Method for determining the aging of a single battery cell
By evaluating cell thickness changes during charge and discharge cycles, the method distinguishes between aging effects of different active materials in battery cells, enhancing control strategies and data collection for improved battery management.
Patent Information
- Application Number
- DE102023001008
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2043-03-15
AI Technical Summary
Existing methods for determining the aging of individual battery cells, particularly lithium-ion cells, fail to accurately differentiate between the aging effects caused by different active materials, leading to inefficiencies in managing and controlling the aging process.
A method that evaluates the change in cell thickness over charge and discharge cycles to identify characteristic properties of individual active materials, using plateau hysteresis and plateau heights to determine the aging of silicon, graphite, and NMC components separately, allowing for precise aging assessment.
Enables efficient management of aging processes by specifically addressing the impact of each active material, facilitating improved battery control strategies and data collection for better understanding of aging mechanisms.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The invention relates to a method for determining the aging in a single battery cell according to the type defined in more detail in the preamble of claim 1.
[0002] It is generally known from the state of the art that individual battery cells, especially lithium-ion cells, experience a volume increase or decrease with increasing charge and / or discharge. Furthermore, the volume of an individual battery cell also changes with age.
[0003] DE 10 2021 005 418 A1 now takes up this idea to determine the aging state of a single battery cell using a method based on cell thickness. The change in cell thickness of a single battery cell is recorded over the state of charge and then divided into the portion caused by charging or discharging, on the one hand, and the portion caused by the aging of the single battery cell, on the other. This allows conclusions to be drawn about the aging of the single battery cell.
[0004] However, the aging-related change in cell thickness has different effects on different materials. The publication "Volume and thickness change of NMC811|SiO x-graphite large-format lithium-ion cells: from pouch cell to active material level" by Hendrik Pegel et al. in the Journal of Power Sources 537 (2022) 231443 shows the relationships that occur here. Essentially, the result is that the total cell thickness change over a charge and discharge cycle of the individual battery cell is partly made up of the cell thickness change caused by the silicon and graphite (anode side) on the one hand, and the change caused by the manganese-nickel-cobalt material known as NMC (cathode side) on the other. The sum of the cell thickness change is therefore the sum of the cathode aging on the one hand and the sum of the anode aging on the other.
[0005] In this context, reference can also be made to LOUL[, AJ [et a].]: Volume, pressure and thickness evolution of Li-Ion pouch cells with silicon-composite negative electrodes. In: Journal of the Electrochemical Society, Vol 2017. No. 12. S. A2689-A2696. - ISSN 1945-7111. Dol: 10 1149 / 2.1691712jes.
[0006] Regarding the general state of the art, reference can also be made to US 2016 / 0 116 548 A1, which deals with the thickness measurement of battery cells.
[0007] The features of the preamble of claim 1 are known in one form or another from US 2019 / 0 178 944 A1.
[0008] The object of the present invention is to provide a method for determining the aging of a single battery cell that is improved compared to the prior art and in which conclusions can be drawn about the aging caused by the respective active material.
[0009] According to the invention, this object is now achieved by the method having the features in claim 1, and in particular in the characterizing part of claim 1. Advantageous embodiments and further developments emerge from the dependent claims.
[0010] Similar to the prior art mentioned above, the cell thickness change of the individual battery cell as a whole is recorded here. This cell thickness change over the state of charge, in particular over a charge and discharge cycle of the individual battery cell, then results in a corresponding cell thickness change curve. This curve is then evaluated for each individual battery cell to determine, based on characteristic properties, the contribution of at least one of the active materials to the cell thickness change and thus ultimately the aging of this specific active material. The characteristic properties that the individual active materials have on the cell thickness change are known in principle from the aforementioned scientific publication.These characteristic properties are now used to infer the contribution of the active material used to a cell thickness change from a recorded age-related change. This ultimately makes it possible to determine the aging of this specific active material, for example, the removal of graphite or silicon in the anode area or the loss of active material in the cathode area, for example, through plating processes or similar.
[0011] This makes it possible to specifically exclude or adjust the battery control settings that have a particularly strong impact on the aging of one or another active material. This makes it possible to effectively halt the progression of aging processes.
[0012] Furthermore, the method allows for the simple measurement of cell thickness changes to break down the influence of individual active materials on this change. This makes it relatively easy to collect data under real-world operating conditions in a fleet of electric or hybrid vehicles, which can be used to further develop our understanding of the aging processes of such individual battery cells.
[0013] In principle, the analysis of the curve according to the invention based on characteristic properties of at least one active material can be used to determine its contribution to the cell thickness change occurring over the lifetime of the individual battery cell. According to a very advantageous development, this is done accordingly for all active materials, for example, silicon, graphite, NMC, lithium metal, and lithium iron phosphate, assuming a linear relationship between the volumetric proportion of the respective active material and its influence on the cell thickness change.
[0014] For this purpose, according to the invention, a plateau hysteresis of the cell thickness change between a charging plateau and a discharging plateau is evaluated to determine silicon aging. The curve of the cell thickness change of the entire battery cell will always exhibit a characteristic plateau during charging on the one hand and a characteristic plateau above it during discharging on the other. The distance between these two plateaus is referred to here as the plateau hysteresis. This plateau hysteresis can then be evaluated to determine the proportion of this cell thickness change caused by silicon from the measured cell thickness change of the entire battery cell. In particular, it has been shown that the plateau hysteresis is significantly greater at the beginning of the life of a battery cell than when this battery cell has already aged. The silicon aging can therefore be derived from the magnitude of the plateau hysteresis.Studies have shown that silicon aging, determined by the plateau hysteresis in the characteristic cell thickness change curve for silicon, corresponds to that determined by the cell thickness change curve of the full cell. Silicon aging can therefore be determined by comparing the thickness values of the first and second plateaus.
[0015] For this purpose, according to the invention, the height of the discharge plateau of the cell thickness change is evaluated to determine graphite aging. Here, too, the height of the discharge plateau corresponds to the cell thickness change caused by graphite aging. In particular, if silicon aging is already known and thus the silicon share in the cell thickness change of the discharge plateau is known, the graphite-related share of the height of the discharge plateau can be easily deduced from the difference, so that graphite aging can be calculated accordingly. If silicon aging is known, NMC aging plays virtually no role in the area of the second discharge plateau, so its share can be neglected here without any loss of accuracy.
[0016] To determine NMC aging according to the invention, the maximum cell thickness change over the discharge state can be evaluated. Typically, this maximum will be in the range of the fully charged cell, i.e., a state of charge of 100%. A maximum occurring in this range then allows inferences to be drawn about the characteristic minimum in the cell thickness change caused by NMC that typically occurs in this range. With known values for silicon and graphite aging, NMC aging can be easily determined in this way.
[0017] According to a very advantageous development of the invention, it is therefore provided that silicon aging is determined first, then graphite aging, and finally NMC aging based on the cell thickness changes characteristic of the respective active material. This has the advantage that the known plateau height in the cell thickness change caused by the silicon can already be included in the determination of graphite aging, and that the other two values can already be taken into account in determining the absolute value of the minimum in the NMC-induced cell thickness change.
[0018] In order to be able to determine this across relevant parts and in particular the entire state of charge, a very advantageous development of the method according to the invention proposes that a value of the silicon-induced cell thickness change over the state of charge, determined from the plateau hysteresis, be used to compress a known initial curve of the silicon-induced cell thickness change at the beginning of the life cycle over the state of charge in the direction of the cell thickness change, in order to obtain an age-related curve of the silicon-induced cell thickness change over the entire state of charge during charging and discharging. The measured value of the plateau hysteresis also allows conclusions to be drawn about the cell thickness changes that occurred in the respective plateau and thus makes it possible to determine the height of the plateau in the curve accordingly.From this, a current curve of the silicon-induced cell thickness change can be calculated starting from a known curve of the silicon-induced cell thickness change at the beginning of a cell's life by compressing this curve using the determined values. This current curve thus indicates the value of the silicon-induced cell thickness change at the current aging state of the individual battery cell over the entire charging and discharging range. This curve can then be subtracted from the measured overall curve to obtain the proportion of graphite- and NMC-induced cell thickness change at the current aging state. To determine this, characteristic ranges for the respective material are used, in particular the height of the final charge plateau in the sense described above for determining the graphite-induced cell thickness change and thus ultimately the graphite aging.
[0019] Analogous to the use of the value recorded from the plateau hysteresis for the silicon-related cell thickness change, a known curve at the beginning of the life of the single battery cell can now be compressed accordingly for the proportion of the graphite-related cell thickness change from the height of the discharge plateau for the graphite-related cell thickness change, in order to obtain not only the age-related silicon-related cell thickness change but also the age-related graphite-related cell thickness change as a new curve in the current aging state of the single battery cell.
[0020] In particular, these two curves can be used to determine the proportion of the cell thickness change of the entire cell caused exclusively by the NMC, in order to easily and efficiently identify the peak in the minimum of the NMC curve and, from its size, to determine the NMC-related cell thickness change and thus the aging state of the NMC, essentially the cathode.
[0021] Specifically, according to an advantageous embodiment, the cell thickness difference between a charging plateau of the cell thickness change versus state of charge curve and a discharge plateau of this curve can be evaluated to determine silicon aging. A decreasing distance between the plateaus, i.e., a decreasing plateau hysteresis, indicates greater silicon aging.
[0022] According to an advantageous development, to determine graphite aging, a graphite-related height of the discharge plateau can be determined from the difference between the recorded height from the cell thickness change curve of the full battery single cell and the previously determined silicon-related height change of the discharge plateau. As the size or height of the graphite-related cell thickness change of the discharge plateau decreases, greater graphite aging is then inferred. Furthermore, using the two previously determined aging values, it can be provided that the respective maxima of the cell thickness change, which are caused by silicon and graphite, are determined during full charge, and that the minimum of the cell thickness change due to NMC occurring during full charge is determined from the difference between the total maximum and the graphite- and silicon-related maxima. As the absolute value of the minimum decreases, increasing NMC aging is inferred.
[0023] Simply by evaluating the corresponding characteristics in the curve, it is possible to easily and efficiently determine the breakdown of the aging-related cell thickness change among the various active materials involved, i.e., their influence on the respective amount of cell thickness change. As already mentioned above, this can be used to improve the control or operating strategy for such a battery, as well as for comprehensive data collection to further analyze and understand aging processes in such individual battery cells.
[0024] The method according to the invention is explained in detail below using an exemplary embodiment, for which reference is made to the following figures.
[0025] Showing: Fig. 1 a diagram of the methodology applied with the process according to the invention; Fig. 2 a schematic representation of the percentage expansion of the individual battery cell in percent over the state of charge, with curves for the entire cell, the anode, essentially made of silicon and graphite, and the cathode made of NMC being shown; Fig. 3 two curves of the percentage expansion in percent of the cell thickness, i.e. the cell thickness change over the state of charge, once at the beginning of the life of a single battery cell (a) and in an aged state (b); Fig. 4 the silicon-related share of the cell thickness change according to Fig. 3; Fig. 5 the graphite-related part of the cell thickness change analogous to Fig. 3 and Fig. 4; and Fig. 6 the NMC-related contribution to the cell thickness change analogously or in addition to the Fig. 3, Fig. 4 and Fig. 5.
[0026] In the presentation of the Fig. Figure 1 is a flowchart describing the methodology of the procedure presented here. The first block, labeled 1 on the far left, describes the in-operando measurement in a vehicle. This measurement records the change in the expansion of a single battery cell as a function of the state of charge. This is also referred to below as cell thickness change and essentially represents the percentage change in the thickness of the single battery cell over the state of charge, starting from an empty single battery cell to full charge and then to the next discharge.
[0027] The middle block of the diagram of the Fig. 2, which is designated here with 2, essentially describes a battery control unit 2. Based on the in-operando measurement 1 in the vehicle, the measured cell thickness change over the state of charge is then transmitted to this battery control unit 2. In a first block 2a, the theoretical knowledge about the distribution of the cell thickness change among its components determined by the respective active material is then applied in order to establish a relationship between the cell thickness change and the aging of the active materials over the aging of the individual battery cell. This is symbolized by the block designated 2b. The corresponding target information 3 is then used further, either in the battery control unit itself to adapt the control system to minimize the aging effects, or to collect data that helps to better understand the aging.
[0028] In the presentation of the Fig. Figure 2 shows the percentage expansion of the cell thickness, referred to below as the cell thickness change, expressed as a percentage change over the state of charge. This curve represents the initial state of a single battery cell at the beginning of its life. The cell thickness change varies between -1% and approximately +5.5%. The state of charge has full charge in the middle, so that discharging is shown to the left of the middle and charging is shown to the right of the middle. Charging takes place to the left of the middle, hence on the x-axis from 0% to 100% SOC is in the middle, and then discharging to the right of the middle, from 100% SOC to 0% SOC. The in-operando measured cell thickness change is indicated by the solid, bold curve. It is broken down into the individual components, first into the cathode component, which is shown with a dotted line, and then the anode component, which is shown with a two-dotted line.The proportion of the cathode-related cell thickness change x over the state of charge (SOC) essentially corresponds directly to the NMC-related aging, as this is the main material of the cathode. The anode-related cell thickness change is in turn divided into the two active materials of the anode: silicon on the one hand and graphite on the other. The silicon-related cell thickness change is shown with a dashed line, the graphite-related cell thickness change with a dotted line. This is also maintained in the following figures, although a repeated representation of the anode-related cell thickness change, which is in fact only the sum of the silicon-related and graphite-related cell thickness changes, will be omitted below.
[0029] As already mentioned, in the in-operando measurement 1 in the vehicle, the cell thickness change x is measured over the state of charge SOC in the block labeled 1. In the representation of the Fig. 3a this is analogous to the representation in Fig. 2 is shown again in the diagram alone. The state in the diagram of the Fig. 3a shows the state of cell thickness change at the beginning of the life of the battery single cell. In addition, in the Fig. Figure 3b shows essentially the same curve, i.e., the cell thickness change x of the entire cell, at a later time point, with increased aging of the individual battery cell. Each curve indicates an unknown superposition of the proportions of the individual active materials in the respective aging state (a), b).
[0030] This curve also already shows some characteristic elements such as a final loading plateau marked 4 and a loading plateau marked 5 as well as a maximum marked 6, which are characteristic points or areas of the curve both in Fig. 3a, at the beginning of the life of the battery cell, as well as in Fig. 3b, i.e. in an already aged single battery cell.
[0031] The difference between the final loading platform 4 and the loading platform 5 is in Fig. 3a as Δx P,Z,1 In the case of the cell thickness change x of the aged battery single cell, this difference between the charging plateau 5 and the discharge plateau 4 is also shown and denoted by Δx P,Z,2 The plateau hysteresis, i.e. the distance between the discharge plateau 4 and the charge plateau 5 in the direction of the cell thickness change, has noticeably decreased.
[0032] In the presentation of the Fig. 4a and in the Fig. 4b is now at the start of the life cycle of the battery single cell in Fig. 4a and in the aged battery single cell in Fig. 4b, the curve for the proportion of silicon-related aging is plotted accordingly. The silicon-related aging itself, which is often expressed as ϑ Sican therefore be calculated from the ratio of the current plateau hysteresis Δx P,Z,2 and the plateau hysteresis of the new battery single cell Δx P,Z1 This value, multiplied by 100, gives the percentage value for silicon aging or a silicon aging degree. Fig. 4a, b it can now be seen that the values of the plateau hysteresis Δx determined from the cell thickness change of the single battery cell P,Z,1 , Δx P,Z,2 those in the silicon curve Δx P,Si,1 Δx P,Si,2 This means that: ϑSi=ΔxP,Si,2ΔxP,Si,1⋅100=ΔxP,Z,2ΔxP,Z,1,1⋅100
[0033] This correspondence now allows the entire curve to be Fig. 2 known silicon contribution to the cell thickness change by compression in the direction of the cell thickness change.
[0034] Analogous to the previous presentation, the Fig. 5a and Fig. 5b shows the graphite-induced aging. Characteristic of the graphite-induced aging or the graphite-induced change in cell thickness x is the level of the discharge plateaus 4 above the zero line of the cell thickness change. The height x P,Ent,2 of the final loading plateau 4 of the solid curve is therefore composed of an addition of the graphite-related height x P,Gr,2 the discharge plateau 4 and the silicon-related height x P,Gr,1 of the end loading platform 4. xP,Ent,2=xP,Si,2+xP,Gr,2
[0035] Theoretically, the NMC-induced cell thickness change x P,NMC,2 the cathode plays a minimal role. In practice, however, this is so small that it can be completely neglected in the area of discharge plateau 4.
[0036] With a known silicon-related height of the discharge plateau 4 from the Fig. 4 described relationship, the graphite-related plateau height x P,Gr,2 be determined. xP,Gr,2=xP,Ent,2−xP,Si,2
[0037] The graphite aging ϑ Gr can then be removed from the plateau height x P,Gr,2 of the aged cell in relation to the plateau height x P,Gr,1 of the cell at the beginning of its life and multiply by 100 as a percentage. ϑGr=xP,Gr,2xP,Gr,1⋅100
[0038] Similar to the curve for the corresponding ageing state of the battery single cell for silicon, the graphite can now also be Fig. 2 fundamentally known initial curve according to the recorded values of the discharge plateau, so that ultimately, in addition to the curve of the cell thickness change of the single battery cell, the silicon or graphite-related cell thickness changes, shown here again as dashed and dotted lines, can be entered.
[0039] As can also be seen from the illustration in Fig. 2 is a characteristic point for determining the NMC-related cell thickness change x and thus the NMC aging ϑ NMC the minimum in the range of 100% SOC.
[0040] The known maxima of the silicon-induced cell thickness changes and, above all, the graphite-induced cell thickness changes can be offset accordingly. The total maximum x M,Z,2 in Fig. 6b is therefore made up of the sum xM,Z,2=xM,Si,2+xM,Gr,2+xM,NMC,2 together, so that ultimately x M,NMC,2can be calculated by determining the difference between the maximum in the full cell and the two silicon or graphite-related maxima. xM,NMC,2=xM,Z,2−xM,Si,2=xM,Gr,2
[0041] For NMC-related aging, the following applies: ϑNMC=xM,NMC,2xM,NMC,1⋅100
[0042] Here, too, the decreasing value of the minimum indicates increasing aging of the NMC or cathode.
Claims
[1] Method for determining the ageing of a single battery cell in a lithium-ion battery constructed from several such single battery cells, for which purpose a cell thickness change (x) of the single battery cell is recorded over the state of charge (SOC) in order to draw conclusions about the ageing of the single battery cell, whereby a curve of the cell thickness change (x) over the state of charge (SOC) during charging and discharging of the respective individual battery cell is evaluated, characterized by , that the evaluation is carried out in such a way that, based on characteristic properties of the curve, a conclusion is drawn as to the involvement of at least one of the active materials (Si, Gr, NMC) in the cell thickness change (x) and thus in the aging, whereby the silicon aging (ϑ Si ) a plateau hysteresis (Δx P ) the cell thickness change (x) between a loading plateau (5) and a final loading plateau (4) is evaluated; to determine graphite aging (ϑ Gr ) a height (x p ) of the discharge plateau (4) of the cell thickness change (x) is evaluated; and / or to determine NMC aging (ϑ NMC ) the maximum (x m ) of the cell thickness change (x) over the state of charge (SOC) is evaluated. [2] Method according to claim 1, characterized by that the aging of at least silicon (Si), graphite (Gr) and NMC is concluded, whereby a linear relationship between the volumetric fraction of the respective active material (Si, Gr, NMC) and its influence on the cell thickness change (x) is assumed. [3] Method according to claim 1, characterized by that first the silicon aging (ϑ Si ), then the graphite aging (ϑ Gr ) and finally the NMC aging (ϑ NMC ) is evaluated based on the recorded proportions of the cell thickness change (x). [4] Method according to one of claims 1 to 3, characterized bythat at least one of the plateau hysteresis (Δx P ) is used to compress a known initial curve of the silicon-related cell thickness change (x) over the state of charge (SOC) in the direction of the cell thickness change (x) in order to obtain a curve of the cell thickness change (x) over the entire state of charge (SOC) during charging and discharging that corresponds to the current aging. [5] Method according to one of claims 1 to 4, characterized by that at least one from the height (x P ) of the discharge plateau (4) is used to compress a known initial curve of the graphite-induced cell thickness change (x) over the state of charge (SOC) in the direction of the cell thickness change (x) in order to obtain a curve of the cell thickness change (x) corresponding to the current aging over the entire state of charge (SOC) during charging and discharging. [6] Method according to one of claims 1 to 5, characterized bythat to determine the silicon aging (ϑ Si ) the plateau hysteresis (Δx P ) of the cell thickness change (x) between the loading plateau (5) and the final loading plateau (4) is evaluated, whereby a reduction in the plateau hysteresis (Δx P ) to a higher silicon aging (ϑ Si ) is closed. [7] Method according to claim 6, characterized by that to determine the graphite aging (ϑ Gr ) a graphite-related height (x p,Gr ) of the discharge plateau (4) from the difference between the recorded height from the curve of the full cell and the previously determined silicon-related height (x P,si ) of the discharge plateau (4) is determined, whereby with decreasing graphite-related height (x P,Gr ) to a higher graphite aging (ϑ Gr ) is closed. [8] Method according to claims 6 and 7, characterized by that with known silicon and graphite aging (ϑ Si , ϑ Gr ) the respective maxima (xM ) of the cell thickness change (x), which is caused by silicon (Si) and graphite (Gr), are determined at full charge, so that the minimum occurring at full charge (x M,NMC ) of the cell thickness change (x) by NMC from the difference between the total maxima and the Gr- and Si-related maximum (x M ), whereby with decreasing amount of the minimum (x M,NMC ) to increasing NMC aging (ϑ NMC ) is closed.
Citation Information
Patent Citations
Method for determining the aging state of a battery cell, and monitoring device
DE102021005418A1
Circuitry and techniques for determining swelling of a battery / cell and adaptive charging circuitry and techniques based thereon
US20160116548A1
Battery fuel gauges, battery management systems, and methods of managing battery life cycle
US20190178944A1