Magnesium alkoxide catalyst support and process for its production and its use

The production method for magnesium alkoxide catalyst support addresses the challenges of particle morphology and size distribution by using surfactants and controlled conditions, resulting in catalysts suitable for diverse olefin polymerization processes.

DE102018130009B4Active Publication Date: 2024-12-05PETROCHINA CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
DE102018130009
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-01
Filing Date
2018-11-27
Publication Date
2024-12-05
Estimated Expiration
2038-11-27

AI Technical Summary

Technical Problem

Existing catalysts for olefin polymerization, particularly those based on magnesium chloride, fail to meet the requirements of particle morphology, uniform size distribution, and high bulk density while maintaining high catalyst activity and stereoregularity, as they either destroy particle shape or require complex processes with non-ideal results.

Method used

A method for producing magnesium alkoxide catalyst support involves mixing metallic magnesium, a monohydric alcohol, a halogenating agent, and surfactants like n-butyl titanate or triethyl phosphite under controlled conditions, followed by washing with an inert solvent to achieve controlled particle size and morphology.

Benefits of technology

The method produces magnesium alkoxide catalyst supports with uniform particle shape and size distribution, facilitating easy handling and suitability for various polymerization processes by adjusting particle size for specific applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A process for producing a magnesium alkoxide catalyst support, characterized in that the process comprises the following steps: Mixing a metallic magnesium, a monohydric alcohol, a halogenating agent and a surfactant at 0°C to 90°C under an inert gas atmosphere, and subsequently washing the resulting product with an inert solvent to obtain the magnesium alkoxide catalyst support; wherein the monohydric alcohol is added in an amount of 2 mol to 50 mol, the halogenating agent is added in an amount of 0.0025 mol to 0.03 mol, and the inert organic solvent is added in an amount of 2 mol to 50 mol, based on 1 mol of metallic magnesium; wherein the surfactant is added in a volume of 0.01% to 10%, based on the volume of the monohydric alcohol, and the surfactant used is one or more aliphatic or aromatic esters with 1 to 20 carbon atoms from the group consisting of n-butyl titanate, triethyl phosphite, 1,2-butane diol tosylate, catechol di-p-tosylate, ethylene glycol diacetate and triacetin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The invention relates to a catalyst support and a process for its preparation, in particular to a magnesium alkoxide catalyst support and a process for its preparation, and concerns the technical field of catalysts and their preparation. background

[0002] Currently, one of the most commonly used catalysts for olefin polymerization is the Ziegler-Natta catalyst supported on magnesium chloride. The magnesium chloride-supported Ziegler-Natta catalyst is typically a solid catalyst composition consisting of magnesium, titanium, halogen, and electron-donating organic compounds. When used in the polymerization of an α-olefin such as propylene, it can be blended with an organoaluminum compound as a cocatalyst and an organosilane compound as a stereoregularity regulator in a suitable ratio for use.Since supported catalysts for olefin polymerization are used in various commercial polymerization processes, such as slurry polymerization, bulk polymerization, or gas-phase polymerization, they must meet various requirements regarding particle morphology, such as suitable particle size and shape, uniform particle size distribution, few larger particles, and high bulk density, as well as exhibit essential properties such as high catalyst activity and stereoregularity. However, there is no catalyst that can simultaneously meet the above-mentioned various requirements.

[0003] Supported catalysts with magnesium alkoxide as the support can exhibit even more excellent properties. For example, as described in Chinese patent applications CN101014558A (Application No.: CN200580028649.3A), CN 101027327A (Application No.: CN200580032074.2A), and CN1420130A (Application No.: CN01137496.9A), magnesium alkoxide is used as a support to improve various catalyst properties. Therefore, it is necessary to develop techniques for producing magnesium alkoxide with excellent performance.

[0004] Patent application WO2018026330A1 discloses a production process for magnesium alkoxides in which magnesium powder reacts with an alcohol and an activator in the presence of a modifier. In contrast to the present application, however, this process does not disclose the advantageous use of surfactants selected from the group consisting of n-butyl titanate, triethyl phosphite, 1,2-butanediol ditosylate, catechol di-p-tosylate, ethylene glycol diacetate, and triacetin.

[0005] Patent application EP3438083A1 discloses a production process for a magnesium alkoxide catalyst support using a carboxylic acid ester and a corresponding magnesium alkoxide catalyst support. This process also does not disclose the advantageous use of surfactants selected from the group consisting of n-butyl titanate, triethyl phosphite, 1,2-butanediol ditosylate, catechol di-p-tosylate, ethylene glycol diacetate, and triacetin.

[0006] The described methods for producing spherical magnesium dialkoxides mainly include the following methods: (1) First, reacting an alcohol with metallic magnesium to form magnesium dialkoxide and then mechanically pulverizing the resulting product to adjust its particle size; (2) A production method in which metallic magnesium and ethanol are reacted such that the final ratio of magnesium to ethanol is controlled within a range of 1 / 9 to 1 / 15, and then the ethanol is refluxed so that ethanol and magnesium are reacted intermittently or continuously (JP3074341B); (3) A production method in which an alcohol solution of carboxylated magnesium carboxylate is subjected to spray drying followed by decarboxylation to obtain fine spherical particles (JP6087773B); (4).a production process in which metallic magnesium is reacted with ethanol under saturated hydrocarbon conditions (JP6304815B); (5) a production process in which Mg(OR)2 is dispersed in R'OH and the resulting product is subjected to spray drying to obtain solid particles suspended in ROH, and R'OH is removed by distillation to obtain spherical particles (JP62051633B).

[0007] However, the above prior art methods have various disadvantages. For example, in method (1), mechanical pulverization can destroy the original shape of the particles. In method (2), it is regulated that the ratio of magnesium to ethanol is controlled within the range of 1 / 9 to 1 / 15. However, it has been found through research that the viscosity of the reaction system increases sharply in the second half of the reaction when the addition ratio is set to 1 / 9, and the particles agglomerate without sufficient agitation when the conversion rate exceeds 80%, so that uniformly spherical particles were not obtained in the experiment, whereas the shape of the particles is destroyed when forcibly stirred (JP8073388).On the other hand, if the initial addition ratio is set to 1 / 15, the reaction takes place with a larger amount of ethanol, allowing for easy stirring as the viscosity increases in the final stage of the reaction. However, the resulting particles have an insufficiently round shape and a much lower bulk density, thus failing to meet the above requirements. Methods (3) to (5) have complicated operations and use other raw materials besides Mg and ROH, and therefore cannot meet the requirements. Summary

[0008] The present invention was made in view of the above technical problems. An object of the present invention is to provide a process for producing a magnesium alkoxide catalyst support with a controlled particle size and good morphology.

[0009] To achieve the above technical object, the present invention provides a process for producing a magnesium alkoxide catalyst support comprising the following steps: Mixing a metallic magnesium, a monohydric alcohol, a halogenating agent and a surfactant at 0°C to 90°C under an inert gas atmosphere, and then washing the obtained product with an inert solvent to obtain the magnesium alkoxide catalyst support; wherein the monohydric alcohol is added in an amount of 2 mol to 50 mol, the halogenating agent is added in an amount of 0.0025 mol to 0.03 mol, and the inert organic solvent is added in an amount of 2 mol to 50 mol, based on 1 mol of the metallic magnesium; wherein the surfactant is added in a volume of 0.01% to 10%, based on the volume of the monohydric alcohol, and the surfactant used is one or more surfactants selected from aliphatic esters or aromatic esters having 1 to 20 carbon atoms from the group of n-butyl titanate, triethyl phosphite, 1,2-butanediol ditosylate, catechol di-p-tosylate, ethylene glycol diacetate and triacetin.

[0010] In the process for preparing the magnesium alkoxide catalyst support provided by the present invention, the surfactant used is one or more surfactants selected from n-butyl titanate, triethyl phosphite, 1,2-butanediol tosylate, catechol di-p-tosylate, ethylene glycol diacetate and triacetin.

[0011] In the process for producing the magnesium alkoxide catalyst support provided by the present invention, the metallic magnesium, the monohydric alcohol, and the halogenating agent used are added at once or in multiple steps; more preferably, they are added in multiple steps.

[0012] In the process for producing the magnesium alkoxide catalyst support provided by the present invention, the metallic magnesium is not particularly limited in its form. As long as the reaction properties are good, metallic magnesium in any form, such as granules, strips, or powder, can be used.

[0013] In the process for producing the magnesium alkoxide catalyst support provided by the present invention, the metallic magnesium used has a particle size of 0.5 µm to 300 µm.

[0014] In the method for producing the magnesium alkoxide catalyst support provided by the present invention, the monohydric alcohol used is not particularly limited, and the monohydric alcohol used includes one or more monohydric alcohols selected from aliphatic alcohols or aromatic alcohols having 1 to 10 carbon atoms. The monohydric alcohol used includes one or more monohydric alcohols selected from methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, isohexanol, n-heptanol, isoheptanol, n-octanol, isooctanol, n-nonanol, isononanol, n-decanol, isodecanol, phenol, phenylmethanol, phenylethanol, and phenylpropanol. Most preferably, the monohydric alcohol used comprises one or more monohydric alcohols selected from methanol, ethanol, propanol and butanol.

[0015] In the process for producing the magnesium alkoxide catalyst support provided by the present invention, the halogenating agent used is not particularly limited, and the halogenating agent used includes one or more halogenating agents selected from iodine, bromine, chlorine, magnesium iodide, magnesium bromide, magnesium chloride, calcium iodide, calcium bromide, calcium chloride, mercuric iodide, mercuric bromide, mercuric chloride, carbon tetraiodine, carbon tetrabromide, carbon tetrachloride, and alkoxymagnesium halide. More preferably, the halogenating agent used includes one or more halogenating agents selected from iodine, carbon tetrachloride, magnesium iodide, magnesium chloride, and alkoxymagnesium halide.

[0016] According to a particular embodiment of the invention, the iodine used can be introduced into the reaction in pure form or in solution, preferably in the form of a solution of iodine in anhydrous ethanol.

[0017] In the process for producing the magnesium alkoxide catalyst support provided by the present invention, the mixed product can be washed with an alcohol used to produce the magnesium alkoxide, washed with an organic solvent used in the reaction, or washed with other inert organic solvents. There are no particular restrictions on the washing treatment and its frequency.

[0018] In the process for preparing the magnesium alkoxide catalyst support provided by the present invention, the inert organic solvent used comprises one or more inert organic solvents selected from hexane, heptane, octane, decane, benzene, toluene, xylene, chlorobenzene, a toluene derivative, a xylene derivative and a chlorobenzene derivative.

[0019] In the process for producing the magnesium alkoxide catalyst support provided by the present invention, the monohydric alcohol is added in an amount of 5 mol to 20 mol, and the halogenating agent is added in an amount of 0.0025 mol to 0.01 mol based on 1 mol of the metallic magnesium.

[0020] The process for producing the magnesium alkoxide catalyst support according to the present invention is carried out in an inert gas, and the inert gas used includes argon gas and nitrogen gas, preferably nitrogen gas.

[0021] In the process for producing the magnesium alkoxide catalyst support according to the present invention, the starting materials (the metallic magnesium, the monohydric alcohol, and the halogenating agent) can be added at once or in multiple steps; the multiple-step addition can prevent the instantaneous generation of a large amount of hydrogen gas and thus prevent splashing of alcohol or halogen caused by the instantaneous generation of a large amount of hydrogen gas.

[0022] The inert organic solvent used to disperse the material in the invention dilutes the material so that the resulting liquid can be reacted with good stirring, which facilitates the release of reaction heat, avoids violent reaction, and also avoids electrostatic charges so that the products can maintain good particle morphology.

[0023] The present invention further provides a magnesium alkoxide catalyst support prepared by the above-described process for preparing a magnesium alkoxide catalyst support.

[0024] The above magnesium alkoxide catalyst support according to the present invention is used to catalyze olefin polymerization.

[0025] The magnesium alkoxide catalyst support produced by the process for producing the magnesium alkoxide catalyst support according to the present invention has a controllable size. Magnesium alkoxide catalyst supports of various sizes can be obtained by varying the surfactant types, so that the magnesium alkoxide catalyst supports of various sizes can be used for various polymerization processes. When the average particle size (D50) of the surfactant is about 20 µm, it can be used in a gas-phase polymerization process, and when the average particle size (D50) is about 50 µm, it can be used in a bulk polymerization process.

[0026] The magnesium alkoxide catalyst support produced by the above process for producing the magnesium alkoxide catalyst support according to the present invention simultaneously has the following advantages: uniform particle shape, easy handling, and controllable size. Detailed description

[0027] The technical solutions of the present invention are described in detail below for a better understanding of the technical features, objects and advantages of the present invention, which is not intended to limit the scope of the invention. Particle size distribution:

[0028] The particle size of the magnesium alkoxide was determined using a Malvern MastersizerTMX; Average particle size (D50): a particle size corresponding to 50% cumulative weight; The particle size of the magnesium alkoxide and its distribution index Span = (D90-D10) / D50 are used to characterize the uniformity of the particle size distribution. Example 1

[0029] This example provides a magnesium alkoxide catalyst support prepared by the following procedures.

[0030] A reflux condenser, a thermometer, and a burette were installed on a reactor equipped with a stirrer. The upper part of the reflux condenser was connected to a tube, which was connected at the other end to an oil seal device to facilitate the observation of H2. After sufficient substitution with nitrogen, 2 g of magnesium powder, 10 ml of decane, 30 ml of absolute ethanol, 0.2 g of iodine, and 1.5 ml of n-butyl titanate were added to the reactor. The resulting product was heated for 15 minutes after the reaction was activated until the reaction temperature for the reaction system was reached. The addition of magnesium powder, alcohol, iodine, and decane in the same amount as in the previous feed was repeated after no more H2 was released from the reaction system, so that the addition was carried out a total of 5 times.After the final batch was added and no more H2 was generated by the reaction, the reaction system was allowed to age for 2 hours. After the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0031] The particle size and distribution of the product were determined using a particle size distribution meter. The results are presented in Table 1. Example 2

[0032] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0033] The same steps as in Example 1 were performed, except that 1.5 ml of tributyl phosphate was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0034] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 3

[0035] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0036] The same steps as in Example 1 were performed, except that 1.5 ml of di-n-butyl phthalate was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0037] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 4

[0038] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0039] The same steps as in Example 1 were performed, except that 1.5 ml of ethylene glycol diacetate was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0040] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 5

[0041] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0042] The same steps as in Example 1 were performed, except that 1.5 ml of triacetin was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0043] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 6

[0044] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0045] The same steps as in Example 1 were performed, except that 0.5 ml of triacetin was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0046] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 7

[0047] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0048] The same steps as in Example 1 were performed, except that 1.5 ml of catechol di-p-tosylate was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0049] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 8

[0050] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0051] The same steps as in Example 1 were performed, except that 1.5 ml of triethyl phosphite was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0052] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Example 9

[0053] This example provides a magnesium alkoxide catalyst support prepared by the following procedure.

[0054] The same steps as in Example 1 were performed, except that 0.5 ml of n-butyl titanate and 0.5 ml of di-n-butyl phthalate were added to the reaction system, and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0055] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Comparison example 1

[0056] The same steps as in Example 1 were performed, except that no surfactant was added to the reaction system and the reaction was carried out at 78°C for 4 hours. After completion of the final reaction, the product was washed, separated, and dried to obtain a white solid powder with good flowability.

[0057] The obtained product was characterized in the same manner as in Example 1. The results are presented in Table 1. Table 1 Particle shape Average particle size D50 (µm) Particle size distribution index Example 1 spherical 22.2 1.3 Example 2 spherical 43.7 1.2 Example 3 spherical 54.7 1.1 Example 4 spherical 39.3 1.1 Example 5 spherical 23.5 1.2 Example 6 spherical 16.5 1.3 Example 7 spherical 51.4 0.9 Example 8 spherical 42.5 1.3 Example 9 spherical 35.8 1.2 Comparison example 1 spherical 51.3 1.3

[0058] As can be seen from Table 1, when no surfactant was added in Comparative Example 1, only a support of approximately 50 µm was obtained with a limited size control range. In contrast, magnesium alkoxide catalyst supports of various sizes were obtained by changing the surfactant types according to the preparation method in Example 1.

[0059] The above examples demonstrate that the process for producing a magnesium alkoxide catalyst support according to the present invention can produce magnesium alkoxide particles with excellent particle morphology and a uniform particle size distribution. Supports of various sizes can be obtained by varying the surfactant types, and the support can be used selectively for various olefin polymerization processes. The process according to the present invention has obvious advantages over other processes. The magnesium alkoxide catalyst support produced according to the present invention is an excellent support for catalyzing olefin polymerization.

Claims

[1] Process for the preparation of a magnesium alkoxide catalyst support, characterized by that the procedure includes the following steps: Mixing a metallic magnesium, a monohydric alcohol, a halogenating agent and a surfactant at 0°C to 90°C under an inert gas atmosphere, and then washing the obtained product with an inert solvent to obtain the magnesium alkoxide catalyst support; wherein the monohydric alcohol is added in an amount of 2 mol to 50 mol, the halogenating agent is added in an amount of 0.0025 mol to 0.03 mol, and the inert organic solvent is added in an amount of 2 mol to 50 mol, based on 1 mol of the metallic magnesium; wherein the surfactant is added in a volume of 0.01% to 10%, based on the volume of the monohydric alcohol, and the surfactant used is one or more aliphatic or aromatic esters having 1 to 20 carbon atoms from the group of n-butyl titanate, triethyl phosphite, 1,2-butanediol tosylate, catechol di-p-tosylate, ethylene glycol diacetate and triacetin. [2] A process for producing a magnesium alkoxide catalyst support according to claim 1, characterized by that the metallic magnesium, the monohydric alcohol and the halogenating agent are added all at once or in several steps. [3] A process for producing a magnesium alkoxide catalyst support according to claim 2, characterized by that the metallic magnesium, the monohydric alcohol and the halogenating agent are added in several steps. [4] A process for producing a magnesium alkoxide catalyst support according to claim 1, characterized bythat the metallic magnesium has a particle size of 0.5 µm to 300 µm. [5] A process for producing a magnesium alkoxide catalyst support according to claim 1, characterized by that the monohydric alcohol comprises one or more monohydric alcohols selected from aliphatic alcohols or aromatic alcohols having 1 to 10 carbon atoms, wherein the monohydric alcohol comprises one or more monohydric alcohols selected from methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, n-pentanol, isopentanol, n-hexanol, isohexanol, n-heptanol, isoheptanol, n-octanol, isooctanol, n-nonanol, isononanol, n-decanol, isodecanol, phenol, phenylmethanol, phenylethanol and phenylpropanol. [6] A process for producing a magnesium alkoxide catalyst support according to claim 5, characterized by that the monohydric alcohol comprises one or more monohydric alcohols selected from methanol, ethanol, propanol and butanol. [7] A process for producing a magnesium alkoxide catalyst support according to claim 1, characterized by that the halogenating agent comprises one or more halogenating agents selected from iodine, bromine, chlorine, magnesium iodide, magnesium bromide, magnesium chloride, calcium iodide, calcium bromide, calcium chloride, mercuric iodide, mercuric bromide, mercuric chloride, carbon tetraiodine, carbon tetrabromide, carbon tetrachloride and alkoxymagnesium halide. [8] A process for producing a magnesium alkoxide catalyst support according to claim 7, characterized by that the halogenating agent comprises one or more halogenating agents selected from iodine, carbon tetrachloride, magnesium iodide, magnesium chloride and alkoxymagnesium halide. [9] A process for producing a magnesium alkoxide catalyst support according to claim 1, characterized bythat the inert organic solvent comprises one or more inert organic solvents selected from hexane, heptane, octane, decane, benzene, toluene, xylene, chlorobenzene, a toluene derivative, a xylene derivative and a chlorobenzene derivative. [10] A process for producing a magnesium alkoxide catalyst support according to claim 1, characterized by that the monohydric alcohol is added in an amount of 5 mol to 20 mol and the halogenating agent in an amount of 0.0025 mol to 0.01 mol, based on 1 mol of the metallic magnesium. [11] Magnesium alkoxide catalyst support, characterized by that the magnesium alkoxide catalyst support is produced by the process for producing a magnesium alkoxide catalyst support according to any one of claims 1-10. [12] Use of the magnesium alkoxide catalyst support according to claim 11, characterized bythat the magnesium alkoxide catalyst support is used to catalyze olefin polymerization.

Citation Information

Patent Citations

  • Magnesium compound, solid catalyst component, olefin polymerization catalyst, and method for producing polyolefin

    CN101014558A

  • Method of preparation of spherical support for olefin polymerization catalyst

    CN101027327A

  • Method for producing pneumatic tire and pneumatic tire

    CN101137496A

  • Polyolefin cafalyst, preparing method thereof, use method and polymer obtained therewith

    CN1420130A

  • Alkoxy magnesium, method for producing alkoxy magnesium, solid catalyst component for olefin polymerization use, catalyst for olefin polymerization use, and method for producing olefin polymer

    EP3438083A1