Silicon-based wafers and methods for the production of silicon-based wafers
By employing a controlled TDM process with defined silicon oxide layer thickness on an amorphous silicon substrate, the production of silicon wafers with optimized crystallite structure addresses inefficiencies in existing methods, enhancing mechanical integrity and solar cell efficiency.
Patent Information
- Application Number
- DE102020132900
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-10
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-12-10
AI Technical Summary
Existing methods for producing silicon-based wafers, particularly for polycrystalline silicon absorbers in solar cells, face inefficiencies due to high material loss and thickness requirements that exceed the necessary thickness for sunlight absorption, leading to mechanical integrity issues and reduced efficiency due to defect distribution and charge carrier recombination at grain boundaries.
A process involving a substrate with an amorphous silicon layer covered by a native silicon oxide layer, followed by partial or complete removal of the native oxide layer and growth of a crystalline silicon layer using the Temperature Difference Method (TDM) with controlled silicon oxide layer thickness, resulting in stochastically oriented crystallites with defined edge lengths.
This process reduces material waste, enhances mechanical integrity, and minimizes charge carrier recombination, enabling higher efficiency in solar cells by controlling the crystallization process and optimizing the structure of the silicon wafers.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a method for producing silicon-based wafers and the wafers themselves. Technological background
[0002] The largest market segment for solar cells today consists of those with polycrystalline silicon absorbers. For these, large blocks of silicon are pre-formed to be developed into wafers during further processing (bulk forming). The various bulk wafer forming processes all involve working from the melt, which means temperatures exceeding 1414 °C for silicon (Si). During processing, a significant portion of the material is lost during sawing. To maintain mechanical integrity, the final wafers retain a thickness of over 150 µm. This thickness also represents a waste of material, as complete absorption of sunlight requires only 50 µm of silicon.
[0003] Alternatives include bottom-up growth methods on inexpensive (glass) substrates, such as the temperature difference method (TDM). The temperature difference method is a specialized form of liquid phase epitaxy (LPE). LPE is a group of primary forming processes for thin crystalline films made of semiconductor materials. LPE generally utilizes solution differences between the material to be deposited (usually an elemental semiconductor such as silicon) in a metallic solvent (in the case of silicon, for example, molten tin (Sn) or indium (In)). An example of LPE is the deposition of crystalline gallium arsenide (GaAs) from gallium (Ga) solution. For this, arsenic (As) is dissolved in molten Ga at temperatures near, but below, the melting point of GaAs. After contact with a crystalline substrate, the temperature is slowly lowered.This lowers the equilibrium ratio of the components in the melt, and GaAs precipitates. Deposition via LPE occurs near energetic equilibrium and therefore produces high-quality crystals (Baliga, BJ (1986) 'Silicon Liquid Phase Epitaxy: A Review', Journal of the Electrochemical Society, 133(1), pp. 5C-14C).
[0004] With silicon as the deposition material, TDM utilizes the solubility difference of silicon in molten tin at different temperatures. Unlike conventional LPE processes, the temperature is not reduced over time, but rather maintained continuously between the silicon source and the substrate. At an example source temperature of around 605 °C, this results in a solubility of 0.346 × 10⁻⁶. 3 at-% silicon in tin, while the solubility at 600°C on the substrate is only 0.31·10 -3The temperature difference is at-%. Due to the mixing of the melt, the melt at the source is always slightly undersaturated and at the substrate always supersaturated. Ultimately, this leads to crystal formation and growth. Compared to conventional bulk molten silicon processes, TDM thus enables process temperatures far below the melting point of silicon and therefore avoids impurities in the silicon that can negatively affect the electrical properties of the polycrystalline silicon absorber. TDM can be used on various substrates, but its strength lies in growth on amorphous silicon (a-Si) substrates on glass. Here, TDM creates crystalline nuclei in the a-Si and then grows them epitaxially into crystallites.
[0005] The efficiency of a solar cell is influenced, among other things, by the fact that the smaller the crystallites, the lower the achieved efficiency. This relationship is due to the defect distribution and, in part, to the recombination of optically generated charge carrier pairs at electrically active grain boundaries. The defect distribution in polycrystalline silicon and the resulting charge carrier lifetime profile are determined by the incorporation of defects directly during crystallization and the subsequent cooling phase. Therefore, there is particular interest in being able to selectively influence the crystallization processes in order to obtain an optimal microstructure of the polycrystalline silicon.
[0006] The following approaches to microstructure control in primary forming from melts have been described so far (Easton, MA, Qian, MA and StJohn, DH (2016) 'Grain Refinement in Alloys: Novel Approaches', Reference Module in Materials Science and Materials Engineering, pp. 1-7): • Finer structure through inoculation with fine particles: When high-melting or poorly soluble particles are added to a melt, they act as nucleation centers when the solidification temperature is undershot, thus ensuring an increased number of crystallites. • Finer microstructure through the addition of elemental microstructures: In metals, the addition of alloying elements that preferentially segregate at the grain boundaries leads to a stronger tendency for nucleation. Boron is known to act as such a grain former in many metals. • Coarser structure due to slow cooling: due to slower cooling, fewer nuclei form when the solidification temperature is undershot, or the nucleation reaction is disadvantaged compared to the growth reaction.
[0007] However, these approaches cannot be readily transferred to bottom-up growth methods, so there is a continuing need for efficient methods for microstructure control. Further examples can be found in DE 10 2010 044 014 A1 and US 2006 / 0 030 131 A1; as well as in Nagel, N. et al. (“The coalescence of silicon layers grown over SiO2 by liquid-phase epitaxy: I: Growth and coalescence of defect-free silicon layers”, Applied physics A. Solids and surfaces, 1993, Vol. 57, pp. 249–254) and Bansen R. et al. (“Continuous polycrystalline silicon layers on glass grown from tin solutions”, CrystEngComm, 2016, Vol. 18, no. 11, pp. 1911–1917). Summary of the invention
[0008] The invention relates to a method for producing silicon-based wafers, which comprises the sequence of the following steps: a) Providing a substrate with an amorphous silicon layer on the surface of the substrate and a native silicon oxide layer covering the amorphous silicon layer (30); b) partial or complete removal of the native silicon oxide layer and creation of an artificial silicon oxide layer with a defined thickness on the amorphous silicon layer; or c) Growth of a crystalline silicon layer on the surface of the artificial silicon oxide layer using the temperature difference method (TDM) from metallic melt.
[0009] Another aspect of the invention relates to a silicon-based wafer, comprising: a substrate with an amorphous silicon layer on the surface of the substrate; a silicon oxide layer covering the amorphous silicon layer with a layer thickness of 1 nm to 20 nm; and A crystalline silicon layer deposited directly onto the silicon oxide layer. The wafer is characterized in that the crystalline silicon layer comprises (stochastically oriented) crystallites with edge lengths of 14 µm to 16 µm, preferably 15 µm. The wafers can be produced in particular according to the inventive method.
[0010] The invention is explained in more detail below with reference to exemplary embodiments and accompanying drawings. Brief description of the characters
[0011] The figures show: Fig. Figure 1 shows the schematic sequence of the inventive method, starting from a substrate coated with an amorphous silicon layer and a silicon oxide layer lying on it. Fig. Figure 2 shows the schematic process flow of an embodiment according to the invention. Fig. Figure 3 shows the schematic process flow of a further embodiment according to the invention. Fig. Figure 4 shows images of the surface morphology of wafers produced according to the invention under the scanning electron microscope. Detailed description of the invention
[0012] The inventive method for producing silicon-based wafers comprises the sequence of the following steps. Fig. 1 illustrated steps: a) Providing a substrate 10 with an amorphous silicon layer 20 on the surface of the substrate and a native silicon oxide layer 30 covering the amorphous silicon layer 20 (directly); b) partial or complete removal of the native silicon oxide layer 30 and creation of an artificial silicon oxide layer 32 with a defined layer thickness on the amorphous silicon layer 20; c) Growth of a crystalline silicon layer 40 on the surface of the artificial silicon oxide layer 32 using the temperature difference method (TDM) from metallic melt.
[0013] According to the invention, the native silicon oxide layer 30 is partially or preferably completely removed in step b), and an artificial silicon oxide layer 32 is subsequently produced or deposited in a controlled manner with a predetermined thickness. A second alternative of step b) (this alternative is not within the scope of the invention) involves removing only part of the native silicon oxide layer 30 down to a defined thickness. In either case, both variants ultimately result in a silicon oxide layer with a defined thickness on the amorphous silicon layer 20. The variant with complete removal of the native silicon oxide layer 30 is preferred because the thickness of the native silicon oxide layer 30 can vary within a single substrate, but especially between a multitude of substrates to be treated.On the fully exposed amorphous silicon layer 20, a homogeneous artificial silicon oxide layer 32 with a uniform layer thickness can then be produced directly afterwards by controlled regrowth.
[0014] The method according to the invention enables the continuous growth of the crystalline silicon layer 40 and the targeted formation of (stochastically oriented) large crystallites with edge lengths of 14 µm to 16 µm, preferably 15 µm, resulting in a reduction of charge carrier recombination processes at the grain boundaries. The quality of the microstructure is ensured by scanning electron microscopy followed by optical evaluation. Grain boundaries are defined here as the interfaces between two single crystals (crystallites) of the same material with different spatial orientations. The thickness of the crystalline silicon layer 40 is preferably 50 µm and is determined by profilometry.
[0015] Furthermore, the process allows for the storage of the substrates from step a) for any desired length of time, since the adjustment of the defined layer thickness of the silicon oxide layer in step b), which determines the microstructure (morphology) of the crystalline silicon layer, preferably takes place promptly, in particular immediately before step c). Due to the thus adjustable morphology of the crystalline silicon layer and the overall small layer thickness of the wafer produced according to the invention, the process is particularly suitable for the production of wafers for photovoltaics, for example for thin-film solar cells.
[0016] In a preferred embodiment, the substrate consists of glass. Preferably, the substrate is covered with an amorphous silicon layer (so-called seed layer) having a layer thickness of 1 µm to 3 µm.
[0017] According to another variant, a further step is added before the above-mentioned procedure (see...). Fig. 2), in which the amorphous silicon layer 20 is applied to the provided substrate 10, for example by means of physical vapor deposition (PVD), and subsequently a native silicon oxide layer 30 is formed by passivation of the surface of the amorphous silicon layer 20 in air.
[0018] Furthermore, a functionalization layer 12 can be present between substrate 10 and amorphous silicon layer 20. Such a functionalization layer 12 can improve the adhesion between substrate 10 and amorphous silicon layer 20 and prevent delamination of the individual wafer components. An example of such a functionalization layer 12 is a layer of silicon oxide, silicon nitride, and silicon oxynitride, which is deposited onto the substrate by chemical vapor deposition.
[0019] For this purpose, the inventive method can be used in a special embodiment (see Fig. 3) further steps may be taken in which the functionalization layer 12 is applied to a provided substrate 10, followed by the deposition of an amorphous silicon layer 20, for example by means of physical vapor deposition (PVD), onto the functionalization layer 12, after which a native silicon oxide layer 30 is formed by passivation of the surface of the amorphous silicon layer 20 in air.
[0020] One aspect of the process according to the invention is to partially or completely remove the native silicon oxide layer 30 formed by passivation in air on the amorphous silicon layer 20 (also called seed layer). Subsequently, according to a preferred embodiment, the artificial silicon oxide layer 32 is grown in a controlled manner such that a predetermined layer thickness is achieved. This controlled growth can be carried out under reduced pressure. Furthermore, the controlled growth can be carried out in a hydrogen atmosphere.
[0021] It has been shown that the morphology of the subsequently deposited crystalline silicon layer 40, applied by TDM, can be controlled by precisely adjusting the thickness of the silicon oxide layer. The silicon oxide layer preferably has a thickness of 1 nm to 20 nm, and particularly preferably 5 nm to 10 nm. By precisely maintaining these layer thicknesses in the large-scale production process, solar cells with increased efficiency can be produced, particularly due to reduced defects at the grain boundaries. This is achieved with edge lengths of 14 to 16 µm, preferably 15 µm. The layer thickness can be determined by interferometry or ellipsometry.
[0022] In a preferred embodiment, the artificial silicon oxide layer is produced in step b) by hydrofluoric acid etching (so-called HF dip). The hydrofluoric acid treatment is preferably carried out with 2% to 4% hydrofluoric acid in deionized water. Furthermore, the resistance of the deionized water used should be at least 4 MΩcm.
[0023] The etching process in hydrofluoric acid can preferably last from 20 seconds to 5 minutes. Furthermore, the etching process can be followed by a rinsing step in deionized water. Subsequently, in step b), the artificial silicon oxide layer can be generated (controlled growth) under reduced atmospheric pressure, preferably in the range of 10 -5 up to 10 -8 mbar. In addition, the generation (controlled growth) of the artificial silicon oxide layer can be achieved by flying in a H2 atmosphere.
[0024] In a further preferred embodiment, the complete or partial removal of the native silicon oxide layer in step b) is carried out using a temperature difference method from a metallic melt (TDM) via a so-called melt-back step. Here, the temperature difference between the substrate and a silicon source is adjusted such that the silicon oxide layer of the substrate dissolves in a silicon-undersaturated (tin) melt and is reduced to the predetermined layer thickness or completely removed. Preferably, the temperature difference between the substrate and the silicon source is 1°C to 6°C, with the silicon source being colder. By subsequently reversing the temperature difference, the growth of the crystalline silicon layer (step c) can occur without further delay to the process (e.g., without changing the reactor).
[0025] In a further preferred embodiment, the complete or partial ablation of the native silicon oxide layer in step b) is carried out using a pulsed nanosecond laser. Ablation with a pulsed nanosecond laser can be performed under a hydrogen atmosphere to prevent uncontrolled oxidation of the amorphous silicon layer. Preferably, a pulsed laser beam with pulse durations of 0.5 to 10 ns, particularly preferably 1.4 ns, can be used. The pulse energies can range from 0.5 µJ to 100 µJ. The ablation can also be performed using a mirror-raster system. The laser can preferably be focused such that the surface lies in a concentrated but slightly defocused plane. Preferably, the exposed area can have a diameter of 25 µm to 200 µm. The laser briefly heats the surface of the silicon oxide to over 800°C, causing the silicon oxide to react with the chamber atmosphere.
[0026] Fig. Figure 4 shows images of the surface morphology of different wafers taken under a scanning electron microscope. The differences in surface morphology can be deliberately induced by varying the thickness of the silicon oxide layer. a) very large number of crystallites and dense growth layer (thin oxide layer) b) large number of crystallites and dense growth layer (middle oxide layer) c) few, large crystallites, growth layer not closed (thick oxide layer).
[0027] Fig. Figure 4b shows the morphology of a wafer produced according to the invention, which predominantly has crystallites with an edge length of 15 µm, thereby minimizing electrical recombination at the grain boundaries. Fig. 4c, on the other hand, has larger crystallites, which means that a closed layer is no longer guaranteed and more defects may occur.
Claims
[1] A process for producing silicon-based wafers, comprising the sequence of the following steps: a) providing a substrate (10) having an amorphous silicon layer (20) on the surface of the substrate (10) and a native silicon oxide layer (30) covering the amorphous silicon layer (20); b) partially or completely removing the native silicon oxide layer (30) and producing an artificial silicon oxide layer (32) with a defined layer thickness on the amorphous silicon layer (20); and c) growing a crystalline silicon layer (40) on the surface of the artificial silicon oxide layer (32) by means of the temperature difference method (TDM) from metallic melt. [2] Method according to claim 1, wherein the partial or complete removal of the silicon oxide layer (30) in step b) is carried out by etching in 2 to 4% aqueous hydrofluoric acid (HF). [3] The method of claim 2, wherein the etching is carried out in aqueous hydrofluoric acid for 20 seconds to 5 minutes. [4] Method according to claim 1, wherein the partial or complete removal of the silicon oxide layer (30) in step b) is carried out by means of the temperature difference method from metallic melt. [5] Method according to claim 1, wherein the partial or complete removal of the silicon oxide layer (30) in step b) is carried out by means of a pulsed nanosecond laser. [6] Method according to claim 5, wherein the ablation is carried out by means of a pulsed nanosecond laser under a hydrogen atmosphere. [7] Method according to claim 5 or 6, wherein the ablation is carried out by means of a pulsed nanosecond laser with pulse lengths of 0.5 to 10 ns and with a pulse energy between 0.5 and 100 µJ. [8] A method according to any one of the preceding claims, wherein the substrate is glass. [9] A process product prepared according to the process of claim 1. [10] Silicon-based wafer comprising: a substrate (10) having an amorphous silicon layer (20) on the surface of the substrate (10); a silicon oxide layer covering the amorphous silicon layer (20) with a layer thickness of 1 to 20 nm; and a crystalline silicon layer (40) deposited directly on the silicon oxide layer, characterized by that the crystalline silicon layer (40) has crystallites with edge lengths of 13 µm to 16 µm.
Citation Information
Patent Citations
Crystallization process for forming semiconductor material-containing crystalline layer for absorber layer of silicon solar cell, involves coating amorphous coating on substrate, depositing metallic solvent on amorphous layer and heating
DE102010044014A1
Method for fabricating crystalline silicon
US20060030131A1