current collector can be 3.5 N / m or more. Thus, in a nonaqueous electrolyte secondary battery provided with the positive electrode, superior battery properties (such as power output density or energy density) can be stably demonstrated over a long period of time. SHORT DESCRIPTION OF THE CHARACTERS Fig. 1 is a flowchart illustrating a method for manufacturing a positive electrode for a nonaqueous electrolyte secondary battery according to an embodiment. Fig. 2 is a longitudinal cross-sectional view schematically illustrating a non-aqueous electrolyte secondary battery. Fig. Figure 3 is a graph showing the relationship between a material mixing ratio and the peeling strength of a positive electrode active material layer. Fig. Figure 4 is a graph showing the relationship between a material mixing ratio and a battery resistance. DESCRIPTION OF THE EMBODIMENTS
[0013] The following provides an explanation of preferred embodiments of the present invention. In addition, matters other than those specifically mentioned in the present invention that are necessary to carry out the present invention (such as battery components (e.g., negative electrode and non-aqueous electrolyte) or conventional manufacturing methods not described in the present invention) can be understood by a person of ordinary skill in the art as design matters based on the prior art in the relevant art. The present invention can be carried out based on the contents disclosed in the present specification and on common technical knowledge in the relevant art. < <Herstellungsverfahren der Positivelektrode für die Sekundärbatterie mit nichtwässrigem Elektrolyt> >
[0014] As shown in the flowchart in Fig. 1, the manufacturing method of a positive electrode for a non-aqueous electrolyte secondary battery disclosed herein generally comprises the following three steps: (S10) a first kneading step for kneading electrically conductive carbon fine particles and a hydrophobic binder in N-methyl-2-pyrrolidone (NMP); (S20) a second kneading step of adding a positive electrode active material and a prescribed amount of water to a first kneaded product obtained in the first kneading step, followed by additional kneading; and (S30) a step of forming a positive electrode active material layer on the surface of a positive electrode current collector by layering a second kneaded product obtained in the second kneading step on the positive electrode current collector.
[0015] This process is characterized by the high degree of control over the moisture (water) content in each of the kneading steps (S10) and (S20). Thus, there are no particular restrictions on other conditions, and these can be appropriately determined according to different objectives and applications.
[0016] The following provides a sequential explanation of each step. <s 10: erster knetschritt>>
[0017] In the manufacturing process disclosed herein, electrically conductive carbon fine particles and a hydrophobic binder that gels when contacted with water are first kneaded in a liquid medium in the form of N-methyl-2-pyrrolidone (NMP). At least one of the electrically conductive carbon fine particles, the hydrophobic binder, and the NMP typically contains moisture. In this step, it is essential to regulate the ratio of the mass of moisture to the mass of NMP (moisture / NMP) to 0.002 or less.
[0018] Electrically conductive carbon fine particles exhibit strong cohesive force. Consequently, when a large amount of moisture is included in the present step, lumps are formed in the solvent (NMP) or a plurality of particles aggregate, easily resulting in the formation of aggregates ranging in size from several tens to several hundred micrometers. According to a study conducted by the present inventor, this results in inefficient electrically conductive paths being formed between the electrically conductive fine particles and the positive electrode active material in the second kneading step (S20) to be described below, resulting in a risk of increased resistance when assembling a battery.In the manufacturing process disclosed herein, this formation of aggregates is suppressed and the electrically conductive carbon fine particles are uniformly dispersed in NMP because the moisture content relative to the amount of NMP is maintained at 0.002 or less.
[0019] One type or two or more types of carbon materials conventionally used in non-aqueous electrolyte secondary batteries can be used as the electrically conductive carbon fine particles without limitation. Preferred examples thereof include various types of carbon black (such as acetylene black (AB), furnace black, Ketjen Black (KB), channel black, lamp black, or gap black), coke, activated charcoal, graphite powder, carbon fiber (such as PAN-based carbon fiber or pitch-based carbon fiber), and carbon nanotubes. Of these, carbon black, especially acetylene black, can be advantageously used.
[0020] Electrically conductive carbon fine particles that easily form a chain-like or group-like structure in which primary particles are connected to a certain extent are preferred as electrically conductive carbon fiber particles from the viewpoint of realizing advantageous electrical conductivity. This chain of primary particles is also called a structure. The degree of formation of this structure can be determined by measuring the particle size distribution (by dynamic light scattering) or examining it with an electron microscope (either a scanning or transmission type can be used). Electrically conductive fine particles that easily form a structure in which the primary particles are connected are capable of effectively forming advantageous electrically conductive paths between the positive electrode and the active material particles.As a result, superior electrical conductivity can be imparted to the positive electrode active material layer by using a smaller amount of electrically conductive carbon fine particles in the second kneading step (S20) to be described below. On the other hand, since fine particles with such a structure are easily caught or entangled in a solvent, this makes it difficult to disperse the particles both uniformly and evenly. From this point of view, the electrically conductive carbon fiber particles preferably have a primary structure diameter (also referred to as aggregate diameter) of approximately 0.01 μm to 3 μm, and more preferably 0.01 μm to 0.1 μm.
[0021] In addition, it is preferable that the specific surface areas of the electrically conductive carbon fiber particles are normally in the range of 1 to 1000 m 2 / g, e.g. 10 to 500 m 2 / g and typically 10 to 100 m 2 / g. Generally, the larger the specific surface area, the greater the increase in contact area with the positive electrode active material, and electrically conductive paths are more easily formed between the positive electrode active material particles. On the other hand, since fine particles with a large specific surface area are very bulky, they tend to cause a decrease in energy density. Both favorable electrical conductivity and high energy density can be realized to a large extent by ensuring that the specific surface area is within the above-mentioned ranges.
[0022] In addition, the specific surface area obtained by analyzing a value measured by the nitrogen adsorption method using the BET method (BET specific surface area) can be used as the specific surface area.
[0023] As described above, the density of the electrically conductive carbon fine particles is preferably relatively low from the viewpoint of high energy density and is typically in the range of 0.01 to 0.5 g / cm 3 and e.g. 0.01 to 0.3 g / cm 3 .
[0024] In addition, a measured value as defined in JIS K1469 (2003) can be used as the density.
[0025] In particular, electrically conductive carbon fine particles that satisfy one or two or more of the above-mentioned preferred properties, namely, degree of structural development, specific surface area, and bulk density, can be particularly preferably used. Examples of such electrically conductive carbon fine particles include carbon black such as acetylene black or Ketjenblack. Acetylene black, in particular, tends to easily form a structure in which primary particles are bonded. As a result, favorable electrical conductivity can be realized while using a comparatively small amount, making it preferable. Furthermore, since uniform dispersion in NMP is difficult, the application of the present invention can be said to be particularly effective.
[0026] The hydrophobic binder is a binder that gels when contacted with water, and one type or two or more types of substances conventionally used in non-aqueous electrolyte secondary batteries can be used without any particular restrictions. Typical examples include various types of polymer materials that dissolve or disperse in a non-aqueous solvent. Preferred examples include polyvinylidene fluoride (PVdF), polyvinylidene chloride (PVdC), and polyethylene oxide (PEO).
[0027] Furthermore, the concept of PVdF, as referred to herein, can include both homopolymers of vinylidene fluoride and copolymers of vinylidene fluoride and other monomers, denatured forms thereof, modified forms thereof, and the like. In the above-mentioned copolymers, monomers capable of copolymerizing with vinylidene fluoride can be one or more types selected, for example, from fluorine-based monomers such as vinyl fluoride, ethyl trifluoride, ethylene trifluorochloride, chlorotrifluoroethylene, ethylene tetrafluoride, or propylene hexyl fluoride, and non-fluorine-based monomers such as ethylene, methyl methacrylate, or acrylic acid. The copolymerization rate of vinylidene fluoride in the copolymer is preferably 50% by mass or more (and typically 70% by mass or more, and e.g., 85% by mass or more).Examples of the above-mentioned denatured forms include carboxylic acid denatured forms of homopolymers and copolymers of vinylidene fluoride.
[0028] Non-aqueous N-methyl-2-pyrrolidone (NMP) is used as the liquid medium (hydrophobic solvent). In the manufacturing process disclosed here, the amount of NMP used is reduced from the perspectives of cost reduction, which reduces environmental pollution and improves productivity. The amount of solvent used (NMP) is usually 800 to 1200 parts by mass, and preferably 900 to 1100 parts by mass, based on 100 parts by mass of electrically conductive carbon fine particles. As a result, the effect of strongly adsorbing the hydrophobic binder onto the surface of the electrically conductive carbon fine particles occurs. As a result, the adhesiveness and durability (mechanical strength) of the positive electrode can be improved.
[0029] The mass ratio of the hydrophobic binder to the electrically conductive carbon fine particles is typically 1:2 to 1:6, and preferably 1:3 to 1:5. As a result, a positive electrode capable of exhibiting both electrical conductivity and mechanical strength at a high level can be realized.
[0030] Furthermore, in a preferred aspect, the mass ratio of the amount of hydrophobic binder used to the amount of solvent (NMP) used is 0.24 to 0.26. If the amount of hydrophobic binder used is excessively small, the degree of gelation in the second kneading step (S20) to be described below will be low, and the effect of the present invention may be reduced. Furthermore, the integration of the positive electrode active material layer and the adhesion between the positive electrode active material layer and the positive electrode current collector may be reduced, and durability may decrease.On the other hand, if the amount of hydrophobic binder used is excessively large, the electrical conductivity of the positive electrode active material layer decreases because the proportion of the surface of the positive electrode active material covered by the hydrophobic binder becomes high, and this may lead to an increase in resistance. As a result of being within the above-mentioned range, the effects of the present invention can be exhibited more stably and at a higher level.
[0031] Furthermore, in the present step, various additives such as dispersants may be added in addition to the electrically conductive fine particles and the hydrophobic binder for the purpose of improving handling, dispersion stability, and the like. For example, polymeric compounds having a hydrophobic chain and a hydrophilic chain (generally alkali salts, typically sodium salts), anionic compounds having a sulfate, sulfonates, or phosphates, and cationic compounds such as amines can be used as dispersants. Preferred examples thereof include polymeric materials such as carboxymethyl cellulose. The addition of a dispersant makes it possible to more appropriately control the high dispersibility (the degree to which the primary particles are bonded) of the electrically conductive carbon fine particles.
[0032] Various conventionally known types of stirring and kneading devices, such as a ball mill, roller mill, mixer, disperser, or kneading device, can be suitably used for kneading. As a result of kneading, the hydrophobic binder can be strongly adsorbed onto the surface of the electrically conductive carbon fine particles. Furthermore, although electrically conductive carbon fine particles generally have the property of easily aggregating in solvents, as a result of kneading, secondary particles of the electrically conductive carbon fine particles are suitably broken up, which makes it possible to adjust the first kneaded product to a low viscosity. Furthermore, the electrically conductive carbon fine particles can be prevented from forming coarse aggregates. As a result, favorable layer-forming ability can be ensured.
[0033] The preferred kneading time during kneading is the time required for the electrically conductive carbon fine particles and the hydrophobic binder to be dispersed in NMP. Although it varies depending on the equipment, design, and kneading conditions, from the perspective of improving productivity, the kneading time is usually approximately 10 minutes to 3 hours, and preferably 10 minutes to 30 minutes.
[0034] Although there are no particular restrictions on the properties of the first kneaded product obtained in this way, the solid concentration (NV) is adjusted from the viewpoint of improving productivity and reducing costs, for example, to about 5 to 20%, typically 7% or more, and preferably 10% or more.
[0035] Furthermore, in the manufacturing process disclosed here, electrically conductive carbon fine particles are highly dispersed in NMP, for which the moisture content has been adjusted. As a result, the viscosity of the kneaded product can be kept at a low level. Furthermore, the viscosity of the first kneaded product is adjusted to approximately 100 to 300 mPa s.
[0036] In addition, a measured value (25°C) as defined by JIS K7117 (1999) using a B-type viscometer can be used as viscosity. <S20: Zweiter Knetschritt>
[0037] In the manufacturing process disclosed here, a positive electrode active material and water are next added to the first kneaded product, followed by additional kneading. In this step, it is essential that water be added at a mass fraction of 0.0022 to 0.0115 based on the mass of NMP.
[0038] In typical electrode manufacturing processes, gelation of a binder and uniformity of the kneaded product are achieved, for example, by reducing the moisture content of the solvent. However, in such cases, when the solid concentration of the first kneaded product is increased, the electrically conductive paths are shortened because the network of electrically conductive carbon fine particles remains disrupted due to the application of energy (shear stress). As a result, when the positive electrode active material layer is formed, the electronic conductivity in the positive electrode active material and / or between the positive electrode active material layer and the positive electrode current collector decreases, resulting in a risk of an increase in battery resistance.
[0039] Therefore, in the manufacturing method disclosed herein, it is intentionally arranged to cause the hydrophobic binder to swell by adding an amount of water sufficient to allow the hydrophobic binder to gel (namely, at a mass fraction of 0.0022 or more (2200 ppm or more) based on the mass of NMP). As a result, aggregates of, for example, several tens to several hundred micrometers can be formed, incorporating the electrically conductive carbon fine particles and the positive electrode active material. Namely, complexes of electrically conductive carbon fine particles and positive electrode active material can be formed while maintaining a slightly dispersed state of the electrically conductive carbon fine particles.As a result, the surface (periphery) of the positive electrode active material is uniformly covered by electrically conductive fine particles with a small particle diameter, and an electrically conductive network can be efficiently created between the electrically conductive carbon fine particles and the positive electrode active material. As a result, a positive electrode can be obtained in which the resistance is reduced compared to the case where no water is added in the current step.
[0040] On the other hand, if the amount of added water is excessive, the gelation of the binder will progress excessively and the aggregates will become excessively large, leading to the risk that the electrically conductive carbon fine particles will not be able to effectively cover the surface of the positive electrode active material. As a result, the electrical conductivity of the positive electrode decreases and the resistance increases, leading to the risk of a reduction in the effective areas of the positive electrode active material and a decrease in capacity. Accordingly, the proportion of added water is 0.0115 or less (11500 ppm or less) based on the mass of NMP.
[0041] Furthermore, if moisture is present in a conventionally prepared electrode, it can lead to a deterioration in resistance. However, the boiling point of the added water in the current step is approximately 100°C, which is significantly lower than the boiling point of NMP (approximately 202°C). As a result, the water is preferentially removed by the drying step following the step of forming the positive electrode active material layer (S30), which will be described below. As a result, the water does not cause this problem (deterioration in resistance).
[0042] As the positive electrode active material, one type or two or more types of different materials known to be used as positive electrode active materials of nonaqueous electrolyte secondary batteries can be used. Preferred examples thereof include layered or spinel-based lithium composite metal oxides such as LiNiO2, LiCoO2, LiMn2O4, LiFeO2, LiNi 0,5 Mn 1,5 O4, LiCrMnO4, or LiFePO4. Of these, lithium-nickel-cobalt-manganese composite oxides with a layered structure (and typically a layered rock salt structure) are preferred from the perspectives of improved thermal stability retention and high energy density.
[0043] Lithium composite metal oxides prepared by a conventionally known method can be used as the lithium composite metal oxide as they are. Although there are no particular restrictions on their properties, the average particle diameter (D 50 ) e.g., 1 to 25 µm and those with an average particle diameter of 2 to 10 µm can be preferably used. As a result, the electrically conductive fine particles can be preferentially arranged in the gaps between the positive electrode active material particles. As a result, the electrical conductivity in the positive electrode active material layer can be further improved.
[0044] In addition, a cumulative frequency of 50% by volume from the side of the fine particles with a small particle diameter in a volume-based particle size distribution based on a conventional laser light diffraction method (also called D 50 or median diameter) corresponding particle diameter can be used as the average particle diameter.
[0045] The mass ratio of positive electrode active material to electrically conductive carbon fine particles is usually approximately 1:0.07 to 1:0.11, and preferably approximately 1:0.08 to 1:0.10. As a result, a positive electrode capable of achieving both high electrical conductivity and energy density can be realized.
[0046] Alternatively, the mass ratio of positive electrode active material to hydrophobic binder is usually about 1:0.01 to 1:0.04, and preferably about 1:0.02 to 1:0.03. As a result, a positive electrode exhibiting superior mechanical strength can be realized.
[0047] In addition, various conventionally known stirring and kneading devices as described above can be suitably used as the kneading device. Furthermore, the kneading device may be the same as or different from that used in the first kneading step (S10).
[0048] A second kneaded product obtained in this way is adjusted to have properties suitable for the coating process described below. The addition of a suitable solvent can be used to achieve this goal. NMP or a non-aqueous solvent that can mix evenly with NMP can be used as the solvent.
[0049] For example, even if there are no particular restrictions on the properties of the second kneaded product, the solid concentration (NV) is approximately 40 to 80%, and is adjusted to 50% or more, and preferably 50 to 60%, from the viewpoint of improving productivity (such as shortening the drying time).
[0050] In addition, the viscosity of the second kneaded product is adjusted to approximately 1000 to 7000 mPa·s (e.g., 2000 to 4000 mPa·s). As a result of adjusting to such a viscosity, the stability (storability) of the kneaded product can be improved. As a result, even in the case of using a kneaded product for which a certain amount of time has elapsed since the time of production, coating streaks or uneven thicknesses, etc., can be prevented from occurring in the positive electrode active material layer forming step (S30) to be described later. Thus, a uniform positive electrode active material layer can be stably formed. <S30: Positivelektrodenaktivmaterialbildungsschritt>
[0051] Next, in the manufacturing method disclosed herein, the second kneaded product is coated on a positive electrode current collector to form a positive electrode active material layer on the surface of the positive electrode current collector. Since electrically conductive carbon fine particles are kept in a slightly dispersed state in the second kneaded product, few coarse aggregates are present, the coatability is favorable, and problems during coating are unlikely to occur. As a result, the positive electrode active material layer can be formed precisely.
[0052] An electrically conductive member made of a metal with favorable electrical conductivity (such as aluminum or nickel) can preferably be used as the positive electrode current collector. Furthermore, a conventionally known coating device such as a gap coater, a melt coater, a comma coater, a gravure coater, or a dip coater can be suitably used to coat the kneaded product.
[0053] Although there are no particular restrictions in this regard, the mass of the positive electrode active material layer stacked per unit area of the positive electrode current collector (mass on one side in a design with the positive electrode active material layer on both sides of the positive electrode current collector) is, for example, 3 mg / cm from the viewpoint of realizing a high energy density. 2 or more, e.g. 5 mg / cm 2 or more and typically 7 mg / cm 2 or more. From the perspective of realizing superior power output characteristics, the mass of the positive electrode active material layer per side of the positive electrode current collector is 100 mg / cm 2 or less, e.g. 70 mg / cm 2 or less and typically 50 mg / cm 2 or less.
[0054] In a typical aspect, moisture and solvent (NMP) included in the kneaded product are subsequently removed by drying the positive electrode active material layer with a suitable drying agent. Specifically, the water added in the second kneading step (S20) is first removed by drying, followed by the removal of NMP with a higher boiling point than water by drying. Air drying, blow drying, low-humidity drying, vacuum drying, or infrared drying, and the like, can be used alone or in a suitable combination when drying the positive electrode active material layer.
[0055] From the perspective of realizing high energy density, it is appropriate to ensure that the proportion of the positive electrode active material in the entire positive electrode active material layer is approximately 50% by mass or more (and typically 60 to 95% by mass), and this proportion is normally approximately 80 to 95% by mass. From the perspective of realizing both high power output characteristics and energy density at a high level, the proportion of electrically conductive carbon fine particles in the entire positive electrode active material layer may be, for example, 1 to 20% by mass, and is normally approximately 2 to 10% by mass. From the perspective of ensuring mechanical strength (shape retention), the proportion of hydrophobic binder in the entire positive electrode active material layer may be, for example, approximately 0.5 to 10% by mass, and is normally 1 to 5% by mass.
[0056] In addition, properties of the positive electrode active material layer, such as thickness or density, can be adjusted by performing an appropriate pressing treatment (using a method such as roll pressing or plate pressing) after drying. The average thickness per side of the positive electrode active material layer is, for example, 20 µm or more (and typically 40 µm or more) and 100 µm or less (and typically 80 µm or less). Furthermore, the density of the positive electrode active material layer is, for example, 1.0 g / cm 3 or more (and typically 2.0 g / cm 3 or more) and 4.5 g / cm 3 or less (and typically 4.0 g / cm 3 or less). As a result, high energy density, high power delivery density, and superior mechanical strength can be offered at an even higher level.
[0057] The positive electrode for a nonaqueous electrolyte secondary battery can be obtained in this way. This positive electrode exhibits both reduced internal resistance and superior durability (mechanical strength with respect to, for example, the integration of the positive electrode current collector and the positive electrode active material layer). For example, the peel strength of the positive electrode active material layer from the positive electrode current collector is preferably 3 N / m, and more preferably 3.5 N / m or more. Particularly in applications requiring strength, the peel strength is 3.7 N / m or more, and, for example, 3.8 N / m or more. <Sekundärbatterie mit nichtwässrigem Elektrolyt>
[0058] The positive electrode can preferably be used to manufacture a nonaqueous electrolyte secondary battery. A nonaqueous electrolyte secondary battery is provided, which is provided with the positive electrode, a negative electrode, and a nonaqueous electrolyte.
[0059] The negative electrode is typically provided with a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. An electrically conductive material made of a metal with favorable electrical conductivity (such as copper or nickel) is preferably used as the negative electrode current collector.
[0060] The negative electrode active material layer comprises at least one negative electrode active material. Carbon materials such as graphite, non-graphitizable carbon (hard carbon), or graphitizable carbon (soft carbon) are considered for use as the negative electrode active material, and a graphite-based carbon material (such as a carbon material in which graphite accounts for 50% or more by mass of the total mass of the negative electrode active material) is particularly preferred. Furthermore, the negative electrode active material layer may comprise one type or two or more types, as required, in addition to the negative electrode active material, which can be used as components of the negative electrode active material layer in conventional nonaqueous electrolyte secondary batteries. Examples of such materials include binders and various types of additives.Preferred examples of binders include styrene-butadiene rubber (SBR) and polytetrafluoroethylene (PTFE). Preferred examples of thickeners include cellulose-based materials such as carboxymethylcellulose (CMC).
[0061] The non-aqueous electrolyte is typically a liquid at normal temperature (e.g., 25°C) and is preferably always a liquid over the temperature range in which it is used (-30 to 60°C). A non-aqueous electrolyte comprising a conductive salt (such as a lithium salt in a lithium-ion secondary battery) in a non-aqueous solvent can preferably be used as the non-aqueous electrolyte.
[0062] A conductive salt similar to that used in a conventional non-aqueous electrolyte battery can be suitably selected and used as the conductive salt, as long as it contains a charge carrier (such as lithium ions, sodium ions, or magnesium ions, and in the case of a lithium-ion secondary battery, lithium ions). For example, if the charge carrier is lithium ions, examples of the conductive salt include lithium salts such as LiPF6 or LiBF4. The concentration of the conductive salt in the non-aqueous electrolyte is, for example, 0.7 to 1.3 mol / L. < <Eine Ausführungsform einer Sekundärbatterie mit nichtwässrigem Elektrolyt (nicht Teil der Erfindung)> >
[0063] Although not intended to be particularly restrictive, the Fig. 2 schematically illustrates a secondary battery (single cell) as an example to explain the approximate structure of a non-claimed embodiment. In the following drawings, the same reference numerals are used to denote components or locations that have the same function, and duplicate explanations are omitted or simplified. The dimensional relationships in each figure (such as length, width, and thickness) do not necessarily reflect actual dimensional relationships.
[0064] Fig. 2 is a longitudinal cross-sectional view schematically illustrating the cross-sectional structure of a nonaqueous electrolyte secondary battery 100. The nonaqueous electrolyte secondary battery 100 includes an electrode body (wound electrode body) 80 in which an elongated positive electrode sheet 10 and an elongated negative electrode sheet 20 are flatly wound with a separator sheet 40 interposed therebetween, and a nonaqueous electrolyte (not shown). The electrode body and the nonaqueous electrolyte are enclosed in a battery case 15 having a shape that allows the wound electrode body to be enclosed (flat box shape).
[0065] The battery case 50 is provided with a battery case body 52 in the shape of a flat rectangular parallelepiped (box-shaped) with the upper end thereof open, and a cover 54 covering the opening. The upper surface of the battery case 50 (namely, the cover 54) is provided with a positive electrode terminal 70 for external connection, which is electrically connected to the positive electrode of the wound electrode body 80, and a negative electrode terminal 72, which is electrically connected to the negative electrode of the wound electrode body 80. The cover 54 is also provided with a safety valve 55 for discharging gas generated in the battery case 50 from the battery case 50, in the same manner as a battery case of a conventional nonaqueous electrolyte secondary battery.
[0066] The flat wound electrode body 80 is enclosed in the battery case 50 together with a non-aqueous electrolyte (not shown). The wound electrode body 80 is provided with an elongated sheet-shaped positive electrode (positive electrode sheet) 10 and an elongated sheet-shaped negative electrode (negative electrode sheet) 20. The positive electrode sheet 10 is provided with an elongated positive electrode current collector and a positive electrode active material layer 14 formed along the longitudinal direction on at least one surface thereof (and typically on both sides). The negative electrode sheet 20 is provided with an elongated negative electrode current collector and a negative electrode active material layer 24 formed along the longitudinal direction on at least one surface thereof (and typically on both sides).Furthermore, two elongated sheet-shaped separators 40 are arranged between the positive electrode active material layer 14 and the negative electrode active material layer 24 in the form of insulating layers that prevent direct contact between the two. In addition to insulating the positive electrode and negative electrode, the separators 40 have the functions of retaining and sealing the non-aqueous electrolyte. Preferred examples thereof include porous resin sheets (films) formed from a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide.
[0067] The positive electrode active material layer 14 formed on a surface of the positive electrode current collector and the negative electrode active material layer 24 formed on a surface of the negative electrode current collector overlap at the center of the wound electrode body in the thickness direction defined as the end-to-end direction in the winding axial direction of the wound electrode body 80, resulting in the formation of a densely laminated wound core. Furthermore, a positive electrode active material non-formation region of the positive electrode sheet 10 and a negative electrode active material non-formation region of the negative electrode sheet 20 each protrude outward from the wound core at both ends in the winding axial direction of the wound electrode body 80.The positive electrode current collector is fixed to the protruding portion of the positive electrode side, while the negative electrode current collector is fixed to the protruding portion of the negative electrode side, and these are electrically connected to the positive electrode terminal 70 and the negative electrode terminal 72, respectively. <<Anwendung der Sekundärbatterie mit nichtwässrigem Elektrolyt> >
[0068] Although the non-aqueous electrolyte secondary battery disclosed herein can be used in various applications, it is characterized in that both high power output density and high durability can be realized at a higher level compared to the prior art due to the effects of reducing the resistance of the positive electrode and superior durability (mechanical strength). Thus, by utilizing these properties, the non-aqueous electrolyte secondary battery disclosed herein can be particularly preferably used in applications requiring both high power output density and high durability. Examples of such applications include drive power sources for driving a motor installed in a vehicle such as a plug-in hybrid vehicle (PHV), hybrid vehicle (HV), or electric vehicle (EV).Furthermore, this non-aqueous electrolyte secondary battery can typically be used by connecting a plurality of them in series and / or in parallel in the form of a battery pack. [Production of positive electrodes]
[0069] Here, after the Fig. 1, 25 types of positive electrodes (Examples 1 to 25) were prepared.
[0070] In the first kneading step (S10), electrically conductive fine particles in the form of acetylene black (AB, trade name: “HS-100 ® ", Denki Kagaku Kogyo Kabushiki Kaisha) and a binder in the form of polyvinylidene fluoride (PVdF, trade name Kureha KF Polymer ® #7300", Kureha Corp.) were gently mixed so that the mass ratio of these materials was roughly such that the ratio of PVdF to AB was 1:4. A solvent in the form of N-methylpyrrolidone (NMP) was then added thereto so that the mass ratio of PVdF to NMP was as shown in Table 1, followed by stirring and mixing for 30 minutes at a rotation speed of 3000 rpm using an ultra-high-speed multi-mixing system ("Robomix ® ", Primix Corp.) to obtain a first kneaded product. In addition, the solid content of the first kneaded product was roughly 10 to 20% by mass, and the viscosity (25°C) was roughly 100 to 300 mPa s. In addition, the moisture content of the first kneaded product, when measured by the Karl Fischer method (heating temperature: 120°C), was such that the mass fraction of moisture based on the amount of NMP was roughly 0.001 to 0.018, satisfying the relationship of (moisture / NMP) ≤ 0.0020 in all cases.
[0071] In the second kneading step (S20), a positive electrode active material in the form of LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (LNCM, average particle diameter: 6 µm, specific surface area: 0.7 m 2 / g) was added to the first kneaded product obtained as described above so that the ratio of LNCM to PVdF was 1:0.025. Next, an amount of water (ion-exchange water) was added so that the ratio of water to NMP was as shown in Table 1, followed by stirring and mixing for 30 minutes at a rotation speed of 3000 rpm to obtain a second kneaded product. Furthermore, the solid content of the second kneaded product was roughly 50 to 60% by mass, and the viscosity (25°C) was roughly 2000 to 4000 mPa s. [Table 1] Table 1 Material mixing ratios (mass ratios) Testbeispiele (S10) PVdF / NMP 0,020 0,024 0,025 0,026 0,030 (S20) Wasser / NMP 0,0020 Bsp. 1 Bsp.6 Bsp.11 Bsp.16 Bsp.21 0,0022 Bsp.2 Bsp.7 Bsp. 12 Bsp.17 Bsp.22 0,0069 Bsp.3 Bsp.8 Bsp. 13 Bsp.18 Bsp.23 0,0115 Bsp.4 Bsp.9 Bsp.14 Bsp.19 Bsp.24 0,0120 Bsp.5 Bsp.10 Bsp. 15 Bsp.20 Bsp.25
[0072] In the positive electrode active material formation step (S30), the second kneaded product obtained in the manner described above with a mass per unit area of 13.5 mg / cm 2 per side on a positive electrode current collector in the form of an aluminum foil, followed by drying (drying temperature: 80°C, drying time: 5 minutes) to form a positive electrode active material layer on the surface of one side of the aluminum foil. Furthermore, the average thickness of the positive electrode active material layer was roughly 50 µm.
[0073] As a result, positive electrodes (Examples 1 to 25) for a nonaqueous electrolyte secondary battery were prepared. [Measurement of peel strength]
[0074] The adhesion between the current collector and the active material layer of the positive electrodes prepared as described above was evaluated. Specifically, a 90° peel test, as defined in JIS-K6854-1 (1999), was performed on the positive electrodes. The results are shown in Table 2 and Fig. 3 shown. [Table 2] Table 2 90° peel strength of the positive electrode active material layer (N / m) Abschälfestigkeit (N / m) (S10) PVdF / NMP 0,020 0,024 0,025 0,026 0,030 (S20) Wasser / NMP 0,0020 2,8 3,5 3,7 3,8 4,1 0,0022 2,8 3,7 3,5 3,9 4,2 0,0069 2,9 3,7 3,6 4,2 4,2 0,0115 2,7 3,5 3,8 3,9 4 0,0120 2,6 3,5 3,5 3,8 3,9
[0075] As shown in Table 2 and Fig. As shown in Figure 3, the peel strength tended to increase as the PVdF / NMP mass ratio of the first kneading step (S10) increased, or in other words, as the amount of PVdF increased. When a practical level of durability is assumed, the 90° peel strength is, for example, preferably roughly 3 N / m or more, and more preferably 3.5 N / m or more. Based on the above results, it was determined that the PVdF / NMP mass ratio in the first kneading step (S10) should be 0.024 or more (and, for example, 0.025 or more). In addition, the water added in the second kneading step (S20) was not found to have any effect, and it was assumed that it was removed from the positive electrode active material layer without any problems in the above-mentioned drying step. [Manufacture of secondary batteries with non-aqueous electrolyte]
[0076] Using the 25 types of positive electrodes obtained in the above-described manner, non-aqueous electrolyte secondary batteries were fabricated. Specifically, a negative electrode active material in the form of amorphous coated graphite (C), a binder in the form of styrene butadiene rubber (SBR), and a thickener in the form of carboxymethyl cellulose (CMC) were placed in a kneader such that the mass ratio of these materials was such that C:SBR:CMC was 98:1:1, followed by kneading while adjusting the viscosity with ion-exchange water. This was then coated on a negative electrode current collector in the form of a copper foil, followed by drying (drying temperature: 100°C, drying time: 5 minutes) to prepare a negative electrode.
[0077] The positive electrode and negative electrode formed as described above were overlapped with a separator (a porous polyethylene (PE) sheet was used here) sandwiched between them to form an electrode body. The electrode body was then sealed in a battery case together with a non-aqueous electrolyte (an electrolyte obtained by dissolving a conductive salt in the form of LiPF6 with a concentration of approximately 1 mol / L in a mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 3:4:3) to prepare non-aqueous electrolyte secondary batteries (Examples 1 to 25). [Measuring resistance]
[0078] The resistance of the batteries prepared as described above was measured. Specifically, after initial charging with a constant current (CC) in a temperature environment of 25°C and at a rate of 1 / 3C until the battery voltage reached 4.1V, charging with a constant voltage (CV) was performed until the current flow rate reached 1 / 50C to achieve a fully charged state. Subsequently, the batteries were discharged with a constant current (CC) at a rate of 1 / 3C until the battery voltage reached 3.0V, and the CC discharge capacity at this time was considered the initial capacity.
[0079] Next, CC charging was performed on the batteries, followed by discharging at a rate of 1 / 3C and a temperature environment of 25°C until the SOC (state of charge) reached 60%, when the initial capacity was 100%. After the SOC was adjusted to 60%, the batteries were discharged for 10 seconds at a constant current of 15C, and the voltage drop was measured for 10 seconds. An IV resistance (mΩ) was then calculated by dividing the value of this change in voltage (V) by the corresponding current flow value. The results are shown in Table 3 and Fig. 4 shown. [Table 3] Table 3 Battery DC resistance (mΩ) Gleichstromwiderstand (mΩ) (S10) PVdF / NMP 0,020 0,024 0,025 0,026 0,030 (S20) Wasser / NMP 0,0020 3,5 3,5 3,5 3,6 3,5 0,0022 3,1 2,9 2,9 2,8 3,5 0,0069 3 2,9 3 2,8 3,5 0,0115 2,8 2,8 2,9 2,9 3,6 0,0120 3,4 3,5 3,8 3,8 4
[0080] As shown in Table 3 and Fig. As shown in Figure 4, based on the results of this study, it was determined that by adding a prescribed amount of water in the second kneading step, the DC resistance can be reduced compared to the case of not adding water. This is believed to be due to the addition of water, which promotes the gelation of PVdF and results in the efficient formation of electrically conductive paths between the positive electrode active material and the electrically conductive fine particles. However, if the amount of added water is excessively large, the gelation of PVdF proceeds excessively, and the electrically conductive fine particles become entangled or entangled, which is believed to prevent efficient covering of the surface of the positive electrode active material.Based on the above results, it was determined that the mass ratio of water / NMP in the second kneading step (S20) should be 0.0022 to 0.0115.
[0081] Furthermore, the DC resistance generally tended to increase as the PVdF / NMP mass ratio in the first kneading step (S10) increased (or, in other words, as the added amount of PVdF increased). The DC resistance is more preferably 3 mΩ or less, especially when considering high power output density applications such as vehicle-mounted batteries.
[0082] Based on the above results, it was determined that the mass ratio of PVdF / NMP in the first kneading step (S10) is more preferably 0.024 to 0.026 and that the mass ratio of water / NMP in the second kneading step (S20) is more preferably 0.0022 to 0.0115.
[0083] As described above, the manufacturing method disclosed herein can produce a positive electrode that is resistant to separation of the positive electrode active material layer and has low resistance. Furthermore, the use of this positive electrode makes it possible to realize a nonaqueous electrolyte secondary battery with superior power output characteristics and durability. These results indicate the technical significance of the present invention.
[0084] Although the above specification has provided a detailed description of certain examples of the present invention, these examples are intended to be exemplary only. Reference character list 10 positive electrode sheets (positive electrode) 14 Positive electrode active material layer 20 negative electrode sheets (negative electrode) 24 Negative electrode active material layer 40 separator sheets (separator) 50 battery cases 52 Battery housing body 54 Cover 55 Safety valve 70 Positive electrode connection 72 Negative electrode connection 80 wound electrode body 100 secondary battery with non-aqueous electrolyte< / s>
Claims
[1] A method of manufacturing a positive electrode for a non-aqueous electrolyte secondary battery, the method comprising: a first kneading step for kneading electrically conductive carbon fine particles and a hydrophobic binder that gels when contacted by water in N-methyl-2-pyrrolidone (NMP); a second kneading step of adding a positive electrode active material and water to a first kneaded product obtained in the first kneading step, followed by additional kneading; and a step of forming a positive electrode active material layer on the surface of a positive electrode current collector by layering a second kneaded product obtained in the second kneading step on the positive electrode current collector, wherein the first kneaded product comprises moisture, the ratio of the mass of moisture to the mass of NMP in the first kneaded product is 0.002 or less, and in the second kneading step, the water is added at a mass fraction of 0.0022 to 0.0115 based on the mass of NMP; wherein the ratio of the mass of the hydrophobic binder to the mass of the NMP in the first kneading step is 0.024 to 0.026; and where polyvinylidene fluoride (PVdF) is used as the hydrophobic binder. [2] The manufacturing method according to claim 1, wherein acetylene black is used as the electrically conductive carbon fine particles.
Citation Information
Patent Citations
Method of manufacturing positive electrode for lithium-ion secondary battery, method of manufacturing lithium-ion secondary battery, positive electrode for lithium-ion secondary battery, and lithium-ion secondary battery
JP2010157361A
Mixture slurry, and method for manufacturing the same
JP2012186054A
Nonaqueous electrolyte secondary battery
JP2014049390A
Battery electrode sheet, method and battery with the same
US20100248027A1
Rectangular nonaqueous electrolyte secondary battery and method for manufacturing the same