MANUFACTURING PROCESS INCLUDING ACTIVATION OF DOTENS

The method of creating lattice vacancies and using LTA for dopant activation in semiconductor devices addresses the challenge of efficient dopant activation in deep junctions and field stop layers, achieving improved electrical performance in IGBTs and diodes.

DE102016114264B4Active Publication Date: 2024-10-24INFINEON TECHNOLOGIES AG
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE102016114264
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2016-08-02
Publication Date
2024-10-24
Estimated Expiration
2036-08-02

AI Technical Summary

Technical Problem

Existing methods for activating implanted dopants in semiconductor devices, such as ion implantation followed by thermal annealing, face challenges in efficiently and selectively activating dopants without damaging the crystal lattice or affecting previously formed structures, particularly in deep junctions and field stop layers of IGBTs and diodes.

Method used

A method involving lattice vacancy creation in a pretreated section of a semiconductor layer, followed by laser thermal annealing (LTA) to activate dopants, where lattice vacancies are generated and then healed by a laser beam, allowing deeper and more efficient dopant activation with controlled dopant density transitions.

Benefits of technology

The method achieves deeper and more efficient activation of dopants, with controlled dopant density transitions, improving the performance of semiconductor devices like IGBTs and diodes by enhancing the electrical properties of deep junctions and field stop layers without significant crystal damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for manufacturing semiconductor devices, comprising: generating lattice vacancies in a pretreated section (710) of a semiconductor layer (700) directly adjacent to a process surface (701), wherein a resulting lattice vacancy density is greater than 1E17 cm-3; implanting dopants at least into the pretreated section (710), wherein the lattice vacancies are generated by implanting impurities through the process surface (701) into a melt section of the semiconductor layer (700), wherein the implanted impurities and / or the implanted dopants pass through an energy filter unit (870) before reaching the semiconductor layer (700), wherein the energy filter unit (870) modifies a vertical distribution of the implanted impurities and / or the implanted dopants in the pretreated section (710) such that the vertical distribution is approximately uniform;and heating, at a lattice vacancy density greater than 1E17cm-3, of the melt section (712) of the semiconductor layer (700) by irradiating the process surface (701) with a laser beam (850) which activates the implanted dopants at least in the melt section (712), wherein the melt section (712) has a vertical extent (v3) that is smaller than a vertical extent (v1) of the pretreated section (710).
Need to check novelty before this filing date? Find Prior Art

Description

BACKGROUND

[0001] Ion implantation involves ionizing, isolating and accelerating dopant atoms and scanning a ion beam containing ionized dopant atoms along a wafer surface. The dopant ions enter the wafer and come to rest below the wafer surface. The depth the implanted ions reach in the wafer is a function of the entry energy of the ions, which in the wafer by electronic interaction and by physical collisions with the host atoms in the wafer. The implanted ions are arranged around a tip on the The ions damage the crystal lattice in a section of the wafer, which they pass by colliding with host atoms and by removing the host atoms from their lattice sites. Implanted dopant atoms that do not occupy regular lattice sites are electrically inactive and have no influence on the electrical properties of the substrate. Typically Heat treatments restore the crystal lattice and electrically activate the dopant atoms by converting them into regular Move grid positions.

[0002] Conventional furnace heating techniques, for example RTP (rapid thermal processing), affect all previously formed structures in the wafer. An LTA (laser thermal anneal) directly heats only a section of the semiconductor crystal and has less influence on previously formed structures in the wafer in a distance from the heated section.

[0003] In an LTA, the absorption depth depends on the wavelength of the laser beam. The absorption depth of a Laser beam with a wavelength of 308 nm is typically 10 nm, and a melting depth down to which the The depth of melting of crystalline silicon by a laser beam with 308 nm is in a range of up to about 500 nm. The melting depth can can be increased to a certain extent by applying anti-reflective coatings or anti-reflective coatings used so that more energy of the laser beam is coupled into the semiconductor substrate.

[0004] The document US 2014 / 0 246 755 A1 describes a method for forming a cathode layer and a Field stop zone on the back of the semiconductor body of a vertical IGBT or a vertical diode. Electron beam treatment creates crystal defects throughout the semiconductor body. Protons are irradiated through the back implanted and activated by a furnace process, whereby the crystal defects created by the electron beam treatment increase the formation rate of proton donors and, moreover, largely heal. The activated proton Donors form the field stop zone. Then, dopant ions are implanted through the back and activated an LTA. The activated dopant ions form a junction between the field stop zone and the back of the semiconductor body a cathode layer.

[0005] From the document DE 10 2009 019 278 A1 it is known that during the ion beam implantation of the dopant for a deep n-buffer of an IGBT inherent lattice defects in the area of ​​the shallow p-emitter of the ions irradiated IGBTs are produced.

[0006] C. Sabatier et al., ´´Laser annealing of double implanted layers for IGBT Power Devices, in RTP'08, 2008, pp.177-181 describe an LTA process for the simultaneous activation of a boron-doped collector layer and a Phosphorus-doped buffer layer of an IGBT. Depending on the laser energy density and the implantation conditions For the LTA, a process window for high activation rates of boron in the melting phase and for Phosphorus in the solid phase.

[0007] There is a need to improve methods for activating implanted dopants. SUMMARY

[0008] The object is achieved by the subject matter of claim 1. Dependent claims relate to further Embodiments.

[0009] A method for manufacturing semiconductor devices comprises implanting impurities or Foreign atoms through a process surface into a semiconductor layer, whereby lattice vacancies (crystal lattice vacancies, Crystal vacancies) in a pretreated section of the semiconductor layer. Dopants are at least implanted into the pretreated section. A melting section of the semiconductor layer is heated by the process surface is irradiated with a laser beam which irradiates the implanted dopants at least in the melt section activated.

[0010] A semiconductor diode comprises a back structure forming a pn junction with an anode layer, and a weakly doped drift zone in the rear structure. A highly doped cathode structure is directly adjacent to a Metal cathode electrode. A field stop layer forms a first transition with the cathode structure and a second transition with the drift zone. A second transition depth of the second transition with respect to a Interface between the metal cathode electrode and the cathode structure is larger than 500 nm, and in the second transition, a dopant density changes by at least one order of magnitude per 50 nm.

[0011] An insulated gate bipolar transistor comprises a backside structure comprising pn junctions with body regions of transistor cells formed on a front side and further comprises a lightly doped drift zone in the rear structure. A highly doped collector structure is directly adjacent to a metal collector electrode. Field stop layer forms a first junction with the collector structure and a second junction with the drift zone. second junction depth of the second junction with respect to an interface between the metal collector electrode and the Collector structure is larger than 500 nm, and at the second transition a dopant density changes by at least one Order of magnitude per 50 nm.

[0012] Those skilled in the art will appreciate additional features and advantages after reading the following detailed description and considering the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The accompanying drawings are included to provide a further understanding of embodiments of the invention, and they are incorporated in and form a part of this disclosure. The drawings illustrate the embodiments of the present invention and together with the description serve to Explain the principles of the invention. Other embodiments of the invention and intended advantages will become immediately appreciated because they are better understood with reference to the following detailed description. Fig. 1A shows a region of a semiconductor substrate illustrating thermal annealing with Laser acting on a pretreated section containing vacancies, after generating of lattice vacancies and implantation of dopants. Fig. 1B is a schematic diagram showing vertical distributions of vacancies and implanted dopant atoms along a line BB of Fig. 1A. Fig. 1C is a schematic cross-sectional view of the semiconductor substrate area of ​​Fig. 1A during an LTA with a melting depth greater than a vertical dimension of the pretreated section. Fig. 1D is a schematic diagram showing a vertical distribution of activated dopants along a line D- D in Fig. 1C shows. Fig. 1E is a schematic cross-sectional view of the semiconductor substrate area of ​​Fig. 1A during an LTA with a melting depth that is smaller than a vertical dimension of the pretreated section. Fig. 1F is a schematic diagram showing a vertical distribution of activated dopants along a line F- F in Fig. 1E shows. Fig. 2A is a schematic diagram showing vertical distributions of implanted and activated dopants -2 to illustrate the effects of an LTA at 4 Jcm. Fig. 2B is a schematic diagram showing vertical distributions of implanted and activated -2 dopants to illustrate the effects of an LTA at 8 Jcm. Fig. 3A is a schematic diagram showing irradiation of a semiconductor substrate with an ion beam passing through an energy filter to illustrate another method for producing to illustrate semiconductor devices. Fig. 3B is a schematic diagram showing vertical distributions of implanted dopants and activated Dopants in the semiconductor substrate shown in Fig. 3A. Fig. 4A is a schematic diagram showing a vertical distribution of lattice vacancies according to a Embodiment showing the lattice vacancies created by a single damage implantation. Fig. 4B is a schematic diagram showing a vertical distribution of lattice vacancies according to a Embodiment showing that the lattice vacancies are created by at least two damage implantations. Fig. 4C is a schematic diagram showing a vertical distribution of lattice vacancies according to a embodiment that creates the lattice vacancies by a single implantation of dopant atoms, where an energy filter is inserted into an implantation beam. Fig. 4D is a schematic diagram showing a vertical distribution of lattice vacancies according to a Embodiment showing the lattice vacancies by at least two implantations of dopant atoms generated. Fig. 5A is a schematic diagram showing vertical distributions of vacancies, implanted Dopants and activated dopants according to one embodiment, relating to a tip at the end of the range of implanted Dopants near the process surface in a pretreated section containing vacancies. Fig. 5B is a schematic diagram showing vertical distributions of vacancies, implanted dopants and activated dopants according to one embodiment, concerning a tip at the end of the Range of implanted dopants in a vertical center of a lattice vacancy containing pretreated section. Fig. 5C is a schematic diagram showing vertical distributions of vacancies, implanted dopants and activated dopants according to one embodiment, concerning a tip at the end of the Range of implanted dopants near the buried edge of the vacancy-containing pretreated section. Fig. 6A is a schematic cross-sectional view of a portion of a semiconductor device containing a doped Target area formed by an LTA, according to one embodiment, wherein the doped target area directly adjacent to the process surface. Fig. 6B is a schematic diagram showing vertical distributions of vacancies, implanted dopants and activated dopants along a line BB- of Fig. 6A. Fig. 6C is a schematic cross-sectional view of a portion of a semiconductor device comprising a LTA formed doped target region, according to one embodiment, wherein the doped target region is in a distance to the process surface. Fig. 6D is a schematic diagram showing vertical distributions of vacancies, implanted dopants and activated dopants along a line BB of Fig. 6C. Fig. 7A is a schematic vertical cross-sectional view of a portion of a semiconductor diode according to a Embodiment relating to a field stop layer with a box-shaped vertical dopant distribution. Fig. 7B is a schematic diagram showing vertical dopant distributions on a backside of the Semiconductor diode of Fig. 7A. Fig. 8A is a schematic vertical cross-sectional view of a portion of an IGBT (Integrated Bipolar Transistor) insulated gate) according to an embodiment relating to a field stop layer with a box-shaped vertical dopant distribution. Fig. 8B is a schematic diagram showing vertical dopant distributions on a backside of the IGBT of Fig. 8A illustrates this. Fig. 9A is a schematic vertical cross-sectional view of a portion of a semiconductor diode according to a Embodiment concerning a CIBH (controlled injection of backside holes, controlled injection of backside holes) Holes) structure with a box-shaped vertical dopant distribution. Fig. 9B is a schematic diagram showing vertical dopant distributions on a backside of the Semiconductor diode of Fig. 9A. Fig. 10A is a schematic vertical cross-sectional view of a portion of an IGBT according to a Embodiment relating to a CIBH structure with a box-shaped vertical dopant distribution. Fig. 10B is a schematic diagram showing vertical dopant distributions on a backside of the IGBT of Fig. 10A illustrates this. Fig. 11A is a schematic vertical cross-sectional view of a region of a semiconductor according to a Embodiment relating to a semiconductor diode with a deeply implanted back emitter. Fig. 11B is a schematic diagram showing vertical dopant distributions on a backside of the Semiconductor diode of Fig. 11A. Fig. 12A is a schematic vertical cross-sectional view of a portion of an IBGT according to a Embodiment relating to a collector layer with a box-shaped vertical dopant distribution. Fig. 12B is a schematic diagram showing vertical dopant distributions on a backside of the IGBT of Fig. 12A illustrates this. Fig. 13A is a schematic vertical cross-sectional view of a portion of a semiconductor diode according to a Embodiment concerning a charge carrier compensation zone. Fig. 13B is a schematic diagram showing vertical dopant distributions on a backside of the Semiconductor diode of Fig. 13A. DETAILED DESCRIPTION

[0014] In the following detailed description, reference is made to the accompanying drawings which form a part of the disclosure and in which, for purposes of illustration, specific embodiments are shown in which the invention can be embodied. It is to be understood that other embodiments used and structural or logical changes can be made without departing from the scope of the present invention. For example, features illustrated for one embodiment or described, in or in connection with other embodiments to achieve yet another It is intended that the present invention encompass such modifications and Modifications are included. The drawings are not to scale and are for illustrative purposes only. Corresponding elements are provided with the same reference numerals in the different drawings, unless something else is determined.

[0015] The terms ´´have´´, ´´contain´´, ´´comprise´´, ´´have´´ and similar terms are open terms, and These terms indicate the presence of the structures, elements or characteristics identified, but exclude the The presence of additional elements or features is not sufficient. The indefinite articles and the definite Articles should include both the plural and the singular, unless the context clearly indicates otherwise. results.

[0016] The term ´´electrically connected´´ describes a permanent low-resistance connection between electrically connected elements, for example a direct contact between the elements in question or a low-resistance connection via a metal and / or a highly doped semiconductor. The term "electrically coupled" comprises one or more intermediate elements designed for signal transmission being arranged between the electrically coupled elements may be present, for example elements that temporarily have a low-resistance connection in a first state and a high-impedance electrical decoupling in a second state. - +

[0017] The figures illustrate relative doping concentrations by indicating ´´ ´´ or ´´ ´´ next to the - Doping type ´´n´´ or ´´p´´. For example, ´´n ´´ means a doping concentration that is lower than the + doping concentration of an ´´n´´-doping region, while an ´´n ´´-doping region has a higher Doping concentration has as an ´´n´´-doping region. Doping regions of the same relative Doping concentrations do not necessarily have the same absolute doping concentration. For example, two different ´´n´´ doping regions can have the same or different absolute doping concentrations have.

[0018] Figures 1A to 1D refer to the activation of dopant atoms in a surface layer of a semiconductor substrate 700a.

[0019] The semiconductor substrate 700a consists of or contains a semiconductor layer 700 made of crystalline Semiconductor material, for example silicon (Si), germanium (Ge), silicon germanium (SiGe), silicon carbide (SiC) or an A B semiconductor. At least a portion of the semiconductor substrate 700a may be formed from a crystal ingot, e.g., by sawing. III V For example, the semiconductor layer 700 may be an epitaxial layer formed by epitaxy on a semiconductor base obtained from a crystal ingot, wherein the semiconductor base after forming the Semiconductor layer 700 is thinned or completely removed.

[0020] In addition to the semiconductor layer 700, the semiconductor substrate 700a may contain further layers of an insulating material, semiconducting material and / or conductive material. For example, the semiconductor substrate 700a may comprise a preprocessed silicon wafer with electronic elements formed on a first side.

[0021] The semiconductor substrate 700a has a planar process surface 701 on a first side and on a opposite side a support surface 702 parallel to the process surface 701. A normal to the Process surface 701 defines a vertical direction. Directions orthogonal to the vertical direction are horizontal Directions.

[0022] Lattice vacancies are formed in a pretreated portion 710 of the crystalline semiconductor layer 700, wherein the pretreated section 710 directly borders the process surface 701. A vertical extension v1 of the pretreated section 710 is at least 500 nm, for example at least 750 nm or at least 1 µm, where a vertical extension v1 of the pretreated section 710 is defined as the distance to the process surface 701 can be determined where a lattice vacancy density (vacancy density, crystal vacancy density, vacancy concentration) on a value which is less than 80% or less than half the difference between a maximum Lattice site density in the pretreated section 710 and an average lattice site density in a section of the Semiconductor layer 700 outside the pretreated section 710 and directly adjacent thereto. The Lattice vacancies include unoccupied regular lattice sites.

[0023] The lattice vacancies can be created, for example, by one or more damage implantations. The implanted Atoms can be dopant atoms such as phosphorus, boron, arsenic, selenium or sulfur atoms or can be auxiliary substances, i.e. i.e. non-doping atoms such as atoms of silicon, germanium or noble gases, ie hydrogen, neon, argon, krypton and xenon. Alternatively or additionally, lattice vacancies can be created by using a biased or biased plasma or irradiation with electrons.

[0024] Dopant atoms may be implanted into the semiconductor layer 700, wherein the dopant atoms are at least pass through a section of the pretreated section 710. For example, a peak 811 is located at the end of the range of the implanted dopant atoms within the pretreated section 710, at the buried edge of the pretreated section 710 or beyond the pretreated section 710. In the embodiment, as shown in Fig. 1A and Fig. 1B illustrates a distance p1 of the implantation tip between a tip 811 at the end of the range and the process surface 701 is smaller than the vertical extent v1 of the pretreated section 710.

[0025] The dopant atoms can be added before the vacancies are created or after the vacancies are created implanted. Implanting the dopant atoms can contribute to the creation of lattice vacancies. Implanting the further impurities increases the density of vacancies to a level that is significantly higher than that produced by the sole implantation of the dopants intended for activation. -3

[0026] Typically, the resulting increased maximum local vacancy density exceeds 1E13 cm , e.g. -3 -3 -3 at least 1E14 cm , at least 1E15 cm or at least 1E16 cm . According to one embodiment, the - 3 maximum local vacancy density at least 1E17 cm .

[0027] Fig. 1A shows the pretreated section 710 of a semiconductor layer 700 of a semiconductor substrate 700a. vertical extent v1 of the pretreated section 710 may be at least 500 nm, for example at least 750 nm or at least 800 nm. The implanted dopant atoms are concentrated in a doped region 720, which is partially overlaps the pre-treated section 710 or which lies mainly or wholly within the pretreated section 710. The dopant concentration N has a peak value N at a peak distance p1 DA pk to the first surface 701.

[0028] Fig. 1B shows a vertical vacancy distribution 901 resulting from a single damage implantation and a vertical implantation dopant distribution 902 of the implanted dopant atoms according to a Embodiment with the lattice vacancies created partly by the implantation of the dopant atoms and partly by Implanting a non-doping auxiliary material, e.g. light atoms.

[0029] When ions of an auxiliary substance, e.g. light ions such as hydrogen ions (protons), pass through the process surface 701 implanted by means of a non-channeled implantation, most of the light ions eventually reach Loads of crystal damage, e.g. lattice vacancies, at a peak distance p to rest, which is a function of the aux acceleration energy. Only a few ions penetrate deeper into the crystal lattice, so that the vacancy density N (x) v beyond the peak distance p decreases abruptly. In the area traversed by the light ions, the vertical aux Lattice vacancy distribution 901 may be approximately constant or increase slightly with increasing penetration depth.

[0030] The total vacancy distribution 904 shows the sum of the vacancies caused by the Damage implantation and dopant implantation. The overall vacancy distribution 904 may include two maxima if the peaks at the end of the range of the two implantations are different distances to the process surface 701.

[0031] According to one embodiment, the pretreated section 710 is not amorphized, ie more than half of the theoretical bonds of a complete crystal lattice exist even before the LTA. A total dopant dose to Generation of the lattice vacancies in the pretreated section 710 is at least a factor of three or even a Magnitude below a threshold above which the crystal is usually considered amorphous.

[0032] The vertical distribution 902 of implantation dopants may have a peak at the end of the range of the Dopant atoms within the pretreated section 710 with a peak value N at a peak distance p1 to pk first process surface 701. A falling edge of the vertical distribution 902 of Implantation dopants facing away from the process surface 701 may have a Gaussian distribution where for boron (B) the vertical implantation dopant distribution 902 is within about 100 nm by a magnitude from the peak value N. A rising edge of the vertical implantation dopant distribution pk 902, the facing the process surface 701 may be flatter than the trailing edge.

[0033] Between the process surface 701 and the tip at the end of the range, the continuous Dopant ions further increase the density of lattice vacancies.

[0034] A laser beam is then applied to the process surface 701 to create a portion of the crystalline semiconductor layer 700 down to a melting depth v3. In Fig. 1C and Fig. 1D, the melting depth v3 greater than the vertical extent v1 of the pretreated section 710, and in Fig. 1E and Fig. 1F the melting depth v3 shallower or not deeper than the vertical extent v1 of the pretreated section.

[0035] Fig. 1C shows a laser beam 850 striking the process surface 701 and forming a melting section 712 of the Semiconductor layer 700 is directly heated. The melting section 712 can at least partially heat the pretreated section 710 In the melting section 712, the laser beam 850 heats the pretreated section 710 to a temperature of at least 1450°C, e.g. at least 1410°C, so that the semiconductor material is heated for at least 100 µs and at most 10 ms liquefied.

[0036] In this example, therefore, a vertical extent or melting depth v3 of the melting section 712 is greater or equal to the first vertical extent v1 of the pretreated section 710, so that a large part of the Crystal damage caused by the damage and dopant implantations is healed.

[0037] The laser beam 850 may have a wavelength in a range of 150 nm to 1100 nm, e.g. 308 nm, and a -2 - 2 energy density of at least 1 Jcm , e.g. 4 Jcm . Unlike heat treatment in a furnace, the LTA does not significantly directly contact areas of the semiconductor substrate 700a at a distance from the pretreated section 710, to Example on an opposite side of the semiconductor layer 700.

[0038] Where in an undamaged crystal lattice a part of the energy applied by a laser beam crystal atoms from their regular lattice sites, the lattice vacancies that lead to the time the LTA is applied, the immediate transfer of dopant atoms from Interstitial sites to regular lattice sites. The transfer of dopant atoms to free lattice sites consumes less energy than replacing occupied lattice sites with dopant atoms. Therefore, a Irradiation with the laser beam 850 triggered heat wave implanted ions in a greater depth of the pretreated Section 710 as in a semiconductor layer without vacancies and even beyond the melting depth. -2

[0039] Where conventionally a typical laser beam 850 with 308 nm and with an energy density of 4 Jcm Dopants are only activated down to a depth of 500 nm, prior damage to the crystal lattice enables greater melting depth and allows activation of dopants by a laser beam with 308 nm and with a -2 Energy density from 4 Jcm down to at least 500 nm, for example at least 750 nm.

[0040] Fig. 1D shows a vertical distribution of 903 activated dopants. The dopants are only present in the melt section 712 between the process surface 701 and the melting depth v3. Implanted dopants outside the Melt section 712, as indicated by the hatched area, remain predominantly at their Interstitial sites, where they are electrically inactive and do not provide electrons or holes.

[0041] From the semiconductor substrate 700a, semiconductor dies for power Semiconductor diodes, power IGFETs and IGBTs.

[0042] The LTA can, to some extent, modify the implantation profile between the tip 811 at the end of the range and the process surface 701, but to a lesser extent than heat treatment in a furnace.

[0043] A falling flank of the vertical distribution 903 of active dopants is comparatively steep, for example, falling by at least one, e.g. two orders of magnitude within less than 50 nm, which is significantly steeper than ordinary sloping flanks of implantation profiles before any heat treatment.

[0044] The effect is achieved without any anti-reflection coating, so that in silicon at least 60% of the Laser beam energy of a 308 nm laser beam is reflected. Increasing the effective depth of the laser beam by Formation of lattice vacancies can be combined with approaches that increase the penetration depth of the LTA by using anti-reflective coatings.

[0045] In Fig. 1E and Fig. 1F, the melting depth v3 is smaller than the first vertical extension v1 of the pretreated Section 710. Compared to the previous example, steeper transitions can be formed at the expense of crystal quality become.

[0046] According to Fig. 1F, the vertical distribution of 903 activated dopants decreases steeply at or near the melting depth v3.

[0047] According to another embodiment, the dopants are also distributed beyond the melting section 712, e.g. over at least 50% of or over the entire vertical extent v1 of the pretreated section 710. With the same vertical distribution 902 of implantation dopants and the same total vacancy distribution 904 as in Fig. 1F, the resulting vertical distribution 903 of active dopants for 0 ≤ x ≤ v3 can be the same as in Fig. 1F, follows the vertical distribution 902 of implantation dopants for v3 < x ≤ v1 and decreases steeply around x = v1.

[0048] Figures 2A and 2B illustrate the effect of lattice vacancies on melting depth.

[0049] Dopant atoms, e.g. boron(B) atoms, are irradiated at approximately the same dose at six different Acceleration energy levels were implanted. The resulting vertical distribution of 912 implanted dopants approximates a ´´box´´ with a comparatively uniform dopant concentration in a doped region, which extends from the process surface at x = 0 to a distance of about 2.5 µm. The vertical distribution 912 implanted dopants also gives an approximation of the shape of the vertical vacancy distribution, where the Vacancy density for 0 < x < 2.5 µm can fluctuate or vary around an average vacancy density.

[0050] Only the vertical distribution of 913 active dopants in Fig. 2A falls at a distance of about 1.0 µm to -2 Process surface 701 and shows that an LTA at a wavelength of 308 nm and an energy of 4 Jcm pretreated section and activates the implanted dopants down to a depth of about 1.0 µm. The vertical distribution of 914 active dopants for the same LTA applied to a semiconductor layer whose Lattice is not damaged or is only damaged by implantation of the dopants intended for its activation, -2 shows that an LTA at a wavelength of 308 nm and an energy of 4 Jcm forms a semiconductor layer which has no significant crystal damage in addition to that caused by the implantation of the activated dopants caused by the melting process, down to a depth of only 400 nm.

[0051] The vertical distribution of 915 active dopants in Fig. 2B shows that an LTA at a wavelength of 308 nm and -2 at an energy of 8 Jcm the semiconductor layer melts and the implanted dopants are released down to a depth of 1.75 µm and the implanted dopants are partially activated down to a depth of about 2.75 µm.

[0052] The vertical distribution of a lattice vacancy density N depends on the method used to generate V Lattice vacancies. Fig. 3A and Fig. 3B refer to a method that uses an energy filter that is an implantation beam is introduced to determine the vertical vacancy distribution and the final vertical to modify the distribution of implantation dopants.

[0053] Fig. 3A shows an energy filter unit 870 based on one or more materials which are sufficiently form stable structures at a thickness at which the materials for particle beams, such as those used for implanting Dopant atoms or auxiliary atoms used to create lattice vacancies are sufficiently permeable.

[0054] For example, the energy filter unit 870 is based on materials that form stable, thin substrates. Energy filter unit 870 can be mainly formed on a layer of crystalline silicon having a thickness in a range of 100 nm to 20 µm, which can be coated with a metal-containing layer to ensure stability, insensitivity and / or scattering properties. Permeable or permeable areas of the energy filter unit 870 can Dampen the energy of passing particles.

[0055] The energy filter unit 870 may be a thin substrate, a membrane or a film with an exposure area 871 which may be planar. In contrast to the exposure surface 871, a structured surface 872 may have depressions and Mesa structures, with a middle level of the depressions and mesa structures facing the exposure surface 871 is parallel. The structured surface 872 can be formed by etching, grinding, sawing, or by processes that use a template or use a stencil or a cast, e.g. by casting, by press forming or by embossing, to be structured.

[0056] The structured surface 872 includes notches 875 extending into the energy filter unit 870, as well as Protrusions or elevations 876 between adjacent notches 875. The notches 875 may have the same vertical and horizontal dimensions or different vertical and / or horizontal dimensions. According to a Embodiment, the notches 875 may have a vertical extent in a range of 100 nm to 10 µm, for example in a range of 0.2 µm to 8 µm.

[0057] Vertical cross sections of the notches 875 and the elevations 876 may be rectangles or quadrilaterals with or without rounded or bevelled edges or corners, triangles with or without a flattened top or columns with rounded or semicircular tops.

[0058] An ion beam 880 containing non-doping auxiliary atoms or dopant atoms, or at least two different ion beams, one of which contains non-doping auxiliary atoms and the other dopant atoms pass through the energy filter unit 870 and hit the process surface 701 of the semiconductor layer 700. The The illustrated embodiment refers to an embodiment with a first ion beam 880, which dopant atoms, and a second ion beam containing a sufficient number of lattice vacancies in a pretreated section 710 with a vertical extension v1, wherein the first ion beam, the second Ion beam or both can pass through the energy filter unit 870. For example, the energy filter unit 870 used to form a graded field stop layer with a smooth dopant profile.

[0059] As shown in Fig. 3B, the energy filter unit 870 of Fig. 3A modifies the distribution of the dopants along the vertical direction perpendicular to the process surface 701 such that over a certain vertical range, which is a function of the vertical extent of the notches 875, the vertical distribution 922 of the implantation dopants for 0 < x < v1 is approximately uniform. The vertical vacancy distribution 921 can also be be comparatively uniform or at least above a threshold value.

[0060] Fig. 3B further shows the vertical distribution 923 of active dopants after an LTA performed in a melt section with a vertical extension v3 that is less than, equal to or greater than the vertical extension v1 of the pretreated section.

[0061] Figures 4A to 4D summarize various vacancy distributions N (x) that are determined by one or more V Implantations can be obtained which include doping implantations or non-doping damage implantations under Use of an auxiliary material, where x is the distance to the process surface 701.

[0062] In Fig. 4A, a vertical vacancy distribution 931 results from a single damage implantation with an acceleration energy that has a peak at the end of the range for the auxiliary material at x = p beyond, equal to the aux or less than the expected melting depth. Around the peak at the end of the range, the distribution of lattice vacancies approximate a Gaussian distribution. In the area traversed by the implanted atoms the vertical vacancy distribution 931 can be approximately uniform or can be assumed to have a minimal Lattice vacancy density N at or near the process surface 701 may increase slightly. V0

[0063] In Fig. 4B, two damage implantations are shown with a first peak at the end of a range at x = p aux1 and a second peak at the end of a range at x = p , which is closer to the process surface than the target melting depth aux2 used to determine the vacancy density N (x) in the region crossed by the implanted ions V The vertical vacancy distribution 941 resulting from the two implantations can be almost uniform distribution of lattice vacancies up to a distance beyond or close to the expected melting depth approximate.

[0064] The vertical vacancy distribution 951 in Fig. 4C may result from implanting an auxiliary material or dopant atoms using an energy filter that reduces the energy of the implanted auxiliary or dopant atoms gradually changes, so that the tip at the end of the range of the implanted ions over a depth is spread, which is defined, for example, by vertical dimensions of notches and elevations of the energy filter. Accordingly, the vertical vacancy distribution 951 shows no significant peak or only a flat The energy filter can be designed to achieve an approximately uniform vacancy distribution of the Penetration depth of the implanted ions between a first distance x01 and a second distance x02 to the process surface 701, where x01 can be 0. The energy filter can have a vertical distribution gradient of the Compensate for lattice vacancies in such a way that a comparatively uniform distribution of lattice vacancies along the vertical direction over a wide range of the expected melting depth.

[0065] In Fig. 4D, the total lattice vacancy distribution 961 results from two dopant implantations, where at least one of the dopant implantations has a peak at the end of the range at a second peak distance p2 beyond the melting depth v3, so that the density of vacancies is decoupled from the activated dopants can be.

[0066] In each of the alternatives discussed, any implantation contributing to the formation of lattice vacancies be masked in such a way that the vertical dopant distributions between at least two different profiles with different Penetration depths can be changed locally. The approach can be used for a lateral variation of rear emitter properties e.g. within the framework of a LEBE (locally enhanced backside emitter) concept or an HDR (high dynamic robustness) concept.

[0067] Fig. 5A to 5C combine an approximately box-shaped vacancy distribution 971 with various Implantation energies for dopants, where the dopant atoms are, for example, boron(B), phosphorus(P), arsenic(As), sulfur can be (S) or selenium (Se) atoms.

[0068] In Fig. 5A, the dopants are shown with a peak at the end of the range at a peak distance p1 close to the process surface. The density 972 of the implanted dopants shows a peak at the end of the range within the pretreated section 710 near the process surface at x = 0. By applying an LTA at -2 a wavelength of 308 nm and an energy density of 4 Jcm, the previously formed lattice vacancies allow The heat wave generated by the laser beam is effective up to a melting depth v3 with respect to the process surface. Laser beam melts a melt section between the process surface at x = 0 and the melt depth v3. During the comparatively short melting time, the implanted dopants are fitted into regular lattice sites and can diffuse to a certain extent in the vertical direction. The vertical distribution of 973 activated dopants decreases steeply at x = v3. Dopants beyond the melting depth v3 remain electrically inactive.

[0069] Fig. 5B refers to an implantation of dopants with a tip at the end of the range approximately in the middle of the pretreated section 710. Compared to the distribution of 974 implanted dopants, the Distribution of 975 activated dopants is flatter and decreases abruptly at the melting depth v3. The hatched area indicates the area or part of dopants that remain electrically inactive.

[0070] In Fig. 5C, the distribution of 976 implanted dopants has a peak at the end of the range with a peak distance p1 near the melting depth v3. The resulting distribution of 977 activated dopants has a sharp drop from near the maximum value.

[0071] The presence of the previously formed lattice vacancies allows the activation of dopants down to a Melting depth v3, which is greater than a melting depth for the same process in the case where the crystal is additionally to the lattice vacancies created by implanting the target dopants, no lattice vacancies or only a contains a comparatively small number of lattice vacancies.

[0072] The method described above can be used to detect steep concentration transitions at a distance greater than 500 nm, e.g. up to 1.5 µm, to a die surface on a front side or on the back side of a semiconductor die to to create sharp unipolar junctions or sharp pn junctions.

[0073] Fig. 6A and Fig. 6B refer to a semiconductor device 500 comprising a semiconductor region 100 of a crystalline semiconductor material such as silicon (Si), germanium (Ge), silicon germanium (SiGe), silicon carbide (SiC) or any AB semiconductor. The semiconductor region 100 has a planar die surface 105 which is III V front or back side. The process described above can be used to form doped regions near the front, near the back or both doped areas on the front and doped areas on the The doped regions can be formed over the entire die surface 105 According to other embodiments, the doped regions are only locally in areas of the die- Surface 105 formed.

[0074] In Fig. 6A, the semiconductor region 100 contains a doped layer 180 that directly borders the die surface 105. The doped layer 180 forms a junction j, which can be a pn junction or a unipolar junction, with a neighboring layer 190.

[0075] A distance between the junction j and the die surface 105 may be at least 500 nm, for example at least 600 nm or at least 800 nm. According to one embodiment, the transition j has a Transition depth a0 of at least 1 µm to the die surface 105.

[0076] In the case of a pn junction, the junction depth a0 is defined at a distance to the die surface 105 where the both complementary dopants compensate each other. For a unipolar junction, the junction depth a0 defined by an average between the mean dopant concentrations in the sections of the doped layer 180 and the adjacent layer 190 directly bordering the transition j.

[0077] Fig. 6B shows that at the junction depth a0 a net dopant concentration N (x) of activated dopants is THERE at least two orders of magnitude each 50 nm. Fig. 6C and Fig. 6D refer to a semiconductor device 500 with a first doped layer 181, which directly borders the die surface 105, and a second, complementarily doped layer 182, which has a first Transition j1 ​​with the first doped layer 181 and a second transition j2 with an adjacent layer 190. None, one of the first and second junctions j1, j2, or both can be a pn junction. Both the first and The second transition j1, j2 are also steep with a change of at least one order of magnitude every 50 nm.

[0078] The first and second transitions j1, j2 can be formed successively in a two-stage process. In a In the first stage, an intermediate doped layer is formed by creating lattice vacancies, dopants implanted and a first LTA with a melting depth corresponding to the second transition depth a2 is performed becomes.

[0079] In a second stage, in a region of the intermediate layer bordering the die surface 105, Lattice vacancies are created, dopants are implanted and a second LTA melts the semiconductor down to the first Transition depth a1 to form the first doped layer 181, with a remaining portion of the intermediate layer forming the second doped layer 182.

[0080] Fig. 6D shows the resulting vertical distributions 983, 984 of activated dopants resulting from the first and second dopant implantations. The vertical distributions 983, 984 of activated dopants show steep Edges at both transitions j1, j2. The implantation of the dopants for the first doped layer 181 hardly influences the distribution of 983 activated dopants of the first dopants in the second doped layer 182.

[0081] The method described above can be applied to doped regions or doped layers on a front side or on the back of a semiconductor. The following embodiments refer to the Doped layers formed on the back of the semiconductor die.

[0082] Fig. 7A and Fig. 7B refer to a semiconductor diode 501. A semiconductor region 100 made of, for example, crystalline Silicon includes an anode region 120 directly adjacent to a first surface 101 of the semiconductor region 100, and a highly doped cathode structure 138, which directly borders a second surface 102, which corresponds to the first surface 101 A metal anode electrode 311 may directly adjoin the anode region 120, which may have a horizontal pn- junction pn0 with a backside structure 130, which forms a weakly doped drift zone 131 with a dopant concentration N. A field stop layer 135 can be arranged between the weakly doped drift zone 131 and the D0 highly doped cathode structure 138 and forms a first junction j1 ​​at a first junction depth a1 with the cathode structure 138 and a second junction j2 at a second junction depth a2 with the drift zone 131. - 3 -3 An average dopant concentration N in the field stop layer 135 can be between 1E14 cm and 1E16 cm, DO where the dopant concentration can be approximately uniform. For example, the field stop layer 135 can be an implantation beam passing through an energy filter unit.

[0083] The first transition depth a1 may be in a range from several tens of nm to about 800 nm. The second Transition depth a2 can be in a range from 100 nm to 3.0 µm, for example in a range from 500 nm to 1.5 µm, lay.

[0084] As shown in Fig. 7B, a vertical donor concentration 985 between the two transition depths a1 > x > a2 box-shaped, where within the field stop layer 135 the donor concentration N depends on the mean D Donor concentration N by a deviation N of not more than 50 % of the mean donor concentration N DØ DV DØ deviates.

[0085] For 0 < x < a1 the vertical donor distribution 985 can be approximately uniform, e.g. if the Cathode structure 138 results from thinning a highly doped base substrate. According to other Embodiments, the range of the vertical donor distribution 985, 986 in the cathode structure can be 138 Gaussian or may result from a superposition of several Gaussian distributions. According to other embodiments the vertical donor distribution 985, 986 may result from any of the methods described above.

[0086] According to the vertical donor distribution 986, both the cathode structure 138 and the Field stop layer 135 is formed by six implantations at different acceleration energies, with the three, the second surface 102 implantations closest to a higher dose than the three more distant implantations With the approximately box-shaped dopant profile of the field stop layer 135, for a given amount electrically active dopants to prevent expansion of a depletion zone towards the metal cathode electrode 321 by the highly doped cathode structure 138, a vertical extension v4 of the field stop layer 135 shorter The thinner the field stop layer 135 is, the lower the switching losses, so that the box-shaped vertical distributions 985, 986 result in a reduction of switching losses. Compared with other methods for forming the Field stop layer 135, the method as described above enables a greater distance of the field stop layer 135 to the second surface 102, so that the cathode structure 138 is thicker and less susceptible to adverse effects caused by, for example, B. cosmic radiation can be induced.

[0087] Fig. 8A and Fig. 8B refer to an IGBT 502 with a field stop layer 135 between a weakly doped drift zone 131 and a more heavily doped collector structure 139, which forms an ohmic contact with a metal Collector electrode 322 along the second surface 102. The drift zone 131 forms first pn junctions pn0 with Body regions 125 of transistor cells TC formed along the first surface 101. The transistor cells TC can be IGFET (Insulated Gate Field Effect Transistor) cells of the amplification type, whose gate electrodes are connected to a Gate terminal G are electrically connected and their source zones are electrically connected to an emitter terminal E are.

[0088] In Fig. 8B, a vertical donor distribution 987 in the area of ​​the field stop layer 135 may be box-shaped. A first junction depth a1 of a first pn junction pn1 between the collector structure 139 and the field stop layer 135 with respect to the second surface 102 may be in a range from 10 nm to 800 nm. A second transition depth a2 of the unipolar junction j2 between a field stop layer 135 and the drift zone 131 with respect to the second Surface 102 can be in a range from 500 nm to 5 µm. In the unipolar transition j2, the Concentration of activated dopants can change by at least two orders of magnitude per 50 nm.

[0089] A vertical acceptor distribution 988 in the collector structure 139 may be box-shaped or Gaussian-shaped as According to other embodiments, the vertical acceptor distribution 988 may consist of a Superposition of several Gaussian distributions resulting from diffusion in a melt, if the Implantations for the collector structure 139 and the field stop layer 135 are activated in the same LTA. vertical acceptor distribution 988 can have a steep falling edge at the first transition depth a1 in the case of two separate LTAs for the field stop layer 135 and the collector structure 139 or can be uniform for 0 > x > a1 be, if the collector structure 139 results from a highly doped base substrate, which before implantation of the Donors to form the field stop layer 135.

[0090] A shift of the area in which steep transitions can be formed to a deeper transition depth provides more degrees of freedom for structuring doped regions in a section of the semiconductor region 100 near the Back.

[0091] Fig. 9A and Fig. 9B refer to a semiconductor diode 501 which has a CIBH (controlled back injection holes) concept. For this purpose, the semiconductor diode 501 contains counter-doped regions 136, e.g. p-islands, p- Stripes or a p-lattice in the field stop layer 135 or between the field stop layer 135 and the cathode structure 138, wherein the p-islands, p-stripes or a p-lattice form part of a CIBH (controlled back injection holes) structure. During a reversal recovery, the counter-doped regions inject 136 holes into the drift zone 138 and avoid the development of a high electric field peak along the Cathode structure 138. The injected holes keep the charge carrier plasma in an area close to the cathode structure 138, slow down the removal of the plasma from the drift zone 131 and thus support a gentle Reversal recovery.

[0092] In the semiconductor diode 501 of Fig. 9A and Fig. 9B, the field stop layer 135 can be formed as described above Before an LTA or in the case of separate LTAs after the formation of the field stop layer 135, the counter-doped Regions 136 and / or the cathode structures 138 are formed by forming an LTA with a previous formation used by the grid vacancy.

[0093] Fig. 9B shows a box-shaped vertical acceptor distribution 990 for the counter-doped regions 136 between the first transition depth a1 and a third transition depth a3 as well as a box-shaped vertical donor distribution 989 for the field stop layer 135 at least between the third transition depth a3 and the second transition depth a2.

[0094] Fig. 10A and Fig. 10B extend the CIBH concept to an IGBT, where the counter-doped regions 136 within the field stop layer 135 with a third and a fourth transition depth a3, a4 with respect to the second surface 102 are formed.

[0095] Fig. 10B shows a vertical acceptor distribution 992, which has a box-shaped area for the counter-doped Areas 136 between the third and fourth transition depths a3, a4 and a Gaussian area for the Collector structure 139, as well as a box-shaped vertical donor distribution 991 for the field stop layer 135 at least between between the first transition depth a1 and the second transition depth a2.

[0096] Fig. 11A and Fig. 11B refer to a semiconductor diode 501 with a vertical extension of the Cathode structure 138 of at least 500 nm, for example at least 600 nm, wherein the cathode structure 138 is formed by using one of the methods as described above. The semiconductor diode 501 has a Semiconductor region 100 with a thickness th1 between the first and second surfaces 101, 102 of at most 100 µm -3 - The average dopant concentration in the drift zone 131 is at least 1E13 cm and can be at most 1E14 cm 3 The drift zone 131 can be formed by epitaxial growth on a highly doped base substrate, which is later removed. After removal of the highly doped base substrate, the highly doped cathode structure 138 is formed by implantation through the second surface 102. By applying one of the methods as above a vertical extension a1 of the highly doped implanted cathode structure 138 greater than 500 nm can be described, for example, larger than 750 nm. Thicker cathode structures 138 are less susceptible to defects caused by, for example, caused by cosmic radiation.

[0097] The vertical donor distribution 993 in Fig. 11B shows a comparatively steep transition at a comparatively deep transition depth a1.

[0098] Fig. 12A and Fig. 12B meet equivalent considerations about an implanted field stop layer 135 of a IGBT 502.

[0099] The semiconductor diode of Fig. 13A contains a charge carrier compensation zone 137 which is located between the drift zone 131 and the cathode structure 138, as a further example of a special shaping of Doping gradients near the second surface 102.

[0100] A dopant concentration in the charge carrier compensation zone 137 is higher than in a typical If, for example, cosmic radiation triggers a local avalanche breakdown through impact ionization, which Drift zone 131 is locally flooded with charge carriers, and electrons move towards the cathode electrode 321, the ionized donor atoms in the charge carrier compensation zone compensate the electrons and dampen a local electric field, so that no further formation of charge carriers can be triggered at the back. -3 - 3 Minimum dopant concentration in the charge carrier compensation zone 137 is between 2E16 cm and 1E17 cm -3 and a maximum dopant concentration in a range of 1E18 to 5E18 cm .

[0101] According to Fig. 13B, a gradient ΔN / Δx of a vertical donor distribution is 995 in the direction of D -4 second surface 102 at most 2E21 cm within the charge carrier compensation zone 137. The charge carrier Compensation zone 137 can be used in an IGBT with a p-doped collector structure instead of the n-doped Cathode structure 138 can be implemented.

Claims

1. A method of manufacturing semiconductor devices, the method comprising: Creating lattice vacancies in a pretreated section (710) of a semiconductor layer (700) which is directly connected to a -3 process surface (701), wherein a resulting vacancy density is greater than 1E17 cm ; implanting dopants at least into the pretreated section (710), wherein the lattice vacancies are generated by impurities passing through the process surface (701) into a melting section of the semiconductor layer (700), wherein the implanted impurities and / or the implanted dopants pass through an energy filter unit (870) before reaching the semiconductor layer (700), wherein the Energy filter unit (870) a vertical distribution of the implanted contaminants and / or the implanted Dopants in the pretreated section (710) are modified so that the vertical distribution is approximately uniform; and -3 Heating, at a vacancy density greater than 1E17cm , the melting section (712) of the semiconductor layer (700) by irradiating the process surface (701) with a laser beam (850) which detects the implanted dopants at least in the melting section (712) is activated, wherein the melting section (712) has a vertical extent (v3) which is smaller than a vertical extent (v1) of the previously treated section (710).

2. The method of claim 1, wherein the implanted dopants are connected to a tip (811) at the end of the range within of the pretreated section (710).

3. The method according to any one of claims 1 to 2, wherein the impurities are further dopants.

4. The method according to any one of claims 1 to 3, wherein implanting the impurities does not involve implanting doping auxiliaries.

5. A method according to any one of claims 1 to 4, wherein the implanted impurities comprise ions originating from a group containing germanium, silicon, argon, neon, xenon, krypton, helium and hydrogen ions includes.

6. A method according to any one of claims 1 to 5, wherein the implanted impurities comprise ions originating from a group which includes boron, phosphorus, arsenic, selenium and sulfur.

7. Method according to one of claims 1 to 6, wherein the vertical extent (v1) of the pretreated section (710) is defined as a distance to the process surface (701) up to which a vacancy density is reduced to half a difference between a maximum vacancy density in the pretreated section (710) and an average Lattice vacancy density in a section of the semiconductor layer (700) outside the pretreated section (710) and directly adjacent to the pretreated section (710).

8. The method according to any one of claims 1 to 7, wherein heating the melting portion (712) of the semiconductor layer (700) by irradiating the process surface (701) with a laser beam (850) the implanted dopants also in a Area of ​​the pretreated section (710) beyond the melting section (712) is activated.

9. The method according to any one of claims 1 to 8, wherein heating the melting portion (712) of the semiconductor layer (700) by irradiating the process surface (701) with a laser beam (850) the implanted dopants in the complete pretreated section (710) is activated.

10. The method according to any one of claims 1 to 9, wherein a wavelength of the laser beam (850) is in a range of 150 nm to 1100 nm. -2 11. The method according to any one of claims 1 to 10, wherein the energy density of the laser beam (850) is at least 1 Jcm amounts.

12. The method according to any one of claims 1 to 11, wherein the vertical extent (v3) of the melting section (712) is at least 0.5 µm.

13. The method according to any one of claims 1 to 12, wherein the pretreated portion (710) is not amorphized.

Citation Information

Patent Citations

  • Method of manufacturing a semiconductor device using laser annealing

    DE102009019278A1

  • Semiconductor device and method for producing semiconductor device

    US20140246755A1

  • Semiconductor Device and Method for Forming a Semiconductor Device

    US20150130013A1

  • Method for forming a semiconductor device

    US20150162418A1

  • Adjusting the Charge Carrier Lifetime in a Bipolar Semiconductor Device

    US20160049474A1