Structure and process for SRAM FinFET device
The fabrication method for SRAM FinFET devices through selective thermal oxidation and epitaxial growth with anchor structures addresses the inefficiencies of existing FinFETs, improving performance by inducing strain and enhancing mobility in gate channels.
Patent Information
- Application Number
- DE102015104604
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2014-04-25
- Filing Date
- 2015-03-26
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2035-03-26
AI Technical Summary
Existing FinFET components, such as SRAM FinFETs, have not been satisfactory in every respect, particularly in terms of complexity and efficiency during IC processing and manufacturing, and there is a need for improved methods to adjust vertical dimensions and inrush current characteristics.
A method for fabricating SRAM FinFET devices involves forming fin structures with selective thermal oxidation to create varying semiconductor oxide structures, using epitaxial growth for material layers, and incorporating periodic anchor structures to induce strain for enhanced performance, along with high-k/metal gate stacks and source/drain regions.
The method achieves improved device performance by inducing mechanical tension and strain in the gate channel regions, enhancing mobility and integration flexibility, thereby addressing the limitations of existing FinFET technologies.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND
[0001] The semiconductor integrated circuit (IC) industry has experienced exponential growth. Technical Advances in IC materials and IC design have produced IC generations, where each generation produces smaller and more complex circuits than the previous generation. As ICs have evolved, functional density (i.e. i.e. the number of interconnected components per chip area) has generally increased, while the Geometry size (i.e. the smallest component (or line) that can be formed by means of a manufacturing process This process of scaling down generally realizes benefits by reducing the Increases production efficiency and reduces production-related costs.
[0002] Such downscaling has also increased the complexity of processing and manufacturing ICs; and thus For these advances to be realized, similar developments in IC processing and manufacturing are necessary. For example, a three-dimensional transistor, such as a Static Random-Access Memory (SRAM) fin field-effect Transistor (FinFET) to replace a planar transistor. Although the existing FinFET Devices and methods for manufacturing SRAM FinFET devices generally for their intended purposes have been sufficient, they have not proved satisfactory in all respects.
[0003] US 2008 / 0128796 A1 discloses a semiconductor structure and its manufacturing method comprising several FinFETs with different vertical dimensions for the semiconductor lamellae. One implant species is inserted into a lower part selected semiconductor lamellae where a reduced vertical dimension is desired. The lower part the selected semiconductor lamellae with implant species is selectively converted to the semiconductor material without the implanted species etched, ie to the semiconductor material in the upper part of the semiconductor lamella and other semiconductor lamellae without the implanted species. On the same semiconductor substrate, FinFETs with lamellae with full vertical dimension and high inrush current and FinFETs with fins with reduced vertical dimension and low By adjusting the depth of the implant species, the vertical dimension of the semiconductor laminations can be selected FinFETs.
[0004] Further prior art is known from DE 10 2013 103 798 A1, US 8,582,352 B2, US 2013 / 0292777 A1, US 8,035,199 B2 and US 7,018,876 B2. The invention is defined in the claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] Aspects of the present disclosure are best understood from the following detailed description understood when read in conjunction with the accompanying figures. It is pointed out that according to In accordance with common industry practice, various structural elements are not drawn to scale. The dimensions Illustrated structural elements can be enlarged as needed in the interest of clarity of the discussion or reduced in size. Fig. 1 is a flowchart of an exemplary method for fabricating an SRAM FinFET device according to some embodiments. Fig. 2A is a schematic perspective view of an exemplary SRAM FinFET device that processes, according to some embodiments. Fig. 2B is a cross-sectional view of an exemplary FinFET device taken along line AA in Fig. 2A during Manufacturing stages carried out according to the procedure of Fig. 1. Fig. 3A is a schematic perspective view of an exemplary SRAM FinFET device that processes, according to some embodiments. Fig. 3B is a cross-sectional view of an exemplary SRAM FinFET device taken along line AA in Fig. 3A during manufacturing stages carried out according to the procedure of Fig. 1. Figures 4A and 4B are schematic perspective views of an SRAM FinFET device that processes, according to some embodiments. Fig. 5 is a cross-sectional view of an exemplary SRAM FinFET device taken along line AA in Fig. 4A during manufacturing stages carried out according to the procedure of Fig. 1. Fig. 6A is a cross-sectional view of an exemplary SRAM FinFET device taken along line AA in Fig. 4A during manufacturing stages carried out according to the procedure of Fig. 1. Fig. 6B is a cross-sectional view of an exemplary SRAM FinFET device taken along line BB in Fig. 4B during manufacturing stages carried out according to the procedure of Fig. 1. Figures 7A and 7B are schematic perspective views of an SRAM FinFET device that processes, according to some embodiments. Figures 8A and 8B are schematic perspective views of an SRAM FinFET device that processes, according to some embodiments. Fig. 8C is a cross-sectional view of an exemplary SRAM FinFET device taken along line AA in Fig. 8A during manufacturing stages carried out according to the procedure of Fig. 1. Fig. 8D is a cross-sectional view of an exemplary SRAM FinFET device taken along line BB in Fig. 8B during manufacturing stages carried out according to the procedure of Fig. 1. Fig. 9A is a cross-sectional view of an exemplary SRAM FinFET device taken along line AB-AB in Fig. 8A during manufacturing stages carried out according to the procedure of Fig. 1. Fig. 9B is a cross-sectional view of an exemplary SRAM FinFET device taken along line BB-BB in Fig. 8B during manufacturing stages carried out according to the procedure of Fig. 1. Figures 10A and 10B are schematic perspective views of an SRAM FinFET device that processes, according to some embodiments. Figures 11A and 11B are schematic perspective views of an SRAM FinFET device that processes, according to some embodiments. Figures 12A and 12B are schematic perspective views of an SRAM FinFET device that processes, according to some embodiments. Fig. 13A is a cross-sectional view of an exemplary SRAM FinFET device taken along line AB-AB in Fig. 12A during manufacturing stages carried out according to the procedure of Fig. 1. Fig. 13B is a cross-sectional view of an exemplary SRAM FinFET device taken along line BB-BB in Fig. 12B during manufacturing stages carried out according to the procedure of Fig. 1. DETAILED DESCRIPTION
[0006] The following disclosure provides many different embodiments or examples for implementing various features of the invention. The following are concrete examples of components and arrangements described in order to simplify the present disclosure. For example, the formation of a first structural element above or on a second structural element in the following description embodiments in which the first and second structural elements are formed in direct contact, and can also Embodiments in which additional structural elements between the first and second structural elements so that the first and second structural elements are not necessarily in direct contact. In addition, the present disclosure may use reference numbers and / or letters in the various examples This repetition is for the purpose of simplicity and clarity and does not automatically create a Relationship between the various embodiments and / or configurations discussed.
[0007] The present disclosure relates to (but is not limited to) a fin field effect transistor (FinFET)- Component. The FinFET component can, for example, be a complementary metal oxide semiconductor (CMOS) component, which is a P-type metal oxide semiconductor (PMOS) FinFET device and an N-type metal oxide semiconductor (NMOS) FinFET component. The following disclosure continues with a FinFET example to illustrate various Embodiments of the present invention. It should be understood, however, that the application is not limited to to a specific type of component, unless expressly claimed otherwise.
[0008] Fig. 1 is a flowchart of a method 100 for manufacturing an SRAM FinFET device 200 according to some embodiments. It is understood that additional steps may be implemented before, during, and after the method and that some of the steps described may be replaced or can be omitted. The SRAM FinFET device 200 and the method 100 for manufacturing such a are described together with reference to the different characters.
[0009] Turning to Figures 1 and 2A-2B, the method 100 begins at step 102 by providing a Substrate 210. Substrate 210 may include a bulk silicon substrate. Alternatively, substrate 210 may include a elementary semiconductor, such as silicon or germanium in a crystalline structure, a compound semiconductor, such as silicon germanium, silicon carbide, gallium arsenic, gallium phosphide, indium pho sphide, indium arsenide and / or indium antimonide or combinations thereof.
[0010] In another embodiment, the substrate 210 has a silicon-on-insulator (SOI) structure with a Insulator layer in the substrate. An exemplary insulator layer may be a buried oxide layer (Buried Oxide Layer, BOX). The SOI substrate can be separated using a separation by implantation of oxygen (SIMOx), wafer bonding and / or other suitable processes.
[0011] In the present embodiment, the substrate 210 includes a first semiconductor material layer 212, a second Semiconductor material layer 214 disposed over the first semiconductor material layer 212, and a third Semiconductor material layer 216 disposed over the second semiconductor material layer 214. The second and third Semiconductor material layer 214 and 216 are different from each other. The second semiconductor material layer 214 has a first lattice constant, and the third semiconductor material layer 416 has a second lattice constant which is different from the first Lattice constant is different. In the present embodiment, the second semiconductor material layer 214 contains Silicon germanium (SiGe), and both the first and third semiconductor material layers 212 and 216 contain Silicon. In various examples, the first, second, and third semiconductor material layers 212, 214, and 216 Germanium (Ge), Silicon (Si), Gallium Arsenide (GaAs), Aluminum Gallium Arsenide (AlGaAs), Silicon Germanium (SiGe), Gallium arsenide phosphide (GaAsP) or another suitable material. In the present embodiment the second and third semiconductor material layers 214 and 216 are deposited by epitaxial growth, which is known as a blanket channel epi. In various examples, the epitaxial processes include CVD Deposition techniques (e.g. vapor phase epitaxy (VPE) and / or ultra-high vacuum CVD (UHV-CVD)), Molecular beam epitaxy and / or other suitable processes.
[0012] The substrate 210 may contain various doped structural elements depending on the design requirements as is known to those skilled in the art. In some embodiments, the substrate 210 may, depending on the Design requirements (for example, p-type substrate or n-type substrate) contain different doped regions. In In some embodiments, the doped regions may be doped with p-type or n-type dopants. For example, the doped regions can be doped with p-type dopants, such as boron or BF2; n-type dopants, such as For example, phosphorus or arsenic, and / or combinations thereof. The doped regions can be for an n-type FinFET (NFET) or alternatively configured for a p-type FinFET (PFET).
[0013] Turning to Figures 1 to 3A-3B, the method 100 proceeds to step 104 where a first Fin structure 220 and trenches 230 are formed in the substrate 210. The first fin structure 220 has a first width w1 in a range of about 4 nm to about 10 nm. In one embodiment, a patterned fin hard mask (Fin Hard Mask, FHM) layer 222 is formed over the substrate 210. The structured FHM layer 222 contains Silicon oxide, silicon nitride, silicon oxynitride or other suitable dielectric material. The structured Hardmask layer 222 may contain a single material layer or multiple material layers. The structured FHM Layer 222 can be formed by: depositing a material layer by thermal oxidation, chemical Chemical vapor deposition (CVD), atomic layer deposition (ALD) or any other suitable process, forming a structured Photoresist (resist) layer through a lithography process, and etching the material layer through the openings of the structured photoresist layer for forming the structured FHM layer 222.
[0014] An exemplary photolithography process may include: forming a photoresist layer, exposing the Resists through a lithography exposure process, performing a firing process after exposure, and developing the photoresist layer to form the patterned photoresist layer. The lithography process can alternatively be performed by a other technology, such as electron beam writing, ion beam writing, maskless Structuring or molecular printing.
[0015] The substrate 210 is then etched through the patterned FHM layer 222 to form the first fin structure 220 and the trenches 230 in the substrate 210. In a further embodiment, the structured Photoresist layer directly for the patterned FHM layer 222 used as an etching mask of the etching process to form the first Fin structure 220 and the trenches 230 in the substrate 210. The etching process may be a wet etching process or a dry etching process. In one embodiment, the wet etching solution contains a Tetramethylammonium hydroxide (TMAH), an HF / HNO3 / CH3COOH solution or another suitable solution. Each etching process can be tailored to different etching parameters, such as the used Etchant, etching temperature, etching solution concentration, etching pressure, source power, RF bias voltage, RF bias power, etchant flow rate, and / or other suitable parameters. For example, a wet etching solution NH4OH, KOH (potassium hydroxide), HF (hydrofluoric acid), TMAH (tetramethylammonium hydroxide), other suitable Wet etching solutions or combinations thereof. Dry etching processes include a pre-stressed Plasma etching process that uses a chlorine-based chemical composition. Other dry etching gases include CF4, NF3, SF6 and He. Dry etching can also be anisotropic using a mechanism such as DRIE (Deep Reactive Ion Etching).
[0016] In the present embodiment, the etching depth is controlled such that the third and second Semiconductor material layer 216 and 214 are exposed, but the first semiconductor material layer 212 is partially in the trench 230 exposed. Thus, the first fin structure 220 is formed such that it covers the third semiconductor material layer 216 as a upper portion, the second semiconductor material layer 214 as a middle portion and the first semiconductor material layer 212 as a lower portion.
[0017] In some embodiments, the SRAM FinFET device 200 includes an n-type FinFET (NFET) device configured with designated by reference numeral 200A and referred to as the SRAM FinFET device 200A. The SRAM FinFET Device 200 also includes a PFET device designated by reference numeral 200B, which serves as the SRAM FinFET device 200B.
[0018] Turning to Figures 1 and 4A-4B, the method 100 proceeds to step 106 where a structured Oxidation hard mask (OHM) 310 is formed over the substrate 210, including encasing a portion of the first fin structures 220. In the present embodiment, in the NFET 200A, the structured OHM 310 covers a first region 312 and exposes a second region 314 in the substrate 210. In the PFET 200B, the structured OHM 310 the entire first fin structure 220. The structured OHM layer 310 can be silicon oxide, silicon nitride, silicon oxynitride or other suitable dielectric material. The structured OHM Layer 310 may be formed by: depositing a material layer by thermal oxidation, CVD, ALD or a other suitable method, forming a structured photoresist (resist) layer by a lithography process, and etching the material layer through the openings of the patterned photoresist layer to form the patterned OHM layer 310 to form.
[0019] We also turn to Figures 1, 4A and 5. The method 100 proceeds to step 108 where a thermal oxidation process is performed on the SRAM FinFET device 200. In one embodiment, The thermal oxidation process is carried out in an oxygen environment. In a further embodiment, the thermal oxidation process is carried out in a combination of steam and oxygen environment. second region 314 of the NFET 200A, at least external Layers of the first, second and third semiconductor material layers 212, 214 and 216 into first, second and third semiconductor material layers, respectively. third semiconductor oxide structure element 322, 324 and 326 µm. In the first region 312 of the NFET 200A as well as in the entire PFET 200B, the structured OHM 310 prevents oxidation of the first fin structure 220. Therefore, the thermal Oxidation process is called selective oxidation.
[0020] After the thermal oxidation process, the first fin structure 220 in the second region 324 has a different Structure as the first region 312. In the interest of clarity for a better description, the first fin structure 220 in the second region 314 (with the second semiconductor oxide structure element 324) as a second fin structure 320 Thus, the second fin structure 320 has the third semiconductor material layer 216 as its upper portion, the second semiconductor material layer 214, with the second semiconductor oxide structure element 324 on its outer layer, as its middle section, and the first semiconductor material layer as its lower section.
[0021] In the present embodiment, the thermal oxidation process is controlled such that the second Semiconductor material layer 214 oxidizes much faster than the first and third semiconductor material layers 212 and 216. Or In other words: Compared to the second semiconductor oxide structure element 324, the first and third Semiconductor oxide structural element 322 and 326 is quite thin. As an example, the thermal oxidation process is shown on the SRAM FinFET device 200 in a H2O reaction gas having a temperature in the range of about 400°C to about 600°C and carried out under a pressure in the range of about 1 atm to about 20 atm. After the oxidation process, a Cleaning process is performed to remove the first and third semiconductor oxide structure elements 322 and 326. The Cleaning process can be carried out using dilute hydrogen fluoride (DHF) acid.
[0022] In the present example, the second semiconductor oxide structure element 324 extends in the vertical direction, wherein a horizontal dimension varies from the top to the bottom of the second semiconductor material layer 214. We remain with the present example. The horizontal dimension of the second semiconductor oxide structural element ments 324 reaches its maximum, called a first width w1, and decreases to near zero as it approaches the Top and bottom surfaces of the second semiconductor oxide features 324, resulting in an olive shape in a Cross-sectional view. By tuning the thermal oxidation process, selecting a composition and thickness of the second semiconductor material layer 214 and adjusting the oxidation temperature, a second target width w2 of the second semiconductor oxide structure element 324, which provides adequate mechanical stress to the third Semiconductor material layer 216 in the first fin structure 220, wherein a gate channel is formed under a gate region to define what will be described later.
[0023] In one embodiment, the second semiconductor material layer 214 contains silicon germanium (SiGex1), and both Both the first and third semiconductor material layers 212 and 216 contain silicon (Si). The subscript x1 is a first Ge composition in atomic percent, and they are adjusted to achieve a given volume expansion target In one embodiment, x1 is selected in a range of about 20% to about 85%. An outer layer of the SiGex1 layer 214 is oxidized by the thermal oxidation process, whereby the silicon germanium oxide (SiGeO) structural element 324 is formed. The second width w2 of the SiGeO structural element 324 lies in a range of about 3 nm to 10 nm. A central portion of the SiGex1 layer 214 changes to a second Ge composition x2, which is much higher than x1. The size and shape of the central section of SiGex2 vary according to the Process conditions, such as thermal oxidation temperature and time. In addition, the second Composition x2 in the central section higher than in other sections, such as an upper section, a lower section, a left section and a right section.
[0024] Turning to Figures 1 and 6A-6B, the method 100 proceeds to step 110 where a Dielectric layer 410 is deposited over the substrate 210, including filling the trench 230 both in the NFET 200A as well as in the PFET 200B. First, the patterned OHM layer 310 is removed by an etching process, as for example, a selective wet etching process. The dielectric layer 410 may be silicon oxide, silicon nitride, silicon oxynitride, other suitable materials, or combinations thereof. The dielectric layer 410 may by CVD, physical vapor deposition (PVD), ALD, thermal oxidation, other suitable techniques or a combination of these can be separated.
[0025] Turning to Figures 1 and 7A-7B, the method 100 proceeds to step 112 where the NFET 200A is a structured hard mask (HM) layer 415, whereby a third fin structure 440 in the PFET component 200b is formed. The structured HM layer 415 may be silicon nitride, silicon oxynitride, silicon carbide or another suitable dielectric material. The structured HM layer 415 can be similar to the structured OHM layer 310 may be formed in step 106. In the present embodiment, the structured HM- Layer 415 covers the NFET device 200A and leaves the PFET device 200B uncovered.
[0026] In the PFET device 200B, the third semiconductor material layer 216 in the first fin structure 220 is formed by a suitable etching process, such as a selective wet etching process, a selective Dry etching or a combination thereof. In the present embodiment, the recessing process is controlled that the remaining third semiconductor material layer 216 is set to a first height h1 in order to provide more The fourth semiconductor material layer 430 is then deposited over the recessed third Semiconductor material layer is deposited to form a third fin structure 440. The fourth semiconductor material layer 430 can be deposited by epitaxial growth. The epitaxial process can include CVD deposition techniques, Molecular beam epitaxy and / or other suitable processes. The fourth semiconductor material layer 430 may Germanium (Ge), Silicon (Si), Gallium Arsenide (GaAs), Aluminum Gallium Arsenide (AlGaAs), Silicon Germanium (SiGe), Gallium arsenide phosphide (GaAsP) or another suitable material. In the present embodiment, the fourth semiconductor material layer 430 is the same as the second semiconductor material layer 214, SiGe. Thus, the third Fin structure 440 is formed to have the fourth semiconductor material layer 430 as its upper portion, which third semiconductor material layer 216 as its upper middle section, the second semiconductor material layer 214 as has its lower middle portion and the first semiconductor material layer 212 as its lower portion.
[0027] Thereafter, a CMP process may be carried out to remove excess material of the fourth semiconductor material layer 430 and planarize the top surface of the PFET device 200B. The HM layer 415 in the NFET Device 200A is removed by a suitable etching process, such as a wet etching process, a Dry etching process or a combination thereof.
[0028] Turning to Figures 1 and 8A-8E, the method 100 proceeds to step 114 by depositing the dielectric layer 410 is recessed in both the NFET device 200A and the PFET device 200B. First, the structured HM layer 415 is removed from the NFET device 200A by a suitable etching process, such as For example, a selective wet etching process or a selective dry etching process. The dielectric layer 410 is then recessed in both the NFET device 200A and the PFET device 200B to form the upper portion of the first fin structure 220 (in the NFET device 200A) and the upper portion of the third fin structure 440 (in the PFET device 200B). In the present embodiment, the recess processes are controlled that a top side of the remaining dielectric layer 410 over the second semiconductor material layer 214 has a first distance d1 to increase process integration flexibility. In the present embodiment, the remaining dielectric layer 410 in the trench 230 Shallow Trench Isolation (STI) structural elements.
[0029] In some embodiments, the SRAM FinFET device 200 includes source / drain (S / D) regions and gate Regions. We will stick with this embodiment. One of the S / D regions is a source region, and another of the S / D regions is a drain region. The S / D regions are separated by the gate region. In the interest of clarity for a For better description, the S / D regions and the gate regions in the NFET device 200A are referred to as the first S / D Regions 450A and first gate regions 460A, and the S / D regions and the gate regions in the PFET Device 200B are referred to as second S / D regions 450B and second gate regions 460B.
[0030] We turn to Fig. 9A. In the NFET device 200A, the first S / D regions 450A are separated by the first Gate regions 460A. In the present embodiment, the first S / D region 450A includes a first Subset of the first S / D regions 450AA and a second subset of the first S / D regions 450AB. The first subset of the first S / D regions 450AA is formed in the first region 312, and the second subset of the first S / D Regions 450AB are formed in both the first region 312 and the second region 314 such that the first region 312 is in the middle and the second region 314 is symmetrical next to the first region 312 The first gate regions 360A are formed in the second region 314. The second region 314 contains the second fin structure 320. The first region 312 contains the first fin 220.
[0031] In the present embodiment, the second semiconductor material layer 214 in the first region 312 is formed as a Anchor 470. The second subset of the first S / D region 450AB has a first space s1. A difference Between a width of the anchor 470 and the first space s1 there is a second space s2. The second space s2 has about 10% to about 25% of the size of the first space s1. The armature 470 is designed to move periodically between two first Gate regions 460A, such as every two first gate regions 460A or every three first gate regions 460A or all four first gate regions 460A and so on.
[0032] Turning to Fig. 9B, in the PFET device 200B, the second S / D regions 450B are formed by the second Gate regions 460B are separated. The second S / D regions 450B and the second gate region 460B are formed in the first Region 312 is formed. The first region 312 contains the first fin structure 220.
[0033] Turning to Figures 1 and 10A-10B, the method 100 proceeds to step 116 where a gate stack 510 and sidewall spacers 520 on sidewalls of the gate stack 510 in the first and second gate regions 460A and 460B. In one embodiment, using a gate-last process, the gate Stack 510 is a dummy gate and will be replaced by the final gate stack in a subsequent phase. More precisely said, the dummy gate stacks 510 are later to be replaced by a high-k dielectric layer (HK) and a metal Gate electrode (MG) is replaced after the thermal high temperature processes, such as thermal annealing for an S / D activation during source / drain formation. The dummy gate stack 510 is formed on the substrate 210 formed and is partially over the second fin structure 320 in the first gate region 460A and the third Fin structure 440 is arranged in the second gate region 460B. In one embodiment, the dummy gate stack includes 510, a dielectric layer 512, an electrode layer 514 and a gate hard mask (GHM) 516. The dummy gate Stack 510 is formed by a suitable process including deposition and patterning. The patterning process also includes lithography and etching. In various examples, the deposition CVD, physical vapor deposition (PVD), ALD, thermal oxidation, other suitable techniques or a combination The lithography process includes photoresist (or resist) coating (for example, spin coating), Soft burning, mask alignment, exposure, post-exposure burning, photoresist development, rinsing, Drying (for example, hard firing), other suitable processes and / or combination nations of it. The etching process includes dry etching, wet etching and / or other etching methods (for example, reactive ion etching).
[0034] The dielectric layer 512 contains silicon oxide. Alternatively or additionally, the dielectric layer 512 silicon nitride, a high-k dielectric material, or another suitable material. Electrode layer 514 may contain polycrystalline silicon (polysilicon). The GHM 516 contains a suitable dielectric material, such as silicon nitride, silicon oxynitride, or silicon carbide. The sidewall spacers 520 may be a dielectric material such as silicon oxide, silicon nitride, silicon carbide, silicon oxynitride or Combinations thereof. The sidewall spacers 520 may contain multiple layers. Typical Formation methods for the sidewall spacers 520 include depositing a dielectric material over the gate stack 510 and a subsequent anisotropic etchback of the dielectric material. The etchback process can include multi-step etching to achieve etch selectivity, flexibility, and desired over-etch control.
[0035] Turning again to Figures 1 and 10A-10B, the method 100 proceeds to step 118 where first S / D Structural elements 610A in the first S / D regions 450A and second S / D structural elements 610B in the second S / D regions 450B are formed. In one embodiment, the first S / D structural elements 610A are formed by Omitting a portion of the upper portion of the first fin structures 220 in the first subset of the first S / D Region 450AA and the second fin structures 320 in the second subset of the first S / D region 450AB. The second S / D structural elements 610B are formed by cutting out a portion of the upper portion of the third Fin structures 440 are formed in the second S / D region 450B. In one embodiment, the first Fin structure 220, the second fin structure 320 and the third fin structure 440 are cut out in an etching process. In In a further embodiment, the first fin structure 220, the second fin structure 320 and the third Fin structure 440 is cut out in various etching processes. In the present embodiment, the Recess process is controlled for the purpose of achieving process integration flexibility so that a section of the third semiconductor material layer 216 in the first fin structure 220 and the second fin structure 320 remains and that a portion of the fourth semiconductor material layer 430 remains in the third fin structure 440.
[0036] The first S / D structure elements 610A and the second S / D structure elements 610B are then epitaxially grown on the recessed first fin structure 220 in the first subset of the first S / D region 450AA, the recessed second Fin structure 320 in the second subset of first S / D region 450AB and the recessed third fin structure 440 grown in the second S / D region 450B. The first and second S / D structural elements 610A and 610B contain Ge, Si, GaAs, AlGaAs, SiGe, GaAsP, or another suitable material. The first and second S / D structural elements 610A and 610B can be formed by one or more epitaxial or epitaxial (epi) processes. The first and the second S / D structural elements 610A and 610B may also be doped, and may, for example, be doped in-situ during epi- processes. Alternatively, the first and second S / D structural elements 610A and 610B are not doped in-situ doped, and implantation processes (ie, an interface implantation process) are carried out to form the first and the second S / D structural elements 610A and 610B.
[0037] In one embodiment, the first S / D structural elements 610A are formed by the epitaxially grown Si layer, which is doped with carbon to form Si:Cz, as a lower portion of the first S / D structural elements 610A and by the epitaxially grown Si layer doped with phosphorus to form Si:P as an upper portion of the first S / D Structural elements 610A are formed, where z is a carbon composition in atomic percent. In one embodiment z is in a range of about 0.5% to about 1.5%. The Si:Cz has a thickness that is in a range of about 5 nm to about 15 nm. The Si:P has a thickness that ranges from about 20 nm to 35 nm. In another Embodiment, the second S / D structural elements 610B are formed by the epitaxially grown SiGe layer, which doped with boron to form SiGeαB5, where α is a germanium composition in atomic percent. In a embodiment, α is in a range of about 60% to about 100%.
[0038] Turning to Figures 1 and 11A-11B, the method 100 proceeds to step 120 where an interlayer Dielectric (ILD) layer 720 is formed on the substrate 210 between the gaps of the dummy gate stacks 510. The ILD layer 720 contains silicon oxide, silicon oxynitride, low-k dielectric material, or other suitable dielectric materials. The ILD layer 720 may be a single layer or alternatively multiple layers The ILD layer 720 is formed by a suitable technique, such as CVD, ALD and Spin coating (SOG). A chemical mechanical polishing (CMP) process can then be performed to remove excess ILD layer 720 and the top of the SRAM FinFET to planarize component 200.
[0039] Turning also to Figures 1 and 11A-11B, the method 100 proceeds to step 122 where the Dummy gate stack 510 in the first gate region 460A may be removed to form one or more first gate trenches 810A and removed in the second gate region 460B to form one or more second gate trenches 810B The upper portion of the second fin structure 320 is exposed in the first gate trench 810A, and the upper portion of the third fin structure 440 is exposed in the second gate trench 810B. The dummy gate stacks 510 are etching process (such as a selective wet etching or a selective dry etching) which is used is designed to provide adequate etch selectivity with respect to the third semiconductor material layer 216 in the first gate trench 810A and the fourth semiconductor material layer 430 in the second gate trench 810B. The etching process may include one or several etching steps with respective etchants. The gate hardmask layer 516 and the spacers 520 are also removed. Alternatively, the dummy gate stack 510 may be removed through a series of processes, such as a photolithography patterning and etching process.
[0040] Turning to Figures 1 and 12A-12B, the method 100 proceeds to step 124 where a first and a second high-k / metal gate (HK / MG) stack 910A and 910B are formed over the substrate 210, including a Enclosing a portion of the second fin structure 320 in the first gate trench 810A or a portion of the third Fin structure 440 in the second gate trench 810B. The first and second HK / MG stacks 910A and 910B include a Gate dielectric layer and a gate electrode on the gate dielectric. In one embodiment, the gate Dielectric layer a dielectric material layer with a high dielectric constant (HK dielectric layer - larger than that of the thermal silicon oxide in the present embodiment), and the gate electrode contains metal, Metal alloy or metal silicide. The formation of the first and second HK / MG stacks 910A and 910B contains Depositions to form various gate materials and a CMP process to remove the excess gate Materials and planarizing the top surface of the NFET device 200A and the PFET device 200B.
[0041] In one embodiment, the gate dielectric layer includes an interfacial layer (IL) formed by a suitable process, such as atomic layer deposition (ALD), CVD, thermal oxidation or Ozone oxidation. The IL contains oxide, HfSiO and oxynitride. A HK dielectric layer is deposited on the IL by a suitable technology such as ALD, CVD, metal-organic CVD (MOCVD), physical vapor deposition (PVD), another suitable technique or a combination thereof. The HK dielectric layer may contain: LaO, AlO, ZrO, TiO, Ta2O5, Y2O3, SrTiO3 (STO), BaTiO3 (BTO), BaZrO, HfZrO, HfLaO, HfSiO, LaSiO, AlSiO, HfTaO, HfTiO, (Ba,Sr)TiO3 (BST), Al2O3, Si3N4, oxynitride (SiON) or other suitable materials. The gate dielectric layers enclose the upper Section of the second fin structures 320 in the first gate region 460A and the upper section of the third Fin structures 440 in the second gate region 460B.
[0042] A metal gate (MG) electrode may comprise a single layer or alternatively a multilayer structure, such as Example of different combinations of a metal layer with a trigger work to increase the component performance (Release work metal layer), a lining layer, a wetting layer, an adhesion layer and a conductive layer of metal, metal alloy or metal silicide. The MG electrode can be Ti, Ag, Al, TiAlN, TaC, TaCN, TaSiN, Mn, Zr, TiN, TaN, Ru, Mo, Al, WN, Cu, W, any suitable materials or a combination thereof. The MG- Electrode can be formed by ALD, PVD, CVD or any other suitable process. The MG electrode can for the NFET 200A and the PFET 200B with different metal layers. A CMP process can be performed to remove excess material from the MG electrode.
[0043] Turning to Fig. 13A, in the NFET device 200A, the first gate region 460A includes the first HM / MG 910A, which envelops the upper portion of the second fin structure 320. The second fin structure 320 includes the Semiconductor material layer 216 as its upper portion, the second semiconductor material layer 214 (with a semiconductor oxide structural element 324 at its outer layer) as its middle section, and the first semiconductor material layer 212 as its lower portion. Therefore, during the formation of the second semiconductor oxide structure element 324 in the second fin structure 320 induces an adequate strain in the first gate region 460A, which increases the mobility in a channel region in the first gate region 460A. In the present embodiment, the second subset of the first S / D region 450AB is provided with the armatures 470 in a periodic arrangement, which in the first gate region 460A-induced stretching is enhanced and mobility in the channel region is increased. The second space s2 creates an adequate separation between the armature 470 and the first gate region 460A to avoid adverse effects such as induced interface states in the first HK / MG 910 by the armature 470.
[0044] Turning to Fig. 13B, in the PFET device 200B, the second S / D region 450B is defined by the second gate Region 460B. The second gate region 460B contains the second HK / MG 910B, which forms the upper section of the third fin structure 440. The third fin structure 440 contains the fourth semiconductor material layer 430 as its upper section, the third semiconductor material layer 216 as its upper middle section, the second semiconductor material layer 214 as its lower middle portion, and the first semiconductor material layer 212 as its lower portion.
[0045] The SRAM FinFET device 200 may be subjected to further CMOS or MOS technological processing to form various structural elements and regions known to those skilled in the art. For example, subsequent processing of various contacts, vias, lines and multilayer interconnects Structural elements (for example, metal layers and interlayer dielectrics) are formed on the substrate 210, which are configured to connect the various structural elements to form a functional circuit that contains one or more SRAM FinFET field-effect transistors. We will stick with this example. A multilayer Interconnect contains vertical interconnect connections, such as vias or contacts, and horizontal interconnect connections, such as metal lines. The various interconnect Structural elements can be implemented using various conductive materials, such as copper, Tungsten and / or silicide. In one example, a damascene and / or dual damascene process is used to To form copper-related multilayer interconnect structure.
[0046] Additional operations may be implemented before, during, and after the method 100, and some above The operations described may be replaced by other embodiments of the method or may be omitted become.
[0047] Based on the above, the present disclosure provides structures of an SRAM FinFET. Structures use the technique of volume expansion and periodic anchor structures in their NFET device, to induce efficient strain in the gate region to improve device performance.
[0048] The present disclosure provides an embodiment of a fin field effect transistor (FinFET) device The device includes a substrate with an n-type FinFET (NFET) region and a p-type FinFET (PFET) region. The device also includes a first fin structure over the substrate in the NFET region, a second Fin structure above the substrate in the NFET region, and a third fin structure above the substrate in the PFET region. The device also includes a first high-k (HK) / metal gate (MG) stack over the substrate in the NFET region, including a wrapper for a portion of the first fin structure. The component also includes a first Subset of Source / Drain (S / D) structural elements adjacent to the first HK / MG stack above the recessed first fin structure and a second subset of S / D structural elements partially over the recessed second Fin structure and partially over the recessed first fin structure around the recessed second fin structure next to another first HK / MG stack. The device also contains a second HK / MG stack above the Substrate in the PFET region, including a cladding of a portion of the third fin structure, and second S / D Structural elements next to the second HK / MG stack above the recessed third fin structure in the PFET region.
[0049] The present disclosure also provides another embodiment of a fin field effect transistor (FinFET) The device includes a substrate with an n-type fin field-effect transistor (NFET) region and a p-type fin field-effect transistor (PFET) region. The device also includes a first fin structure over the Substrate in the NFET gate region. The first fin structure contains an epitaxial silicon (Si) layer as its upper Section and an epitaxial silicon germanium (SiGe), with a silicon germanium oxide (SiGeO) structural element at its outer layer, as its lower section. The component also contains a second fin structure above the Substrate in the NFET region. The second fin structure contains an epitaxial silicon (Si) layer as its upper section and an epitaxial silicon germanium (SiGe) as its lower section. The device also contains a third fin structure above the substrate in the PFET region. The third fin structure contains an epitaxial SiGe layer as its upper section, an epitaxial Si as its middle section, and another epitaxial SiGe layer as its lower section. The device also includes a first subset of source / drain (S / D) regions in a section of the first fin structure, a second subset of S / D regions in a section of the second Fin structure surrounded by the first fin structure, and a second S / D region in a section of the third fin structures.
[0050] The present disclosure also provides a method for fabricating a FinFET. The method comprises providing a substrate having an n-type fin field-effect transistor (NFET) region and a p-type fin field-effect Transistor (PFET) region. The method also includes forming first fin structures in the NFET region and the PFET region. The first fin structure includes a first epitaxial semiconductor material layer as its upper portion, a second epitaxial semiconductor material layer, having a semiconductor oxide structural element on its outer layer, as its middle section, and a third semiconductor material layer as its lower section. The process includes also forming a patterned oxidation hard mask (OHM) over the NFET region and the PFET region to exposing the first fin structure in a first gate region of the NFET region, applying an anneal to form a Semiconductor oxide structural element on the outer layer of the second semiconductor material layer in the first fin structure in the first gate region, depositing a dielectric layer between the first fins, forming a third Fin structure in the PFET device, while the NFET device is covered with a hard mask layer, the Removing the dielectric layer in both the NFET region and the PFET region, forming dummy Gates in a first gate region and a second gate region in the second fin structure, forming first source / Drain (S / D) structural elements in a first S / D region in the first fin structure and in the second fin structure in the NFET region, and forming second S / D structural elements in a second S / D region in the third fin structure in the PFET region.
Claims
1. FinFET device comprising: a substrate (210) having an NFET region (200A) and a PFET region (200B); a first fin structure (320) over the substrate in the NFET region (312); a second fin structure (220) over the substrate in the NFET region (314), wherein the first fin structure (320) and the second fin structure (220) forms a continuous fin; a third fin structure (440) above the substrate in the PFET region (312); a first HK / MG stack, high-k / metal gate stack, (910A) over the substrate in the NFET region, including a Enveloping a portion of the first fin structure (320); a first subset of S / D structural elements, source / drain structural elements, (610A) next to the first HK / MG stack above the first fin structure (320); a second subset of S / D structural elements (610A) partially over the second fin structure (220) and partially above the first fin structure (320), wherein the first HK / MG stack is between the first and the second subset of S / D structural elements (61oA); a second HK / MG stack (910B) over the substrate in the PFET region including a cladding of a section the third fin structure (440); and second S / D structural elements (610B) next to the second HK / MG stack above the third fin structure (440) in the PFET Region; wherein the first fin structure (320) comprises: a first semiconductor material layer (216) as its upper portion; and a second semiconductor material layer (214) having a semiconductor oxide structural element (324) on its outer layer, as its lower portion, wherein the semiconductor oxide structural element (324) forms a thickened region of the first fin structure (320) in the region of the lower section and is not present in the upper section; wherein the second fin structure (220) does not have the semiconductor oxide structural element (324), wherein the second Semiconductor material layer (214) of the second fin structure (220), in which no semiconductor oxide structural element (324) is present, a further first semiconductor material layer (216) is grown, which forms an anchor of the second subset of the S / D structural elements (610A).
2. Component according to claim 1, wherein the second fin structure includes: the first semiconductor material layer (216) as its upper portion; and the second semiconductor material layer (214) as its lower portion.
3. Component according to claim 1 or 2, wherein the third fin structure (440) includes: a third semiconductor material layer (430) as its upper portion; the first semiconductor material layer (216) as its central portion; and the second semiconductor material layer (214) as its lower portion.
4. Component according to one of the preceding claims, wherein the second semiconductor material layer (214) is so is that it oxidizes faster than the first semiconductor material layer (216).
5. Component according to one of the preceding claims, wherein the second subset of the first S / D structural elements (61oA), which is above the second fin structure (220) is formed, from the semiconductor oxide structural element (324) of the first fin structure (320) surrounded by.
6. The component according to claim 5, wherein a width of the semiconductor oxide structural element (324) comprising the first fin structure (320) is in a range of about 10% to about 25% of a width of the first fin.
7. Component according to one of the preceding claims, wherein the second subset of S / D structural elements each every two or three or four first HK / MG stacks.
8. Component according to one of the preceding claims and claim 3, wherein: the first semiconductor material layer contains epitaxial silicon; the second semiconductor material layer contains epitaxial silicon germanium; the semiconductor oxide structural element contains silicon germanium oxide; and the third semiconductor material layer contains epitaxial silicon.
9. A component according to any one of the preceding claims, wherein the first and second S / D structural elements are epitaxially contain grown semiconductor material.
10. Static Random-Access Memory FinFET device containing: a substrate with an NFET region (200A) and a PFET region (200B); a first fin structure (320) over the substrate in the NFET region, the first fin structure including: an epitaxial Si layer (216) as its upper portion; and an epitaxial SiGe (214), having a SiGeO structural element (324) at its outer layer, as its lower portion; a second fin structure (220) over the substrate in the NFET region, the second fin structure including: an epitaxial Si layer (216) as its upper portion; and an epitaxial SiGe (214) as its lower section; a third fin structure (440) above the substrate in the PFET region, the third fin structure including: an epitaxial SiGe layer (430) as its upper portion; an epitaxial Si (216) as its central section; and another epitaxial SiGe layer (214) as its lower portion; a first subset of first S / D regions (610A) in a portion of the first fin structure; a second subset of first S / D regions in (61oA) a section of the second fin structure separated from the first surrounded by a fin structure; and second S / D regions (610B) in a section of the third fin structures.
11. The component of claim 10, further comprising: first gate regions (460A) in a portion of the first fin structure (320) formed by the first subset or the second subset of the S / D region (61oA) are separated; and a first HK / MG stack (910A) in the first gate region, including a cladding of a portion of the upper Section of the first fin structure (320).
12. The device according to claim 11, wherein the second subset of S / D structural elements (610A) comprises every two first HK / MG stack is arranged.
13. The device of claim 11, wherein the second subset of S / D structural elements (610A) comprises all three first HK / MG stack is arranged.
14. The device of claim 11, wherein the second subset of S / D structural elements (610A) comprises all four first HK / MG stack is arranged.
15. Component according to one of claims 10 to 14, wherein a width of the SiGeO structural element (324) comprising the first fin structure (320) is in a range of about 10% to about 25% of a width of the first fin structure.
16. Component according to one of claims 10 to 15, further comprising: a second gate region (460B) in a portion of the third fin structure (440) defined by the second S / D regions is separated; and a second HK / MG stack (910B) in the second gate region, including a cladding of a portion of the upper Section of the third fin structure (440).
17. A component according to any one of claims 10 to 16, wherein the first and second S / D structural elements (610A, 610B) contain epitaxially grown semiconductor material.
18. Procedure comprising: Providing a substrate having an NFET region (200A) and a PFET region (200B); Forming first fin structures (220) in the NFET region and the PFET region, wherein the first fin structure has the following includes: a first epitaxial semiconductor material layer (216) as its upper portion; a second epitaxial semiconductor material layer (214) as its middle section; and a third semiconductor material layer (212) as its lower portion; Forming a patterned oxidation hard mask (310) over the NFET region and the PFET region to form the first to expose fin structure in (220) a first gate region of the NFET region; Applying an anneal to form a semiconductor oxide feature (324) on the outer layer of the second forming a semiconductor material layer in the first fin structure to form a second fin structure (320); Depositing a dielectric layer (410) between the first fin structures (220) and the second fin structures (320); Forming a third fin structure (440) in the PFET region while the NFET region is covered with a hard mask layer (415) is covered; Retaining the dielectric layer (410) in both the NFET region and the PFET region; Forming dummy gates (510) in the first gate region in the NFET region and a second gate region in the second fin structure in the PFET region; Forming first source / drain (S / D) structural elements (610A) in a first S / D region in the first fin structure (220) and in the second fin structure (320) in the NFET; and Forming second S / D structural elements (610B) in a second S / D region in the third fin structure (440) in the PFET Region.
19. The method of claim 18, further comprising: Replacing the dummy gates (510) with a first high-k / metal gate, HK / MG, (9104) in the NFET region, including an enclosing of an upper portion of the first fin structure (220) in the first gate region; and Replacing the dummy gates with a second HK / MG (91oB) in the PFET region, including encapsulation of a upper portion of the second fin structure (320) in a second gate region.
20. The method of claim 18 or 19, wherein forming the third fin structure (440) includes: Removing the upper portion of the first fin structure (220); and epitaxial growth of a semiconductor layer over the recessed first fin structure.
Citation Information
Patent Citations
Integrated circuit devices with voltage-ambient effects and methods of manufacturing the same
DE102013103798A1
Triple gate and double gate finfets with different vertical dimension fins
US20080128796A1
Structure for FinFETs
US20130292777A1
Transistor with vertical dielectric structure
US7018876B2
Semiconductor device and method for manufacturing the same
US8035199B2