Solid electrolyte, its manufacturing process and gas sensor

A solid electrolyte with adjacently arranged low concentration phase particles in partially stabilized zirconia addresses thermal expansion issues, ensuring high reliability and stability in gas sensors by matching thermal expansion coefficients with dissimilar materials, preventing damage in high-temperature conditions.

DE112018005236B4Active Publication Date: 2024-11-07DENSO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE112018005236
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-11-03
Filing Date
2018-10-12
Publication Date
2024-11-07
Estimated Expiration
2038-10-12

AI Technical Summary

Technical Problem

The difference in thermal expansion coefficients between solid electrolytes made of partially stabilized zirconia and dissimilar material components, such as alumina or spinel, leads to damage like peeling and cracking in gas sensors, especially in high-temperature environments, which are increasingly required for vehicles to meet fuel efficiency and emissions regulations.

Method used

A solid electrolyte composed of partially stabilized zirconia with stabilizer low and high concentration phase particles, where low concentration phase particles are arranged adjacently, reducing thermal stress and forming a thermally stable phase, thereby matching the thermal expansion coefficient of dissimilar materials.

Benefits of technology

The solution prevents damage from thermal expansion differences, ensuring high reliability and stability of the gas sensor even in high-temperature environments exceeding 1,000°C, reducing peeling and cracking between the solid electrolyte and dissimilar material components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

solid electrolyte (1), comprising: partially stabilized zirconium dioxide (2) in which a stabilizer forms a solid solution in zirconium dioxide, wherein: the partially stabilized zirconium dioxide as crystal particles (3) which configure the partially stabilized zirconium dioxide as follows: stabilizer low-concentration phase particles (33) whose stabilizer concentration at a particle center (O) is less than 4.7 mol%, and stabilizer high-concentration phase particles (34) whose stabilizer concentration at the particle center (O) is greater than 4.7 mol%, and an adjacent particle section (35) in which two or more particles of the stabilizer low-concentration phase particles, whose average particle size is greater than or equal to 0.1 µm, are arranged adjacently; a frequency fraction of the stabilizer high-concentration phase particles on a cross-section of the solid electrolyte with respect to an area ratio relative to all crystal particles is greater than or equal to 70%; and the areas of the adjacent particle segments (35) are areas of circles having radii which are half the length of the respective particle sizes, and the presence of the adjacent particle segments (35) can be confirmed by a SEM / EDX analysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a solid electrolyte made of partially stabilized zirconia, its manufacturing method, and a gas sensor including the solid electrolyte. State of the art

[0002] A gas sensor element is used in an exhaust system of an internal combustion engine and the like for the purpose of detecting oxygen concentration, air-fuel ratio, and the like in the exhaust gas. Such a gas sensor element uses an oxide ion-conductive solid electrolyte such as zirconium dioxide.

[0003] For example, PTL 1 discloses a ceramic laminate including a solid electrolyte layer. Such a ceramic laminate is used in gas sensors and the like. The solid electrolyte layer is used, for example, in a state where the solid electrolyte layer is in contact with a dissimilar material component made of alumina or the like. The solid electrolyte layer is used, for example, in a state where the solid electrolyte layer is in contact with a dissimilar material component of a ceramic heater including alumina.Additionally, the solid electrolyte is used in a cup-type gas sensor having a bottomed cylindrical solid electrolyte in a state where the solid electrolyte is in contact with a dissimilar material component, a protective layer covering a surface of the solid electrolyte and made of spinel or the like, or a state where the solid electrolyte is covered with an approximately 1 µm electrode by a protective layer. The protective layer is formed, for example, by plasma spraying.

[0004] Furthermore, PTL 2 and PTL 3 disclose prior art solid electrolyte materials. Patent literature PTL 1: JP 2000-202406 A PTL 2: WO 2012 / 105579 A1 PTL 3: JP 2009-104990 A Summary of the invention

[0005] However, a difference in thermal expansion coefficient may occur between the solid electrolyte made of partially stabilized zirconia and the component made of a dissimilar material. Therefore, during a cooling / heating cycle, damage may occur between the solid electrolyte and the component made of a dissimilar material, which is attributed to the difference in thermal expansion coefficient. In a gas sensor, for example, the difference in thermal expansion coefficient leads to the occurrence of peeling and cracking between the solid electrolyte and the ceramic heater, the protective layer, and the like.

[0006] In recent years, due to changes in mounting positions and the like, reliability in even higher-temperature environments has been required for on-board or in-vehicle gas sensors, for example, as vehicles are required to comply with strict fuel efficiency and emission regulations. However, with the popularity of hybrid vehicles, cars with automatic start-stop systems, and the like, frequent engine stopping and starting has become more common. In addition, heaters are often turned off during stops to reduce power consumption. Therefore, high reliability is required with regard to an increase in load during the cooling / heating cycle.

[0007] In this case, the solid electrolyte used in gas sensors and the like also requires additional stability during the cooling / heating cycle. This means, for example, stability is required in a higher temperature range exceeding 1,000°C. In a conventional solid electrolyte, stability can be improved.

[0008] An object of the present invention is to provide a solid electrolyte, a manufacturing method thereof, and a gas sensor using the solid electrolyte, in which the solid electrolyte is capable of preventing damage caused, for example, by a difference in a coefficient of thermal expansion with a member made of a dissimilar material such as alumina or spinel.

[0009] One aspect of the present invention provides a solid electrolyte comprising partially stabilized zirconia in which a stabilizer forms a solid solution in zirconia. The partially stabilized zirconia contains stabilizer low-concentration phase particles whose stabilizer concentration at a particle center is less than 4.7 mol% and stabilizer high-concentration phase particles whose stabilizer concentration at the particle center is greater than or equal to 4.7 mol% as the crystal particles configuring the partially stabilized zirconia. The partially stabilized zirconia includes an adjacent particle section in which two or more of the stabilizer low-concentration phase particles whose average particle size is greater than or equal to 0.1 µm are adjacently arranged.The frequency fraction of the stabilizer high-concentration phase particles on a cross-section of the solid electrolyte is greater than or equal to 70% in terms of an area ratio relative to all crystal particles. The areas of the adjacent particle segments are areas of circles with radii equal to half the length of the respective particle sizes. The presence of the adjacent particle segments can be confirmed by SEM / EDX analysis.

[0010] Another aspect of the present invention provides a gas sensor including the solid electrolyte described above.

[0011] Yet another aspect of the present invention provides a manufacturing method of a solid electrolyte, the manufacturing method including: a mixing step of obtaining a mixture by mixing: a first raw material powder made of zirconia particles, a second raw material powder made of aggregated particles in which a plurality of zirconia particles are aggregated, and a stabilizer raw material powder; a molding step of obtaining a molded body by molding the mixture; and a sintering step of obtaining a solid electrolyte made of partially stabilized zirconia by sintering the molded body.The mixing step includes a first mixing step (S11) in which the first raw material powder and the stabilizer raw material powder are mixed, and a second mixing step (S12) in which, after the first mixing step, the second raw material powder is further mixed. The d50 particle size of the first raw material powder (221) is within a range of 0.2 to 0.5 µm, and the d50 particle size of the second raw material powder (222) is within a range of 1 to 5 µm.

[0012] For example, with the solid electrolyte configured as described above, the coefficient of thermal expansion approaches that of a dissimilar material component such as alumina or spinel. Therefore, damage attributed to the difference in coefficient of thermal expansion between the solid electrolyte and the dissimilar material component can be prevented. For example, with the solid electrolyte, thermal stress with the dissimilar material component can be reduced even during a cooling / heating cycle in which the solid electrolyte is exposed to a high-temperature region exceeding 1,000°C. Consequently, peeling and cracking can be prevented from occurring in a contacting portion when the solid electrolyte is used in such a manner as to be in contact with the dissimilar material component.

[0013] For example, in the solid electrolyte having the adjacent particle portion, the adjacent particle portion does not easily receive compressive stress from the high-concentration phase particles and the like in the periphery during manufacturing by sintering and the like. This is considered to be because compressive stress at particle boundaries of the two or more low-concentration phase particles configuring the adjacent particle portion is reduced. As a result, a thermally stable phase is easily formed at the adjacent particle portion during manufacturing. That is, an unstable phase is considered to be reduced. As a result, the coefficient of thermal expansion is considered to approach that of the dissimilar material component, as described above.

[0014] For example, the gas sensor described above incorporates a solid electrolyte whose thermal expansion coefficient differs from that of a component made of a dissimilar material, such as alumina or spinel, as described above. Therefore, internal damage to the gas sensor is not easily caused. The gas sensor exhibits high reliability, even withstanding high-temperature environments exceeding 1,000°C.

[0015] The above-described solid electrolyte is obtained by performing the mixing step, the molding step, and the sintering step. In the mixing step, the first raw material powder, the second raw material powder, and the stabilizer raw material powder are mixed. The second raw material powder is made of aggregated particles of zirconia particles. Such aggregated particles do not easily react with the stabilizer raw material powder during the sintering step. The stabilizer does not easily form a solid solution in the zirconia particles, which configure the aggregated particles. As a result, the above-described stabilizer low-concentration phase particles are produced. In addition, the adjacent particle portion is formed in which two or more of the stabilizer low-concentration phase particles are adjacently arranged.In this way, the solid electrolyte of the configuration described above can be obtained.

[0016] During the sintering step, compressive stress is typically applied to the zirconia particles. However, the aggregated particles have a surface that is not subjected to compressive stress. As a result, a more thermally stable phase can be easily formed during the sintering step, for example, during a temperature reduction. Therefore, the solid electrolyte obtained by the above-described manufacturing process is expected to reduce a thermally unstable phase.

[0017] As described above, according to the above-described aspects, a solid electrolyte that can prevent damage caused by a difference in a coefficient of thermal expansion with a member made of a dissimilar material such as alumina or spinel even when exposed to a high-temperature region exceeding, for example, 1,000 °C, its manufacturing method, and a gas sensor using the solid electrolyte can be provided.

[0018] Reference numerals in the parentheses in the scope of claims indicate corresponding relationships with specific means described according to embodiments described below and do not limit the technical scope of the present invention. Short description of the drawings

[0019] The above-described object, other objects, features, and advantages of the present invention will become clear from the detailed description below with reference to the accompanying drawings. An overview of the drawings is as follows: Fig. 1 is a schematic diagram of a cross section of a solid electrolyte according to a first embodiment; Fig. 2 is a schematic diagram of a microstructure of partially stabilized zirconia composing the solid electrolyte according to the first embodiment; Fig. 3 is an explanatory diagram of a particle center and a particle size of a crystal particle according to the first embodiment; Fig. 4 is an explanatory diagram of a particle size of an adjacent particle portion according to the first embodiment; Fig.5 is an explanatory diagram of a manufacturing method of the solid electrolyte according to the first embodiment; Fig. 6 is an explanatory diagram of a mixing step of raw materials according to the first embodiment; Fig. 7 is a schematic diagram of a microstructure of partially stabilized zirconia composing a solid electrolyte in Comparative Example 1; Fig. 8 is a cross-sectional view of a gas sensor according to a second embodiment; Fig. 9 is a cross-sectional view of a lamination-type gas sensor element according to the second embodiment; and Fig. 10 is an explanatory diagram of a cross section of a cup-type gas sensor element according to the second embodiment. Description of the embodimentsFirst embodiment

[0020] A solid electrolyte according to an embodiment is described with reference to Fig. 1 to Fig. 6. As shown in examples in Fig. 1 and Fig. 2, as shown by (a) and (b), a solid electrolyte 1 is made of partially stabilized zirconia 2. The partially stabilized zirconia 2 is a so-called sintered body. The partially stabilized zirconia 2 is a sintered body in which a stabilizer forms a solid solution in zirconia.

[0021] Yttrium oxide, calcium oxide, magnesium oxide, scandium oxide, ytterbium oxide, and the like are exemplified as the stabilizer. The partially stabilized zirconia may contain at least one of the foregoing as the stabilizer.

[0022] The partially stabilized zirconia 2 contains, as crystal particles 3 that configure the partially stabilized zirconia 2, stabilizer low-concentration phase particles 33 and stabilizer high-concentration phase particles 34. The stabilizer low-concentration phase particle 33 is accordingly referred to as "low-concentration phase particle 33." The stabilizer high-concentration phase particle 34 is accordingly referred to as "high-concentration phase particle 34."

[0023] The low-concentration phase particles 33 and the high-concentration phase particles 34 are the crystal particles 3 that configure the partially stabilized zirconia 2, which are classified based on the solid solution state of the stabilizer. That is, the low-concentration phase particles 33 and the high-concentration phase particles 34 are the crystal particles 3 viewed from the perspective of the solid solution state of the stabilizer. The solid solution state can also be referred to as the solid solution concentration state of the stabilizer.

[0024] The low-concentration phase particle 33 refers to the crystal particle 3 whose concentration of the stabilizer, such as yttrium oxide, at a particle center O is less than 4.7 mol%. Measurement of the stabilizer concentration is performed by measuring the concentration of metal elements, such as yttrium, in the stabilizer through scanning electron microscope / energy-dispersive X-ray spectroscopy (SEM / EDX analysis), which is described below. A specific measurement method will be described below for an experimental example.

[0025] As in an example in Fig.As shown in Figure 3, the particle center of the crystal particle 3 denotes a center of gravity of a rectangle in which the crystal particle is surrounded by maximum particle widths in a horizontal direction and a vertical direction. This similarly applies not only to the low-concentration phase particles 33, but also to the high-concentration phase particles 34.

[0026] The high-concentration phase particle 34 described above refers to the crystal particle that does not correspond to the low-concentration phase particle 33. That is, the high-concentration phase particle 34 refers to the crystal particle whose concentration of the stabilizer, such as yttrium oxide, at the particle center O is equal to or greater than 4.7 mol%.

[0027] In a production process for the partially stabilized zirconia 2, it is considered that the stabilizer forms a solid solution from the surface of a zirconia particle toward the center. It is assumed that a concentration gradient in which the solid solution concentration of the stabilizer decreases from the surface toward the center is likely to form. Therefore, it is assumed that for the high-concentration phase particle 34 whose stabilizer concentration at the particle center is equal to or greater than 4.7 mol%, the stabilizer usually forms a sufficient solid solution throughout the entire crystal particle 3. A total amount of the high-concentration phase particles 34 and the low-concentration phase particles 33 is 100%.

[0028] The partially stabilized zirconia 2 includes a contiguous particle section 35 in which two or more low-concentration phase particles 33, whose average particle size is equal to or greater than 0.1 μm, are adjacently arranged. That is, it can be considered that, in a solid solution state crystal structure of the partially stabilized zirconia 2, the low-concentration phase particle 33 forms a primary particle, and a connected particle section in which a plurality of low-concentration phase particles 33 are adjacently arranged forms a secondary particle.

[0029] If the average particle size of the low-concentration phase particles 33 configuring the adjacent particle portion 35 is less than 0.1 μm, the advantages achieved by forming the connected particle portion are lost. As a result, for example, a difference in a thermal expansion coefficient with a member made of a dissimilar material may increase. From the perspective of further reducing the difference in a thermal expansion coefficient, the average particle size of the low-concentration phase particles 33 is preferably equal to or greater than 0.2 μm, more preferably equal to or greater than 0.25 μm, and even more preferably equal to or greater than 0.3 μm.

[0030] On the other hand, from the viewpoint of further improving the material strength, the average particle size of the low concentration phase particles 33 configuring the adjacent particle portion 35 is preferably less than or equal to 1 µm, further preferably less than or equal to 0.5 µm, and even more preferably less than or equal to 0.4 µm.

[0031] As in the example in Fig. As shown in Figure 3, the particle size of the low-concentration phase particle 33 is expressed by an arithmetic mean of a length L1 in the horizontal direction and a length L2 in the vertical direction of a rectangle in which the particle is enclosed in the horizontal direction and the vertical direction by the maximum widths of the particle. The average particle size of the low-concentration phase particle 33 is an arithmetic mean of the particle sizes of at least 30 low-concentration phase particles 33.

[0032] In the adjacent particle portion 35, two or more of the low-concentration phase particles 33 are arranged adjacently. In the solid electrolyte having such an adjacent particle portion 35 in the crystal structure, for example, during sintering in the manufacture of the solid electrolyte, compressive stress is not easily experienced or absorbed by the high-concentration phase particle 34 made of a cubic phase (C phase).

[0033] One reason for this is that stress is reduced at a particle boundary of each low-concentration phase particle 33, which configures the adjacent particle section 35. Therefore, during a sintering temperature reduction process, a transformation from the tetragonal phase (T phase) to a monoclinic phase (M phase) easily occurs. As a result, the thermodynamically unstable T phase diminishes, and the solid electrolyte becomes thermodynamically stable. As a result, the difference in thermal expansion coefficient with the component made of dissimilar materials, such as alumina and spinel, decreases.

[0034] From the viewpoint of further enhancing this effect, partially stabilized zirconia 2 of the solid electrolyte preferably has the adjacent particle portion 35 in which three or more particles of the low concentration phase particle 33 are adjacently arranged, further preferably has the adjacent particle portion 35 in which five or more particles of the low concentration phase particle 33 are adjacently arranged, and still further preferably has the adjacent particle portion 35 in which ten or more particles of the low concentration phase particle 33 are adjacently arranged.

[0035] On a cross section of the solid electrolyte, the frequency ratio of the adjacent particle segments 35 in terms of an area ratio relative to the low-concentration phase particles 33 is preferably greater than or equal to 50%. That is, the frequency ratio of the adjacent particle segments 35 relative to all the low-concentration phase particles 33 is preferably greater than or equal to 50% in terms of an area ratio. In this case, the above-described effect achieved by forming the adjacent particle segments 35 is further enhanced. That is, the difference in a coefficient of thermal expansion with the component made of dissimilar materials, such as alumina and spinel, is further reduced.

[0036] Here, from a thermodynamic perspective, the low-concentration phase particles 33 can be considered the M phase. From the perspective of further reducing the difference in a thermal expansion coefficient, the frequency ratio of the adjacent particle segments 35 relative to all low-concentration phase particles 33 is further preferably greater than or equal to 70%, and even more preferably greater than or equal to 80%.

[0037] Regarding the calculation of the area ratio, the area of ​​the low-concentration phase particles 33 is calculated using a product of the ratio of a circumference of a circle to its diameter π and the particle size / 2 squared. This similarly applies to the high-concentration phase particles 34 and the adjacent particle segments 35. That is, the areas of the low-concentration phase particles 33, the high-concentration phase particles 34, and the adjacent particle segments 35 are areas of circles having radii half the length of the respective particle sizes.

[0038] The frequency ratio of the adjacent particle segments 35 is preferably 8% to 16% in terms of an area ratio relative to all the crystal particles. More specifically, the frequency ratio of the adjacent particle segments 35 is preferably 8% to 16% in terms of an area ratio relative to a total of 100% of the high-concentration phase particles 34 and the low-concentration phase particles 33. In this case, moreover, the above-described effect achieved by forming the adjacent particle segments 35 is further enhanced. That is, the difference in a coefficient of thermal expansion with the member made of dissimilar materials such as alumina and spinel is further reduced.

[0039] The average particle size of the adjacent particle segments 35 is preferably greater than or equal to 1 µm. In this case, the above-described effect of not easily experiencing the compressive stress during sintering in the production of the solid electrolyte becomes significant. Therefore, the unstable T phase is further reduced, and the difference in a coefficient of thermal expansion with the component made of dissimilar material is further reduced. From the perspective of further reducing the T phase, the average particle size of the adjacent particle segments 35 is further preferably greater than or equal to 2 µm, and even more preferably greater than or equal to 3 µm.

[0040] In addition, the average particle size of the adjacent particle segments 35 is preferably less than or equal to 5 µm. In this case, stress generated during a transition from the T phase to the M phase can be reduced. Therefore, the occurrence of cracking and the like is prevented, and the strength of the solid electrolyte is improved. From the perspective of further improving the strength, the average particle size of the adjacent particle segments 35 is further preferably less than or equal to 4 µm, and even more preferably less than or equal to 3.5 µm.

[0041] As in an example in Fig.As shown in Figure 4, the particle size of the adjacent particle segment 35 is expressed by an arithmetic mean of a length L3 in the horizontal direction and a length L4 in the vertical direction of a rectangle enclosed in the horizontal and vertical directions by the maximum widths of the particles. The average particle size of the adjacent particle segments 35 is an arithmetic mean of the particle sizes of at least 30 adjacent particle segments 35.

[0042] In addition, the frequency ratio of the high-concentration phase particles 34 on the cross section of the solid electrolyte 1 is greater than or equal to 70% in terms of an area ratio relative to all crystal particles 3. The frequency ratio of the high-concentration phase particles 34 is an area ratio occupied by the high-concentration phase particles 34 relative to all crystal particles 3, that is, a sum of the low-concentration phase particles 33 and the high-concentration phase particles 34.

[0043] When the abundance ratio of the high-concentration phase particles 34 is less than 70%, the thermal expansion coefficient of the solid electrolyte 1 decreases. As a result, for example, when the solid electrolyte 1 is used in such a manner that it is placed in contact with the dissimilar material component made of alumina, spinel (MgAl2O4) or the like whose thermal expansion coefficient is 7 to 10 ppm / °C, the difference in thermal expansion coefficient between the solid electrolyte 1 and the dissimilar material component 4 increases.

[0044] As a result, internal damage may occur within a device such as a gas sensor using the solid electrolyte 1. More specifically, peeling or cracking may occur between the solid electrolyte 1 and the dissimilar material component 4. From the perspective of further reducing the difference in a thermal expansion coefficient between the dissimilar material component 4, such as alumina or spinel, and the solid electrolyte 1, the abundance ratio of the high-concentration phase particle 34 is preferably equal to or greater than 75%, and further preferably equal to or greater than 80%.

[0045] On the other hand, from the viewpoint of a crystal system, it can be considered based on common technical knowledge that the partially stabilized zirconia 2 contains at least monoclinic phase particles 31 and cubic phase particles 32 as the crystal particles 3 configuring the partially stabilized zirconia 2.

[0046] In the following description, the monoclinic phase is accordingly referred to as the "M phase." The cubic phase is accordingly referred to as the "C phase." In addition, the partially stabilized zirconia 2 may contain a tetragonal phase. The tetragonal phase is accordingly referred to as the "T phase." The C phase, M phase, and T phase are the crystal particles 3 that configure the partially stabilized zirconia 2, which are classified based on a crystal phase structure. That is, the C phase, M phase, and T phase are crystal particles viewed from the perspective of the crystal system that configures the crystal phase. Although this is common technical knowledge, the C phase, M phase, and T phase can be determined by X-ray diffraction analysis.

[0047] Based on the crystal system, it can be considered that the high-concentration phase particle 34 is made of the C phase at room temperature. Based on the crystal system, it can be considered that the low-concentration phase particle 33 is made of the M phase or the T phase at room temperature. The low-concentration phase particles 33 contain particles made of the M phase and particles made of the T phase.

[0048] From the viewpoint of sufficiently achieving the above-described effect achieved by forming the adjacent particle portions 35, the low-concentration phase particles 33 are preferably made of the M phase. The crystal particle made of the M phase can be referred to as an M-phase particle. The coefficient of thermal expansion of the M phase is 2 to 3 ppm / °C. The crystal particle made of the C phase can be referred to as a C-phase particle. The coefficient of thermal expansion of the C phase is 10 to 11 ppm / °C. The crystal particle made of the T phase can be referred to as a T-phase particle. The coefficient of thermal expansion of the T phase is 10 to 11 ppm / °C.

[0049] As in the example in Fig.2, the low-concentration phase particles 33 and the adjacent particle portions 35 are formed on the particle boundaries of the high-concentration phase particles 34. For example, the average particle size of the low-concentration phase particles 33 is smaller than the average particle size of the high-concentration phase particles 34.

[0050] The average particle size of the high-concentration phase particles 34 is preferably greater than or equal to 1 µm. In this case, the compressive stress applied from the high-concentration phase particles 34 to the low-concentration phase particles 33 during sintering in the preparation of the solid electrolyte is reduced. As a result, the advantages achieved by forming the adjacent particle sections 35 are not easily achieved.

[0051] From the viewpoint of sufficiently achieving the above-described effect achieved by forming the adjacent particle portions 35, the average particle size of the high concentration phase particles 34 is preferably equal to or greater than 2.5 μm, and more preferably equal to or greater than 3 μm.

[0052] The average particle size of the high-concentration phase particles 34 is preferably less than or equal to 5 μm. In this case, the strength of the partially stabilized zirconia 2 itself, which configures the solid electrolyte 1, can be prevented from decreasing. From the perspective of further improving the strength, the average particle size of the high-concentration phase particles 34 is further preferably less than or equal to 4 μm, and even more preferably less than or equal to 3.5 μm.

[0053] The particle size of the high-concentration phase particles 34 is expressed as an arithmetic mean of the length L1 in the horizontal direction and the length L2 in the vertical direction of a rectangle enclosed in the horizontal and vertical directions by the maximum widths of the particles. The average particle size of the high-concentration phase particles 34 is an arithmetic mean of the particle sizes of at least 30 high-concentration phase particles 34.

[0054] For example, the solid electrolyte 1 can be used in a manner such that it is placed in contact with the dissimilar material component made of alumina, spinel, or the like. For example, during the cooling / heating cycle in which the solid electrolyte configured as described above is exposed to a high-temperature region exceeding 1,000°C, the coefficient of thermal expansion can be made equal to that of the dissimilar material component up to the high-temperature region. Therefore, thermal shock fracture damage can be sufficiently prevented even in uses in which the solid electrolyte 1 is exposed to a high-temperature region.

[0055] From the perspective of achieving the effects of the present invention, the type of stabilizer is not particularly limited. However, from the perspective of ensuring favorable chemical stability, the stabilizer is preferably made of yttrium oxide.

[0056] As in Fig.1, the solid electrolyte preferably has a contacting portion configured to contact the dissimilar material component. In this case, as a result of reducing the difference in thermal expansion coefficient between the solid electrolyte and the dissimilar material component, the effect of preventing peeling and cracking between the dissimilar material component and the solid electrolyte can be more accurately obtained. Here, the dissimilar material component is a component made of a material different from that of the solid electrolyte.

[0057] It is only required that the contacting portion be a portion that is at least partially in contact. A contact surface, for example, is also included in the contacting portion. "The solid electrolyte has a contacting portion configured to come into contact with the dissimilar material component" means that the solid electrolyte is used in such a way that it is in contact with the dissimilar material component, that is, it has a constituent portion placed in contact with the dissimilar material component. Actual contact with the dissimilar material component is not necessarily required. The solid electrolyte 1 can be used, for example, in a gas sensor. Such a solid electrolyte 1 can include a gas contacting portion configured to come into contact with a measurement gas such as exhaust gas.

[0058] Next, a manufacturing process of the solid electrolyte will be described. As shown in the examples in Fig. 5 and Fig. 6, the solid electrolyte is obtained by performing a mixing step S1, a forming step S2 and a sintering step S3.

[0059] In the mixing step S1, a first raw material powder 221, a second raw material powder 222, and a stabilizer raw material powder 211 are mixed. As a result, a mixture 20 is obtained. The first raw material powder 211 and the second raw material powder 222 are both made of zirconia. However, the second raw material powder 222 is made of aggregated particles in which a plurality of zirconia particles are aggregated. The stabilizer raw material powder 211 is made of a stabilizer such as yttrium oxide. The second raw material powder 222 is a powder whose average particle size is larger than that of the first raw material powder 221.

[0060] Yttrium oxide powder, calcium oxide powder, magnesium oxide powder, scandium oxide powder, ytterbium oxide powder, or the like can be used as the stabilizer raw material powder 211. At least one of the foregoing can be used as the stabilizer raw material powder 211.

[0061] The second raw material powder 222 can be manufactured by subjecting a raw material powder made of zirconia powder to a heat treatment. As a result of the heat treatment, the zirconia particles are aggregated together. Thus, the second raw material powder 222 made of aggregated particles is obtained. The aggregated particles can be considered secondary particles formed by aggregating the zirconia particles (i.e., primary particles).

[0062] The average particle sizes of the first raw material powder 221 and the second raw material powder 222 indicate the particle size at 50% volume integration with respect to a particle size distribution determined by a laser diffraction / scattering method. Accordingly, the particle size at 50% volume integration with respect to the particle size distribution determined by a laser diffraction / scattering method is referred to as a "d50 particle size."

[0063] The d50 particle size of the first raw material powder 221 is within a range of 0.2 to 0.5 µm. In contrast, the d50 particle size of the second raw material powder 222 is within a range of 1 to 5 µm.

[0064] The mixing step S1 further includes a first mixing step S11 and a second mixing step S12. In the first mixing step S11, the first raw material powder 221 and the stabilizer raw material powder 211 are mixed. After the first mixing step S11, in the second mixing step S12, the second raw material powder 222 is further mixed with the mixture of the first raw material powder 221 and the stabilizer raw material powder 211, and a mixture 20 is obtained.

[0065] A slurry can be prepared from the mixture 20 prior to molding. A liquid such as water, alcohol, or a liquid organic substance can be used to prepare a slurry from the mixture 20. Preferably, a water-based liquid is used. The mixture from which a slurry is prepared can be granulated.

[0066] Next, the molding step S2 is performed. In the molding step S2, the mixture 20 containing the first raw material powder 221, the second raw material powder 222, and the stabilizer raw material powder 211 is molded. As a result, a molded body is obtained.

[0067] The molding method is not particularly limited. Compression molding, compression molding, extrusion molding, injection molding, hot pressing, isotropic cold press molding, grinding, and the like can be used. As a result of molding, a molded body having a desired shape can be obtained based on an intended use. For example, molded bodies having various shapes such as a board shape, a sheet shape, a hollow sheet shape, a rod shape, a cylindrical shape, and a bottomed cylindrical shape can be obtained. Milling can be performed on the molded body if necessary.

[0068] Next, the molded body is sintered in sintering step S3. As a result of sintering, partially stabilized zirconia 2 is produced, and solid electrolyte 1 is obtained. A sintering temperature can be changed accordingly or as appropriate based on a composition and the like, but is, for example, 1,300°C to 1,500°C.

[0069] In the above-described manufacturing method, the second raw material powder 222, which is made of aggregated particles that do not easily react with the stabilizer, is used as a portion of the zirconia raw material. As a result, the above-described low-concentration phase particles 33 are formed in the sintering step. In addition, the adjacent particle portions 35 are formed. In this way, the solid electrolyte 1 according to the present embodiment can be obtained.

[0070] The solid electrolyte 1 according to the present embodiment is made of partially stabilized zirconia 2, in which the stabilizer forms a solid solution in zirconia. The partially stabilized zirconia 2 includes low-concentration phase particles 33 and high-concentration phase particles 34 as the crystal particles 3 that configure the partially stabilized zirconia 2. The frequency ratio of the high-concentration phase particles 34 is equal to or greater than 70%.

[0071] In addition, the partially stabilized zirconia 2 has the adjacent particle portion 35 in which two or more particles of the low concentration phase particles 33 whose average particle size is equal to or greater than 0.1 µm are adjacently arranged.

[0072] For example, because the solid electrolyte 1 is configured in this way, the thermal expansion coefficient of the solid electrolyte 1 approaches that of the component made of a dissimilar material, such as alumina or spinel. Therefore, damage attributed to the difference in thermal expansion coefficient between the solid electrolyte 1 and the component 4 made of a dissimilar material can be prevented.

[0073] One reason for this is that, for example, in the solid electrolyte 1 having the adjacent particle portions 35, the adjacent particle portion 35 does not easily receive compressive stress from the high-concentration phase particles 34 and the like during manufacturing by sintering and the like. That is, it is considered that one reason for this is that compressive stress at the particle boundaries of the two or more particles is reduced by low-concentration phase particles 33 that configure the adjacent particle portion 35.

[0074] As a result, it is assumed that a thermally stable phase is easily formed in the adjacent particle section 35 during manufacturing, and an unstable phase is reduced. Here, the thermally stable phase is considered the M phase, and the unstable phase is considered the T phase. That is, it is assumed that a transition from the unstable T phase to the stable M phase easily occurs in the adjacent particle section 35 during sintering, and the T phase is reduced.

[0075] Therefore, for example, with the solid electrolyte 1, thermal stress with the dissimilar material component 4 can be reduced even during the cooling / heating cycle in which the solid electrolyte 1 is exposed to a high-temperature region exceeding 1,000°C. Consequently, peeling and cracking can be prevented from occurring in the contacting portion when the solid electrolyte 1 is used, for example, in contact with the dissimilar material component 4. Comparison example 1

[0076] Next, a solid electrolyte of a comparative example will be described. A solid electrolyte 9 of a comparative example 1 is manufactured by a method similar to that of the first embodiment, except that the second raw material powder is not used.

[0077] Specifically, the first raw material powder 221 and the stabilizer raw material powder are mixed. Next, the mixture is formed into a slurry, molded, and sintered. The solid electrolyte 9 of the present example can be obtained in this way.

[0078] As in an example in Fig. 7, partially stabilized zirconia 90, which composes the solid electrolyte 9 of the present example, contains C-phase particles 91 and M-phase particles 92 as the crystal particles 3.

[0079] In the present example, the second raw material powder made of aggregated particles is not used. Therefore, a reactivity between the first raw material powder 221 and the stabilizer is high. As a result, in addition to the C-phase particles 91, the stabilizer also forms a solid solution inside the M-phase particles 92, although a solid solution state is omitted in the drawings. This can be confirmed by SEM / EDX. The solid electrolyte 9 of the present example does not have a neighboring particle portion like that according to the first embodiment. Consequently, the difference in a coefficient of thermal expansion increases with the dissimilar material member.

[0080] Therefore, the thermal expansion coefficient of the solid electrolyte tends to diverge significantly from that of the dissimilar material component, for example, during the cooling / heating cycle. As a result, the difference in thermal expansion coefficient between the solid electrolyte and the dissimilar material component becomes large, for example, when the solid electrolyte is used in contact with the dissimilar material component made of alumina, spinel (MgAl2O4), or the like.

[0081] Delamination and cracking can occur between the solid electrolyte and the component made of dissimilar materials. In particular, the divergence in the coefficient of thermal expansion increases, for example, during the cooling / heating cycle, in which the solid electrolyte is exposed to a high-temperature region exceeding 1,000 °C, and delamination and cracking occur more easily. Experimental example 1

[0082] A plurality of solid electrolytes of an experimental example and a comparative example were manufactured, and their performances were compared and evaluated. A manufacturing process for the solid electrolyte of the present example is described below.

[0083] First, an yttrium oxide powder and a zirconia powder with a d50 particle size of 0.30 µm were mixed and measured. Further, as a result of heat-treating the zirconia powder with a d50 particle size of 0.30 µm at 1,100 °C, the zirconia particles aggregated together. As a result, an aggregated zirconia powder was obtained, which was made from aggregated particles of the zirconia powder.

[0084] Next, aggregated zirconia powder was mixed with the mixture of zirconia powder and yttrium oxide powder. The zirconia powder, whose d50 particle size is 0.30 µm, corresponds to the first raw material powder, and the aggregated zirconia powder corresponds to the second raw material powder described above. The yttrium oxide powder corresponds to the stabilizer raw material powder described above. Their mixing ratio can be adjusted based on a target composition.

[0085] Next, the mixture of zirconia powder, yttrium oxide powder, and aggregated zirconia powder was mixed with water to obtain a slurry of the mixture. To increase the fluidity of the raw material particles that comprise the mixture and facilitate molding into a desired shape, the slurry of the mixture was granulated. Granulation is carried out, for example, by spray granulation.

[0086] Next, the mixture was molded, resulting in a molded body. Molding is performed, for example, by compaction. In the present example, the mixture was molded into a test mold, which will be used in the evaluations described below.

[0087] Next, the molded body was sintered at a temperature of 1,400 °C. Thus, the solid electrolyte was obtained. In the present example, the solid electrolytes of Samples 1 to 13 shown in Table 1 were manufactured by varying the average particle sizes of the raw materials, mixing ratios, and the like. Determination of low-concentration phase particles and high-concentration phase particles and confirmation of the presence of adjacent particle segments

[0088] A sample with a width of 5 mm, a length of 20 mm, and a thickness of 2 mm was cut from each sample. After the surface of the sample was ground, thermal etching was performed. Thermal etching was performed by heating the sample at a temperature of 1,200 °C for 1 hour. Y element assignment was performed on five surfaces through composition analysis using SEM / EDX analysis. Among the observed particles, the Y concentration at the particle center was measured for particles with low Y concentrations.

[0089] As a result, it was determined that particles whose Y concentration at the particle center was less than 4.7 mol% were the low-concentration phase particles. Conversely, particles whose Y concentration at the particle center was greater than or equal to 4.7 mol% were the high-concentration phase particles.

[0090] Additionally, the presence of adjacent particle segments, where a plurality of low-concentration phase particles are arranged adjacently, has been confirmed by SEM / EDX analysis. The low-concentration phase particles arranged adjacently can be confirmed, for example, by the presence of particle boundaries between the low-concentration phase particles. However, by observing an image obtained by SEM / EDX analysis, it is usually easy to confirm that the low-concentration phase particles are arranged adjacently.

[0091] The observation conditions for SEM are as follows: Apparatus: "SU8220," manufactured by Hitachi High-Technologies Corporation; accelerating voltage: 5 kV; WD setting: 8.0 mm; current: 10 mA; magnification: 10,000x. In addition, the measurement conditions for EDX are as follows: Apparatus: "XFlash 6|60," manufactured by Bruker Corporation; accelerating voltage: 5 kV; WD setting: 14 mm; current: 5 to 15 mA; magnification: 50,000x. The current was adjusted so that the acquisition amount was 40 to 55 kcps.

[0092] Next, a total of 30 low-concentration phase particles were selected from the five areas described above, and their particle sizes were measured using the method described above. The average particle size of the low-concentration phase particles was determined by the arithmetic mean of the particle sizes of the low-concentration phase particles.

[0093] In addition, the particle sizes of all low-concentration phase particles present in isolation in the image of the above-described five areas obtained by SEM / EDX analysis and the particle sizes of all adjacent particle segments were determined, respectively. The respective areas S of the low-concentration phase particles present in isolation and the adjacent particle segments were calculated from particle sizes r by an expression (1) below. Next, a frequency ratio S3 (unit: %) of the adjacent particle segments relative to all low-concentration phase particles was calculated from a total value S1 of the areas of the low-concentration phase particles present in isolation and a total value S2 of the areas of the adjacent particle segments by an expression (2) below. Each area is an area of ​​12 μm × 9 μm. S=πr2 / 4 S3=100×S2 / (S1+S2)

[0094] In addition, the frequency fraction of the neighboring particle segments relative to all crystal particles is calculated by dividing the above-described total value S2 of the areas of the neighboring particle segments by the area of ​​an observation area. The frequency fraction of the neighboring particle segments is expressed as an arithmetic mean of the frequency fractions of the five areas. The frequency fraction of the neighboring particle segments is expressed as a percentage. Frequency fraction of high concentration phase particles relative to all crystal particles

[0095] In a similar manner to the method described above, in addition to Y-element mapping performed on ten areas of the measurement sample, SEM / EDX analysis was performed. The particle sizes of all high-concentration phase particles included in the areas were measured, and the areas of the high-concentration phase particles were calculated using expression (1). The abundance ratio of the high-concentration phase particles in each area was calculated by dividing the total area of ​​the high-concentration phase particles by the area of ​​the observation area. The abundance ratio of the high-concentration phase particles is expressed by the arithmetic mean of the abundance ratios of the ten areas. The abundance ratio of the high-concentration phase particles is expressed as a percentage. Coefficient of thermal expansion

[0096] A test sample with a width of 5 mm, a length of 20 mm, and a thickness of 2 mm was cut from each sample. The thermal expansion behavior of the test samples was measured between room temperature and 1,050 °C. The room temperature was 25 °C. A thermomechanical analyzer (TMA) was used to measure the thermal expansion behavior. The TMA used was a TMA 4000 SA manufactured by Bruker AXS Corporation. A reference sample used for the measurement was a sintered body made of aluminum oxide.

[0097] The measurement was performed five times for each sample. In addition, regarding thermal expansion behavior, a gradient of 500°C to 600°C was set as the thermal expansion coefficient. Table 1 shows the average value of the measurements performed five times. One criterion for determining the thermal expansion coefficient is that, from the perspective of matching the thermal expansion coefficient with that of the dissimilar material, the sample is determined to be "good" if the thermal expansion coefficient is 8 to 9 ppm / °C, "excellent" if the thermal expansion coefficient is 8.3 to 8.7 ppm / °C, and "no good" if the thermal expansion coefficient is less than 8 ppm / °C or more than 9 ppm / °C. Table 1 Sample No. Frequency fraction of high concentration phase particles relative to all crystal particles (area ratio) Presence of adjacent particle segments Average particle size of low concentration phase particles Frequency fraction of neighboring particle sections relative to all low concentration phase particles (area ratio) Frequency fraction of neighboring particle sections relative to all crystal particles (area ratio) Coefficient of thermal expansion ppm / °C Determination 1 85 % none 0,28µm 9,5 Not good 2 86 % available 0,25µm 42 % 79,5 % 8,9 Good 3 70 % available 0,26µm 55 % 16% 8,2 Good 4 60 % available 0,26µm 80 % 30 % 7,5 Not good 5 86 % available 0,25µm 42 % 7 % 8,9 Good 6 84 % available 0,1µm 48 % 8 % 9 Good 7 84 % available 0,05µm 46 % 9 % 9,7 Not good 8 85 % available 0,31µm 50 % 8 % 8,7 Excellent 9 84 % available 0,32µm 81 % 13 % 8,5 Excellent 10 85 % available 0,35µm 80 % 7 % 9 Good 11 88 % available 0,26µm 78 % 10% 8,7 Excellent 12 80 % available 0,31µm 83 % 16% 8,3 Excellent 13 77 % available 0,32µm 77 % 18 % 8,1 Good

[0098] As can be seen from Table 1, as well as Sample 2, Sample 3, Sample 5, Sample 6 and Sample 8 to Sample 13, the coefficient of thermal expansion in the solid electrolyte whose frequency ratio of the high concentration phase particles relative to all crystal particles is greater than or equal to 70%, and in which the adjacent particle portion in which two other particles of the low concentration phase particles whose average particle size is greater than or equal to 0.1 µm are adjacently arranged is present, is 8 to 9 ppm / °C.

[0099] Therefore, with these solid electrolytes, the difference in thermal expansion coefficient with a dissimilar material component made of alumina, spinel, or the like is small. Consequently, peeling and cracking between the solid electrolyte and the dissimilar material component can be prevented during a cooling / heating cycle.

[0100] In addition, as shown in Table 1, the difference in thermal expansion coefficient with the component made of dissimilar material, such as alumina or spinel, is further reduced when the frequency ratio of the adjacent particle segments relative to the low-concentration phase particles on a cross section of the solid electrolyte is greater than or equal to 50% in terms of an area ratio. Furthermore, the difference in thermal expansion coefficient with the component made of dissimilar material is further reduced as a result of the frequency ratio of the adjacent particle segments also being set to 8 to 16% in terms of an area ratio relative to all crystal particles. Experimental example 2

[0101] In a similar manner to Experimental Example 1, a plurality of solid electrolytes are manufactured, and their performance is compared and evaluated. In this example, a performance evaluation is also conducted from the perspective of strength.

[0102] First, in a similar manner to Experimental Example 1, solid electrolytes of Samples 14 to 21 shown in Table 2 were prepared by changing the average particle sizes of the raw materials, mixing ratios, and the like. In addition to measurements similar to those in Experimental Example 1, the following measurements were also performed for each sample. Average particle size of neighboring particle sections

[0103] In a manner similar to Experimental Example 1, the presence / absence of the adjacent particle segment was confirmed, and the particle size of the confirmed adjacent particle segment was measured by the method described above. In addition, a total of 30 adjacent particle segments were selected from a plurality of areas, and the average particle size of the adjacent particle segments was determined by an arithmetic mean of the particle sizes of the adjacent particle segments. Average particle size of high concentration phase particles

[0104] In a manner similar to Experimental Example 1, a determination of the high-concentration phase particle was performed, and the particle size of the confirmed high-concentration phase particle was measured by the method described above. In addition, a total of 30 high-concentration phase particles were selected from a plurality of areas, and the average particle size of the high-concentration phase particles was determined by an arithmetic mean of the particle sizes of the high-concentration phase particles. strength

[0105] A test specimen was cut with a width of 5 mm, a length of 45 mm, and a thickness of 5 mm. A strength evaluation specimen was fabricated from the test specimen based on a four-point bending strength test described in JIS R 1601:2008. Next, the four-point bending strength test was performed based on JIS R 1601:2008. The result of this test is the strength.

[0106] The test was performed ten times for each sample. The table shows the average value of the tests. The strength was determined to be "good" at 250 MPa or more and "poor" at less than 250 MPa. For example, if the strength is less than 250 MPa, cracks may occur when the solid electrolyte is installed in a sensor or the like. Therefore, from the perspective of ensuring strength when installed in a device, the strength of the solid electrolyte is preferably 250 MPa or greater.

[0107] In addition, the sample is evaluated as "X" if the determination of either the thermal expansion coefficient or strength is "no good." In addition, the sample is evaluated as "OO" if the determination of neither the thermal expansion coefficient nor the strength is "no good" and the determination of at least one is "excellent." Furthermore, the sample is evaluated as "O" if the determinations of both the thermal expansion coefficient and strength are "good." These are evaluations of suitability when the solid electrolyte is applied to a lamination-type gas sensor element. "OO" means excellent suitability, and "O" means good suitability. "X" means poor suitability. Table 2 Sample No. Frequency fraction of high concentration phase particles relative to all crystal particles (area ratio) Presence of adjacent particle segments Average particle size of low concentration phase particles Frequency fraction of neighboring particle segments relative to all low-concentration phase particles (area ratio) Frequency fraction of neighboring particle sections relative to all crystal particles (area ratio) Average particle size of neighboring particle sections Average particle size of high concentration phase particles Coefficient of thermal expansion ppm / °C strength Evaluation 14 85 % available 0,27µm 81 % 12 % 0,5µm 3,0µm 8.8 (Good) Good O 15 86 % available 0,31µm 80 % 12 % 1,0µm 2,8µm 8.6 (Excellent) Good OO 16 84 % available 0,3µm 78 % 11 % 5,0µm 3,3µm 8.5 (Excellent) Good OO 17 86 % available 0,28µm 75 % 12 % 8,2µm 3,2µm 8.8 (Good) Not good X 18 83 % available 0,33µm 83 % 13 % 2,8µm 0,6µm 8.5 (Excellent) Good O 19 87 % available 0,32µm 75 % 11 % 3,5µm 1,0µm 8.5 (Excellent) Good OO 20 86 % available 0,32µm 80 % 12 % 3,2µm 5,0µm 8.5 (Excellent) Good OO 21 85 % available 0,28µm 86 % 12 % 3,1µm 8,2µm 8.5 (Excellent) Not good X

[0108] As can be seen from Table 2, the thermal expansion coefficient of the solid electrolyte in which the frequency fraction of the high-concentration phase particles is equal to or greater than 70% and in which the adjacent particle portion in which two other particles of the low-concentration phase particles whose average particle size is equal to or greater than 0.1 μm are adjacently arranged is present, is 8 to 9 ppm / °C. Therefore, with respect to these solid electrolytes, the difference in thermal expansion coefficient with a dissimilar material component made of alumina, spinel, or the like is small. Consequently, peeling and cracking between the solid electrolyte and the dissimilar material component can be prevented during a cooling / heating cycle.

[0109] In addition, the difference in thermal expansion coefficient with the dissimilar material is further reduced when the average particle size of the adjacent particle segments is 1 to 5 µm. Furthermore, the strength of the solid electrolyte is improved. Furthermore, the difference in thermal expansion coefficient with the dissimilar material is further reduced when the average particle size of the high-concentration phase particles is also 1 to 5 µm. Furthermore, the strength of the solid electrolyte is improved. Second embodiment

[0110] Next, an embodiment of a gas sensor 5 using a solid electrolyte will be described. Here, among the reference numerals used in the second and subsequent embodiments, reference numerals identical to those used in a previous embodiment indicate constituent elements and the like similar to those used in the previous embodiments, unless specifically stated otherwise.

[0111] As in Fig. 8 and Fig. As shown in Figure 9, the gas sensor 5 according to the present embodiment includes a sensor element 6. The sensor element 6 according to the present embodiment is a gas sensor element that detects gas. The sensor element 6 includes the solid electrolyte 1, a detection electrode 62, a reference electrode 63, and a diffusion resistance layer 66. That is, the gas sensor 5 includes the solid electrolyte 1 within the sensor element 6.

[0112] The detection electrode 62 and the reference electrode 63 are formed on both surfaces 601A and 602A of the solid electrolyte 1, respectively. The detection electrode 62 and the reference electrode 63 form a pair of electrodes formed in positions opposite to each other. The diffusion resistance layer 66 restricts a flow amount of measured gas such as exhaust gas G from reaching the detection electrode 62. The gas sensor 5 is of a limiting current type that detects an oxygen concentration (i.e., an air-fuel ratio) in the exhaust gas G based on a magnitude of a limiting current generated between the pair of electrodes 62 and 63 in a state where a voltage is applied across the pair of electrodes 62 and 63.

[0113] The gas sensor 5 according to the present embodiment will be described in detail below. Here, in the description below, a side in an axial direction X of the gas sensor 5 exposed to the measured gas, such as the exhaust gas G, is referred to as a distal end side X1, and the opposite side thereof is referred to as a base end side X2. Gas sensor

[0114] The gas sensor 5 is used in such a way that it is arranged in an exhaust pipe of an internal combustion engine of a vehicle or the like. As in the present embodiment, the limit flow type gas sensor 5 is used as an air-fuel ratio sensor that quantitatively detects the air-fuel ratio of the exhaust gas G flowing through the exhaust pipe. The gas sensor 5 can quantitatively determine the air-fuel ratio in both a case where the air-fuel ratio is on a rich side and a case where the air-fuel ratio is on a lean side.

[0115] Here, the air-fuel ratio of the exhaust gas G refers to the mixture ratio of fuel and air during combustion in an internal combustion engine. Additionally, the rich side refers to the situation where the air-fuel ratio of the exhaust gas G is such that the fuel is on the higher side compared to the theoretical air-fuel ratio when the fuel and air are completely combusted. The lean side refers to the air-fuel ratio of the exhaust gas G where the fuel is on the lower side compared to the theoretical air-fuel ratio.

[0116] In the gas sensor 5 according to the present embodiment, the air-fuel ratio of the exhaust gas is detected as a result of detecting the oxygen concentration in the exhaust gas G. The gas sensor 5, which serves as the air-fuel ratio sensor, essentially detects the oxygen concentration in the exhaust gas G on the lean side and, on the other hand, detects an unburned gas concentration in the exhaust gas G on the rich side.

[0117] As in Fig.As shown in Fig. 8, the gas sensor 5 includes, in addition to the sensor element 6, a housing 71, a distal end-side cover 72, a proximal end-side cover 73, and the like. The housing 71 is attached to the exhaust pipe and holds the sensor element 6 with an insulator 74. The distal end-side cover 72 is attached to the distal end side X1 of the housing 71 and covers the sensor element 6. The distal end-side cover 72 has a double-layer structure and is made of an inner cover 721 and an outer cover 722. The proximal end-side cover 73 is attached to the proximal end side of the housing 71 and covers a terminal 75 for electrical wiring and the like of the sensor element 6. Sensor element

[0118] As in an example in Fig.For example, as shown in Fig. 9, a lamination-type sensor element is used as the sensor element 6. That is, the sensor element 6 may be configured by a lamination body in which the reference electrode 63, the plate-shaped solid electrolyte 1, and the detection electrode 62 are sequentially laminated.

[0119] As in the example in Fig. 9, the sensor element 6 includes, for example, the plate-shaped solid electrolyte 1. The solid electrolyte 1 has a measurement gas surface 601A and a reference gas surface 602A. The measurement gas surface 601A is a surface exposed to the measured gas, such as the exhaust gas G. In contrast, the reference gas surface 602A is a surface exposed to the reference gas, such as the atmospheric air A. The measurement gas surface 601A and the reference gas surface 602A are surfaces of the solid electrolyte 1 that are arranged opposite to each other.

[0120] The detection electrode 62 is provided on the measurement gas surface 601A of the solid electrolyte 1. On the other hand, the reference electrode 63 is provided on the reference gas surface 602A. When the sensor element 6 is configured by such a lamination-type sensor element, a heat generating member 641, which configures a heater 64, is laminated onto the solid electrolyte 1 with an insulator 642. The insulator 642 is made of, for example, alumina.

[0121] The detection electrode 62 is arranged facing a measurement gas chamber 68. The measured gas, or measurement gas G, which has passed through the porous diffusion resistance layer 66, is introduced into the measurement gas chamber 68. The measurement gas chamber 68 is a space surrounded by the solid electrolyte 1, a measurement gas chamber formation layer 681, and the diffusion resistance layer 66.

[0122] The detection electrode 62 is formed to contact the solid electrolyte 1. Furthermore, the measurement gas chamber formation layer 681, which is a structural component of the measurement gas chamber 68, is formed to contact the solid electrolyte 1. The detection electrode 62 is exposed to the measured gas, such as the exhaust gas G, and is a portion that performs gas detection together with the reference electrode 63. The detection electrode 62 is electrically connected to the terminal 75, to which a lead wire 76 is connected.

[0123] The reference electrode 63 is arranged facing a reference gas chamber 69. The reference gas, such as atmospheric air A, is introduced into the reference gas chamber 69 from the near-end side X2 through a through hole 731 in the cover 73 on the near-end side. Here, instead of the lamination-type sensor element, a cup-type sensor element described below can also be used as the sensor element 6.

[0124] The detection electrode 62 is exposed to the measured gas, such as exhaust gas G, flowing into the cover 72 on the distal end side through through holes 723, 724, and 725 provided in the cover 72 on the distal end side. The reference electrode 63 is exposed to the reference gas, such as atmospheric air A, flowing through the through hole 731 provided in the cover 73 on the proximal end side and from within the cover 73 on the proximal end side into the reference gas chamber 69 of the solid electrolyte 1.

[0125] The heater 64 generates heat through energization. The heater 64 heats the solid electrolyte 1 and the electrodes 62 and 63 to an activation temperature during start-up of the internal combustion engine and the gas sensor 5 or the like. The heater 64 is configured by the insulator 642 made of a sintered body of alumina and the heat-generating body 641 formed inside the heater 64.

[0126] The alumina sintered body constitutes the insulator 642, which is in contact with the solid electrolyte. In other words, the sensor element 6 is a structural body in which the solid electrolyte 1 and the dissimilar material component 4 made of an alumina sintered body are in contact with each other. The solid electrolyte 1 has a contacting portion 1A (more precisely, a contacting surface) with the dissimilar material component 4 made of alumina. The insulator 642, which configures the heater, is also a structural component that forms the reference gas chamber 69 and also serves as a reference gas chamber formation layer.

[0127] In addition, in the solid electrolyte 1, the measurement gas chamber formation layer 681, which configures the measurement gas chamber 68, is laminated and formed on the measurement gas surface 601A side. The measurement gas chamber formation layer 681 is made of alumina. That is, the solid electrolyte 1 contacts the insulator 642 (i.e., the dissimilar material member 4) on the reference gas surface 602A side, which configures the heater 64 described above, and the measurement gas chamber formation layer 681 (i.e., the dissimilar material member 4) on the measurement gas surface 601A side. The solid electrolyte 1 comes into contact with the measured gas at the measurement gas surface 601A. The measurement gas surface 601A can be regarded as the gas contacting portion described above.

[0128] The diffusion resistance layer 66 is made of, for example, a porous spinel body. In addition, a shielding layer 60 made of aluminum oxide is provided on a surface of the diffusion resistance layer 66. The shielding layer 60 is made of a dense body that does not transmit gas. The exhaust gas G flowing into the cover 72 on the distal end side passes through the diffusion resistance layer 66 and reaches a measuring section 50 of the detection electrode 62. In the configuration of the sensor element 6, which is in Fig. 9 as an example, the diffusion resistance layer 66 is not in contact with the solid electrolyte 1. However, a configuration may also be used in which the diffusion resistance layer 66 is in contact with the solid electrolyte 1. In this case, the diffusion resistance layer 66 serves as the dissimilar material component 4. Solid electrolyte

[0129] The solid electrolyte 1 is made of partially stabilized zirconia 2. Specifically, the solid electrolyte described in the first embodiment is used. The solid electrolyte 1 has a small difference in a coefficient of thermal expansion with alumina and spinel. Thus, in the cooling / heating cycle, peeling and cracking do not easily occur between the heater 64 and the measurement gas chamber formation layer 681 and the solid electrolyte 1. In addition, the difference in a coefficient of thermal expansion at hysteresis and the difference in a coefficient of thermal expansion with alumina and spinel in the high-temperature region are small even in a cooling / heating cycle in which the solid electrolyte 1 is exposed to, for example, a high-temperature region exceeding 1,000°C.

[0130] Therefore, even when the solid electrolyte 1 is exposed to a high-temperature region, peeling and cracking do not easily occur between the solid electrolyte 1 and the component 4 made of dissimilar materials, such as the heater 64 and the measurement gas chamber formation layer 681. This means that the gas sensor 5 is capable of detecting a measured gas while maintaining high reliability even when the gas sensor 5 is applied to temperatures exceeding 1,000°C. electrode

[0131] The material of the detection electrode 62 according to the present embodiment is not particularly limited as long as the material has catalytic activity relative to oxygen and the like. The detection electrode 62 may contain, as a noble metal component, for example, a composition of Pt (platinum), Au (gold), Ag (silver), a mixture or alloy of Pd (palladium) and Ag, and a mixture or alloy of Pt and Au. In addition, the material of the reference electrode 63 is also not particularly limited and may contain Pt, Au, Ag, Pd, and the like as the noble metal component.

[0132] In addition, instead of the lamination type sensor element, for example, a bottomed cylindrical type sensor element (more specifically, a cup type) may also be used as the sensor element 6, as shown in an example in Fig.10. Such a cup-type sensor element includes a bottomed, cylindrically shaped (more precisely, cup-shaped) solid electrolyte 1, a detection electrode 62, and a reference electrode 63. The detection electrode 62 is provided on an outer peripheral surface 601A of the solid electrolyte 1. The reference electrode 63 is provided on an inner peripheral surface 602A of the solid electrolyte 1. In such a cup-type sensor element, a rod-shaped heater (not shown) is inserted inside the sensor element 6. The heater heats the sensor element 6 to a desired temperature.

[0133] The detection electrode 62 is provided on the outer peripheral surface 601A of the solid electrolyte 1. In addition, a porous protective layer 625 is formed on the outer peripheral surface 601A of the solid electrolyte. Fig.10, the protective layer 625 is a porous body and is made of, for example, spinel. In this case, peeling and cracking do not easily occur between the solid electrolyte 1 and the component 4 made of a dissimilar material, such as the protective layer 625, in a manner similar to that of the lamination-type sensor element described above.

[0134] Therefore, even in the gas sensor 5 including the cup-type sensor element, the gas sensor 5 is capable of detecting a measured gas while maintaining high reliability. Here, the detection electrode 62 is located in the example. Fig.10 between the protective layer 625 and the solid electrolyte 1. However, the detection electrode 62 is not necessarily formed on the entire outer peripheral surface 601A. Typically, a non-formation portion is present. Therefore, a portion in which the protective layer 625 and the solid electrolyte 1 are in contact exists, although a configuration is omitted from the drawings.

[0135] In addition, the reference electrode 63 is provided on the inner peripheral surface of the cup-shaped solid electrolyte 1. However, the reference electrode 63 may be provided on the entire inner peripheral surface, or it may be partially provided. In cases where the reference electrode 63 is partially provided, alumina configuring the heater and the solid electrolyte may come into contact. In this case, too, in a similar manner to that in the lamination-type sensor element, peeling and cracking do not easily occur between the solid electrolyte 1 and the member 4 made of dissimilar material, such as the heater, because the solid electrolyte 1 is thermally stable.

[0136] The present invention is not limited to the embodiments described above.

[0137] The solid electrolyte according to the first embodiment can also be used in a solid oxide fuel cell (SOFC), for example. In this case, the solid electrolyte has contact surfaces with an anode layer and a cathode layer, for example. Although one configuration is omitted from the drawings, the solid electrolyte can be applied to a fuel cell unit cell in which the anode layer, an electrolyte layer made of the solid electrolyte, and the cathode layer are sequentially laminated. In addition, as a result of laminating a plurality of fuel cell unit cells with a separator, a stack-type fuel cell can be constructed. Furthermore, in addition to the air-fuel ratio sensor, an oxygen sensor, a NOx sensor, and the like are provided as the gas sensor. The solid electrolyte can also be applied to these sensors.

Claims

[1] Solid electrolyte (1), comprising: partially stabilized zirconia (2) in which a stabilizer forms a solid solution in zirconia, wherein: the partially stabilized zirconia comprises, as crystal particles (3) configuring the partially stabilized zirconia, stabilizer low-concentration phase particles (33) whose concentration of the stabilizer at a particle center (O) is less than 4.7 mol%, and stabilizer high-concentration phase particles (34) whose concentration of the stabilizer at the particle center (O) is greater than 4.7 mol%, and an adjacent particle portion (35) in which two or more particles of the stabilizer low-concentration phase particles whose average particle size is greater than or equal to 0.1 µm are adjacently arranged; a frequency fraction of the stabilizer high-concentration phase particles on a cross-section of the solid electrolyte in terms of an area ratio relative to all crystal particles is greater than or equal to 70%; and the areas of the adjacent particle segments (35) are areas of circles having radii that are half the length of the respective particle sizes, and the presence of the adjacent particle segments (35) can be confirmed by SEM / EDX analysis. [2] Solid electrolyte according to claim 1, wherein: the frequency fraction of the adjacent particle sections on a cross-section of the solid electrolyte with respect to an area ratio relative to the stabilizer low concentration phase particles is greater than or equal to 50%. [3] Solid electrolyte according to claim 1 or 2, wherein: the frequency fraction of the adjacent particle sections on a cross-section of the solid electrolyte in terms of an area ratio relative to all crystal particles is 8 to 16%. [4] Solid electrolyte according to one of claims 1 to 3, wherein: an average particle size of the neighboring particle sections is 1 to 5 µm. [5] Solid electrolyte according to one of claims 1 to 4, wherein: an average particle size of the stabilizer high concentration phase particle is 1 to 5 µm. [6] Solid electrolyte according to one of claims 1 to 5, wherein: the stabilizer contains yttrium oxide. [7] Solid electrolyte according to one of claims 1 to 6, further comprising: a contacting section (1A) configured such that the solid electrolyte is in contact with a component (4) made of dissimilar material, wherein: the component is made of dissimilar material such as aluminum oxide or spinel. [8] Gas sensor (5), comprising: a solid electrolyte according to any one of claims 1 to 7. [9] A manufacturing method of a solid electrolyte according to any one of claims 1 to 7, wherein the manufacturing method comprises: a mixing step (S1) in which a mixture (20) is obtained by mixing: (i) a first raw material powder (221) comprising zirconia particles, (ii) a second raw material powder (222) comprising aggregated particles in which a plurality of zirconia particles are aggregated, and (iii) a stabilizer raw material powder (211); a molding step (S2) in which a molded body is obtained by molding the mixture; and a sintering step (S3) in which a solid electrolyte comprising partially stabilized zirconium dioxide is obtained by sintering the molded body, wherein: the mixing step comprises the following: a first mixing step (S11) in which the first raw material powder and the stabilizer raw material powder are mixed; and a second mixing step (S12) in which, after the first mixing step, the second raw material powder is further mixed, wherein the d50 particle size of the first raw material powder (221) is within a range of 0.2 to 0.5 µm, and the d50 particle size of the second raw material powder (222) is within a range of 1 to 5 µm.

Citation Information

Patent Citations

  • Organic matter disposal device

    JP2000202406A

  • Method of manufacturing electrolyte sheet for solid oxide fuel cell and electrolyte sheet

    JP2009104990A

  • Solid electrolyte material and solid oxide fuel cell provided with same

    WO2012105579A1

  • JP002009104990A