METHOD FOR MANUFACTURING A SEMICONDUCTOR DEVICE

By optimizing impurity concentrations and ion implantation energies in JTE regions, the semiconductor device achieves high withstand voltage and reliability, addressing avalanche breakdown issues.

DE112013006513B4Active Publication Date: 2024-11-14MINEBEA POWER SEMICON DEVICE INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE112013006513
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2013-03-05
Filing Date
2013-12-10
Publication Date
2024-11-14
Estimated Expiration
2033-12-10

AI Technical Summary

Technical Problem

Existing semiconductor devices face issues with insufficient withstand voltage and reliability due to high impurity concentration differences between JTE regions, leading to avalanche breakdown and reduced performance.

Method used

The semiconductor device is manufactured with specific impurity concentration ranges for the first and second JTE regions, minimizing concentration differences and optimizing ion implantation energies to reduce electric field concentration at the JTE region boundaries.

Benefits of technology

The solution results in a semiconductor device with high withstand voltage and reliability, exceeding 90% of ideal performance, and maintains integrity under harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for manufacturing a semiconductor device, wherein the semiconductor device is a Schottky diode, and wherein in the method: the semiconductor device is formed with a main transition region on a drift region (2) with an n-type conductivity and a p-type JTE region (6) that is formed adjacent to the main transition region, in the JTE area (6) a first JTE area (7) and a second JTE area (8), whose fault concentration is lower than that of the first JTE area (7), are provided, the first JTE area (7) is provided in such a way that it is sandwiched between sections of the second JTE area (8), the fault concentration in the first JTE area (7) to 4.4 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or is placed below it, and the fault concentration in the second JTE area (8) is reduced to 2 × 10 17 cm-3 or is placed below it, and the first JTE area (7) and the second JTE area (8) are formed by a multi-stage ion implantation with first ion implantation energies for the first JTE area (7) and second ion implantation energies for the first and second JTE areas (7, 8), wherein the highest ion implantation energy of the first ion implantation energies is made lower than the second ion implantation energies.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a method for manufacturing a semiconductor device. TECHNICAL BACKGROUND

[0002] Non-Patent Document 1 discloses a vertical pn diode in which a JTE (junction termination extension) region formed in a termination region of the diode is divided into two regions by using two implantation cans.

[0003] The vertical pn diode described in Non-Patent Document 1 comprises a vertical pn junction structure of an n + -conducting SiC substrate, an n - -conducting drift region, a p +-conducting main junction, a cathode and an anode and a termination structure provided with a JTE region consisting of an annular first JTE region (high concentration implantation region) and an annular second JTE region (low concentration implantation region) on the surface of the n - -conducting drift region.

[0004] The first JTE region and the second JTE region, as described in Non-Patent Document 1, are formed by multi-stage ion implantation of a p-type impurity such as Al, and the implantation dose ratio between them is 3 to 1. Although not described in Non-Patent Document 1, the maximum implantation energy in both the first JTE region and the second JTE region is 700 keV, as explained in the presentation at the meeting.

[0005] Non-Patent Document 2 discloses that an impurity concentration of a first JTE region is 2 × 1019 cm -3 and an impurity concentration of a second JTE region is 2 × 10 18 cm -3 or 2 × 10 17 cm -3 is.

[0006] Non-Patent Document 3 discloses that the broadening of the concentration distribution of Al ion-implanted into SiC in the depth direction depends on the implantation energy. PRIOR ART DOCUMENTS NON-PATENT DOCUMENTS Non-patent document 1: KAJI, Naoki [et al.]: Design and fabrication of 20 kV-class SiC PiN diodes with space-modulated JTE. In: Kōen yokōshū, 2012 shūki: (73.) Ōyō Butsuri Gakkai gakujutsu kōenkai ; Matsuyama, September 11-14, 2012. Tōkyō : Ōyō-Butsuri-Gakkai, 2012. Art. 12p-H7-6 (1 p.) - ISBN 978-4-86348-276-0 Non-patent document 2: PÉREZ, Raúl [et al.]: Planar edge termination design and technology considerations for 1.7-kV 4H-SiC PiN diodes. In: IEEE Transactions on Electron Devices, Vol. 52, 2005, No. 10, pp. 2309-2316. ISSN 0018-9383. Non-patent document 3: MOCHIZUKI, Kazuhiro ; ONOSE, Hidekatsu: Dual-Pearson approach to model ion-implanted Al concentration profiles for high-precision design of high-voltage 4H-SiC power devices. In: Materials Science Forum, Vol. 600-603, 2008, pp. 607-610. ISSN 1662-9752. PATENT DOCUMENTS

[0007] US 2009 / 0 212 301 A1, DE 10 2006 056 139 B4, DE 10 2010 060 229 A1, US 2013 / 0 140 582 A1 and US 2012 / 0 132 924 A1 disclose further conventional semiconductor devices. SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0008] Because the impurity concentration could not be specified based on the description of Non-Patent Document 1 and the content of the presentation, an experimental test was conducted with the impurity concentration changed. It was found that the withstand voltage was insufficient in some cases.

[0009] In order to understand the existing phenomenon, the inventors conducted a device simulation test in which the Al ion implantation dose was varied in a range disclosed in Non-Patent Document 1 up to 2 × 10 13 cm -3 This showed that although an avalanche breakdown occurred near the surface when the surface charge density described in Non-Patent Document 2 was 7 x 10 12 cm -2 an avalanche breakthrough at the boundary between the first JTE area and the second JTE area (for example, a boundary indicated by a reference number 9 in Fig. 8) near a gap between the JTE region and the drift region (typically at a depth of about 0.7 to 0.9 µm, but depending on the withstand voltage) when the interfacial charge density was less than 7 × 10 12 cm -2 was.

[0010] The first JTE region and the second JTE region, as disclosed in Non-Patent Document 2, have very high impurity concentrations, and the impurity concentration of the first JTE region is ten times higher than that of the second JTE region. Accordingly, an avalanche breakdown is likely to occur at a boundary between a first JTE region and a second JTE region (for example, a boundary indicated by a reference numeral 9 in Fig. 8) in a diode with a high withstand voltage such as a 3.3 kV diode, causing the reduction in withstand voltage.

[0011] An object of the present invention is to provide a semiconductor device with a high withstand voltage and high reliability. MEANS TO SOLVE THE PROBLEM

[0012] The above object is achieved by the manufacturing methods defined in the claims. These include, among other things, the following steps: forming a semiconductor device having a main junction region on a drift region with an n-type conductivity and a p-type JTE region formed adjacent to the main junction region; providing a first JTE region and a second JTE region having an impurity concentration lower than that of the first JTE region in the JTE region; providing the first JTE region so that it is sandwiched between the second JTE regions; setting the impurity concentration in the first JTE region to 4.4 x 10 17 cm -3or above and 8 x 10 17 cm -3 or below and setting the impurity concentration in the second JTE region to 2 x 10 17 cm -3 or below in the case of a Schottky diode and setting the impurity concentration in the first JTE region to 6 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or below and setting the impurity concentration in the second JTE region to 2 × 10 17 cm -3 or below in the case of a junction barrier Schottky diode.

[0013] It should be noted that it is desirable that the impurity concentration difference between the first JTE region and the second JTE region in a pn junction depth is substantially eliminated so that the first JTE region and the second JTE region have almost the same impurity concentration.

[0014] It is also desirable that the ratio between the width and the spacing of the second JTE regions in an in-plane direction decreases according to the distance from the main transition region. EFFECTS OF THE INVENTION

[0015] According to the present invention, a semiconductor device having a high withstand voltage and high reliability can be provided. BRIEF DESCRIPTION OF THE DRAWING

[0016] They show: Fig. 1 is a plan view of a semiconductor device according to a first embodiment, Fig. 2 is a sectional view of the semiconductor device according to the first embodiment, Fig. 3 is a plan view of a semiconductor device according to a second embodiment, Fig. 4 is a sectional view of the semiconductor device according to the second embodiment, Fig. 5 is a graph showing a concentration distribution of Al in the depth direction in a JTE region of the semiconductor device according to the first embodiment and the second embodiment; Fig. 6 is a graph showing a concentration distribution of Al in the depth direction in a JTE region of a semiconductor device according to the first embodiment and the second embodiment; Fig. 7 is a graph showing a concentration distribution of Al in the depth direction according to a comparative example, and Fig. 8 is a sectional view of a semiconductor device according to the comparative example. DETAILED DESCRIPTION OF PREFERRED EMBODIMENTS

[0017] Embodiments of the present invention are described below. First embodiment

[0018] Fig. 1 is a plan view of a semiconductor device (protective films and others are omitted) according to the first embodiment, and Fig. 2 is a sectional view of the semiconductor device.

[0019] The semiconductor device according to the first embodiment is a Schottky diode with a SiC substrate. This semiconductor device includes a drift layer 2, which is an n-type semiconductor region formed by epitaxial growth on a semiconductor substrate 1, a Schottky electrode 10 formed in a main junction region located on an upper surface of the drift layer 2, a p-type semiconductor region 3, into which a p-type impurity such as Al is implanted and which forms a guard ring around the Schottky electrode 10, and a cathode 4 formed on the back surface of the semiconductor substrate 1. Furthermore, the semiconductor device includes a JTE (Junction Termination Extension) region 6, which consists of a ring-shaped p-type semiconductor region so as to surround the main junction region.

[0020] The semiconductor substrate 1 is an n +-conductive semiconductor substrate consisting mainly of SiC in which an n-type impurity such as N is implanted at a high concentration.

[0021] The drift layer is a n - -conductive semiconductor layer consisting primarily of SiC, into which an n-type impurity such as N is implanted. Its impurity concentration is lower than that of the semiconductor substrate 1.

[0022] The JTE region 6 consists of high impurity density regions (first JTE regions) 7 and low impurity density regions (second JTE regions) 8, and the ratio between the width and the spacing of the second JTE regions gradually increases in a direction outward from the main junction 3.

[0023] According to the first embodiment, the first JTE region and the second JTE region are formed by multi-stage Al ion implantation using the following ion implantation energies.

[0024] First ion implantation energy (first JTE region): 25, 55, 95, 150, 220 and 320 keV.

[0025] Second ion implantation energy (first JTE region and second JTE region): 25, 55, 95, 150, 220, 320 and 450 keV.

[0026] The maximum Al concentration (peak concentration in the box profile) in the first JTE area is 6 × 10 17 cm -3 and the maximum Al concentration of the second JTE region is set to 2 × 10 17 cm -3 However, by making the highest ion implantation energy for a highly doped region (first ion implantation energy) lower than the second ion implantation energy, the concentration difference between the first JTE region and the second JTE region in the horizontal direction at the depth of the pn junction becomes almost zero, as shown by the Al concentration distribution in Fig. 5 is shown.

[0027] As a comparison example, Fig. 7 shows an Al concentration distribution in the depth direction in the case where the first ion implantation and the second ion implantation are performed with the same implantation energy as in Non-Patent Document 1. In this example, a large discontinuity in the Al concentration distribution in the horizontal direction (substrate in-plane direction) occurs at a depth (depth of 0.7 to 0.9 μm) of a pn junction formed between the drift layer 2 and the JTE region 6. In particular, unlike the case where the ion implantation energy is set to a value as high as 700 keV as in Non-Patent Document 1, the Al ion lattice guidance cannot be ignored when the ion implantation energy is less than or equal to 450 keV as disclosed in Non-Patent Document 3.Specifically, if the Al ion implantation of the first JTE region and the second JTE region is carried out with an implantation dose ratio of 3 to 1 between the first JTE region and the second JTE region as in Non-Patent Document 1 and with the same multi-stage energy with a maximum value of 450 keV or less, the Al concentration even in the depth remains 0.6 μm or more in a graph of the Al concentration distribution in the depth direction as shown in FIG. Fig. 7, its state. Therefore, the diode can be connected to the Fig. 8 can only achieve an actual withstand voltage of at most about 70% of the ideal withstand voltage in the case where the diode has an infinite size, namely in the case where there is no peripheral region and the diode can be regarded as a one-dimensional structure in the vertical direction.

[0028] On the other hand, the Fig. 1 has a withstand voltage exceeding 90% of the ideal withstand voltage in the case where the diode has an infinite size. This is believed to be because the concentration values ​​of the first JTE region and the second JTE region are matched, and the concentration difference between the first JTE region and the second JTE region in the horizontal direction at the depth of the pn junction is almost zero, so that an electric field is less likely to concentrate at a boundary between the first JTE region and the second JTE region.

[0029] Also, the field intensity of a protective insulating film (in Fig. 2 not shown) at the outermost edge position of the second JTE region at the maximum Al concentration (peak concentration in the box section) in the JTE region according to the first embodiment is not 2 MV / cm, so that the problem of breakdown of the insulating film does not occur in the measurement of the initial characteristics.

[0030] Furthermore, as a result of the measurement in which the diode was kept at 125°C for 1000 hours while setting the reverse bias voltage to 80% of the rated withstand voltage and then cooled to room temperature while applying the reverse bias voltage, no breakdown of the Schottky diode was observed upon application of a voltage less than or equal to an initial withstand voltage. This is believed to be because the maximum concentration of the first JTE region is high, and accordingly, the withstand voltage is not affected even under the harsh test condition where the interfacial charge density is 7 x 10 12 cm -2 exceeds.

[0031] Also, the withstand voltage of the Schottky diode exceeded 90% of the ideal withstand voltage when the maximum Al concentration in the first JTE region was set to 4 × 10 17 cm -3 and the maximum Al concentration in the second JTE area was set to 2 × 1017 cm -3 However, as a result of the measurement in which the diode was kept at 125 °C for 1000 hours while maintaining the reverse bias voltage at 80% of the rated withstand voltage, and then cooled to room temperature while applying the reverse bias voltage, a breakdown of the Schottky diode was observed upon application of a voltage less than or equal to the initial withstand voltage. The presence of a positive charge with a density of approximately 1 x 10 12 cm -2 up to 2 x 10 12 cm -2at an interface between an insulating film and the semiconductor in an initial state was known in the case of a semiconductor device using SiC, and it is assumed that the interface charge changes to a larger positive value during the test, thereby reducing the withstand voltage and causing the breakdown of the Schottky diode. When the maximum Al concentration in the first JTE region is increased to 6 × 10 17 cm -3 and the maximum Al concentration in the second JTE area was set to 2 × 10 17 cm -3 as was the case according to the first embodiment, no breakdown of the Schottky diode was observed at all. Another test was then carried out in which the maximum Al concentration in the first JTE region was gradually increased from 4.0 × 10 17 cm -3 to 4 × 10 16 cm -3 was increased, while the maximum Al concentration in the second JTE region was fixed at 2 × 1017 cm -3 As a result of the test, it was found that no breakdown of the Schottky diode occurred when the maximum Al concentration in the first JTE region was greater than or equal to 4.4 x 10 17 cm -3 Furthermore, it was also found that the initial withstand voltage itself was reduced when the maximum Al concentration in the first JTE region was increased to 8.4 x 10 17 cm -3 Accordingly, the range of maximum concentration of the first JTE region is desirably between 4.4 × 10 17 cm -3 and 8 × 10 17 cm -3 to achieve a Schottky diode as a high reliability semiconductor device.

[0032] As described above, according to the first embodiment, it is possible to increase the withstand voltage of a semiconductor device such as a Schottky diode using SiC and thus achieve high reliability of the semiconductor device. Second embodiment

[0033] Fig. 3 is a plan view of a semiconductor device according to the second embodiment, and Fig. 4 is a sectional view of the semiconductor device.

[0034] The main difference from the first embodiment is that the first JTE regions are arranged discretely under the Schottky electrode 10 and annularly around the Schottky electrode 10 instead of the p-type semiconductor region 3 using a guard ring, thereby forming a JBS diode. The implantation energy of the first JTE region and the second JTE region is the same as that of the first embodiment, and the implantation dose of the first JTE region is controlled such that the maximum Al concentration in the first JTE region has three values, such as 4.4 × 10 17 cm -3 (not shown), 6 × 10 17 cm -3 ( Fig. 5) and 8 × 10 17 cm -3 ( Fig. 6), and the implantation dose of the second JTE region is controlled so that the maximum Al concentration in the second JTE region is 2 × 10 17 cm -3 becomes ( Fig. 5 and Fig. 6).

[0035] In the JBS diode manufactured according to the second embodiment, when the maximum Al concentration in the first JTE region is 4.4 × 10 17 cm -3 was reduced to 60% of the ideal withstand voltage in the case where the diode had an infinite size. This is believed to be due to the maximum Al concentration in the first JTE region of 4.4 × 10 17 cm -3 was too low for the replacement of the p-type semiconductor region 3 according to the first embodiment. However, if the maximum Al concentration in the first JTE region was 6 × 10 17 cm -3 and 8 × 10 17 cm -3 was, the withstand voltage exceeded 90% of the ideal withstand voltage in the case where the diode had an infinite size. Then, when the maximum Al concentration in the first JTE region was 6 x 10 17 cm -3 and 8 × 10 17 cm -3In the measurement in which the diode was kept at 125 °C for 1000 hours in the state where the reverse bias voltage was applied to 80% of the rated withstand voltage, and then cooled to room temperature while the reverse bias voltage was applied, no breakdown of the JBS diode was observed at all when a voltage less than or equal to an initial withstand voltage was applied. Accordingly, the range of the maximum concentration of the first JTE region is desirably between 6 × 10 17 cm -3 and 8 × 10 17 cm -3 to achieve a JBS diode as a high reliability semiconductor device.

[0036] According to the second embodiment, it is possible to achieve a JBS diode type semiconductor device using SiC with high reliability and also to avoid a process in which the p-type semiconductor region 3 is formed as a guard ring according to the first embodiment, thereby reducing the manufacturing cost of the semiconductor device.

[0037] The present invention has been described above specifically based on embodiments. However, it goes without saying that the present invention is not limited to the above embodiments, and various modifications and alterations can be made within the scope of the present invention. List of reference symbols 1 semiconductor substrate 2 Drift area 3 p-conducting semiconductor region 4 Cathode 6 JTE area 7 First JTE area with high implantation dose 8 Second JTE area with small implantation dose 9 Example of the position of an avalanche breakthrough 10 Schottky electrode

Claims

[1] A method of manufacturing a semiconductor device, wherein the semiconductor device is a Schottky diode, and wherein in the method: the semiconductor device is formed with a main junction region on a drift region (2) having an n-conductivity and a p-conducting JTE region (6) formed adjacent to the main junction region, in the JTE region (6) a first JTE region (7) and a second JTE region (8) whose impurity concentration is lower than that of the first JTE region (7) are provided, the first JTE region (7) is provided so as to be sandwiched between sections of the second JTE region (8), the impurity concentration in the first JTE region (7) to 4.4 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or below, and the impurity concentration in the second JTE region (8) is set to 2 × 10 17 cm-3 or below, and the first JTE region (7) and the second JTE region (8) are formed by a multi-stage ion implantation with first ion implantation energies for the first JTE region (7) and second ion implantation energies for the first and second JTE regions (7, 8), wherein the highest ion implantation energy of the first ion implantation energies is made lower than the second ion implantation energies. [2] A method of manufacturing a semiconductor device, wherein the semiconductor device is a junction barrier Schottky diode, and wherein in the method: the semiconductor device is formed with a main junction region on a drift region (2) having an n-conductivity and a p-conducting JTE region (6) formed adjacent to the main junction region, in the JTE region (6) a first JTE region (7) and a second JTE region (8) are provided, the impurity concentration of which is lower than that of the first JTE region (7), the first JTE region (7) is provided so as to be sandwiched between sections of the second JTE region (8), the impurity concentration in the first JTE region (7) to 6 × 10 17 cm -3 or above and 8 × 10 17 cm -3 or below, and the impurity concentration in the second JTE region (8) is set to 2 × 10 17 cm -3 or below, and the first JTE region (7) and the second JTE region (8) are formed by a multi-stage ion implantation with first ion implantation energies for the first JTE region (7) and second ion implantation energies for the first and second JTE regions (7, 8), wherein the highest ion implantation energy of the first ion implantation energies is made lower than the second ion implantation energies. [3] A method of manufacturing a semiconductor device according to claim 1 or 2, wherein the ratio between the width and the pitch of the portions of the second JTE region (8) decreases according to the distance from the main junction region.

Citation Information

Patent Citations

  • semiconductor device with an improved structure for high withstand voltage

    DE102006056139B4

  • Semiconductor device with semiconductor zones, manufacturing process for this and integrated circuit

    DE102010060229A1

  • Double Guard Ring Edge Termination for Silicon Carbide Devices and Methods of Fabricating Silicon Carbide Devices Incorporating Same

    US20090212301A1

  • Silicon carbide semiconductor device and manufacturing method therefor

    US20120132924A1

  • Semiconductor device and method for manufacturing same

    US20130140582A1