Semiconductor devices and methods for their manufacture

The method of epitaxially forming doped and undoped semiconductor layers within substrate depressions in semiconductor devices addresses material loss issues, ensuring layer integrity and reducing contact resistance for improved device performance.

DE102015104596B4Active Publication Date: 2024-11-07TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE102015104596
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-04-14
Filing Date
2015-03-26
Publication Date
2024-11-07
Estimated Expiration
2035-03-26

AI Technical Summary

Technical Problem

The manufacturing of semiconductor devices often results in inadvertent loss of material from the semiconductor substrate, which can adversely affect the device's performance and integrity.

Method used

A method involving epitaxial growth of a doped semiconductor material within a substrate depression, followed by the formation of an undoped semiconductor layer and optionally a third layer, with specific etching processes to protect the underlying layers during contact formation.

Benefits of technology

The method prevents material loss during etching, maintains layer integrity, and reduces contact resistance, enhancing the reliability and performance of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for manufacturing a semiconductor device, the method comprising the following: Providing (102) a substrate (202) with a depression (204); epitaxial formation (104) of a first layer (206) comprising a doped semiconductor material within the well (204), wherein a top surface (206a) of the first layer (206) is substantially flush with a top surface (202a) of the substrate (202); and epitaxial formation (106) of a second layer (208) comprising an undoped semiconductor material over at least one section of the well (204); wherein a thickness (T2) of the second layer is in a range of about 1 nanometer to about 6 nanometers.
Need to check novelty before this filing date? Find Prior Art

Description

BACKGROUND

[0001] Semiconductor devices are used in a wide variety of electronic applications, such as personal computers, mobile phones, digital cameras, and other electronic equipment. Semiconductor devices are typically manufactured by processing a semiconductor substrate, for example, by successively depositing insulating or dielectric layers, conductive layers, and semiconducting layers of material onto the substrate and structuring the various material layers using lithography or etching to create circuit components and elements.

[0002] The processing of the semiconductor substrate can lead to an unintended loss of material (for example, semiconductor material) from a section of the substrate, which can adversely affect the manufactured semiconductor device. There is a need to solve the problem described above, and new methods for manufacturing semiconductor devices may be required.

[0003] From US patent 2013 / 0295752A1, a method for the chemical-mechanical polishing of a semiconductor wafer is known, in which recesses of a substrate are filled with a first material and a second material that differs from the first material.

[0004] DE 10 2013 105 763 A1 discloses a semiconductor device comprising a substrate in which depressions are formed. A first and a second semiconductor layer are conformally formed on the substrate and the inner walls of the depressions.

[0005] DE 10 2009 014 507 A1 describes a method for forming an electrical contact between a carrier wafer and a surface of an upper silicon layer, in which a cavity is etched in the silicon layer and an epitaxial layer is formed in the cavity.

[0006] From US patent 2013 / 0105861A1, a method for forming a semiconductor device is known in which three epitaxial layers are formed on top of each other over a depression, wherein the uppermost of the three epitaxial layers is doped.

[0007] US Patent 2013 / 0109144A1 discloses a method in which a semiconductor device with a depression is formed. The depression is filled with two epitaxial layers, on which a third epitaxial layer is formed. The third epitaxial layer protrudes from a surrounding substrate and may be doped. SUMMARY OF THE INVENTION

[0008] The present invention relates to a method for manufacturing a semiconductor device according to claim 1, a method for manufacturing a semiconductor device according to claim 11 and a semiconductor device according to claim 14. Preferred embodiments are specified in the accompanying dependent claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] Aspects of this disclosure are best understood by reference to the following detailed description, when read in conjunction with the accompanying figures. It should be noted that, in accordance with common industry practice, various structural elements are not drawn to scale. The dimensions of illustrated structural elements may be enlarged or reduced as necessary for the clarity of the discussion. Fig. Figure 1 shows a method for manufacturing a semiconductor device according to some embodiments. Fig. 2A to Fig. Figures 2F show a process flow illustrating a method for manufacturing a semiconductor device comprising a first layer and a second layer according to some embodiments. Fig. Figure 3 shows a method for manufacturing a semiconductor device according to some embodiments. Fig. 4A to Fig. Figure 4F shows a process flow illustrating a method for manufacturing a semiconductor device comprising a first layer, a second layer and a third layer, according to some embodiments. Fig. 5 to Fig. Figure 7 shows various semiconductor devices according to some embodiments. DETAILED DESCRIPTION

[0010] The following disclosure provides many different embodiments or examples for implementing various features of the subject matter discussed herein. Specific examples of components and arrangements are described below to simplify the present disclosure. For example, the formation of a first structural element above or on top of a second structural element in the following description may include embodiments in which the first and second structural elements are in direct contact, and may also include embodiments in which additional structural elements may be formed between the first and second structural elements, so that the first and second structural elements are not necessarily in direct contact. Furthermore, the present disclosure may repeat reference numerals and / or letters in the various examples.This repetition serves the purpose of simplicity and clarity and does not automatically create a relationship between the various designs and / or configurations discussed.

[0011] Furthermore, spatially relative terms, such as "below," "under," "lower," "above," "upper," and the like, may be used in this text to simplify the description and to describe the relationship of one element or structural element to one or more other elements or structural elements, as illustrated in the figures. These spatially relative terms are intended to encompass not only the orientation shown in the figures but also other orientations of the device during use or operation. The device may also be oriented differently (rotated 90 degrees or otherwise), and the spatially relative descriptors used in this text may be interpreted accordingly.

[0012] Fig. Figure 1 shows a method 100 for manufacturing a semiconductor device according to one or more embodiments.

[0013] Method 100 may include: providing a substrate with a well (in 102); epitaxially forming a first layer containing a doped semiconductor material within the well (in 104); and epitaxially forming a second layer containing an undoped semiconductor material over at least one section of the well (in 106).

[0014] Method 100 may optionally include: forming a mask layer over the second layer and a section of the substrate (in 108); and etching a section of the mask layer arranged over the second layer (in 110).

[0015] Fig. 2A to Fig. Figures 2F show a process flow illustrating the process 100 for manufacturing a semiconductor device according to one or more embodiments.

[0016] As in Fig. As shown in a cross-sectional view 201, the method 100 for manufacturing a semiconductor device may include providing a substrate 202 with a depression 204.

[0017] The substrate 202 can have a top surface 202a. In one or more embodiments, the top surface 202a can refer to a surface of the substrate 202 that can be processed (for example, by etching, by depositing material, etc.).

[0018] The substrate 202 can contain (or consist of) a semiconductor material. According to one embodiment, the semiconductor material can contain (or consist of) at least one material selected from the following group: silicon, germanium, gallium nitride, gallium arsenide, and silicon carbide, although according to other embodiments, other materials may also be possible.

[0019] In one or more embodiments, the substrate 202 can be a doped substrate, for example, a doped semiconductor substrate. In one embodiment, the doped semiconductor substrate can be (or comprise) a doped silicon substrate, a doped germanium substrate, a doped gallium nitride substrate, a doped gallium arsenide substrate, or a doped silicon carbide substrate, although other doped semiconductor substrates are possible according to other embodiments. In this context, the term "doped substrate" can include an embodiment where the entire substrate 202 is doped, as well as another embodiment where only a part (for example, an upper part) of the substrate 202 is doped.

[0020] The substrate 202 can be a p-doped substrate (or, in other words, a substrate 202 doped with a p-type dopant) or an n-doped substrate (or, in other words, a substrate 202 doped with an n-type dopant). According to one embodiment, the dopants for doping the substrate 202 can contain (or consist of) at least one material selected from the following group of materials: boron, aluminum, gallium, indium, antimony, phosphorus, arsenic, and antimony, although other materials are possible according to other embodiments. For example, the substrate 202 can be a silicon substrate doped with a p-type dopant, such as boron. Or, according to another example, the substrate 202 can be a silicon substrate doped with an n-type dopant, such as phosphorus, arsenic, or antimony.

[0021] In one or more embodiments, the substrate 202 may contain (or be) a bulk semiconductor substrate.

[0022] In one or more embodiments, the substrate 202 can contain (or consist of) a substrate with at least one semiconductor layer, such as a silicon-on-insulator (SOI) semiconductor substrate. According to one embodiment, the at least one semiconductor layer can contain (or consist of) at least one material selected from the following group of materials: silicon, germanium, gallium nitride, gallium arsenide, and silicon carbide, although other materials are possible according to other embodiments.

[0023] In one or more embodiments, the substrate 202 can contain (or consist of) a substrate with at least one dielectric layer, such as a silicon-on-insulator (SOI) semiconductor substrate. According to one embodiment, the at least one dielectric layer can contain at least one material selected from the following group of materials: an oxide, a nitride, and an oxynitride, although other materials are possible according to other embodiments.

[0024] As in Fig. As shown in Figure 2A, the depression 204 can be arranged on the top surface 202a of the substrate 202. For example, an opening of the depression 204 can be arranged on the top surface 202a of the substrate 202.

[0025] In one or more embodiments, the depression 204 can extend partially through the substrate 202. Or, in other words, the depth D of the depression 204 can be less than the thickness T1 of the substrate 202. In one embodiment, the depth D of the depression 204 can be in the range of approximately 15 nm to approximately 60 nm, for example, in the range of approximately 20 nm to approximately 40 nm, or approximately 30 nm, although other values ​​are possible according to other embodiments.

[0026] The recess 204 can include at least one side wall 204a and a bottom surface 204b. According to one embodiment, the at least one side wall 204a of the recess 204 can be inclined. For example, in one embodiment, an angle α formed by the at least one side wall 204a and a line parallel to the top surface 202a of the substrate 202 (for example, line AB in Fig. 2A) is included, in the range of approximately 20° to approximately 70°, for example in the range of approximately 30° to approximately 60°, for example approximately 55°, although according to other embodiments other values ​​may also be possible.

[0027] According to one embodiment, the width W of the recess 204 can be measured as the widest lateral extent of the recess 204. For example, the width W can be measured as the lateral extent of the recess 204 on the top surface 202a of the substrate 202, as in the example of Fig. 2A shown. As another example, the width W can be measured as the lateral extent of the opening of the depression 204, which can be located on the top surface 202a of the substrate 202.

[0028] In one or more embodiments, the width W of the recess 204 can be in the range of about 30 nm to about 100 nm, for example about 60 nm, although other values ​​may be possible according to other embodiments.

[0029] In one embodiment, the recess 204 can be formed by means of an etching process. The etching process can include (or be) a wet etching process and / or a dry etching process (for example, a plasma etching process) or other suitable etching processes.

[0030] According to one embodiment, the etching process can be carried out in conjunction with a structured etching mask that can be formed over a portion of the top surface 202a of the substrate 202. The structured etching mask can be formed by depositing a masking material over the substrate 202 and structuring the masking material to create the structured etching mask. The structuring of the masking material can include (or consist of) a lithographic process (for example, a photolithographic process). The structured etching mask can be removed after the formation of the depression 204.

[0031] As in Fig. As shown in Figure 2A, the depression 204 can be arranged in a region 202R of the substrate 202. In one embodiment, the region 202R can contain (or be) an active region or area of ​​the substrate 202. In this context, the term "active region" or "active area" can contain (or be) a region or area of ​​the substrate 202 that is defined for further processing (for example, by etching, by material deposition, etc.). In one embodiment, the region 202R of the substrate 202 in which the depression 204 is arranged can contain or be a source region or a drain region of the semiconductor device, as defined in Figure 2A. Fig. 1 shown procedure 100 and / or the one in Fig. 2A to Fig. The process flow shown in 2F is produced.

[0032] As in Fig. As shown in a cross-sectional view 203 in Figure 2B, the method 100 for fabricating a semiconductor device can include the epitaxial formation of a first layer 206 containing a doped semiconductor material within the well 204. The epitaxial process for fabricating the first layer 206 is shown in Fig. 2B is shown as arrow 205.

[0033] In the Fig. In the embodiment shown in Figure 2B, a top surface 206a of the first layer 206 can be at least substantially flush with the top surface 202a of the substrate 202. In a further embodiment, the top surface 206a of the first layer 206 can be arranged at a level below the top surface 202a of the substrate 202 (which is shown, for example, below with respect to Fig. 7 is described). Or, put another way: In such an embodiment (for example, in Fig. (as shown in Figure 7) the top surface 206a of the first layer 206 can be closer to the bottom surface 204b of the depression 204 than the top surface 202a of the substrate 202 is to the bottom surface 204b of the depression 204.

[0034] The doped semiconductor material of the first layer 206 can contain (or be) a doped semiconductor material that can be formed (for example, grown and / or deposited) by means of the epitaxial process 205. In one embodiment, the doped semiconductor material of the first layer 206 can contain (or be) doped silicon, although according to other embodiments, other doped semiconductor materials (for example, doped silicon-germanium) are also possible.

[0035] The doped semiconductor material of the first layer 206 can have a conductivity type that may be different from the conductivity type of the substrate 202.

[0036] For example, in one embodiment, the doped semiconductor material of the first layer 206 can contain n-type dopants, and the substrate 202 can contain (or be) a semiconductor substrate doped with a p-type dopant. For example, the doped semiconductor material can contain (or be) phosphorus-doped silicon (for example, Si:P) or arsenic-doped silicon (for example, Si:Als), and the substrate 202 can contain (or be) boron-doped silicon (for example, Si:B) or boron-doped silicon-germanium (for example, SiGeB).

[0037] As another example, in one embodiment the doped semiconductor material of the first layer 206 can contain p-type dopants, and the substrate 202 can contain (or be) a semiconductor substrate doped with an n-type dopant. For example, the doped semiconductor material can contain (or be) boron-doped silicon (for example, SiB) or boron-doped silicon-germanium (for example, SiGeB), and the substrate 202 can contain (or be) phosphorus-doped silicon (for example, SiP).

[0038] The concentration of dopant atoms in the doped semiconductor material of the first layer 206 can be in the range of approximately 1 × 10 20 atoms per cubic centimeter up to about 3 × 10 21atoms per cubic centimeter. For example, in one embodiment, the concentration of phosphorus atoms in a phosphorus-doped semiconductor material (for example, SiP) of the first layer 206 can be in the range of approximately 2 × 10 20 atoms per cubic centimeter up to about 2 × 10 21 atoms per cubic centimeter.

[0039] As described above, the first layer 206 can be formed (for example, grown and / or deposited) by means of the epitaxial process 205. The epitaxial process 205 can include at least one liquid-phase epitaxial process, one molecular-beam epitaxial process, and one vapor-phase epitaxial process. For example, in one embodiment, the first layer 206 can be formed (for example, grown and / or deposited) by means of a vapor-phase epitaxial process.

[0040] In one or more embodiments, the first layer 206 can contain several sublayers. Each sublayer of the multiple sublayers of the first layer 206 can be formed by means of the epitaxial process 205.

[0041] In one embodiment, the first layer 206 can comprise a first sublayer 206-1 near the bottom surface 204b of the depression 204 and a second sublayer 206-2 near the top surface 202a of the substrate 202. The top surface 206a of the first layer 206 can comprise or be the top surface of the second sublayer 206-2 of the first layer, as in the example of Fig. 2B shown.

[0042] In the Fig. In the embodiment shown in Figure 2B, the first sublayer 206-1 and the second sublayer 206-2 of the first layer 206 can have top surfaces that are at least substantially parallel to the bottom surface 204b of the depression 204 or to the top surface 202a of the substrate 202, or to both. However, in another embodiment, the top surfaces of the first sublayer 206-1 and the second sublayer 206-2 can follow a contour or shape of one of the at least one side wall 204a and the bottom surface 204b of the depression 204 (as, for example, in the embodiment shown in Figure 2B). Fig. 7 shown).

[0043] In one embodiment, the thickness of the first sublayer 206-1 of the first layer 206 can be in the range of about 5 nanometers to about 10 nanometers, although other thicknesses are possible according to other embodiments. The thickness of the second sublayer 206-2 of the first layer 206 can be in the range of about 10 nanometers to about 30 nanometers, although other thicknesses are possible according to other embodiments.

[0044] In one embodiment, the first layer 206 can be a third sublayer (in Fig. (2B not shown) which is arranged above the second sublayer 206-2. In one embodiment, the top surface of the third sublayer can be at least substantially flush (i.e., coplanar) with the top surface 202a of the substrate 202. In another embodiment, the top surface of the third sublayer can be arranged within the recess 204. In such an embodiment, the top surface of the third sublayer can be at a level below the top surface 202a of the substrate 202. In one embodiment, the thickness of the third sublayer of the first layer 206 can be in the range of about 4 nanometers to about 9 nanometers, although other thicknesses are possible according to other embodiments.

[0045] As in Fig. As shown in a cross-sectional view 207, the method 100 for fabricating a semiconductor device can include the epitaxial formation of a second layer 208, which contains an undoped semiconductor material over at least one section of the well 204. The epitaxial process for fabricating the second layer 208 is shown in Fig. 2C is shown as arrow 209.

[0046] The undoped semiconductor material of the second layer 208 can contain (or be) an undoped semiconductor material that can be formed (for example, grown and / or deposited) by means of the epitaxial process 209. In one embodiment, the undoped semiconductor material of the second layer 208 can contain (or be) undoped silicon.

[0047] The second layer 208 can have a top surface 208a, which can be arranged at a higher level than the top surface 202a of the substrate 202. In the embodiment shown in Fig. 2C, a bottom surface 208b of the second layer 208 can be at least substantially flush (i.e., coplanar) with the top surface 202a of the substrate. However, in another embodiment, the bottom surface 208b of the second layer 208 can also be arranged above—or at a level below—the top surface 202a of the substrate (which is shown, for example, below with respect to Fig. 7 is described).

[0048] In the embodiment shown in Fig. In 2C, the bottom surface 208b of the second layer 208 can be in contact (for example, in direct contact, for example, in direct physical contact) with the top surface 206a of the first layer 206. However, in another embodiment, the bottom surface 208b of the second layer 208 can be arranged above the top surface 206a of the first layer 206 and need not be in contact with it (which is shown, for example, below with respect to Fig. 6 and Fig. 7 is described).

[0049] The thickness T2 of the second layer 208 can be measured from the bottom surface 208b to the top surface 208a of the second layer 208. The thickness T2 of the second layer 208 can be in a range of approximately 1 nanometer to approximately 6 nanometers, for example, in a range of approximately 1 nanometer to approximately 3 nanometers or in a range of approximately 2 nanometers to approximately 5 nanometers.

[0050] In one embodiment, the second layer 208 can further comprise a doped semiconductor material (for example, doped silicon). In one embodiment, the undoped semiconductor material can be contained in one sublayer of the second layer 208, while the doped semiconductor material can be contained in another sublayer of the second layer 208.

[0051] In one embodiment, the doped semiconductor material of the second layer 208 (for example, the sublayer containing the doped semiconductor material of the second layer 208) can be arranged near the top surface 202a of the substrate 202, and the undoped semiconductor material of the second layer 208 (for example, the sublayer containing the undoped semiconductor material of the second layer 208) can be arranged away from the top surface 202a of the substrate 202.

[0052] The doped semiconductor material of the second layer 208 (for example, the sublayer containing the doped semiconductor material of the second layer 208) can have a constant doping profile or a graded doping profile. In an embodiment where the doped semiconductor material of the second layer 208 (for example, the sublayer containing the doped semiconductor material of the second layer 208) can have a graded doping profile, the dopant concentration can be higher near the top surface 202a of the substrate 202, while the dopant concentration can be lower at a distance from the top surface 202a of the substrate 202.

[0053] In one embodiment, the concentration of dopant atoms (for example, phosphorus atoms) of the doped semiconductor material (for example, doped silicon) of the second layer 208 can be in the range of about 0 atoms per cubic centimeter to about 1 × 10 18atoms per cubic centimeter, although other concentrations of dopant atoms may be possible according to other embodiments.

[0054] As described above, the second layer 208 can be formed (for example, grown and / or deposited) by means of the epitaxial process 209. The epitaxial process 209 for forming the second layer 208 can include at least one liquid-phase epitaxial process, one molecular-beam epitaxial process, and one vapor-phase epitaxial process. For example, in one embodiment, the second layer 208 can be formed (for example, grown and / or deposited) by means of a vapor-phase epitaxial process.

[0055] The epitaxial process 209 can contain (or be) at least one of a cyclic deposition set (CDE) process and a selective epitaxial growth (SEG) process.

[0056] The epitaxial process 209 can be carried out at a temperature in a range of about 600 °C to about 750 °C, for example about 680 °C.

[0057] The epitaxial process 209 can be carried out with a precursor gas containing the undoped semiconductor material. For example, in an embodiment where the undoped semiconductor material contains or is silicon, the precursor gas can contain (or be) at least one of silane (SiH4), disilane (Si2H6), and dichlorosilane (SiH2Cl2).

[0058] In one embodiment, silane or disilane may be preferred to dichlorosilane, since silane or disilane may lead to a higher deposition rate of undoped silicon in the epitaxial process 209.

[0059] In one embodiment, chlorine present during the epitaxial process 209 can help to desorb hydrogen from the top 206a of the first layer 206 and / or the top 202a of the substrate 202, thereby promoting the deposition and / or growth of the undoped semiconductor material (for example, undoped silicon) of the second layer 208.

[0060] As described above, the second layer 208 can be formed over at least one section of the recess. In one embodiment, the lateral extent L of the second layer 208 can be smaller than the width W of the recess 206. In another embodiment, the lateral extent L of the second layer 208 can be at least substantially equal to the width W of the recess 206.

[0061] In the Fig. In the example shown in Figure 2C, the lateral extent L of the second layer 208 can be smaller than the width W of the recess 206. Furthermore, the lateral extent L of the second layer 208 can be arranged within the width W of the recess 206. In another embodiment, the lateral extent L of the second layer 208 can be at least substantially equal to the width W of the recess 206, and the lateral extent L of the second layer 208 can completely overlap the width W of the recess 206.

[0062] As in Fig. As shown in a 2D cross-sectional view 211, the method 100 for manufacturing a semiconductor device can optionally include the formation of a mask layer 210 over the second layer 208 and a section 202P1 of the substrate 202.

[0063] In one or more embodiments, the mask layer 210 can contain (or consist of) a dielectric material. According to one embodiment, the mask layer 210 can contain (or consist of) at least one material selected from the following group of materials: an oxide, a nitride, and an oxynitride, although other materials are possible according to other embodiments. For example, the mask layer 210 can contain (or consist of) silicon dioxide (SiO2) and / or silicon nitride (Si3N4).

[0064] The substrate 202 may contain a further section 202P2, which may be free of the mask layer 210. The section 202P2 of the substrate 202, which is free of the mask layer 210, can be processed (e.g., etched) using the mask layer 210 as a processing mask (for example, an etching mask). Or, in other words, the mask layer 210 can protect the second layer 208, the underlying first layer 204, and section 202P1 of the substrate 202 during processing of section 202P2 of the substrate 202. Processing of section 202P2 is not in Fig. Shown in 2D.

[0065] After processing section 202P2 of the substrate 202, the second layer 208 can be exposed, for example by removing section 210P of the mask layer 210 that is arranged above the second layer 208, as for example in Fig. 2E shown in a cross-sectional view 213.

[0066] Section 210P of the mask layer 210, which is located above the second layer 208, can be etched using a wet etching process (in Fig. 2E (shown as arrow 215) can be removed, which can be done with an acid, for example hot phosphoric acid.

[0067] One effect achieved by the second layer 208, which contains the undoped semiconductor material, can be increased selectivity during the removal of section 210P of the mask layer 210. For example, the undoped semiconductor material of the second layer 208 can be highly resistant to the wet etching process 215 (e.g., acid in the wet etching process 215, for example, hot phosphoric acid in the wet etching process 215). In this way, the undoped semiconductor material of the second layer 208 is exposed for the wet etching process 215, and the underlying first layer 204 is protected by the second layer 208 from etch-induced material loss (e.g., SiP material loss).

[0068] As described above, in an embodiment where the second layer 208 may further contain a doped semiconductor material (for example, with a constant or graded doping profile), the undoped semiconductor material of the second layer 208 may be arranged at a distance from the top surface 202a of the substrate 202, while the doped semiconductor material of the second layer 208 may be arranged close to the top surface 202a of the substrate 202. In such an embodiment, the resistance of the second layer 208 to the wet etching process 215 is maintained, since the undoped semiconductor material of the second layer 208, which lies above the doped semiconductor material of the second layer 208 and the underlying first layer 204, is exposed to the wet etching process 215.In this way, the underlying doped semiconductor material of the second layer 208 and the first layer 204 is protected from etch-induced material loss (for example, SiP material loss) by the undoped semiconductor material of the second layer 208.

[0069] After the in Fig. In the process shown in Figure 2E, an electrical contact 219 can be formed above the first layer 206, as for example in Fig. 2F shown in a cross-sectional view 217.

[0070] The electrical contact 219 may contain a silicide layer (in Fig. 2F not shown), which can be in contact (for example, in direct physical contact) with the top surface 206a of the first layer 206. The electrical contact 219 can be formed after exposing the top surface 206a of the first layer 206.

[0071] Exposing the top surface 206a of the first layer 206 may involve removing at least a section of the second layer 208 that lies above the first layer 206. The section of the second layer 208 that lies above the first layer 206 may be removed during the wet etching process 215. Accordingly, the Fig. The second layer 208 shown in Figure 2E is just thick enough to be consumed and / or removed by the wet etching process 215, while the underlying first layer 206 remains unchanged. Therefore, one effect achieved by the thickness T2 of the second layer 208, which lies in the range described above of approximately 1 nanometer to approximately 6 nanometers, can be the prevention of losses due to contact resistance, which can be caused, for example, by the second layer 208 forming during the formation of the electrical contact 218 over the first layer 206, as in Fig. 2F is shown, it is present.

[0072] Fig. Figure 3 shows a method 300 for manufacturing a semiconductor device according to one or more embodiments.

[0073] Method 300 may include: providing a substrate with a well (in 302); epitaxially forming a first layer containing a doped semiconductor material within the well (in 304); and epitaxially forming a second layer containing an undoped semiconductor material over at least one section of the well (in 306).

[0074] Method 300 can optionally include the epitaxial formation of a third layer containing a semiconductor material over a surface of the first layer, wherein the epitaxial formation of the second layer includes the epitaxial formation of the second layer over the first layer and the third layer (in 308).

[0075] Method 300 may optionally include: forming a mask layer over the second layer and a section of the substrate (in 310); etching a section of the mask layer arranged over the second layer (in 312); and forming an electrical contact over the first layer (in 312).

[0076] Fig. 4A to Fig. Figure 4F shows a process flow illustrating the process 300 for manufacturing a semiconductor device according to one or more embodiments.

[0077] The reference symbols in Fig. 4A to Fig. 4F, which are the same as in Fig. 2A to Fig. 2F denotes the same or similar elements as in Fig. 2A to Fig. 2F. Therefore, these elements will not be described in detail again here, and reference is made to the description above. The differences between Fig. 4A to Fig. 4F and Fig. 2A to Fig. 2F are described below.

[0078] As in Fig. As shown in cross-sectional view 400, the first layer 206 within the depression 208 can be formed epitaxially, similar to the above in conjunction with Fig. 2A to Fig. 2B described.

[0079] As in Fig. As shown in a cross-sectional view 401 in Figure 4B, the method 300 for fabricating a semiconductor device can include the epitaxial formation of a third layer 402, which contains a semiconductor material over a surface (for example, the top surface 206a) of the first layer 206. The epitaxial process for fabricating the third layer 402 is shown in Figure 4B. Fig. 4B shown as arrows 403.

[0080] In the Fig. In the embodiment shown in Figure 4B, the third layer 402 can have a top surface 402a that may be arranged at a higher level than the top surface 202a of the substrate 202. However, in another embodiment, the top surface 402a of the third layer 402 can be at least substantially flush (i.e., coplanar) with the top surface 202a of the substrate (as shown, for example, below with respect to Fig. 7 is described).

[0081] In the Fig. In the embodiment shown in Figure 4B, a bottom surface 402b of the third layer 402 can be at least substantially flush (i.e., coplanar) with the top surface 202a of the substrate. However, in another embodiment, the bottom surface 402b of the third layer 402 can be arranged at a level below the top surface 202a of the substrate 202 (as shown, for example, below with respect to Fig. 7 is described).

[0082] In the Fig. In the embodiment shown in 4B, the bottom surface 402b of the third layer 402 can be in contact (for example, in direct contact, for example, in direct physical contact) with the top surface 206a of the first layer 206.

[0083] In the Fig. In the embodiment shown in 4B, the third layer 402 can be formed over the entire lateral extent of the top surface 206a of the first layer 206. Or, in other words, the third layer 402 can completely cover the top surface 206a of the first layer 206 in the embodiment shown in 4B. Fig. 4B cover. However, in another embodiment, the third layer 402 can be formed above the top surface 206a of the first layer 206 and can cover a section of it.

[0084] The thickness T3 of the third layer 402 can be measured from the bottom surface 402b to the top surface 402a of the third layer 402. The thickness T3 of the third layer 402 can be in a range of approximately 1 nanometer to approximately 5 nanometers, for example, in a range of approximately 1 nanometer to approximately 3 nanometers or in a range of approximately 2 nanometers to approximately 5 nanometers.

[0085] The semiconductor material of the third layer 402 can contain (or be) a semiconductor material that can be formed (for example, grown and / or deposited) by means of the epitaxial process 403. For example, in one embodiment, the semiconductor material of the third layer 402 can contain at least one material selected from the following group of materials: silicon carbide (SiC) and silicon phosphorus carbide (SiCP).

[0086] In one embodiment, the third layer 402 can contain carbon. The concentration of carbon in the third layer 402 can be in the range of about 0.5 mol percent to about 2 mol percent, for example about 1 mol percent, although other concentrations are possible according to other embodiments.

[0087] In one embodiment, the semiconductor material of the third layer 402 can contain dopants (for example, phosphorus atoms). The concentration of dopants in the semiconductor material of the third layer 402 can be less than or equal to approximately 2 × 10⁻⁶. 20 atoms per cubic centimeter, for example less than - or equal to - approximately 1 × 10 20 atoms per cubic centimeter. The concentration of dopant atoms in the third-layer semiconductor material 402 can be selected based on various factors, which are related to Fig. 4D will be discussed.

[0088] As described above, the third layer 402 can be formed (for example, grown and / or deposited) by means of the epitaxial process 403. The epitaxial process 403 for forming the second layer 208 can include at least one liquid-phase epitaxial process, one molecular-beam epitaxial process, and one vapor-phase epitaxial process. For example, in one embodiment, the third layer 402 can be formed (for example, grown and / or deposited) by means of a vapor-phase epitaxial process.

[0089] The epitaxial process 403 may contain (or be) at least one of a cyclic deposition set (CDE) process and a selective epitaxial growth (SEG) process.

[0090] The epitaxial process 403 can be carried out at a temperature in the range of about 600 °C to about 750 °C, for example, about 680 °C. The epitaxial process 403 can be carried out with a precursor gas containing the semiconductor material. For example, in an embodiment where the semiconductor material contains or is silicon, the precursor gas can contain (or be) at least one of silane (SiH4), disilane (Si2H6), and dichlorosilane (SiH2Cl2).

[0091] In one embodiment, chlorine present in the epitaxial process 403 can help to desorb hydrogen from the top 206a of the first layer 206 and / or the top 202a of the substrate 202, thereby requiring the deposition and / or growth of the semiconductor material (for example, silicon) of the third layer 402.

[0092] As in Fig. As shown in cross-sectional view 405 in Figure 4C, the method 300 for fabricating a semiconductor device can include the epitaxial formation of the second layer 208, which contains the undoped semiconductor material above the first layer 206 and the third layer 402. For example, the third layer 402 can be arranged between the first layer 206 and the second layer 208.

[0093] In the Fig. In the embodiment shown in Figure 4C, the second layer 208 can be formed over the entire lateral extent of the top surface 402a of the third layer 402. Or, in other words, the second layer 208 can completely cover the top surface 402a of the third layer 402 in the embodiment shown in Figure 4C. Fig. 4B cover. However, in another embodiment, the second layer 208 can be formed above the top surface 402a of the third layer 402 and cover a section of it.

[0094] As in Fig. As shown in a 4D cross-sectional view 407, the method 300 for fabricating a semiconductor device can optionally include forming the mask layer 210 over the second layer 208 and section 202P1 of the substrate 202, similar to the above in conjunction with Fig. Described in 2D.

[0095] As in Fig. As shown in a cross-sectional view 409, the method 300 for fabricating a semiconductor device can optionally include the removal of section 210P of the mask layer 210, which is arranged above the second layer 208, similar to the above in conjunction with Fig. 2E described.

[0096] Section 210P of the mask layer 210, which is located above the second layer 208, can be etched using a wet etching process (in Fig. 4E (shown as arrow 215) can be removed, which can be done with an acid, for example hot phosphoric acid.

[0097] One effect achieved by the third layer 402 is increased selectivity during the removal of section 210P from the mask layer 210. For example, the third layer 402 can act as a barrier layer that prevents or reduces (for example, by slowing down) the diffusion (e.g., upward diffusion) of dopant atoms from the doped semiconductor material of the underlying first layer 206 into the second layer 208. Accordingly, the undoped semiconductor material of the second layer 208 can remain free of dopant atoms with the help of the third layer 402 (e.g., barrier layer, diffusion barrier layer). Therefore, the second layer 208 can be highly resistant to the wet etching process 215 (e.g., the acid of the wet etching process 215, for example, hot phosphoric acid of the wet etching process 215).Consequently, the underlying first layer 204 is protected from etch-induced material loss (for example, SiP material loss in the first layer 204) by the second layer 208.

[0098] As described above, the semiconductor material of the third layer 402 can contain dopants. These dopants can be deliberately added during the epitaxial process 403. The concentration of dopants in the semiconductor material of the third layer 402 can be selected based on various factors, such as the etch rate of the semiconductor material (for example, silicon carbide) of the third layer 402 and the contact resistance of an electrical contact that can subsequently be formed over the first layer 206.

[0099] After the in Fig. In the process shown in Figure 4E, an electrical contact 419 can be formed above the first layer 206, as for example in Fig. 4F shown in a cross-sectional view 411.

[0100] The electrical contact 419 can have a silicide layer (in Fig. 4F (not shown) which can be in contact (for example, in direct contact, for example, in direct physical contact) with the top surface 206a of the first layer 206. The electrical contact 419 can be formed after the top surface 206a of the first layer 206 has been exposed.

[0101] Exposing the top surface 206a of the first layer 206 may involve removing at least a section of the third layer 402 and the second layer 208 that lies above the first layer 206. This section of the third layer 402 and the second layer 208 that lies above the first layer 206 can be removed during the wet etching process 215. Accordingly, the total thickness of the third layer 402 and the second layer 208 (i.e., the sum of thickness T2 and thickness T3) may be just sufficient for the third layer 402 and the second layer 208 to be consumed and / or removed by the wet etching process 215, while leaving the underlying first layer 206 unchanged.Therefore, an effect achieved by having the thickness T2 of the second layer 208 within the range described above of approximately 1 nanometer to approximately 6 nanometers, and by having the thickness T3 of the third layer 402 in a range of approximately 1 nanometer to approximately 5 nanometers, can be the prevention of losses due to contact resistance, which can be caused, for example, by the fact that the second layer 208 is present over the first layer 206 during the formation of the electrical contact.

[0102] Fig. Figure 5 shows a semiconductor device 500 according to one or more embodiments.

[0103] Reference numeral in Fig. 5, which are the same as in Fig. 2A to Fig. 2F and Fig. 4A to Fig. 4F denotes the same or similar elements as in Fig. 2A to Fig. 2F and Fig. 4A to Fig. 4F. Therefore, these elements will not be described in detail again here, and reference is made to the description above.

[0104] The semiconductor device 500 can include: a substrate 202 having a well 204, a first layer 206 containing a doped semiconductor within the well 204, and a second layer 208 containing an undoped semiconductor material over at least one section of the well 204.

[0105] In the Fig. In the embodiment shown in Figure 5, the top surface 206a of the first layer 206 can be at least substantially flush with the top surface 202a of the substrate 202. Furthermore, in the embodiment shown in Fig. In the embodiment shown in Figure 5, the bottom surface 208b of the second layer 208 is in contact (for example, in direct contact, for example, in direct physical contact) with the top surface 206a of the first layer 206.

[0106] The semiconductor device 500 can include a gate layer 502 (for example, a metal gate layer and / or a polysilicon gate layer) arranged on the top surface 202a of the substrate and adjacent to the recess 206. The semiconductor device 500 can further include an insulating layer 504 arranged on one or more side walls of the gate layer 502.

[0107] In one embodiment, the semiconductor device 500 can be a metal-oxide-semiconductor field-effect transistor (MOSFET). In another embodiment, the semiconductor device 500 can be a finned field-effect transistor (FINFET).

[0108] Fig. Figure 6 shows a semiconductor device 600 according to one or more embodiments.

[0109] The reference symbols in Fig. 6, which are the same as in Fig. 2A to Fig. 2F, Fig. 4A to Fig. 4F and Fig. 5 are, denote the same or similar elements as in Fig. 2A to Fig. 2F, Fig. 4A to Fig. 4F and Fig. 5. Therefore, these elements will not be described in detail again here, and reference is made to the description above.

[0110] The semiconductor device 600 can include: a substrate 202 having a cavity 204, a first layer 206 containing a doped semiconductor within the cavity 204, a second layer 208 containing an undoped semiconductor material over at least one section of the cavity 204, and a third layer 402 containing a semiconductor material arranged between the first layer 206 and the second layer 208.

[0111] In the Fig. In the embodiment shown in Figure 6, the third layer 402 can have a top surface 402a which can be arranged at a higher level than the top surface 202a of the substrate 202.

[0112] In the Fig. In the embodiment shown in Figure 6, the bottom surface 208b of the second layer 208 can be arranged above the top surface 206a of the first layer 206 and need not be in contact with it.

[0113] In one embodiment, the semiconductor device 600 can be a metal-oxide-semiconductor field-effect transistor (MOSFET). In another embodiment, the semiconductor device 600 can be a finned field-effect transistor (FINFET).

[0114] Fig. Figure 7 shows a semiconductor device 700 according to one or more embodiments.

[0115] The reference symbols in Fig. 7, which are the same as in Fig. 2A to Fig. 2F, Fig. 4A to Fig. 4F, Fig. 5 and Fig. 6 are, denote the same or similar elements as in Fig. 2A to Fig. 2F, Fig. 4A to Fig. 4F, Fig. 5 and Fig. 6. Therefore, these elements will not be described in detail again here, and reference is made to the description above.

[0116] The semiconductor device 700 can include: a substrate 202 having a cavity 204, a first layer 206 containing a doped semiconductor within the cavity 204, a second layer 208 containing an undoped semiconductor material over at least one section of the cavity 204, and a third layer 402 containing a semiconductor material arranged between the first layer 206 and the second layer 208.

[0117] In the Fig. In the embodiment shown in Figure 7, the first layer 206 can comprise a first sublayer 206-1 and the second sublayer 206-2, which is arranged above the first sublayer 206-1. In the embodiment shown in Fig. In the embodiment shown in Figure 7, the upper surfaces of the first sublayer 206-1 and the second sublayer 206-2 can follow a contour or shape of the at least one side wall 204a and bottom surface 204b of the recess 204.

[0118] In the Fig. In the embodiment shown in Figure 7, the top surface 402a of the third layer 402 can be at least substantially flush (i.e. coplanar) with the top surface 202a of the substrate.

[0119] In the Fig. In the embodiment shown in Figure 7, the top surface 206a of the first layer 206 can be arranged at a level below the top surface 202a of the substrate 202.

[0120] In the Fig.In the embodiment shown in Figure 7, the bottom surface 402b of the third layer 402 can be in contact (for example, in direct contact, for example, in direct physical contact) with the top surface 206a of the first layer 206. Accordingly, the bottom surface 402b of the third layer 402 can be arranged at a level below the top surface 202a of the substrate 202.

[0121] The bottom surface 402b can be inclined, for example because the top of the first layer 206 follows a contour or shape of at least one side wall 204a and the bottom surface 204b follows the depression 204.

[0122] In one embodiment, the semiconductor device 700 can be a metal-oxide-semiconductor field-effect transistor (MOSFET). In another embodiment, the semiconductor device 700 can be a finned field-effect transistor (FINFET).

[0123] According to various embodiments presented in this text, an effect achieved by the second layer 208, which contains the undoped semiconductor material, can be increased selectivity during the removal of section 210P of the mask layer 210. For example, the undoped semiconductor material of the second layer 208 can be highly resistant to the wet etching process 215 (e.g., acid in the wet etching process 215, for example, hot phosphoric acid in the wet etching process 215). In this way, the undoped semiconductor material of the second layer 208 is exposed to the wet etching process 215, and the underlying first layer 204 is protected by the second layer 208 from etch-induced material loss (e.g., SiP material loss).

[0124] According to various embodiments presented in this text, an electrical contact can be formed across the first layer 206, for example, after exposing the top surface 206a of the first layer 206, for example, by removing at least a section of the second layer 208 that lies above the first layer 206. The section of the second layer 208 that lies above the first layer 206 can be removed during the wet etching process 215. Accordingly, the second layer 208 can be just thick enough to be consumed and / or removed by the wet etching process 215, while the underlying first layer 206 remains unchanged.Therefore, an effect achieved by ensuring that the thickness T2 of the second layer 208 is within the range described above of approximately 1 nanometer to approximately 6 nanometers can be the prevention of losses due to contact resistance, which can be caused, for example, by the presence of the second layer 208 over the first layer 206 during the formation of the electrical contact.

[0125] According to various embodiments presented in this text, a third layer 402 can be arranged between the second layer 208 and the first layer 206. One effect achieved by the third layer 402 can be increased selectivity during the removal of section 210P of the mask layer 210. For example, the third layer 402 can act as a barrier layer that can prevent or reduce (for example, by slowing down) the diffusion (e.g., upward diffusion) of dopant atoms from the doped semiconductor material from the underlying first layer 206 into the second layer 208. Accordingly, the undoped semiconductor material of the second layer 208 can remain free of dopant atoms with the help of the third layer 402 (e.g., barrier layer, diffusion barrier layer).Therefore, the second layer 208 can be highly resistant to the wet etching process 215 (for example, the acid of the wet etching process 215, for example, hot phosphoric acid of the wet etching process 215). Consequently, the underlying first layer 204 is protected by the second layer 208 from etch-induced material loss (for example, SiP material loss in the first layer 204).

[0126] According to various embodiments presented in this text, an electrical contact can be formed above the first layer 206, for example, after exposing the top surface 206a of the first layer 206, for example, by removing at least a section of the third layer 402 and the second layer 208 that lies above the first layer 206. The section of the third layer 402 and the second layer 208 that lies above the first layer 206 can be removed during the wet etching process 215. Accordingly, the total thickness of the third layer 402 and the second layer 208 (i.e., a sum of thickness T2 and thickness T3) can be just sufficient to allow the third layer 402 and the second layer 208 to be consumed and / or removed by the wet etching process 215, while the underlying first layer 206 remains essentially unchanged.Therefore, an effect achieved by ensuring that the thickness T2 of the second layer 208 is within the range described above of approximately 1 nanometer to approximately 6 nanometers, and that the thickness T3 of the third layer 402 is in a range of approximately 1 nanometer to approximately 5 nanometers, can be the prevention of losses due to contact resistance, which can be caused, for example, by the presence of the second layer 208 over the first layer 206 during the formation of the electrical contact.

Claims

[1] A method of manufacturing a semiconductor device, the method comprising: Providing (102) a substrate (202) having a recess (204); epitaxially forming (104) a first layer (206) comprising a doped semiconductor material within the recess (204), wherein a top surface (206a) of the first layer (206) is substantially flush with a top surface (202a) of the substrate (202); and epitaxially forming (106) a second layer (208) comprising an undoped semiconductor material over at least a portion of the recess (204); wherein a thickness (T2) of the second layer is in a range of about 1 nanometer to about 6 nanometers. [2] The method of claim 1, wherein the undoped semiconductor material of the second layer (208) includes undoped silicon. [3] A method according to any one of the preceding claims, further comprising: Forming (108) a mask layer (210) over the second layer (208) and a portion (202P1) of the substrate (202); and Removing a portion (21oP) of the mask layer (210) disposed over the second layer (208). [4] The method of claim 3, wherein removing the portion (21oP) of the mask layer (210) comprises a wet etching process. [5] The method of any preceding claim, wherein the second layer (208) further comprises a doped semiconductor material, wherein the undoped semiconductor material of the second layer (208) is spaced from a top surface of the substrate (202) and the doped semiconductor material of the second layer is proximate the top surface (202a) of the substrate (202). [6] The method of claim 5, wherein the doped semiconductor material of the second layer (208) has a graded doping profile, wherein a dopant concentration is higher near the top surface (202a) of the substrate (202), and wherein the dopant concentration is lower at a distance from the top surface (202a) of the substrate (202). [7] A method according to any one of the preceding claims, further comprising: epitaxially forming (308) a third layer (402) comprising a semiconductor material over a surface (206a) of the first layer (206), wherein epitaxially forming the second layer (208) comprises epitaxially forming the second layer (208) over the first layer (206) and the third layer (402). [8] The method of claim 7, wherein a top surface (402a) of the third layer is disposed over a top surface (202a) of the substrate (202). [9] The method of any one of claims 7 to 8, wherein a thickness (T3) of the third layer (402) is in a range of about 1 nanometer to about 5 nanometers. [10] The method of any one of claims 7 to 9, wherein the semiconductor material of the third layer (402) comprises at least one material selected from a group of materials consisting of SiC and SiCP. [11] A method of manufacturing a semiconductor device, the method comprising: Providing (302) a substrate (202) having a recess (204); epitaxially forming (304) a first layer (206) containing a doped semiconductor material within the recess (204); epitaxially forming (306) a second layer (208) containing an undoped semiconductor material over at least a portion of the recess (204); Forming (310) a mask layer (210) over the second layer (208) and a portion (202P) of the substrate (202); Etching (312) a portion (202P, 210P) of the mask layer (210) disposed over the second layer (208); and Forming (314) an electrical contact (219, 419) over the first layer (206), the method further comprising: epitaxially forming (308) a third layer (402) containing a semiconductor material over a surface (206a) of the first layer (206), wherein epitaxially forming the second layer (208) comprises epitaxially forming the second layer (208) over the first layer (206) and the third layer (402), wherein the third layer (402) completely covers a top surface (206a) of the first layer (206). [12] The method of claim 11, wherein the mask layer (210) comprises a nitride material. [13] The method of claim 11 or 12, wherein the undoped semiconductor material of the second layer (208) comprises undoped silicon. [14] A semiconductor device (500, 600, 700) comprising: a substrate (202) having a recess (204); a first layer (206) containing a doped semiconductor material within the recess (204), wherein a top surface (206a) of the first layer (206) is substantially flush with a top surface (202a) of the substrate (202); and a second layer (208) containing an undoped semiconductor material over at least a portion of the recess (204), wherein a thickness (T2) of the second layer (208) is in a range of about 1 nanometer to about 6 nanometers. [15] A semiconductor device (600; 700) according to claim 14, further comprising: a third layer (402) comprising a semiconductor material disposed between the first layer (206) and the second layer (208). [16] The semiconductor device (500, 600, 700) of any of claims 14 or 15, wherein the undoped semiconductor material of the second layer (208) comprises undoped silicon.

Citation Information

Patent Citations

  • Method for forming an electrical contact between a carrier wafer and the surface of an upper silicon layer of a silicon-on-insulator wafer and electrical device with such an electrical contact

    DE102009014507A1

  • Semiconductor Device and Method for Manufacturing a Semiconductor Device

    DE102013105763A1

  • Semiconductor device and method of forming epitaxial layer

    US20130105861A1

  • Semiconductor devices and methods of fabricating the same

    US20130109144A1

  • Methods for chemical mechanical planarization of patterned wafers

    US20130295752A1