Wear protection element for a shredding device and use

A ceramic material composition with specific aluminum and zirconium oxide ratios enhances wear resistance and fracture toughness, addressing the high wear issues in shredding devices by enabling quick and cost-effective element replacement.

DE102019201097B4Active Publication Date: 2024-11-28F L SMIDTH & CO AS
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
DE102019201097
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-01-29
Publication Date
2024-11-28
Estimated Expiration
2039-01-29

AI Technical Summary

Technical Problem

Existing wear protection elements in shredding devices suffer from high wear and tear, leading to frequent replacements and significant downtime, especially in production chains where such devices are critical.

Method used

A ceramic material composition comprising 65-85% aluminum oxide, 12-18% tetragonal zirconium oxide, 0.1-6% cubic zirconium oxide, and 1-5% monoclinic zirconium oxide, with optional doping and specific grain sizes, is used to create wear protection elements that are highly wear-resistant and fracture-resistant, allowing for easy replacement and reducing downtime.

Benefits of technology

The ceramic material provides enhanced wear resistance and fracture toughness, minimizing downtime and maintenance costs by ensuring quick and efficient replacement of worn-out elements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Wear protection element for a comminution device, wherein the wear protection element comprises a ceramic material, wherein the ceramic material comprises: - between 65 wt.% and 85 wt.% aluminium oxide, - between 12 wt.% and 18 wt.% tetragonal zirconia, - 0.1 wt.% to 6 wt.% cubic zirconia, - 1 wt.% to 5 wt.% monoclinic zirconia, and - less than 25 wt.% zirconium oxide, wherein the mean grain size of the aluminum oxide is between 300 nm and 1000 nm, wherein the mean grain size of the zirconium oxide is between 100 nm and 500 nm, characterized in that the ceramic material contains 0.01 wt.% to 5 wt.% LaAl 11 O 18 and has a porosity of less than 3%, where the D 90 The pore size value is less than 50 µm.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to hard bodies or wear protection elements and the use thereof, in particular for partial insertion into recesses, for example on the surface of comminution devices for the pressure comminution of granular material.

[0002] The surfaces of shredding devices are subject to high levels of wear. Such surfaces must meet at least the following requirements: They should be highly wear-resistant, be cost-effective to manufacture, exhibit good feed characteristics for the material to be shredded, and, if necessary, be repairable, at least in part, by the operator of the shredding device.

[0003] To protect such surfaces, a grid plating can be used, for example, in which pin-shaped profile elements are inserted into blind holes. The pin-shaped profile elements are replaceable and can be designed to be particularly wear-resistant.

[0004] Grinding rollers, which are used in particular for so-called material bed comminution, face the problem of high wear on the roller surface. It is known that this wear can be counteracted by different designs and coatings of the roller surfaces exposed to wear. For example, the roller surface has pin-shaped profile bodies that are spaced apart from one another in such a way that, during operation of the grinding roller, a portion of the material to be crushed is deposited in the spaces between them, forming autogenous wear protection. Depending on the material to be crushed, the aforementioned profile bodies are omitted and the roller surface is provided with a build-up weld, which can be applied to the roller surface in various patterns.

[0005] Hammer mills are typically used to crush materials such as ore-containing material streams or carbon-containing material streams and / or residues from pig iron production, such as various types of slag. These mills have at least one rotor to which percussive hammers are mounted, spaced circumferentially from one another. Such a hammer mill is known from EP 1 128 908 B1.

[0006] When crushing ores, especially nickel ores, the impact hammers often experience significant wear, which can lead to severe damage or even destruction of the hammer mill. Replacing the impact hammers is very time-consuming and costly.

[0007] DE 10 2006 010 042 A1 discloses a hard body for wear protection of roller surfaces.

[0008] A mill with sintered particles of aluminum oxide and zirconium oxide is known from US 2012 / 0082849 A1.

[0009] EP 2 513 009 B1 discloses a composite material made of aluminum oxide as a ceramic matrix with zirconium oxide dispersed therein.

[0010] EP 2 513 010 B1 discloses a composite material made of aluminum oxide as a ceramic matrix with zirconium oxide dispersed therein.

[0011] From EP 567 136 B1 a mill component comprising a sintered zirconium dioxide body is known.

[0012] WO 2014 / 029757 A1 discloses a composite material with a ceramic matrix made of zirconium oxide.

[0013] An aluminum oxide-zirconia powder is known from US 4 665 040 A.

[0014] A ceramic material containing aluminum and zirconium is known from DE 10 2007 020 473 A1.

[0015] WO 2016 / 008 970 A1 describes a process for producing ceramic grains.

[0016] EP 0 729 927 A1 describes ceramic articles made of alumina and processes for their production.

[0017] JP H11-157918 A describes the production of a sintered zirconia dispersion alumina compact with high strength, high thermal shock resistance and high abrasion resistance.

[0018] EP 1502 650 A1 describes a grinding roller with a roller base body and a plurality of wear protection elements made of hard metal.

[0019] WO 2011 / 083 023 A1 describes a ceramic composite material consisting of the main components aluminum oxide and zirconium oxide and a dispersoid phase.

[0020] If the wear protection elements are worn out, they must be replaced. This results in a system shutdown. This is particularly disadvantageous because shredding devices, for example, are normally part of a production chain. If this occurs, larger production areas can be affected.

[0021] The object of the invention is to create a wear protection element which is particularly wear-resistant and fracture-tough and thus results in short downtimes due to replacement.

[0022] This problem is solved by the wear protection element having the features specified in the independent claims. Advantageous further developments emerge from the subclaims and the following description.

[0023] The wear protection element according to the invention for a comminution device comprises a ceramic material. According to the invention, the ceramic material comprises between 65 wt.% and 85 wt.% aluminum oxide. Furthermore, the ceramic material comprises between 12 wt.% and 18 wt.% tetragonal zirconium oxide. Furthermore, the ceramic material comprises 0.1 wt.% to 6 wt.% cubic zirconium oxide. Furthermore, the ceramic material comprises 1 wt.% to 5 wt.% monoclinic zirconium oxide. Furthermore, the ceramic material comprises less than 25 wt.% zirconium oxide.

[0024] A ceramic material with this composition has proven to be particularly wear-resistant compared to conventional ceramic materials, especially those with 92 wt.% aluminum oxide. In particular, it also exhibits higher fracture toughness, making critical failure due to fracture less likely.

[0025] In a further embodiment of the invention, the ceramic material comprises between 75 wt% and 80 wt% aluminum oxide.

[0026] In a further embodiment of the invention, the tetragonal zirconium oxide has an yttrium doping, a cerium doping or an yttrium-cerium co-doping, preferably an yttrium doping.

[0027] Doping within the meaning of the invention is to be interpreted broadly and includes, for example, the exchange of metal ions in the lattice, the incorporation of the doping element at interstitial sites or mixed oxide phases. Doping does not have to be homogeneous. Doping can, in particular, also include enrichment within the structure, for example, a nucleus of the doping element, or enrichment on the surface.

[0028] In a further embodiment of the invention, the monoclinic zirconium oxide has an yttrium doping, a cerium doping or an yttrium-cerium co-doping, preferably an yttrium doping.

[0029] The ceramic material contains 0.01 wt% to 5 wt% LaAl 11 O 18 This leads in particular to a reduction in the size of the aluminum oxide particles. For example, the LaAl 11 O 18 needle-shaped.

[0030] According to the invention, the mean grain size or the average grain size of the aluminum oxide is between 300 nm and 1000 nm. Preferably, the D 90 Grain size value below 10 µm, particularly preferably below 5 µm.

[0031] According to the invention, the mean grain size or the average grain size of the zirconium oxide is between 100 nm and 500 nm. Preferably, the D 90 Grain size value below 2000 nm, particularly preferably below 1000 nm.

[0032] In a further embodiment of the invention, the aluminum oxide is at least partially doped with lanthanum.

[0033] In a further embodiment of the invention, the ceramic material comprises between 2 wt% and 6 wt% lanthanum oxide.

[0034] The ceramic material has a porosity of less than 3%, preferably less than 2%, particularly preferably less than 1%. The D 90 The pore size is less than 50 µm, preferably less than 30 µm. Large pores, in particular, increase the risk of breakage.

[0035] In a further embodiment of the invention, the wear protection element has a cylindrical shape, wherein the wear protection element can be inserted into a blind hole as a pin-shaped profile body.

[0036] In a further embodiment of the invention, the wear protection element is plate-shaped. Plate-shaped wear protection elements can be, in particular, angular, in particular square, rectangular or hexagonal, round, or oval. For the purposes of the invention, "plate-shaped" refers in particular to a wear protection element with a flat surface, where "flat" for the purposes of the invention means that the radius of curvature of the surface is at least 10 times larger than the edge length of the plate-shaped wear protection element.

[0037] In a further embodiment of the invention, the wear protection element has a thickness of 3 to 350 mm, preferably of 15 to 200 mm, particularly preferably of 25 to 100 mm.

[0038] In a further embodiment of the invention, the ceramic material is bonded to a base plate via an elastomer layer. Polyurethane or rubber, as well as mixtures thereof, can be used as the elastomer layer.

[0039] In a further embodiment of the invention, the wear protection element comprises a composite material, wherein the composite material consists of the ceramic material and a metal, in particular a hard metal.

[0040] In a further embodiment of the invention, the comminution device is a crusher or a mill, in particular a high-pressure roller mill.

[0041] A grinding roller for a roller mill for comminuting granular material comprises, for example, a roller base body having a plurality of edge protection devices on at least one roller end. At least one of the edge protection devices has a wear protection element and a fastening element, wherein the fastening element is arranged and configured such that it fastens a plurality of wear protection elements to the roller base body. In particular, the wear protection elements are detachably fastened to the roller base body.

[0042] The roller mill is preferably designed for crushing granular material such as limestone, ores or clinker and is used in the cement and mineral industries.

[0043] In particular, at least one edge protection device comprises a fastening element to which a plurality of wear protection elements are attached. The wear protection elements are attached to the roller base body by means of the fastening element.

[0044] The grinding roller preferably has a plurality of edge protection devices on at least one end face, which are circumferentially mounted adjacent to one another on the roller base body and, in particular, form a closed ring. The edge protection devices are attached to the radially outward-facing edge of at least one end face of the grinding roller to prevent wear on the respective grinding roller edge.

[0045] Preferably, the fastening element is designed and arranged on the grinding roller in such a way that it fastens two to six, in particular four, wear protection elements to the grinding roller. The wear protection elements are clamped in particular by means of the fastening element.

[0046] A fastening element that attaches a plurality of wear protection elements to the roller base body offers the advantage of quick and easy replacement of the wear protection elements of an edge protection device. It eliminates the need to attach each of the wear protection elements individually to the roller base body. This allows for significant time savings during both assembly and disassembly of the wear protection elements. Furthermore, damaged wear protection elements can be specifically replaced with new and / or reconditioned wear protection elements, resulting in significant cost savings.

[0047] A grinding track preferably comprises at least one base plate designed to withstand the forces acting on the grinding track during comminution of the material to be ground. The base plate has, for example, a curved plate shape to form a cylindrical or semi-tubular grinding track.

[0048] A wear protection assembly that is detachably attached to the base plate offers the advantage that, in the event of wear, only the wear protection assembly needs to be replaced. Removing or replacing the entire base plate is not necessary. This results in significant cost and time savings. Furthermore, the wear assembly is significantly lighter than the base plate, making it considerably easier to replace.

[0049] The wear protection assembly is preferably attached to the base plate by means of screws, with the carrier plate being screwed to the base plate. A screw connection allows for easy removal of the wear protection assembly from the base plate without having to remove the base plate from the grinding track.

[0050] The wear protection arrangement extends, for example, over the entire surface of the base plate, so that it does not come into contact with the material to be crushed and is therefore subject to no or only very minimal wear. According to a first embodiment, a plurality of wear protection arrangements are arranged side by side on the base plate. This realizes a modular design of the grinding track, in particular the base plate, enabling targeted replacement of areas exhibiting high levels of wear.

[0051] A grinding track for a comminution device, in particular a hammer mill or a vertical mill, comprises, for example, at least one base plate and at least one wear protection arrangement mounted on the base plate, which comprises a carrier plate and a wear protection mounted on the carrier plate, wherein the wear protection arrangement is detachably fastened to the base plate.

[0052] A grinding track comprises, for example, the grinding track of a hammer mill, wherein the grinding track is stationary and impact hammers mounted on a rotor rotate relative to the grinding track, so that the material to be ground is comminuted between the impact hammers and the grinding track. A grinding track further comprises a grinding track of a vertical mill, in particular the surface of a grinding table and / or a rolling element rolling thereon or the roller element carrier.

[0053] A percussion hammer for a hammer mill for comminuting materials, in particular material flows, comprises, for example, a hammer head and at least one wear protection element attached to the hammer head, wherein the hammer head comprises a high-temperature-resistant steel and the wear protection element comprises a ceramic material.

[0054] The materials to be crushed, in particular material streams, preferably comprise material streams containing ore or carbon and / or material streams containing residues from pig iron production, such as various types of slag.

[0055] High-temperature-resistant steel is defined as a heat-resistant steel with a high chromium-nickel content, which has a temperature resistance of up to 650 °C, especially up to 1000 °C. Examples of such steels include austenitic chromium-nickel steels, such as GX25CrNiSi18-9, GX40CrNiSi25-12, and GX40NiCrSiNb35-26. Examples of high-temperature-resistant steels up to 600 °C are steels according to DIN EN 10213. Examples of high-temperature-resistant steels up to 1200 °C are steels according to DIN EN 10295.

[0056] A percussion hammer installed in a hammer mill is attached to a rotor rotating about a rotational axis. During operation of the hammer mill, the percussion hammer rotates about the rotational axis of the hammer mill rotor, with the front of the hammer head facing in the direction of rotation of the hammer mill rotor and forming the impact surface for the material to be crushed. The wear protection elements are preferably arranged on the front of the hammer head. For example, wear protection elements are also arranged on the side surfaces and the outer surface of the hammer head, which faces radially outward during rotation.

[0057] A hammer head made of high-temperature-resistant steel and attached wear protection elements made of ceramic materials enable the use of such a percussion hammer for comminuting hot material. Temperatures of approximately 500 to 1000 °C occur, for example, during the comminution of ores, particularly during nickel ore grinding, where hot gases are used to dry the ores before or during grinding. In particular, to dry the ores, hot gases flow through the comminution device during grinding. This hot gas flow simultaneously conveys the material to be comminuted through the comminution device and is therefore in direct contact with the percussion hammer.

[0058] In particular, the combination of the hammer head made of high-temperature-resistant steel and the wear protection element made of a ceramic material enables reliable wear protection for applications in a high-temperature range from 500 °C to approximately 1000 °C. Furthermore, the high-temperature-resistant steel of the hammer head exhibits less hardness loss at high temperatures, such as those encountered during ore crushing, compared to, for example, general structural steel. Therefore, the high-temperature-resistant steel exhibits less wear, ensuring a secure fit of the wear protection elements in the hammer head.

[0059] The high-temperature-resistant steel also allows the surface of the hammer head to be machined, allowing recesses to be created without great effort, for example, by milling, to accommodate the wear protection elements. The use of high-temperature-resistant steel also enables the targeted attachment of the wear protection elements to the most wear-intensive areas of the hammer head, particularly to the radially outer areas of the hammer head during operation. Wear protection elements do not need to be attached to the less wear-prone areas of the hammer head, as the steel used exhibits low wear, particularly at high temperatures. This results in simple and cost-effective production of the impact hammers. Furthermore, the hardness and wear properties of the high-temperature-resistant steel are not affected by a brazing process.

Claims

[1] Wear protection element for a comminution device, wherein the wear protection element comprises a ceramic material, wherein the ceramic material comprises: - between 65% and 85% by weight of aluminium oxide, - between 12 wt% and 18 wt% tetragonal zirconium oxide, - 0.1 wt% to 6 wt% cubic zirconium oxide, - 1 wt% to 5 wt% monoclinic zirconium oxide, and - less than 25 wt.% zirconium oxide, the average grain size of the aluminium oxide being between 300 nm and 1000 nm, the average grain size of the zirconium oxide being between 100 nm and 500 nm, characterized by that the ceramic material contains 0.01 wt% to 5 wt% LaAl 11 O 18 and has a porosity of less than 3%, wherein the D 90 The pore size value is less than 50 µm. [2] Wear protection element according to claim 1, characterized bythat the tetragonal zirconium oxide has an yttrium doping, a cerium doping or an yttrium-cerium co-doping. [3] Wear protection element according to one of the preceding claims, characterized by that the monoclinic zirconium oxide has an yttrium doping, a cerium doping or an yttrium-cerium co-doping. [4] Wear protection element according to one of the preceding claims, characterized by that the aluminum oxide is at least partially doped with lanthanum. [5] Wear protection element according to one of the preceding claims, characterized by that the ceramic material has a porosity of less than 2%, particularly preferably less than 1%. [6] Wear protection element according to one of the preceding claims, characterized by that the wear protection element has a cylindrical shape, wherein the wear protection element can be inserted into a blind hole as a pin-shaped profile body. [7] Wear protection element according to one of claims 1 to 6, characterized by that the wear protection element is plate-shaped. [8] Wear protection element according to claim 7, characterized by that the ceramic material is connected to a base plate via an elastomer layer. [9] Wear protection element according to one of the preceding claims, characterized by that the wear protection element has a thickness of 3 to 350 mm, preferably 15 to 200 mm, particularly preferably 25 to 100 mm. [10] Use of a wear protection element according to one of the preceding claims for a comminution device.

Citation Information

Patent Citations

  • Hard body for the autogenous wear protection of roll surfaces

    DE102006010042A1

  • Ceramic material, its use and sintered shaped body

    DE102007020473A1

  • Mill parts

    EP0567136B1

  • Alumina ceramic articles having cubic spinel on surfaces and methods for preparing alumina ceramic articles and for sintering

    EP0729927A1

  • Hammer crusher

    EP1128908B1