Method for producing an electrode catalyst for fuel cells
The method enhances electrode catalyst performance in fuel cells by using controlled heat treatment to achieve uniform platinum or platinum alloy particles on carbonaceous supports, ensuring high initial activity and long-term stability.
Patent Information
- Application Number
- DE102018206378
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-04-28
- Filing Date
- 2018-04-25
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2038-04-25
AI Technical Summary
Existing electrode catalysts for fuel cells face challenges in achieving high initial activity while maintaining this activity over a long period, with issues in particle size uniformity and stability.
A manufacturing method for electrode catalysts using platinum or platinum alloy particles with a specific surface area and size distribution, achieved through controlled heat treatment of carbonaceous support materials, ensuring uniformity and stability of catalyst particles.
The method results in electrode catalysts with high initial activity and prolonged activity maintenance, attributed to the precise control of particle size and distribution.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical area
[0001] The present invention relates to a process for producing an electrode catalyst for fuel cells. State of the art
[0002] A fuel cell has high energy generation efficiency, is easy to scale down, and has little harmful impact on the environment, making it promising for use in various fields such as personal computers, mobile phones and other mobile devices, cars, trains, and other vehicles.
[0003] A fuel cell comprises a pair of electrodes and an electrolyte. The electrode comprises an electrode catalyst consisting of catalyst metal particles and a support to support them. In the past, fuel cells generally used carbon as the support. Furthermore, platinum or a platinum alloy was used for the catalyst metal particles.
[0004] A fuel cell with a high initial activity of the electrode catalyst and capable of maintaining this activity over a long period of time has been sought. Numerous techniques have been reported for this purpose (Patent Documents 1 to 8).
[0005] DE 10 2015 105 503 A1 discloses an electrode catalyst for a fuel cell comprising a carbon support; and a catalytic metal supported on the carbon support, wherein the catalytic metal is selected from platinum or a platinum alloy, wherein the carbon support has a crystallite size of the (002) plane of carbon in a range of 5.0 nm or more and a specific surface area in a range of 95 m 2 / g up to 170 m 2 / g and wherein the catalytic metal has a crystallite size of the (220) plane of platinum in a range of 4.5 nm or less.
[0006] US 2013 / 0244137 A1 discloses a catalyst for a polymer electrolyte fuel cell comprising platinum catalyst particles supported on a carbon powder support, wherein the carbon powder support contains 0.7 to 3.0 mmol / g (based on the weight of the support) of a hydrophilic group bonded thereto, and wherein the platinum particles have an average particle size of 3.5 to 8.0 nm and a CO adsorption-based platinum specific surface area (COMSA) of 40 to 100 m 2 / g.
[0007] CA 2 998 075 A1 discloses an electrode catalyst layer for a fuel cell comprising a catalyst support having a large specific surface area and a polyelectrolyte, at least a part of which assumes an aggregated form, whereby the electrode catalyst layer for a fuel cell has excellent power generation performance in a high humidity environment.
[0008] US 2009 / 0029216 A1 discloses a method for suppressing corrosion of a carbon material serving as a support in a PEFC catalyst layer. An electrode catalyst is disclosed that is produced by subjecting a carbon material with a noble metal catalyst thereon to a heat treatment in an inert gas atmosphere. [Prior art documents][Patent documents] Patent Document 1: JP 2012-124001 A Patent Document 2: JP 2013-252483 A Patent Document 3: JP 2012-248365 A Patent Document 4: JP 2012-236138 A Patent Document 5: JP 2005-317546 A Patent Document 6: JP 2005-166409 A Patent Document 7: JP 2009-140657 A Patent document 8: WO 2016 / 063968 A1 Patent document 9: WO 2014 / 129597 A1 Summary of the invention[Problem to be solved by the invention]
[0009] The object of the present invention is to provide an electrode catalyst for fuel cells having a high initial activity of the electrode catalyst which is capable of maintaining this activity over a long period of time, and a process for its preparation. [Means of solving the problem]
[0010] The inventors have discovered that the above-mentioned problem can be solved by the present invention which has the following aspects. Aspect 1:
[0011] A manufacturing method for an electrode catalyst for a fuel cell comprising the catalyst metal particles containing a platinum or a platinum alloy and the support particles supporting the catalyst metal particles, wherein the support particles are made of a carbonaceous material having a BET specific surface area of 700 m 2 / g or more and 2500 m2 / g or less, wherein the catalyst metal particles have an average particle size of 2.5 to 4.5 nm, and wherein a standard deviation of the particle size of the catalyst metal particles is 1.30 nm or less, wherein the production process comprises: bringing a platinate solution into contact with the support particles, using an alcohol as a reducing agent to reduce the platinate at 60°C to 90°C for 1 hour to 3 hours to promote metal formation of the catalyst metal particles on the support particles, and heat-treating the support particles that support the metal forming the catalyst metal particles in an inert atmosphere or reducing atmosphere, wherein the heat-treating is carried out at 830°C to 880°C within 2 hours, or at 880°C to 920°C within 1.5 hours, or at 920°C to 980 °C within 0.8 hours,where heat treatment means keeping the temperature within the specified range., Aspect 2:
[0012] The manufacturing process according to aspect 1, wherein the carrier particles consist of a carbonaceous material having a BET specific surface area of 900 to 1500 m 2 / g were produced. Aspect 3:
[0013] The manufacturing method according to aspect 1 or 2, wherein the catalyst metal particles have an average particle size of 2.8 to 3.8 nm and wherein the standard deviation of the particle size of the catalyst metal particles is 0.95 to 1.15 nm. Aspect 4:
[0014] The manufacturing process according to any one of aspects 1 to 3, wherein the catalyst metal particles contain an alloy of a platinum and a cobalt with a molar ratio of 4 to 1 to 11 to 1. Short description of the drawings The Fig. 1 shows a temperature profile of the heat treatment for the examples carried out in the embodiments. The Fig. 2 shows an embodiment of a fuel cell. Detailed description of the inventionElectrode catalyst for a fuel cell
[0015] The electrode catalyst for a fuel cell of the present invention comprises catalyst metal particles containing platinum or a platinum alloy and support particles that support the catalyst metal particles. The support particles consist of a carbonaceous material with a specific surface area of 700 m 2 / g or more, the catalyst metal particles have an average particle size of 2.5 to 4.5 nm, and the standard deviation of the particle size of the catalyst metal particles is 1.30 nm or less.
[0016] When the prior art attempts to obtain catalyst metal particles with an average particle size of 2.5 to 4.5 nm, the particle size distribution tends to become poor in uniformity. When further attempts are made to improve the uniformity of the particle size distribution, the average particle size tends to become too small. In contrast, the inventors discovered that by using a carbonaceous material with a high specific surface area for the support particles and preparing them under specific heat treatment conditions, the obtained catalyst metal particles exhibited a particle size distribution that was impossible to obtain in the prior art (i.e., a combination of an average particle size and a standard deviation).If the average particle size of the catalyst metal particles is small, the initial activity of the electrode catalyst will be higher, but the activity tends not to be maintained for a long period of time. However, it has been found that with the electrode catalyst of the present invention, the activity can be maintained for a long period of time even if the average particle size is small. Catalyst metal particles
[0017] The catalyst metal particles used in the present invention are particles containing platinum or a platinum alloy. Particles made of platinum or a platinum alloy are preferred, and particles made of a platinum alloy are particularly preferred. The average particle size of the catalyst metal particles is 2.5 to 4.5 nm, while the standard deviation of the particle size of the catalyst metal particles is 1.30 nm or less.
[0018] The average particle size of the catalyst metal particles may be 2.6 nm or more, 2.8 nm or more, 3.0 nm or more, 3.2 nm or more, or 3.4 nm or more, and it may be 4.5 nm or less, 4.2 nm or less, 4.0 nm or less, 3.8 nm or less, or 3.6 nm or less. Furthermore, the standard deviation of the particle size of the catalyst metal particles may be 1.25 nm or less, 1.20 nm or less, 1.15 nm or less, 1.10 nm or less, or 1.05 nm or less, and it may be 0.10 nm or more, 0.30 nm or more, 0.50 nm or more, 0.80 nm or more, 0.90 nm or more, or 0.95 nm or more. When the particle size of the catalyst metal particles is in such ranges, the initial activity of the electrode catalyst is high and the activity tends to be maintained for a long period of time.
[0019] The average particle size of the catalyst metal particles is calculated from a single-peak X-ray diffraction measurement using JADE analysis software. In this case, the average particle size becomes the average particle size of the numerically averaged sample. The standard deviation of the particle size of the catalyst metal particles can be calculated using small-angle X-ray scattering with analytical software. Examples of analytical software include Nano-Solver (manufactured by Rigaku).
[0020] When the catalyst metal particles contain a platinum alloy, the type of platinum alloy is not particularly limited as long as it serves as an electrode catalyst for the fuel cell. For example, the platinum alloy may be an alloy of a metal selected from the group consisting of iron, chromium, nickel, cobalt, terbium, yttrium, gadolinium, and ruthenium, and combinations thereof, with platinum. Preferably, it is an alloy of a metal selected from the group consisting of nickel, cobalt, terbium, yttrium, gadolinium, and ruthenium, and combinations thereof, with platinum. More preferably, it is an alloy of platinum and cobalt.
[0021] The molar ratio of platinum to the metal forming the platinum alloy may be 1 or more to 1, 2 or more to 1, 4 or more to 1, 5 or more to 1, or 10 or more to 1, and it may be 100 or less to 1, 50 or less to 1, 30 or less to 1, 20 or less to 1, or 10 or less to 1. For example, the molar ratio of the platinum to cobalt alloy may be 4 to 1 to 11 to 1.
[0022] The proportion of the catalyst metal particles in the electrode catalyst for the fuel cell of the present invention may be 10 wt% or more, 20 wt% or more, 30 wt% or more, 35 wt% or more, 40 wt% or more, or 45 wt% or more, and it may be 70 wt% or less, 60 wt% or less, 55 wt% or less, 50 wt% or less, 45 wt% or less, 40 wt% or less, or 35 wt% or less based on the total weight of the carrier particles and catalyst metal particles. carrier particles
[0023] The carrier particles used in the present invention are made of a carbonaceous material with a BET specific surface area of 700 m 2 / g or more. The BET specific surface area of the carbonaceous material can be 750 m2 / g or more, 800 m 2 / g or more, 850 m 2 / g or more, 900 m 2 / g or more or 950 m 2 / g or more and it can reach 2500 m 2 / g or less, 2000 m 2 / g or less, 1800 m 2 / g or less, 1500 m 2 / g or less or 1200 m 2 / g or less. It has been found that in such ranges, the particle size of the platinum alloy is maintained extremely uniform and at a suitable size.
[0024] The type of carbonaceous material is not particularly limited as long as the BET specific surface area is large, but graphite, activated carbon, carbon black, carbon nanotubes, solid carbon, hollow carbon, dendritic carbon, and combinations thereof can be mentioned. As the solid carbon and hollow carbon, the carbon described in Patent Document 8 can be mentioned. As the dendritic carbon, the carbon described in Patent Document 9 can be mentioned.
[0025] The average particle size of the carrier particles may preferably be 30 μm or less, 20 μm or less, 10 μm or less, and 0.1 μm or more, 0.5 μm or more, 1.0 μm or more, 5.0 μm or more, or 10 μm or more. In this case, the average particle size can be calculated from the number-averaged equivalent diameter based on a large number of photographs taken at arbitrary positions with an electron microscope. Note that the "equivalent diameter" means the diameter of a true circle with an outer circumference equal to the outer circumference of this particle. fuel cell
[0026] The fuel cell of the present invention comprises the above-mentioned electrode catalyst. This fuel cell may comprise electrodes containing the above-mentioned electrode catalyst and an ionomer on a base material and an electrolyte, particularly a polymer electrolyte.
[0027] As the type of ionomer, for example, DuPaft's Nafion® DE2020, DE2021, DE520, DE521, DE1020 and DE1021 and Asaki Kasei Chemicals Aciplex® SS700C / 20, SS900 / 10, SS1100 / 5 and so on can be mentioned.
[0028] The fuel cell type can include a solid polymer fuel cell (PEFC), a phosphoric acid fuel cell (PAFC), a molten carbonate fuel cell (MCFC), a solid oxide fuel cell (SOFC), an alkaline electrolyte fuel cell (AFC), a direct fuel cell (DFC), and so on. Although not particularly limited, the preferred fuel cell is a solid polymer fuel cell.
[0029] The electrodes containing the above-mentioned electrode catalyst can be used as the cathode, they can be used as the anode, or they can be used as both the cathode and the anode. The fuel cell may further include separators. The unit cells of a membrane electrode assembly (MEA), which includes a pair of electrodes (cathode and anode) and an electrolyte membrane sandwiched by a pair of separators, may be stacked to form a cell stack, thereby achieving high electrical performance. The fuel cell may further include gas diffusion layers, etc.
[0030] The Fig. Figure 2 shows a membrane electrode assembly 100 comprising an anode electrode layer 20 and a cathode electrode layer 30 containing the above-mentioned electrode, and an electrolyte membrane 10 having proton conductivity sandwiched between the electrode layers. Furthermore, Fig.2 a fuel cell 200 comprising, as a single cell, the membrane electrode assembly 100, an anode-side gas channel 21, an anode-side gas diffusion layer 22, an anode-side separator 23, a cathode-side gas channel 31, a cathode-side gas diffusion layer 32, and a cathode-side separator 33.
[0031] Method for Producing an Electrode Catalyst for a Fuel Cell The method for producing the electrode catalyst for a fuel cell of the present invention comprises heat-treating the support particles that support the metal constituting the catalyst metal particles at a temperature of 830°C or higher for 2 hours. The electrode catalyst for a fuel cell obtained by the method of the present invention can be the above-mentioned electrode catalyst for a fuel cell. For the catalyst metal particles and the support particles, those explained with respect to the above-mentioned electrode catalyst for a fuel cell can be used.
[0032] In the prior art, for example, the heat treatment was carried out at 700 to 800 °C for about 3 to 6 hours, but the inventors discovered that when a carbonaceous material with a high specific surface area is used as the support particles and these are heat-treated for a short time at a high temperature, the obtained catalyst metal particles have a particle size distribution that could not be obtained in the past (that is, the combination of an average particle size with a standard deviation). Step of supporting
[0033] The method for producing the electrode catalyst for a fuel cell of the present invention may include a step of supporting the catalyst metal particles on the support particles. The step of supporting the catalyst metal particles on the support particles may include contacting a platinate solution with the support particles and using a reducing agent to reduce the platinate. As the platinate solution, for example, a solution of diammine dinitro platinum nitric acid may be mentioned.
[0034] In the step of contacting a platinate solution with the carrier particles, the carrier particles can be dispersed in an aqueous solvent and mixed with a platinate solution. In this case, the aqueous solution can be acidified to suppress the formation of precipitates that may form at the time of mixing with the platinate solution.
[0035] The reducing agent is not particularly limited, but an alcohol, such as ethanol, can be used. During the reduction step, it is possible to add the reducing agent and then perform a heat treatment. The heat treatment conditions vary depending on the type of reducing agent; however, when using ethanol as the reducing agent, for example, it is possible to heat the particles at 60°C to 90°C for 1 to 3 hours.
[0036] After the reduction step, the platinum particles and the support particles can be separated from the dispersion. For example, a filter can be used to separate the platinum particles and the support particles that support them. After separating the platinum particles and the support particles that support them, they can be washed and / or dried.
[0037] When a platinum alloy is used for the catalyst metal particles, the platinum particles and the support particles that support them can be further dispersed in an aqueous solvent to bring them into contact with the salt solution of the metal that forms the platinum alloy. For example, if the metal that forms the platinum alloy is cobalt, it is possible to use a cobalt nitrate solution for the salt solution. In this case, a reducing agent can be used to reduce the metal salt and alloy the metal that forms the platinum alloy and the platinum to some extent. After the reduction step, the platinum alloy particles and the support particles can be separated from the dispersion. For example, a filter can be used for separation to obtain the platinum alloy particles and the support particles that support them.After separating the platinum alloy particles and the carrier particles that support them, they can be washed and / or dried. Heat treatment step
[0038] After the catalyst metal particles have been supported on the support particles in this way, the catalyst metal particles and the support particles are heat-treated at a temperature of 830 °C or higher for 0.2 to 2 hours. In the above-mentioned manner, this heat treatment is carried out in a relatively short time and at a high temperature.
[0039] Heat treatment performed at 830°C or higher can be performed at a temperature of 850°C or higher, 880°C or higher, 900°C or higher, or 930°C or higher. The highest temperature can be 1100°C or lower, 1050°C or lower, 1000°C or lower, 980°C or lower, 950°C or lower, 930°C or lower, 900°C or lower, or 880°C or lower.
[0040] The heat treatment time at 830°C or higher can be within 2 hours, within 1.8 hours, within 1.5 hours, within 1.2 hours, within 1.0 hour, within 0.8 hours, or within 0.5 hours. For this heat treatment, the heat treatment time at 880°C or higher can be within 1.5 hours, within 1.2 hours, within 1.0 hour, within 0.8 hours, or within 0.5 hours, while the heat treatment time at 920°C or higher can be within 1.0 hour, within 0.8 hours, or within 0.5 hours. Furthermore, these heat treatments may be carried out for 0.2 hours or longer, for 0.3 hours or longer, for 0.5 hours or longer, for 0.8 hours or longer, for 1.0 hours or longer, or for 1.5 hours or longer.It was found that when this heat treatment is carried out for a long time, the particle size distribution of the catalyst metal particles tends to become uneven.
[0041] For example, heat treatment at 830°C or higher can be carried out within 2 hours or 1.8 hours at a temperature of 830°C to 880°C; it can be carried out within 1.5 hours or 1.2 hours at a temperature above 880°C to 920°C; or it can be carried out within 0.8 hours or 0.5 hours at a temperature above 920°C to 980°C. For example, it can be carried out within 1.5 hours, 1.0 hours, or 0.5 hours at a temperature of 880°C to 980°C.
[0042] The temperature rise and cooling rates at the time of heat treatment are not particularly limited, as long as they are within the ranges where heat treatment can be sufficiently performed. For example, the temperature rise rate may be 3°C / min or more, 5°C / min or more, 10°C / min or more, or 15°C / min or more, and it may be 30°C / min or less, 20°C / min or less, or 15°C / min or less. The cooling rate may be 10°C / min or more, 20°C / min or more, 30°C / min or more, or 50°C / min or more, and it may be 80°C / min or less, 50°C / min or less, or 30°C / min or less.
[0043] The atmosphere at the time of heat treatment is preferably an inert atmosphere or a reducing atmosphere so that the carbonaceous material is not oxidized. Acid treatment step
[0044] The method for producing the electrode catalyst for the fuel cell of the present invention may further comprise an acid treatment step.
[0045] In the acid treatment step, the PtCo alloy supported by the solid carbon support is treated with an acid, preferably at 70 to 90 °C, and more preferably at 75 to 85 °C. By acid treatment at such a temperature, it is possible to sufficiently remove the Co that does not contribute to the reaction. Therefore, it is possible to suppress the leaching of Co.
[0046] As the acid used in the acid treatment step, for example, inorganic acids (such as nitric acid, phosphoric acid, permanganic acid, sulfuric acid, hydrochloric acid, and so on) and organic acids (such as acetic acid, malonic acid, oxalic acid, formic acid, citric acid, lactic acid, and so on) can be mentioned.
[0047] The present invention will be explained in more detail by the following examples, but the present invention is not limited to them. ExamplesManufacturing examplesExample 1
[0048] 7 g of dendritic carbon with a specific BET surface area of about 1000 m 2 / g were dispersed in 1 liter of a 0.1 N aqueous nitric acid solution. To this dispersion, a solution of diamine-dinitro-platinum nitric acid containing 2.8 g of platinum was added to give a platinum supporting rate of 40 weight percent. Further, 27 g of 99.5% ethanol was added as a reducing agent and sufficiently mixed. Using ethanol as the reducing agent, the metal was assisted by reduction. The dispersion after reduction was repeatedly filtered and washed until the conductivity of the filtrate was 50 µS / cm or less. The powder cake obtained by filtration and washing was dried by air blow drying at 80 °C for 15 hours or more to obtain the platinum-supporting carbon.
[0049] The platinum-supporting carbon was dispersed in pure water in an amount 80 times the amount of carbon, and the cobalt nitrate solution was added dropwise. This aqueous cobalt nitrate solution was prepared by dissolving commercially available cobalt nitrate 6-hydrate in pure water and used to achieve a molar ratio of platinum to cobalt of 7 to 1. The aqueous cobalt nitrate solution was added, and then additional sodium borohydride dissolved in pure water was used as the reducing agent to support the metal through reduction. This dispersion was repeatedly filtered and washed until the conductivity of the filtrate was 5 µS / cm or less. The powder cake obtained by filtration and washing was dried by air-blast drying at 80°C for 15 hours or more to obtain a platinum-supporting carbon.
[0050] The thus obtained carbon supporting the platinum alloy was heated in an argon atmosphere at a rate of 10 °C / min for heat treatment. The temperature increase was stopped when 950 °C was reached. After stopping the temperature increase, the temperature was lowered to about 750 °C within a few minutes. Finally, the carbon was cooled to nearly room temperature. As a result, the electrode catalyst for the fuel cell of Example 1 was obtained. The heat treatment temperature and the elapsed time for Example 1 are shown in the Fig. 1 shown. Example 2
[0051] Except for changing the heat treatment to increase the temperature at 10 °C / min and, when 900 °C was reached, to hold at this temperature for 1 hour, the same procedure as in Example 1 was carried out to obtain the electrode catalyst for the fuel cell of Example 2. The heat treatment temperature and the elapsed time in Example 2 are shown in the Fig. 1 shown. Example 3
[0052] With the exception of the change in heat treatment that the temperature is increased by 10 °C / min and after reaching 850 °C, this temperature is maintained for 1.5 hours and the use of a solid carbon with a BET specific surface area of about 800 m 2 / g, the same procedure as in Example 1 was carried out to obtain the electrode catalyst for the fuel cell of Example 3. The heat treatment temperature and the elapsed time in Example 3 are shown in the Fig. 1 shown. Comparison example 1
[0053] Except for changing the heat treatment to 800 °C for 4 hours, the same procedure as in Example 1 was carried out to obtain an electrode catalyst for the fuel cell of Comparative Example 1. Comparison example 2
[0054] Except that the heat treatment was not performed, the same procedure as in Example 1 was carried out to obtain an electrode catalyst for the fuel cell of Comparative Example 2. Comparison example 3
[0055] In addition to the use of a solid carbon for the carrier particles with a BET specific surface area of about 600 m 2 / g, the same procedure as in Example 1 was carried out to obtain an electrode catalyst for the fuel cell of Comparative Example 3. EvaluationParticle size measurement
[0056] The mean particle size of the prepared catalyst metal particles was calculated from the peak X-ray diffraction data using the JADE analysis software. Furthermore, the standard deviation of the particle size of the catalyst metal particles was calculated from the peak X-ray scattering data using the Nano-Solver analysis software. Initial catalytic activity
[0057] The electrode catalyst prepared according to each of the examples and comparative examples was dispersed in an organic solvent. The dispersion was coated on a Teflon® film to form the electrodes. The electrodes were hot-pressed through a polymer electrolyte membrane, and the diffusion layers were arranged on both sides to produce a unit cell for use in a solid polymer fuel cell.
[0058] The cell temperature was set to 80 °C, the relative humidity of the two electrodes was set to 100%, and a small unit cell evaluation system (manufactured by Toyo) was used for cyclic voltammetry (CV) and IV measurements.
[0059] For the IV measurement, the current was in the range of 0.01 to 1.0 A / cm 2freely controlled. The current value per mass of Pt at the time of 0.86 V was defined as the "initial catalytic activity." Rate of maintenance of activity
[0060] The fuel cell cell tested for initial catalytic activity was repeatedly charged and discharged 2,000 times, and then remeasured for IV. The ratio (%) of the current value after the charge and discharge test relative to the current value of the initial catalytic activity was calculated. This value was defined as the "activity maintenance rate." Results
[0061] The results are shown in the following table. Table 1 BET specific surface area (m 2 / G) average particle size (nm) Standard deviation (nm) initial catalytic activity (A / g@0.86V) Rate of maintenance of activity (%) Example 1 1000 3,0 1,0 0,46 67 Example 2 1000 3,5 1,1 0,46 72 Example 3 800 3,7 1,2 0,37 68 Comparison example 1 1000 3,8 1,4 0,47 56 Comparison example 2 1000 2,2 0,9 0,35 57 Comparison example 3 600 5,1 1,3 0,19 63
[0062] Each of Examples 1 to 3 had a relatively small catalyst metal particle size, so the initial catalytic activity was high. When the catalyst metal particle size is small, there is a concern that the activity maintenance rate would be reduced, but unexpectedly, the activity maintenance rate was high. Although this is not theoretically limiting, it is believed to be due to the uniform particle size of the catalyst metal particles.
[0063] Comparative Example 1 had an average particle size of the catalyst metal particles within the preferred range and sufficient initial catalytic activity, but it had a large standard deviation and the particle size of the catalyst metal particles was not uniform. As a result, the activity maintenance rate became low. Comparative Example 2 had a small average particle size of the catalyst metal particles, so the initial catalytic activity was sufficient, but because the average particle size was too small, even when the particle size of the catalyst metal particles was uniform, the activity maintenance rate fell. Comparative Example 3 had a large average particle size of the catalyst metal particles, so the activity maintenance rate was high, but the initial catalytic activity became low.
Claims
[1] Manufacturing method for an electrode catalyst for a fuel cell, which comprises catalyst metal particles containing a platinum or a platinum alloy and carrier particles supporting the catalyst metal particles, wherein the carrier particles consist of a carbonaceous material with a BET specific surface area of 700 m 2 / g or more and 2500 m 2 / g or less, wherein the catalyst metal particles have an average particle size of 2.5 to 4.5 nm and wherein a standard deviation of the particle size of the catalyst metal particles is 1.30 nm or less, and the manufacturing process comprising: bringing a platinate solution into contact with the carrier particles, using an alcohol as a reducing agent to reduce the platinate at 60 °C to 90 °C for 1 hour to 3 hours to assist in metal forming the catalyst metal particles on the support particles, and heat-treating the support particles supporting the metal forming the catalyst metal particles in an inert atmosphere or reducing atmosphere, the heat-treating being carried out: at 830 °C to 880 °C within 2 hours, or at 880 °C to 920 °C within 1.5 hours, or at 920 °C to 980 °C within 0.8 hours, whereby heat treatment means keeping the temperature within the specified range. [2] A manufacturing process according to claim 1, wherein the carrier particles are made of a carbonaceous material having a BET specific surface area of 900 to 1500 m 2 / g were produced. [3] The manufacturing method according to claim 1 or 2, wherein the catalyst metal particles have an average particle size of 2.8 to 3.8 nm and wherein the standard deviation of the particle size of the catalyst metal particles is 0.95 to 1.15 nm. [4] A manufacturing process according to any one of claims 1 to 3, wherein the catalyst metal particles contain an alloy of a platinum and a cobalt with a molar ratio of 4 to 1 to 11 to 1.
Citation Information
Patent Citations
Fuel cell electrode catalyst layer and manufacturing method therefor, and membrane electrode assembly, fuel cell, and vehicle using catalyst layer
CA2998075A1
Electrode catalyst for a fuel cell and method for its production, and cathode, anode and fuel cell containing the electrode catalyst
DE102015105503A1
Electrode catalyst, catalyst-carrying electrode, fuel cell and MEA therefor
JP2005166409A
Membrane-electrode assembly for fuel cell and fuel cell system including the same
JP2005317546A
Electrode catalyst for fuel cell
JP2009140657A