Method and apparatus for smoothing a plastic surface of an article and articles produced by the method
The method of acetone vaporization under negative pressure in a vacuum chamber effectively addresses the challenges of smoothing 3D printed plastic surfaces, ensuring a smooth and precise finish without thermal energy, enhancing safety and reducing manual labor costs.
Patent Information
- Application Number
- DE102017200191
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2017-01-09
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2037-01-09
AI Technical Summary
Existing methods for smoothing 3D printed plastic surfaces, such as those used in motor vehicle parts, face challenges including poor surface quality, difficulty in processing undercuts, risk of explosions, and high costs due to manual labor and thermal processes, which often result in uneven smoothing and potential loss of small details.
A method involving acetone vaporization under negative pressure at room temperature, using a vacuum chamber to smooth the surface by depositing acetone vapor on the plastic surface, ensuring safety and precision without thermal energy addition, and utilizing a device with a vacuum lock for controlled acetone vapor application.
Achieves a smooth and dimensionally accurate surface finish with enhanced safety and efficiency, avoiding explosions and manual labor, while maintaining the integrity of small details and complex shapes.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a method for smoothing a polymeric surface of an article, in particular an article for a motor vehicle, according to the preamble of patent claim 1. Such a method is known from CN 204 526 140 U. The article is manufactured, for example, by an additive molding process. Furthermore, the invention relates to a device suitable for this method and to an article processed by this method. By smoothing the surface, an originally increased roughness of the surface is reduced to a value similar to that of an article produced by injection molding.
[0002] Motor vehicles, for example, often require spare parts that are no longer so easy to find on the market. A typical example of this is spare parts for classic cars. The injection molds used to produce the items are often no longer available. However, the shape of the item is usually known and can be captured by scanning or other methods, particularly if you have an old, possibly no longer functional item on hand. Once the shape is known, the item can be created using 3D printing. This usually involves printing layer by layer. This results in the surface of the printed item being significantly too rough and of poor surface quality. In particular, it is not smooth.
[0003] An article with a polymeric surface is defined as follows: The article is at least partially made of plastic, more specifically, at least part of the article's surface is made of plastic. This part exhibits the increased roughness that is to be reduced. For example, the article may have a metal core onto which the plastic is applied.
[0004] DE 11 2014 002 879 T5 discloses a process in which a liquid solvent, such as acetone, is first applied to the surface by immersing the article in the liquid solvent. This can be done at room temperature. The solvent is then removed by suction, i.e., applying a vacuum. The suction preferably takes place at elevated temperature in a vacuum oven. The vacuum used is in the range of 100 to 250 Torr. 250 Torr corresponds to approximately 1 / 3 of normal atmospheric pressure or approximately 33 kPa. The application of a gel layer is also described. The gel layer is allowed to harden in order to smooth at least part of the surface while reducing roughness.
[0005] From US 2014 / 0264294 A1 the treatment of surfaces of articles manufactured using the 3D process is known.
[0006] Acetone (C3H6O) is the common name for propanone or dimethyl ketone, the simplest ketone. Acetone is a colorless liquid and is used, among other things, as an aprotic solvent. Acetone is known as a very good solvent. It is used for cleaning in various industries. Its characteristic structural feature is the carbonyl group bonded to two methyl groups. The boiling point is 56 °C, and the vapor pressure is 233 hPa at 20 °C. In higher concentrations, acetone forms an explosive mixture with air. At normal atmospheric pressure, the substance ignites at about 56 °C.
[0007] JP 000H05239240 A1 teaches a method for surface treatment. CN 103192524 A discloses a method and device that uses baths.
[0008] 3D-printed plastic items, which are the focus here, can also be smoothed by sandblasting or grinding, for example. However, narrow sections, undercuts, and other problematic areas cannot be machined, or at least are difficult to machine, and certainly not with sufficient quality. Small details that are important to the item can be lost during machining. The result depends on the skill of the person performing the machining. Machining can usually only be done manually, and this type of machining is costly. During machining, too much material is often removed locally, and frequently too little, so the overall quality is unsatisfactory.
[0009] Instead of sand, other blasting media can be used, such as CO2 ice particles or other particles such as glass beads. These pose similar problems to those described above for sandblasting.
[0010] A common method is to smooth the surface by treating it with acetone. A distinction is made between a cold and a warm process. Acetone is known to dissolve, or at least partially dissolve, a variety of plastics, such as ABS. In the cold process, the printed parts are placed in a container whose bottom is covered with a small amount of acetone. The container is closed. The acetone gradually transforms into a gas and removes approximately 2 µm of the surface of the printed article. Such removal using vapor-colored acetone typically takes 3 hours. Great care must be taken to avoid an explosion.
[0011] The warm process is significantly more explosive than the cold process. In the warm process, heat is applied, actively converting the acetone into a gas. Temperatures of 60 °C and above are used. This makes the process relatively fast, but it must be used with great caution due to the increased risk of explosion.
[0012] This is where the invention comes in. Its objective is to further develop the aforementioned smoothing process according to CN 204 526 140 U and to provide a method, a device, and a correspondingly manufactured article that are advantageous over the prior art. The method can be carried out extremely safely, no thermal energy needs to be added, the device is simple to construct, and the finished article is smooth and dimensionally accurate.
[0013] This object is achieved by a method having the features of claim 1. The object is further achieved by a device having the features of claim 3 and an article having the features of claim 8.
[0014] The solvent acetone is converted into the vapor phase by working under negative pressure. The process according to the invention is preferably carried out at room temperature, although a slight increase to non-critical temperature ranges, for example 30 °C, is possible. In the process, an article, for example a 3D-printed component, is placed in an airtight, sealable chamber. A certain amount of acetone is contained in the chamber. A vacuum pump is used to create a negative pressure, for example of 33 kPa, in the sealed chamber. At the specified pressure of 33 kPa, the acetone begins to boil; the acetone vapor fills the chamber and thus also precipitates on the surface of the article. After a short period of time, in particular between 1-10, preferably 1-2 minutes, the surface is sufficiently smoothed by the vaporous acetone wetting the polymeric surface.Atmospheric pressure can now be restored in the chamber, after which the treated article can be removed.
[0015] Preferably, work is carried out in a largely closed system. The chamber is only opened when atmospheric pressure prevails. At room temperature, however, the acetone is essentially liquid, and only a small amount of vapor escapes when the chamber is opened.
[0016] A vacuum pump is not directly connected to the chamber's interior; rather, its suction side is connected to an air chamber, which is connected to the chamber via a movable diaphragm. As a result, the vacuum pump always pumps only air, not acetone vapor.
[0017] An improvement is also possible, with a lock through which the article to be treated enters and exits the chamber. This lock is preferably designed as a vacuum lock. This allows a constant negative pressure to be maintained in the chamber.
[0018] Further advantages and features emerge from the remaining claims and the following description of a non-limiting embodiment, which is explained in more detail below with reference to the drawing. The drawing shows in Fig. 1 is a schematic representation of a device for smoothing the surface of an article, wherein the surface consists at least partially of plastic, and Fig. 2 a graph of the vapor pressure in kPa of acetone versus temperature.
[0019] Fig. 1 shows a hermetically sealable chamber 1 which is connected to a pipe socket in which an automatic valve 2 is located. This valve opens and closes the path of a compressed air connection 3 into the interior of the chamber 1. Via the compressed air connection 3, for example, compressed air in the range of over 1 bar to 3 bar, in particular approximately 2 bar, can be introduced into the chamber 1. An article 4 is located in the chamber 1, a steering wheel being shown as an example. Associated with the chamber 1 is a container 5, the internal pressure of which is displayed by a pressure indicator 6. The interior of the container 5 contains gaseous acetone 7 and liquid acetone 8. The container 5 is connected to the interior of the chamber 1 via a supply line in which a one-way valve 9 is located. It continues into a distribution pipe 10, which has openings for the escape of acetone vapor.
[0020] The vacuum is generated by a vacuum pump 11. It has an outlet 12 and is connected on its suction side to a working chamber that has two separate compartments: an air zone 13 and an acetone zone 15 separated by a membrane 14. The membrane 14 is designed, for example, as a rolling membrane. Its position within the working chamber can change as desired and follows the pressure conditions. In other words, the internal volume of the working chamber can be divided as desired between the air zone 13 and the acetone zone 15, depending on the position of the membrane 14. The latter's position, in turn, depends on the pressures in the two zones 13 and 14. The membrane 14 can also be implemented as a tightly sealed piston or slide valve that slides in the longitudinal direction of the cylinder in a working chamber with a cylindrical inner surface and hermetically separates the two zones 13 and 15 from each other.The air area 13 is connected to the outside via a pipe section. An air outlet 13 is provided here, which can also function as an air inlet. The pipe section is equipped with a valve.
[0021] The acetone area 16 is in constant communication with the interior of chamber 1 via a connecting pipe. Also shown is a pressure gauge, which indicates the pressure prevailing in the acetone area 16 and thus also in the interior of chamber 1.
[0022] The chamber 1 is connected to a safety one-way valve 17, which opens into an outlet nozzle 18 on the outlet side.
[0023] The procedure is as follows: First, an article 4 to be treated, which has a surface produced using the 3D printing process, is placed in chamber 1. This can be done by opening chamber 1, but an airlock (not shown) can also be used for this purpose. The article 4 is placed in a favorable position within chamber 1, preferably in its center. Several articles 4 can be placed into chamber 1. Subsequently, chamber 1 is hermetically sealed. The air outlet 13 is closed. The automatic valve 2 is closed.
[0024] In the next step, the vacuum pump 11 is started. It pumps air out of the air area 14. This displaces the diaphragm 14; in the illustration, it moves downward. As a result, the total volume of chamber 1 and the acetone area 16, including its connecting pieces, is increased sufficiently that the pressure in this entire area, and thus also in the interior of chamber 1, corresponds to approximately 1 / 3 of atmospheric pressure. The one-way valve 9 opens due to the resulting pressure difference.
[0025] In order to achieve a sufficient increase in the total volume so that the desired negative pressure is achieved, the working space which forms the air region and the acetone region 16 must have a relatively large volume, in any case significantly larger than in the schematic representation. When the internal pressure in chamber 1 and the connected spaces has been sufficiently reduced, the acetone, which is located in particular in container 5, boils. It precipitates, among other things, on the surface of article 4. It is preferentially possible for this article 4 to have a lower temperature than the other internal wall parts of the overall space which forms the total volume, in particular chamber 1. This is achieved by the vapor preferentially precipitating on the cool surface of article 4. It is sufficient if the article is 5 to 30°, in particular 5 to 10°, cooler than other internal wall parts of the overall space.
[0026] After treatment with acetone vapor for 1 to 2 minutes, the surface of article 4 is sufficiently smoothed. The vacuum pump 11 can now be switched off at the latest. Article 4 is now ready for removal. The air outlet valve 13 is opened, thereby reducing the volume of the air area 14 again, and the membrane 15 moves. In the illustration, it moves upwards. The automatic valve 2 can also be opened and compressed air admitted into the interior of chamber 1. Residual acetone vapor can now leave chamber 1 when the excess pressure opens the safety valve 17. They can be collected at the outlet nozzle using suitable means and reused. Chamber 1 is now largely free of acetone vapor and can be opened; the finished product, i.e. article 14, can be removed.
[0027] Out of Fig.Figure 2 shows the vapor pressure in kPa for acetone plotted against temperature in the range of 0-125°C. At a temperature of 56°C, the vapor pressure is 101.3 kPa, i.e., atmospheric pressure. Thus, the boiling point at atmospheric pressure is 56°C. At approximately room temperature (25°C), the boiling point is at a pressure of 30 kPa. The process according to the invention is preferably carried out in a pressure range below 50 kPa, in particular below 40 kPa. A pressure below 10 kPa is possible, but not preferred; such pressure values do not have to be achieved.
[0028] In the method for smoothing a surface of an article 4, in particular a component of a motor vehicle, which surface is formed at least partially from a plastic, at least the following steps are carried out: a) Placing the article in a vacuum-tight chamber 1, b) reducing the pressure in chamber 1 to a negative pressure of not more than 50 kPa, in particular not more than 34 kPa c) Intake of acetone into chamber 1, resulting in evaporation of at least part of the acetone, the vapor being deposited on the surface of article 4, d) Allow the precipitated steam to act on the article 4 for at least 1 minute, e) Opening the chamber 1 so that at least the ambient pressure is established in the chamber 1 and f) Removal of Article 4 from Chamber 1. List of reference symbols 1 chamber 2 automatic valve 3 Compressed air connection 4 articles 5 containers 6 Pressure display 7 gaseous acetone 8 liquid acetone 9 One-way valve 10 distribution pipe 12 Outlet 13 Air outlet 14 Air area 15 Membran 16 Acetone area 17 Safety valve 18 outlet nozzles 14 and 16 together: Working Chamber
Claims
[1] Method for smoothing a surface of an article (4), in particular a component of a motor vehicle, which surface is formed at least partially from a plastic, comprising the following steps a) placing the article in a vacuum-tight chamber (1), b) reducing the pressure in the chamber (1) to a negative pressure, c) introducing solvent into the chamber (1), resulting in evaporation of at least part of the solvent, the vapor being deposited on the surface of the article (4), d) Allow the precipitated steam to act on the article (4) for at least 1 minute, e) opening the chamber (1) so that at least the ambient pressure is established in the chamber (1) and f) removal of article (4) from chamber (1), characterized bythat acetone is used as solvent, that a negative pressure of at most 50 kPa, in particular not more than 34 kPa, is used, that in step b) the pressure is reduced by sucking air out of an air region (14) of a working space, that the working space also includes an acetone region (16), and that in the working space between the air region (14) and the acetone region (16) a movable separating means which is designed as a membrane (15) and separates the two regions from one another is arranged and a reduction in the pressure in the acetone region (16) and the chamber (1) connected thereto takes place due to the displacement of the separating means, the process being carried out at room temperature, ie without the addition of thermal energy. [2] Method according to claim 1, characterized by that in step e) an overpressure is created in the chamber (1), in particular an overpressure of at least 2 bar. [3] Device for carrying out a method according to one of claims 1 or 2, - with an airtight chamber (1) which accommodates at least one article (4) to be treated, - with a container (5) containing acetone and connected to the chamber (1) via a supply line in which a one-way valve (9) is arranged, - with a working chamber which has an air region (14) and an acetone region (16) connected to the chamber (1) and furthermore a movable separating means, namely a membrane (15), which tightly separates the two regions, and - with a vacuum pump (11) having a suction side connected to the air area (14). [4] Device according to claim 3, characterized by that the chamber (1) is connected to a pipe socket in which an automatic valve (2) is located. [5] Device according to one of claims 3 or 4, characterized bythat the chamber (1) is connected to a safety valve (17) which opens into an outlet nozzle (18) on the outlet side, wherein the safety valve (17) is preferably designed as a one-way valve. [6] Device according to one of claims 3 to 5, characterized by that the air area (14) is connected to the outside world via a pipe section, and that a valve (2) is assigned to the pipe section. [7] Device according to one of claims 3 to 6, characterized by that the chamber (1) is connected to a safety valve (17) which opens into an outlet nozzle (18) on the outlet side. [8] Article (4) with a smoothed surface formed at least partly from a plastic, in particular a component of a motor vehicle, characterized by that the article (4) was produced by the method according to one of claims 1 or 2.
Citation Information
Patent Citations
Novel 3D (three dimensional) printed body surface treatment process
CN103192524A
Equipment for three-dimensional printing plastics, resin piece polishing
CN204526140U
treatment of polymeric surfaces of objects
DE112014002879T5
Surface treatment method for low-activity polymer compact
JP1993239240A
Smoothing method for layered deposition modeling