METHOD FOR MANUFACTURING A TRAPEZOIDAL CONNECTION CABLE WITH A Narrow Beol Grid
By employing PVD to reshape trenches into trapezoidal profiles and replacing thick PVD layers with thin conformal barriers, the method addresses the resistance issues in Co/Ru connecting lines, achieving lower resistance and improved chip performance.
Patent Information
- Application Number
- DE112020003469
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-17
- Filing Date
- 2020-08-14
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2040-08-14
AI Technical Summary
Existing methods for forming connecting lines using cobalt (Co) and ruthenium (Ru) face challenges in controlling the thickness of the barrier layer, leading to increased resistance and reduced conductor cross-section due to the limitations of thin film deposition processes like CVD and ALD, which follow the trench profile and further reduce the available space.
A method involving physical vapor deposition (PVD) to create a trapezoidal trench profile by ion bombardment, followed by selective removal of the thick PVD layer and replacement with a thin conformal barrier layer using CVD or ALD, allowing for a larger conductor cross-section and reduced resistance.
The method results in connecting lines with lower resistance and improved electromigration properties, enhancing chip performance by increasing the conductor cross-section and reducing resistance, particularly when using Co, Ru, or copper (Cu) as conductors.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Field of the invention
[0001] The present invention relates to the technology of interconnections, in particular to methods for forming trapezoidal connecting cables with a narrow back-end-of-line (BEOL) pitch. Background of the invention
[0002] Due to their reduced resistance and improved electromigration, cobalt (Co) and ruthenium (Ru) is considered a cost-effective alternative to conventional interconnect metals such as copper (Cu). To fabricate a Co / Ru-based interconnect, an element (e.g. a trench) is usually first Dielectric structured. The element is then lined with a thin barrier layer on which the Co and / or Ru is deposited to form the connecting line.
[0003] The thickness of the barrier layer is an important consideration. The thicker the barrier, the smaller the cross-section of the element available for the Co / Ru filler metal. For smaller element sizes, the The ratio of barrier to filler metal is even more important, since the resistance decreases with decreasing conductor cross-section can increase dramatically.
[0004] Thus, there is a need for methods for controlling the thickness of the lining to achieve practical Implementing interconnection technology with alternative conductors such as Co or Ru can be difficult, since thin-film deposition processes such as chemical vapor deposition (CVD) and atomic layer deposition (ALD), simply follow the trench profile and further reduce an already limited space.
[0005] Therefore, improved methods for manufacturing connecting lines would be desirable.
[0006] The document US 2018 / 0 323 151 A1 relates to a method for producing a conductive structure for a Semiconductor device in which a barrier layer is deposited in a trench formed in a dielectric material and a barrier layer is formed over the barrier layer. A main conductor is formed over the interface layer, and the main conductor is selectively introduced into the interface layer and the barrier layer to a position below a upper surface of the dielectric layer. The interface layer is formed using a chemical composition with an oxidizing agent selectively wet-etched to the main conductor and the barrier layer, The chemical composition is buffered to have a pH value above 7. The barrier layer is selectively etched onto the main conductor and the interface layer. Brief description of the invention
[0007] The invention is described by the features of claim 1. Embodiments are described in the dependent claims stated.
[0008] A method for forming trapezoidal interconnections with narrow back-end-of-line (BEOL) Pitch, in particular a method for forming an interconnection line structure. The method includes a: structuring at least one trench in a dielectric, wherein the at least one trench, as structured, comprises a V-shaped profile with a rounded bottom; depositing a lining in the and lining the at least one trench using physical vapor deposition (PVD), whereby the at least a trench is widened to create a trapezoidal profile in the at least one trench; removing the Lining selectively with respect to the dielectric from the at least one trench, wherein after removal of the at least one trench having the trapezoidal profile in which dielectric remains; depositing a conformal barrier layer in and lining the at least one trench having the trapezoidal profile; Depositing a conductor into and filling the at least one trench having the trapezoidal profile above the conformal barrier layer; and polishing the conductor and the conformal barrier layer down to the dielectric.
[0009] Furthermore, another method for forming an interconnection line structure is provided. The method includes: structuring at least one trench in a dielectric, wherein the at least one trench, such as structured, has a V-shaped profile with a rounded bottom; depositing a lining in the and Lining the at least one trench using PVD, whereby the at least one trench is widened to create a trapezoidal profile in the at least one trench; removing the lining selectively relative to the dielectric from the at least one trench, wherein after removal of the at least one trench, which has the trapezoidal profile in which dielectric remains; depositing a conformal barrier layer in the and lining the at least one trench having the trapezoidal profile using PVD, Atomic layer deposition (ALD) or chemical vapor deposition (CVD), where the conformal bar rier layer contains a material selected from: tantalum (Ta), tantalum nitride (TaN), titanium nitride (TiN) and combinations thereof and wherein the conformal barrier layer has a thickness of less than about 2 nm; depositing a conductor in the and filling the at least one trench having the trapezoidal profile above the conformal barrier layer, wherein the conductor is selected from: cobalt (Co), ruthenium (Ru) and combinations thereof; and polishing the conductor and the conformal barrier layer down to the dielectric.
[0010] In addition, a further method for forming an interconnection line structure is provided. Method includes: structuring at least one trench in a dielectric, wherein the at least one trench, as structured, has a V-shaped profile with a rounded bottom; depositing a lining in the and Lining the at least one trench using PVD, whereby the at least one trench is widened to create a trapezoidal profile in the at least one trench; removing the lining selectively relative to the dielectric from the at least one trench, wherein after removal of the at least one trench, which has the trapezoidal profile in which dielectric remains; depositing a conformal barrier layer in the and lining the at least one trench having the trapezoidal profile using PVD, ALD or CVD, wherein the conformal barrier layer contains a material selected from: Ta, TaN, TiN and combinations thereof and wherein the conformal barrier layer has a thickness of less than about 2 nm; depositing a conformal Wetting layer in the at least one trench having the trapezoidal profile, above the barrier layer under Using ALD or CVD, wherein the conformal wetting layer comprises a material selected from: Co, Ru and combinations thereof and wherein the conformal wetting layer has a thickness of less than about 3 nm; Depositing a conductor into and filling the at least one trench having the trapezoidal profile above the conformal barrier layer and on the conformal wetting layer, wherein the conductor contains copper (Cu); and polishing the conductor and the conformal barrier layer down to the dielectric.
[0011] Furthermore, a connecting line structure is provided. The connecting line structure includes: at least one trench structured in a dielectric having a trapezoidal profile; a conformal Barrier layer lining the at least one trench having the trapezoidal profile, wherein the conformal Barrier layer contains a material selected from: Ta, TaN, TiN and combinations thereof and wherein the conformal Barrier layer has a thickness of less than about 2 nm; and a conductor disposed over the conformal barrier layer in which is arranged at least one trench having the trapezoidal profile.
[0012] A more complete understanding of the present invention as well as further features and advantages of the present Invention will be obtained from the following detailed description and drawings. Brief description of the drawings Fig. 1 is a sectional view showing a V-shaped trench profile having a rounded bottom and a trapezoidal trench profile according to an embodiment of the present invention; Fig. 2 is a cross-sectional view showing at least one trench patterned in a dielectric has been formed, the trench, as structured, having a V-shaped profile with a rounded bottom, according to an embodiment of the present invention; Fig. 3 is a cross-sectional view showing that physical vapor deposition (PVD) is used to deposit a thick conformal lining into the trench and line it, thereby Trench is widened due to ion bombardment against the side walls / bottom of the trench to create a to create a trapezoidal profile of the trench, according to an embodiment of the present invention; Fig. 4 is a cross-sectional view showing that the PVD lining is selective to the dielectric of has been removed from the trench, leaving the (trapezoidal) trench profile intact, according to a Embodiment of the present invention; Fig. 5 is a cross-sectional view showing that atomic layer deposition (ALD) or chemical Chemical vapor deposition (CVD) has been used to deposit a thin conformal barrier layer in the (trapezoidal) trench and lining it, according to an embodiment of the present Invention; Fig. 6 is a sectional view showing that a conductor (e.g. cobalt (Co) and / or ruthenium (Ru)) is inserted into the (trapezoidal) trench has been deposited over the barrier layer and fills it, according to a Embodiment of the present invention; Fig. 7 is a sectional view showing that the conductor and the barrier layer are polished down to the surface of the dielectric, according to an embodiment of the present Invention; Fig. 8 is a sectional view taken from Fig. 2 and showing an alternative embodiment represents that PVD has been used to deposit a thick conformal lining in the trench and to line it, causing the trench to rupture due to ion bombardment against the sides / floor of the trench is widened to create a trapezoidal profile of the trench, according to one embodiment of the present invention; Fig. 9 is a cross-sectional view showing that the PVD lining is selective to the dielectric of has been removed from the trench, leaving the (trapezoidal) trench profile intact, according to a Embodiment of the present invention; Fig. 10 is a cross-sectional view showing that ALD or CVD has been used to produce a thin to deposit a conformal barrier layer into the (trapezoidal) trench and to line it, according to a Embodiment of the present invention; Fig. 11 is a cross-sectional view showing that ALD or CVD has been used to produce a thin to deposit a conformal wetting layer into the (trapezoidal) trench above the barrier layer, according to a Embodiment of the present invention; Fig. 12 is a sectional view showing that a conductor (e.g. copper (Cu)) is inserted into the (trapezoidal) trench has been deposited over the barrier layer and on the wetting layer and fills it, according to a Embodiment of the present invention; Fig. 13 is a sectional view showing that the conductor, barrier layer and wetting layer are polished down to the surface of the dielectric, according to an embodiment of the present Invention; Fig. 14 is a diagram showing a lower line resistance of connecting lines used in formed in a trapezoidal trench, compared to connecting lines laid in a trench with V- shaped profile, according to an embodiment of the present invention; and Fig. 15 is a diagram showing improved chip performance using interconnect lines arranged in formed in a trapezoidal trench, compared to connecting lines laid in a trench with V- shaped profile, according to an embodiment of the present invention. Detailed description of preferred embodiments
[0013] As described above, thin film deposition processes such as chemical Chemical vapor deposition (CVD) and atomic layer deposition (ALD), only in the formation of interconnections with alternative conductors, such as cobalt (Co) or ruthenium (Ru), only a barrier layer that follows the trench profile and This further reduces the already limited space. As a result, the conductor cross-section is minimized, resulting in an increased resistance of the connecting line. The use of physical vapor deposition (PVD) for Barrier deposition can create a trapezoidal trench (i.e. by ion bombardment against the dielectric). A trapezoidal trench provides a larger conductor cross-section. However, a PVD barrier is thick and takes up a too large a cross-section.
[0014] See, for example, Fig. 1. As shown in Fig. 1, a trench, as patterned in a dielectric, has a rounded trench profile and flat sidewall angles, i.e. a V-shaped profile with a rounded bottom. This V-shaped profile provides only a limited cross-section for filling the conductor. Therefore, if CVD or ALD is to be used to simply deposit the barrier into the trench, this limited cross-section would still As shown by dashed lines in Fig. 1, PVD can be used to make the trench (through ion bombardment) to create a trapezoidal profile. As described above, a PVD But the layer is too thick and takes up too much of the conductor cross-section.
[0015] Advantageously, methods are provided herein which take advantage of both the thin film capabilities of CVD or ALD and the capabilities for profile redesign / improvement of PVD by first applying a thick PVD layer is deposited into the trench to create a trapezoidal trench profile with an enlarged cross-section and then the PVD layer is removed and replaced by a (thin) CVD, ALD or PVD barrier.
[0016] The methods described here can be used in conjunction with alternative conductors, such as Co or Ru, and with conventional conductors, such as copper (Cu). For example, in a first exemplary Embodiment that In connection with the description of Figs. 2 to 7, an exemplary procedure for forming a Cu / Ru connecting line. This description is followed by a second exemplary embodiment, which is Forming a Cu interconnect using the same scheme of PVD and then CVD / ALD.
[0017] In the first exemplary embodiment, the method according to Fig. 2 begins with the structuring of at least a trench 204 in a dielectric 202. Suitable dielectrics 202 include, but are not limited to, Oxide materials such as silicon oxide (SiOx), and / or organosilicate glass (SiCOH) and / or Ultra-low &kgr; interlayer dielectric materials (ULK-ILD), e.g. with a dielectric constant κ of less than 2.7. For comparison, silicon dioxide (SiO ) has a dielectric constant κ of 3.9 2 Suitable ultra-low &kgr; dielectric materials include, but are not limited to, porous organosilicate glass (pSiCOH). To pattern the trench 204 into the dielectric 202, standard Lithography and etching processes can be used. Just as an example, a direction-dependent (ie anisotropic) Etching processes such as reactive ion etching (RIE) can be used for trench etching.
[0018] As shown in Fig. 2, the trench 204 has a structured rounded trench profile and flat Side wall angle, ie a V-shaped profile with a rounded bottom, a shape that provides the space required for the conductor filling available cross-section is unnecessarily limited. Simply lining trench 204 with a conformal barrier or Barrier / wetting layer would further reduce the already limited conductor cross-section.
[0019] However, as shown in Fig. 3, PVD is first used to deposit a thick conformal liner 302 into the trench 204 and lining it, whereby by ion bombardment against the side walls / floor of the trench During the PVD process, the trench 204 is widened and a trapezoidal profile of the trench 204 is created. Suitable materials for the liner 302 include, but are not limited to, tantalum (Ta), tantalum nitride (TaN) and / or titanium nitride (TiN). In an exemplary embodiment, the liner 302 is formed to a thickness of greater than about 3 nm, e.g. from about 3.5 nm to about 5 nm and ranges in between.
[0020] Even with this now trapezoidal profile, the thickness of the lining 302 takes up a significant portion of the conductor cross-section of the trench 204. Thus, filling a conductor over the PVD lining 302 would result in a lead to undesirably high resistance. It is advantageously proposed to next apply the PVD lining 302 selectively from the trench 204 to leave the trapezoidal profile and replace it with a thinner (PVD, ALD or CVD) barrier layer. While the deposition of a thicker PVD coating (e.g. over about 3 nm - see above) is required to create a trapezoidal profile of the trench 204, thinner layers of deposited PVD is not associated with sufficient ion bombardment of the dielectric to form the trench 204 to expand and create a trapezoidal profile. Thus, PVD can also be used to deposit the replacement barrier as long as it is kept thin (e.g. less than about 2 nm - see below).
[0021] As shown in Fig. 4, the PVD liner 302 is selective to the dielectric 202 from the trench 204 removed. In an exemplary embodiment, the dielectric 202 is an oxide material, such as SiOx, SiCOH and / or pSiCOH (see above), and the lining 302 (e.g. Ta, TaN and / or TiN) is formed using a selective etching process, such as a selective direction-independent (ie isotropic) wet chemical etching. The Using a selective etching process leaves the trench profile intact. What remains is trench 204, which is a trapezoidal profile, which advantageously has an enlarged conductor cross-section compared to that of the trench such as structured (i.e. a V-shaped profile with a rounded bottom - see Fig. 2 (described above)) provides.
[0022] PVD, ALD or CVD is then used to deposit a thin conformal barrier layer 502 in the (trapezoidal) trench 204 and to line it. See Fig. 5. As shown in Fig. 5, the Barrier layer 502 the trapezoidal profile of the trench 204 (created by the deposition and subsequent Removing the PVD lining 302). Suitable materials for the barrier layer 502 include, without limitation, Ta, TaN and / or TiN. In an exemplary embodiment, the barrier layer 502 is Thickness of less than about 2 nm, e.g. from about 1 nm to about 1.5 nm and ranges therebetween. How As described above, PVD with these small thicknesses will not produce a trapezoidal profile. The barrier layer 502 will prevent diffusion of the conductor (in this case cobalt (Co) and / or ruthenium (Ru)) into the dielectric 202.
[0023] As deposited, the barrier layer 502 is in the trench 204 and on an upper surface of the dielectric 202. See Fig. 5. After filling the conductor, however, the over filling is removed, e.g. using a process such as chemical-mechanical polishing (CMP), and with it the excess barrier layer 502 on the dielectric 202.
[0024] Next, a conductor 602 is deposited over the barrier layer 502 into the (trapezoidal) trench 204 and fills it. See Fig. 6. Suitable conductors include, but are not limited to, Co and / or Ru. As above described, embodiments are also contemplated herein in which more conventional conductors, such as copper (Cu), For depositing the conductor 602 into the trench 204, a method such as evaporation, sputtering, electrochemical plating, etc. As shown in Fig. 6, the as-deposited conductor 602 overfills the Trench 204. This overfill is then removed to avoid short circuits with neighboring structures.
[0025] For example, as shown in Fig. 7, a process such as CMP is used to form the conductor 602 and the Barrier layer 502 down to the surface of the dielectric 202. The result is a trapezoidal (Co and / or Ru) connecting line 702 embedded in a dielectric 202 having a thin (e.g. less than about 2 nm, e.g. from about 1 nm to about 1.5 nm and areas in between - see above) conformal barrier layer 502 which separates the conductor 602 from the dielectric 202.
[0026] As described above, the methods described here can also be used in conjunction with conventional Conductors such as Cu can be used. For example, in another exemplary embodiment shown in In conjunction with the description of Figs. 8 to 13, an exemplary procedure for forming a Cu connecting cable described.
[0027] The process begins in the same general way as in the previous example with structuring at least one trench 204 in a dielectric 202 (e.g., SiOx, SiCOH, and / or pSiCOH). Thus, what is shown in Fig. 8 is shown, from the structure shown in Fig. 2, where like structures are numbered the same in the figures. As described above, the trench 204 structured as with an etching process such as RIE will have a rounded trench profile and flat sidewall angles, i.e. a V-shaped profile with a rounded bottom. This shape unnecessarily limits the cross-section available for filling with conductors. Simply lining trench 204, in this Case with a barrier layer and a wetting layer, this already limited conductor cross-section would be further reduce.
[0028] As shown in Fig. 8, PVD is first used to deposit a thick conformal liner 802 into the trench 204 and lining it. As described above, ion bombardment against the side walls / bottom of the trench during the PVD process to widen the trench 204 to achieve a trapezoidal profile of the trench 204 Suitable materials for the liner 802 include, but are not limited to, Ta, TaN and / or TiN. In an exemplary embodiment, the liner 802 is formed to a thickness greater than about 3 nm, e.g., about 3.5 nm to about 5 nm and areas in between.
[0029] As shown in Fig. 8, the trench 204 now has a trapezoidal profile. As described above, the thick PVD lining 802 can be removed to increase the conductor cross-section. In this embodiment This allows the placement, e.g. using PVD, ALD or CVD, of a thin barrier layer and a thin wetting layer to improve the Cu gap filling properties. Therefore, the PVD lining 802 is now selectively removed from trench 204. See Fig. 9.
[0030] As shown in Fig. 9, the PVD liner 802 is selective to the dielectric 202 from the trench 204 removed. In an exemplary embodiment, the dielectric 202 is an oxide material, such as SiOx, SiCOH and / or pSiCOH (see above), and the lining 802 (e.g. Ta, TaN and / or TiN) is formed using a selective etching process, such as a selective direction-independent (ie isotropic) wet chemical etching. The Using a selective etching process leaves the trench profile intact. What remains is, as shown in Fig. 9, the trench 204 with a trapezoidal profile, which advantageously allows an increased conductor cross-section compared to that of the trench as structured (ie a V-shaped profile with a rounded bottom - see Fig. 2 (above described)).
[0031] Subsequently, as shown in Fig. 10, PVD, ALD or CVD is used to form a thin conformal barrier layer 1002 into the (trapezoidal) trench 204 and to line it. The barrier layer 1002 follows the trapezoidal profile of the trench 204 (created by the deposition and subsequent removal of the thick PVD Lining 802). Suitable materials for the barrier layer 1002 include, but are not limited to, Ta, TaN and / or TiN. In an exemplary embodiment, the barrier layer 1002 is deposited to a thickness of less than about 2 nm, e.g., from about 1 nm to about 1.5 nm and ranges in between. As above As described, PVD with these small thicknesses will not produce a trapezoidal profile. The barrier layer 1002 will Diffusion of the materials of the wetting layer (in this case Co and / or Ru) and / or the conductor (in this case Cu) in prevent the dielectric 202.
[0032] Subsequently, to improve the Cu gap filling properties, ALD or CVD is used to form a thin conformal wetting layer 1102 into the (trapezoidal) trench 204 over the barrier layer 1002. See Fig. 11. Suitable materials for the wetting layer 1102 include, but are not limited to, Co and / or Ru. Filling Cu over Co / Ru shows clear advantages. For example, Cu exhibits excellent wetting on Ru and Cu wets Co better than Ta. In an exemplary embodiment, the wetting layer 1102 is applied to a Thickness of less than about 3 nm, e.g. from about 1.5 nm to about 2 nm and regions therebetween.
[0033] As deposited, the barrier layer 1002 and the wetting layer 1102 are in the trench 204 and on a upper surface of the dielectric 202. See Fig. 11. After filling the conductor, the overfilling removed, e.g. using a process such as CMP, and with it the excess barrier layer 1002 and Wetting layer 1102 on the dielectric 202.
[0034] Next, a conductor 1202 is deposited over the barrier layer 1002 and on the wetting layer 1102 in the (trapezoidal) trench 204 and fills it. See Fig. 12. In this exemplary embodiment, The conductor 1202 is Cu, but is not limited thereto. To deposit the conductor 1202 into the trench 204, a Processes such as evaporation, sputtering, electrochemical plating, etc. As shown in Fig. 12, the conductor 1202 as deposited overfills the trench 204. This overfill is then removed to short circuit with neighboring structures.
[0035] For example, as shown in Fig. 13, a process such as CMP is used to polish conductor 1202, Barrier layer 1002 and wetting layer 1102 down to the surface of the dielectric 202. The The result is a trapezoidal (Cu) interconnect line 1302 embedded in a dielectric 202 that has a thin (e.g. less than about 2 nm, e.g. from about 1 nm to about 1.5 nm and ranges in between - see above) conformal Barrier layer 1002 and a thin conformal (e.g., less than about 3 nm, e.g., from about 1.5 nm to about 2 nm and regions in between - see above) wetting layer 1102 which separates the conductor 1202 from the dielectric 202.
[0036] The present methods are further described by the following non-limiting examples. First, as shown in Fig. 14, for Co-interconnects made using the present methods formed and have a height-to-width aspect ratio of 1.5 and a trapezoidal trench profile with a 2 nm thick ALD barrier layer (labelled as ´´PVD profile´´), a 15% lower R / C value was observed than for a corresponding trench having a V-shaped profile with a rounded bottom (marked as ´´ALD profile´´) In Fig. 14, the critical dimension (CD) of the trench (measured in nanometers (nm)) is shown on the x-axis and the line resistance (measured in ohms per micrometer (ohm / µm)) is plotted on the y-axis. The lower line resistance for the connecting lines formed in a trapezoidal trench can the larger amount of conductors compared to connecting cables laid in a trench with a V-shaped profile (ie like structured) are formed.
[0037] Fig. 15 is a diagram showing improved chip performance, which is also due to the larger amount of conductor in the Connecting lines formed in a trapezoidal trench (marked as ´´PVD profile´´) compared to connecting lines laid in a trench with a V-shaped profile (i.e. as structured) (called ´´ALD profile´´ In particular, in this example, an improvement in the frequency power value (´´frequency performance gauge´´, FPG) of 3% for a 5 nm VTFET using the present co- V-shaped profile interconnect structure with 30 nm pitch observed in the back-end-of-line (BEOL). FPG is a measure of the highest frequency at which a chip can operate, ie the higher the frequency, the faster / more powerful the chip is. In Fig. 15, the power is plotted on the x-axis and the frequency (measured in Gigahertz (GHz)) is plotted on the y-axis.
[0038] In a preferred embodiment of the present invention described herein, a method for Forming a connecting line structure, the method comprising the steps of: structuring at least a trench in a dielectric, wherein the at least one trench, as structured, has a V-shaped profile with a rounded bottom; depositing a lining in the and lining the at least one trench under Use of PVD, whereby the at least one trench is widened to form a trapezoidal profile in the to create at least one trench; removing the lining from the at least one trench selectively with respect to the dielectric, whereby removing at least one trench having the trapezoidal profile in which dielectric remains; Depositing a conformal barrier layer in and lining the at least one trench which defines the trapezoidal profile, using PVD, ALD or CVD, wherein the conformal barrier layer comprises a material selected from the group consisting of: Ta, TaN, TiN and combinations thereof and wherein the conformal barrier layer comprises a thickness of less than about 2 nm; depositing a conductor in and filling the at least one trench, the having a trapezoidal profile, over the conformal barrier layer, wherein the conductor is selected from the group consisting of: Co, Ru and combinations thereof; and polishing the conductor and the conformal barrier layer down to the dielectric.
[0039] In a further preferred embodiment of the invention described herein, a method for forming a connecting line structure, the method comprising the steps of: structuring at least one Trench in a dielectric, wherein the at least one trench, as structured, has a V-shaped profile with a rounded bottom; depositing a lining in the and lining the at least one trench under Use of PVD, whereby the at least one trench is widened to form a trapezoidal profile in the to create at least one trench; removing the lining selectively with respect to the dielectric from the at least one trench, wherein after removal of the at least one trench having the trapezoidal profile, the dielectric; depositing a conformal barrier layer in and lining the at least one Trench having the trapezoidal profile using PVD, ALD or CVD, whereby the conformal Barrier layer comprises a material selected from the group consisting of: Ta, TaN, TiN and combinations thereof and wherein the conformal barrier layer has a thickness of less than about 2 nm; depositing a conformal Wetting layer in the at least one trench having the trapezoidal profile, above the barrier layer under Use of ALD or CVD, wherein the conformal wetting layer comprises a material selected from the group consisting of of: Co, Ru and combinations thereof and wherein the conformal wetting layer has a thickness of less than about 3 nm; depositing a conductor in and filling the at least one trench having the trapezoidal profile over the conformal barrier layer and on the conformal wetting layer, wherein the conductor comprises Cu; and Polishing the conductor and conformal barrier layer down to the dielectric.
Claims
1. A method for forming an interconnection structure, the method comprising the steps of: Structuring at least one trench (204) in a dielectric (202), wherein the at least one trench, such as structured, has a V-shaped profile with a rounded bottom; Depositing a lining (302; 802) in and lining the at least one trench using physical vapor deposition (PVD), whereby the at least one trench is widened to form a trapezoidal profile in the at least one trench, wherein the lining has a thickness of more than 3 nm; Removing the lining selectively with respect to the dielectric from the at least one trench, wherein after Removing at least one trench having the trapezoidal profile in which dielectric remains; Depositing a conformal barrier layer (502; 1002) in and lining the at least one trench which has a trapezoidal profile; Depositing a conductor (602; 1202) into and filling the at least one trench having the trapezoidal profile over the conformal barrier layer; and Polishing the conductor and conformal barrier layer down to the dielectric.
2. The method according to claim 1, wherein the dielectric is selected from the group consisting of: silicon oxide (SiOx), Organosilicate glass (SiCOH), porous organosilicate glass (pSiCOH) and combinations thereof.
3. The method of claim 1, wherein the lining comprises a material selected from the group consisting of: tantalum (Ta), Tantalum nitride (TaN), titanium nitride (TiN) and combinations thereof.
4. The method of claim 1, wherein the liner has a thickness of 3.5 nm to 5 nm and ranges therebetween.
5. The method of claim 1, wherein the conformal barrier layer comprises a material selected from the group consisting of: Ta, TaN, TiN and combinations thereof.
6. The method of claim 1, wherein the conformal barrier layer has a thickness of less than 2 nm.
7. The method of claim 1, wherein the conformal barrier layer has a thickness of 1 nm to 1.5 nm and regions in between.
8. The method of claim 1, wherein the conformal barrier layer is formed using PVD, atomic layer deposition (ALD) or chemical vapor deposition (CVD).
9. The method of claim 1, wherein the conductor is selected from the group consisting of: cobalt (Co), ruthenium (Ru) and combinations thereof.
10. The method of claim 1, wherein the conductor comprises copper (Cu).
11. The method of claim 10, further comprising the step: Depositing a conformal wetting layer (1102) into the at least one trench having the trapezoidal profile over the barrier layer, with the conformal wetting layer being deposited in front of the conductor.
12. The method according to claim 11, wherein the conformal wetting layer comprises a material selected from the group consisting of of: Co, Ru and combinations thereof.
13. The method of claim 11, wherein the conformal wetting layer has a thickness of less than 3 nm.
14. The method according to claim 11, wherein the conformal wetting layer has a thickness of 1.5 nm to 2 nm and regions in between.
15. The method of claim 1, wherein the conformal wetting layer is deposited using ALD or CVD becomes.
Citation Information
Patent Citations
WET ETCH REMOVAL OF Ru SELECTIVE TO OTHER METALS
US20180323151A1