SLIDING CONTACT MATERIAL FOR MOTOR BRUSHES, MOTOR BRUSH AND DC MOTOR
The Ag-Ta2O5-ZnO composite material addresses the challenges of wear and spark resistance in motor brushes, offering improved durability and cost-effectiveness for small DC motors by replacing Pd-based alloys and carbon-based materials.
Patent Information
- Application Number
- DE112022006152
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-24
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-21
AI Technical Summary
Existing motor brush materials for small DC motors face challenges in balancing wear resistance, spark resistance, and cost, particularly due to the high cost of Pd-based alloys and the occurrence of spark discharges with carbon-based materials, which are unsuitable for downsized motors and noisy.
A sliding contact material comprising a pure Ag matrix with dispersed Ta2O5 and ZnO particles, optimized in content and particle size, providing improved wear and spark resistance without Pd, suitable for both high-load and low-load DC motors.
The Ag-Ta2O5-ZnO composite material offers enhanced durability, reduced noise, and lower material costs, making it a viable alternative to carbon-based and Pd-based materials, with demonstrated longevity and resistance to mechanical and spark wear.
Smart Images

Figure 00000015_0000
Abstract
Description
BACKGROUND OF THE INVENTION AREA OF THE INVENTION
[0001] The present invention relates to a sliding contact material, preferably as a material component of motor brushes of small DC motors, in particular a sliding contact material that is improved in both wear resistance and spark resistance, and that is Pd-free and therefore cost-effective, as well as a motor brush with the sliding contact material. DESCRIPTION OF THE STATE OF THE ART
[0002] Small DC motors are widely used in a variety of fields, including automobiles, precision instruments, and household appliances. For example, many electrical components in an automobile, such as an audio system, air conditioning (air conditioning vent), electrically folding mirrors, a steering lock, and automatic door locks, are powered by small DC motors. Furthermore, small DC motors are a key component in household appliances, including razors, electric toothbrushes, and small vacuum cleaners.
[0003] DC motors share a common basic structure and / or configuration, even though they have different applications. A typical DC motor comprises a housing, a permanent magnet mounted on an inner surface of the housing, and a rotor rotatably mounted on a shaft inside the housing. The rotor contains an armature and a commutator, and a brush, acting as a commutator, is electrically connected to the commutator. The motor supplies current from an external power supply to the rotor via the brush and commutator to rotate the rotor. A crucial factor in ensuring stable operation of such a DC motor is the durability of the contact materials used for the brush and commutator.In particular, the brush is located in a harsh environment where the same part is continuously subjected to friction during motor operation, and therefore must have a higher durability than the commutator.
[0004] The selection of a contact material for a small DC motor's motor brush depends on the loads the motor experiences during operation. The correlation between stall torque and stall current determines the load on the small DC motor. Motor brushes of heavily loaded small DC motors with high stall torques and stall currents are subjected to high conduction currents, raising concerns about sparking and arcing when the brush separates from the commutator. Therefore, they must be resistant to spark wear. Furthermore, resistance to mechanical wear is required, a property common to all sliding contact materials.Carbon-based materials, which exhibit low coefficients of sliding friction and superior mechanical wear properties compared to metals, are typically used as contact materials for motor brushes that can meet the requirements for small, high-power DC motors. Known examples of such carbon-based materials are those obtained by mixing carbon powder with metal powders such as precious metal or copper powders, or with ceramic powders (Patent Documents 1, 2). Furthermore, a large-volume, block-like carbon-based brush material, on the order of millimeters, is used to compensate for mechanical wear and sparking in the motor brushes of small, high-power DC motors.The brushes of small, high-power DC motors typically have a structure in which a block of brush material is pressed against a commutator by a spring. Small, high-power DC motors with this type of structure are used in automotive electrical components such as electric folding mirrors, steering wheel locks, and automatic door locks.
[0005] On the other hand, motor brushes of small, low-load DC motors with relatively low stall torques and stall currents are less of a concern due to spark wear from discharge, and therefore, ensuring resistance to mechanical wear is a key objective for these motor brushes. Precious metal-based materials, particularly Ag-Pd alloys, are used as contact materials for motor brushes in small, low-load DC motors. Examples of Ag-Pd alloys include an Ag-50 wt% Pd alloy and an Ag-30 wt% Pd alloy, described in Reference 3. Ag-Pd alloys exhibit extremely high resistance to mechanical wear and are also superior in terms of weldability.
[0006] For the motor brushes of small, low-load DC motors, brush materials are used in which each of these precious metal-based materials is bonded to a base material, including a copper-based material such as beryllium copper and phosphor bronze. In automotive applications, small, low-load DC motors with this configuration are used for air conditioning (HVAC) systems in vehicles, such as air conditioning flaps, audio equipment, and other components. Small, low-load DC motors are also used as general-purpose motors in household appliances such as razors and toys. State of the art documents Patent document Patent document 1 Published Japanese patent application no. Hei 11-4563 Patent document 2 Published Japanese patent application no. 2005-176492 Patent document 3 Published Japanese patent application no. Hei 5-277762 SUMMARY OF THE INVENTION Technical Problem
[0007] The aforementioned sliding contact materials for motor brushes have been used in various small DC motors and applications without any problems to date. However, the increasing demand for small DC motors and the need to reduce product costs necessitate the use of a different type of material for motor brushes, both for small high-load and small low-load DC motors.
[0008] For carbon-based materials used in the motor brushes of small, high-power DC motors, the primary reason for the material change is to respond to the need for miniaturized motors. Carbon-based materials with low minimum arc current values are likely to allow spark discharge and arc discharge to occur during sliding. Previously, carbon-based materials were used as block brush materials to compensate not only for mechanical wear but also for wear caused by spark discharge. However, meeting the downsizing requirement with brush materials on the millimeter scale is challenging.
[0009] Sparks and arc discharges, which are likely to occur with carbon-based materials, cause noise and rotational noise. In recent years, the automotive industry has sought to avoid noise during engine operation, partly due to the increasing preference for high-end products. Accordingly, a sliding contact material has been required for small, high-power DC motors that can replace carbon-based materials, exhibit higher wear resistance, and offer satisfactory spark resistance with a reduced occurrence of spark discharges and similar issues.
[0010] On the other hand, the recent rise in the price of pd has necessitated a change in the materials used in Ag-Pd-based alloys for contact brushes in small, low-load DC motors. While the price of pd was previously relatively low among precious metals, it has risen rapidly over the past two to three years and is now comparable to or higher than that of gold (Au). Ag-Pd-based alloys for motor brush applications include those with a pd content as high as 50% by mass; thus, the price of pd has a direct impact on the material costs of motor brushes. These higher material costs will also affect the product costs of motor brushes used in universal motors for household appliances.
[0011] Due to their extremely high resistance to mechanical wear, as described above, Ag-Pd-based alloys possess unparalleled properties as sliding contact materials. However, the previously mentioned problem of the rapid increase in Pd prices is driving demand for a sliding contact material that, while not exhibiting the high resistance of Ag-Pd-based alloys, is Pd-free and offers a balanced cost-to-performance ratio.
[0012] Although the need for a material change described above has been recognized for both small high-load and small low-load DC motors, few concrete attempts have been made to meet this need. In particular, the material cost problem has further hampered such a change. The present invention was developed in light of these circumstances and provides: a sliding contact material that is preferred as a material component of motor brushes for small high-load DC motors, exhibiting satisfactory resistance to mechanical wear and superior spark resistance; and a cost-effective sliding contact material that is also applicable to motor brushes for small low-load DC motors and capable of replacing Ag-Pd-based alloys. Solution to the problem
[0013] The present invention for solving the problems is directed to a sliding contact material for a motor brush, wherein the sliding contact material comprises: pure Ag as a matrix; and Ta2O5 particles and ZnO particles dispersed in the matrix, wherein the sliding contact material contains a Ta2O S -particle content of 0.1 mass percent or more and 6.0 mass percent or less and a ZnO particle content of 0.1 mass percent or more and 12 mass percent or less.
[0014] The present sliding contact material for a motor brush according to the invention comprises a composite material in which metal oxide particles are dispersed in a matrix comprising silver (Ag). The silver forming the matrix is a metal that is advantageous with respect to its spark discharge properties and in which, unlike carbon-based materials, fewer discharges occur even under high load conditions. Accordingly, the precious metal alloy, mainly made of silver, is considered in the present invention to be more satisfactory with respect to spark resistance than conventional carbon-based materials. This leads to the successful achievement of resistance to spark wear and a reduction in noise generation, which is a problem with carbon-based materials.
[0015] In the present invention, both the Ta oxide Ta2O Sas well as the zinc oxide ZnO, essentially as metal oxides in the form of dispersed particles in the silver matrix. The investigations carried out by the present inventors have shown that Ta₂O₅ contributes to improving wear resistance and spark resistance, and ZnO to further improving spark resistance. As described above, a brush in a DC motor is exposed to a harsher environment with regard to wear and sparking than a commutator. A motor brush that can withstand the harsh conditions described above can be produced by dispersing these two metal oxides in suitable quantities.
[0016] As described above, the present sliding contact material according to the invention for a motor brush achieves material reinforcement with dispersed metal oxide particles and improved spark resistance with an optimized matrix and metal oxide configuration. These features make the present sliding contact material according to the invention satisfactory with regard to both resistance to mechanical wear and spark wear. The present sliding contact material according to the invention is a Pd-free precious metal alloy without inclusions of expensive Pd. Therefore, the present invention is also suitable as a sliding contact material for motor brushes, replacing Ag-Pd alloys. The design of the present sliding contact material according to the invention for a motor brush is described in more detail below.
[0017] (A) Configuration and manufacturing process for the present sliding contact material according to the invention Ag-Matrix (I)
[0018] The matrix of the present inventive sliding contact material for a motor brush is pure silver (Ag). If a metal other than silver is mixed into the matrix, i.e., if the matrix is an silver alloy, the spark resistance properties deteriorate. The use of pure silver as the matrix is an essential requirement for the present inventive contact material for a motor brush. Pure silver is silver that contains no other element than silver and unavoidable impurities. Examples of such unavoidable impurities are the elements iron (Fe), chromium (Cr), palladium (Pd), copper (Cu), nickel (Ni), manganese (Mn), aluminum (Al), silicon (Si), and magnesium (Mg). These unavoidable impurities originate from trace amounts of elements that contaminate silver powder and metal oxide powder as raw materials for the sliding contact material, as well as from material components of a production device (e.g., a crusher, a mixer).Elements that should be particularly restricted among the unavoidable impurities are Fe, Cr, and Ni, as these especially affect spark resistance. The present sliding contact material according to the invention for a motor brush preferably has a total Fe / Cr / Ni content of 0.3% by mass or less. The total Fe / Cr / Ni content is preferably 0.2% by mass or less, and even more preferably 0.1% by mass or less. (II) Dispersed particles (metal oxides)
[0019] In the present sliding contact material according to the invention for a motor brush, oxide particles consist of both ZnO and Ta2O. S Dispersed in the pure Ag matrix. The oxide particle contents are specified in the present invention.
[0020] ZnO contributes to improved spark resistance. For improved spark resistance, the present sliding contact material according to the invention for a motor brush contains, in particular, ZnO in addition to Ta₂O₅. The ZnO content is 0.1% by mass or more and 12% by mass or less, based on the total mass of the sliding contact material. If the ZnO content is less than 0.1% by mass, the effect is not expected to occur. A ZnO content of more than 12% by mass results in impaired processability, which leads to difficulties in processing into a specific shape for assembling a motor brush. The ZnO content is preferably 1% by mass or more and 9% by mass or less, and more preferably 2% by mass or more and 7% by mass or less.
[0021] Ta2O5 contributes to improved wear resistance and spark resistance, and the Ta2O5 content is 0.1% by mass or more and 6.0% by mass or less, based on the total mass of the sliding contact material. If the Ta2O5 content is less than 0.1% by mass, the effect is not expected to occur. S In amounts exceeding 6.0% by mass, Ta₂O₅ has difficulty distributing homogeneously within the matrix and forms aggregates that cause increased contact resistance. Accordingly, an increase in spark resistance is not to be expected. The Ta₂O₅ content is preferably 0.5% by mass or more and 3.0% by mass or less, and more preferably 0.9% by mass or more and 2.0% by mass or less.
[0022] The ZnO and Ta₂O₅ concentrations, which fall within the aforementioned ranges, can be easily measured by any analytical method, including electron beam microanalysis (EPMA), energy-dispersive X-ray analysis (EDX), wavelength-dispersive X-ray analysis (WDX), and X-ray fluorescence analysis (XRF). The sliding contact material according to the invention is bonded to a base material, e.g., a copper-based material, to form a motor brush. If part or all of the contact material can be separated from a base material, the oxide concentrations can be estimated from the metal component concentrations for Zn and Ta measured by inductively coupled plasma atomic emission spectrometry (ICP atomic emission spectrometry) of a separated portion of the material.
[0023] Regarding the particle sizes of the oxide particles, the average particle size of ZnO is preferably 0.5 µm or more and 5 µm or less, and that of Ta₂O₅ is preferably 0.5 µm or more and 5 µm or less. For both ZnO and Ta₂O₅, the effect of improving wear resistance is less pronounced when the average particle size is less than 0.5 µm. When the average particle size of the oxide particles is greater than 5 µm, the oxide particles are only sparsely distributed and, as in the first case, contribute less to wear resistance. To determine the average particle size in the material, a metal structure observation is performed using a SEM or similar instrument to measure the particle sizes of the oxide particles in an image using a biaxial method or similar technique, and the average value is calculated as the average particle size.In this case, if Ta2O5 and ZnO need to be distinguished from each other, it is appropriate to additionally carry out an elemental classification by EPMA or similar.
[0024] The present sliding contact material according to the invention for a motor brush can be produced by powder metallurgy. In powder metallurgy, a mixed powder consisting of Ag powder for the matrix and Ta₂O₅ powder and ZnO powder for the dispersed particles is sintered, resulting in the contact material. The average particle sizes of the Ag powder are preferably 1 µm or more and 15 µm or less, of the Ta₂O₅ powder 0.5 µm or more and 5 µm or less, and of the ZnO powder 0.5 µm or more and 5 µm or less. Preferably, the mixed powder is processed into a billet (compressed form) under pressure before sintering. Preferably, the mixed powder is compressed into a billet (compressed form) under pressure before sintering. Preferably, the mixed powder is compressed during billet production at a pressure of 2.5 × 10⁻⁶. 2 MPa or more and 15× 10 2The material is pressurized to MPa or less. The heating temperature during sintering is preferably 700°C or more and 950°C or less. The contact material, including the sintered body obtained by powder metallurgy, can be processed appropriately. (B) Forming the present sliding contact material according to the invention
[0025] The present sliding contact material according to the invention for assembling a motor brush can be in any shape without restriction and can be machined before use so that it has a shape and dimensions that correspond to the specifications of a motor into which the motor brush is to be installed. However, the motor brush must remain in contact with the commutator with adequate contact pressure, which is why it must be resilient. Therefore, the present sliding contact material according to the invention is preferably combined with a spring-like base material and used in the form of a composite material. The base material is preferably a copper-based material. Examples of copper-based materials are pure copper, nickel silver, beryllium copper, phosphor bronze, and CuNi alloys.The sliding contact material is bonded to at least part of the base material, which contains a copper-based material, creating a composite material for a motor brush.
[0026] The sliding contact material according to the invention costs less than Ag-Pd-based alloys but is more expensive than Cu-based materials. Thus, the use of this composite material even leads to a cost reduction for motor brushes. Furthermore, a motor brush onto which the composite material has been applied, when a base material with suitable spring properties is selected, enables the miniaturization of motors. While carbon-based materials are used for conventional small, high-load DC motors, and brushes containing a carbon-based material in block form and a spring material in combination are used for such motors, the present invention can provide smaller motors than these.
[0027] The composite material has no specifically limited dimensions. The sliding contact material, in the form of a strip, film, or chip, is bonded to part or all of the surface of a base material, also in the form of a strip, film, or chip. Various joining methods, such as cladding, seam welding, and brazing, can be used to bond the sliding contact material to the base material. The resulting composite material is then cut and / or machined as appropriate to create a motor brush.
[0028] Motor brushes to which the contact material according to the invention has been applied are suitable for the small high-load and low-load DC motors described above. The configuration of small DC motors is as described above, and a motor brush and a commutator are essential to the configuration. The motor brush supplies the commutator with current from a power supply outside the motor.
[0029] For motor brushes to which the present sliding contact material according to the invention is applied, Ag alloys are preferred as a material component of a commutator. Examples of such Ag alloys include an Ag alloy containing Ag with a total of 1% or more by mass and a total of 12% or less of one or more of the elements Pd, Cu, Zn, and Ni. Specific examples of such Ag alloys are an Ag-Cu alloy, an Ag-Cu-Ni alloy, and an Ag-Pd-Cu-Zn-Ni alloy.
[0030] Not only the aforementioned Ag alloys (solid solution alloys), but also an oxide-dispersed Ag alloy as in the present invention can be used as a commutator material. One example is an oxide-dispersed Ag alloy in which MgO and ZnO are dispersed in an AgCu alloy matrix. Another example is an oxide-dispersed Ag alloy that uses an Ag alloy (an Ag alloy containing one or more of the elements Fe, Co, Ni, and Cu) as the matrix and Ta₂O. SThe contact material contains particles as well as Mg, Fe, Co, Ni, or Zn oxide particles dispersed in the matrix. This latter contact material for commutators, in which Ta and Zn oxide particles can be distributed, is similar to the present contact material according to the invention for a motor brush, but differs in that an Ag alloy is used as the matrix. The difference lies in the fact that contact materials for motor brushes, as described above, must exhibit higher spark resistance, and Ag alloys containing an additional element in the matrix are disadvantageous. This latter contact material for commutators, which contains an Ag alloy and Ta₂O₅ particles and other particles dispersed in the Ag alloy, is preferably used, in particular, for commutators of small, high-load DC motors.
[0031] A commutator material configuration comprising an Ag alloy is used in accordance with the specification of a small low-load or high-load DC motor. It is only required that the commutator of a small DC motor, regardless of the application, incorporates the aforementioned commutator material in the surface that contacts a motor brush. Alternatively, the commutator can also be configured with a composite material, where a base material is coated with a contact material. In this case, the same copper-based material used as the aforementioned composite material for a motor brush can be used as the base material. Advantageous effects of the invention
[0032] The present sliding contact material according to the invention exhibits high wear resistance and spark resistance for use in motor brushes under harsh operating conditions with regard to mechanical wear, discharge, and sparking, and can exhibit these properties without the use of Pd as a material component. With these improved performance and cost-related properties, the present contact material according to the invention is a promising replacement for carbon-based materials that have been used for motor brushes of small, high-load DC motors and also exhibits high durability combined with a noise-reducing effect.
[0033] The present sliding contact material according to the invention is also available for brushes of small, low-load DC motors. While Ag-Pd alloys have been used as motor brush material for such DC motors, the present invention can be used as an alternative material to Ag-Pd alloys. The present contact material according to the invention, for which no Pd is used (given the recent trend of rising Pd prices), makes it possible to provide universal motors and the like at low cost. BRIEF DESCRIPTION OF THE DRAWING Fig. Figure 1 is a photograph showing the material structure of a sliding contact material (Ag - 1.2 wt% Ta2O5 - 3.0 wt% ZnO) produced in the first embodiment. DETAILED DESCRIPTION OF PREFERRED EXECUTION FORMS
[0034] First embodiment: Preferred embodiments of the present invention are described with examples shown below. In the present embodiment, a sliding contact material in which 1.2 wt% Ta₂O₅ and 3.0 wt% ZnO were dispersed in a pure Ag matrix, and a composite material comprising the sliding contact material were produced. Subsequently, the composite material was processed into a motor brush, which was installed in a small DC motor, and the wear resistance was evaluated. [Production of sliding contact material]
[0035] In the present embodiment, a sliding contact material was produced by powder metallurgy. Pure Ag powder (average particle size: 7 µm), 1.2 wt% Ta₂O SZnO powder (average particle size: 1 µm) and 3.0 wt% ZnO powder (average particle size: 1 µm) were mixed for 5 hours using a ball mill. A cylindrical container was filled with this powder mixture and compressed by applying a pressure of 5 × 10 2 The material was compressed longitudinally at 1 MPa to form a cylindrical billet with a diameter of 50 mm. This cylindrical billet was then sintered by heating at atmosphere at 850°C for 4 hours. The compression and sintering process was repeated three times, yielding a sliding contact material. This sliding contact material was hot-extruded into a coarse wire with a diameter of 6 mm, which was repeatedly drawn and annealed to obtain a wire rod with a diameter of 1 mm. The wire rod was then further rolled to produce a ribbon-shaped sliding contact material. Fig.Figure 1 shows a photograph of the metal structure of the sliding contact material produced in the present embodiment. [Production of composite material for a motor brush]
[0036] The sliding contact material, in the form of a strip, and a base material were then joined together by cladding (inlaying; coating) to create a composite material. Nickel silver for springs (C7701) was used as the base material. The coating was applied using a roller, and the rolled material was then heat-treated at 750°C to produce the composite. The thickness of the sliding contact material within the composite, which was to be manufactured into a motor brush, was 30 µm. [Reference example]
[0037] To ensure the durability of the sliding contact material produced in the present embodiment (Ag - 1.2% Ta2O) STo evaluate the performance of a material with a sliding contact material of an Ag-50% Pd alloy (-3% ZnO), a composite material with a sliding contact material made of an Ag-Pd alloy was produced as a reference example. The reason an Ag-Pd alloy was used as a reference example for evaluation is that the Ag-Pd alloy exhibits very satisfactory wear resistance, as described above, and that the Ag-Pd alloy is a precious metal-based contact material that is also satisfactory with respect to spark resistance, which is key when used under high loads, and can therefore serve as a reference for evaluating spark resistance. In view of the improved material costs, which are one of the objectives of the present application, and the increased price of Pd, the thickness of the Ag-Pd alloy of the reference example was set to 10 µm to match the material costs.Then the same base material as in the present embodiment was coated with the Ag-50% Pd alloy, resulting in a composite material. [Manufacturing a small DC motor and durability test]
[0038] The composite materials produced in the present embodiment and in the reference example were processed into motor brushes, which were actually used to assemble small DC motors, and durability tests were carried out on the sliding contact materials under two test conditions shown below. Commutators for the small DC motors were produced with composite materials, each consisting of a base material comprising a copper-based material coated with a contact material, with different contact materials being used for different test conditions.
[0039] Among the two groups of test conditions in the present embodiment, “Test Conditions 1” simulated a small, low-load DC motor used in a vehicle's heating, ventilation, and air conditioning (HVAC) system and were intended for evaluating durability against mechanical wear. “Test Conditions 2” simulated a small, high-load DC motor used in an electric folding mirror in an automobile and were used to evaluate durability against spark wear. In the durability test, an operating mode was defined as a combination of counterclockwise rotation (CCW) and off (OFF) and clockwise rotation (CW) and off (OFF) as one cycle, and the number of cycles until motor failure was evaluated. Table 1] Test conditions 1 Test conditions 2 Tension DC 13.5 V Electricity 83 mA 200 mA load 1.96 mN-m 2.0 mN-m Rotational frequency 3400 rpm 7000 rpm commutator AgCuZnNi AgCuNi-Ta2O5 +ZnO mode CCW 6 seconds - OFF 2 seconds CW 6 seconds - OFF 2 seconds CCW 3 seconds - OFF 5 seconds CW 3 seconds - OFF 5 seconds Test environment 25°C 65%± 20%RH
[0040] The results of the durability test under the two test conditions showed that Ag-1.2% Ta2O S -3% ZnO, which was the sliding contact material of the present embodiment, exhibited a durability of 683,000 cycles under test conditions 1. In contrast, the Ag-Pd alloy used as a reference example was found to have failed after 473,000 cycles. The evaluation test under test conditions 1 relates to the mechanical wear characteristics of a low-load motor for HVAC, etc., and the sliding contact material of the present embodiment has a higher durability than the Ag-Pd alloy used as a reference example.
[0041] The evaluation results under test conditions 2 showed that the motors did not fail after 100,000 cycles for either Ag-1.2% Ta2O5 - 3% ZnO or the Ag-Pd alloy. Motors for electric folding mirrors must have a durability of 50,000 cycles under test conditions 2 according to the standard, and it was confirmed that these sliding contact materials have a durability twice or more than specified in the standard. The test under test conditions 2 is used to evaluate the spark resistance of a small, high-load DC motor, and it was confirmed that Ag-1.2% Ta2O S -3% ZnO exhibits high spark resistance. The Ag-Pd alloy, as a reference example, is also considered to have high spark resistance, similar to the present embodiment.
[0042] Thus, the evaluation test under the two groups of test conditions in the present embodiment confirmed that Ag-1.2% Ta2O S -3% ZnO, which was the sliding contact material of the present embodiment, even exhibited advantageous wear resistance and spark resistance compared to the Ag-Pd alloy as a reference example.
[0043] Second embodiment: In the present embodiment, several sliding contact materials with Ag-Ta₂O₅-ZnO with varying Ta₂O₅ and ZnO contents were produced and tested for durability. The sliding contact materials were produced by powder metallurgy, as in the first embodiment. The same pure Ag powder, Ta₂O₅ powder, and ZnO powder were used under the same production conditions as in the first embodiment to produce sliding contact materials (thickness: 30 µm), each comprising an Ag-Ta₂O₅-ZnO alloy, and motor brushes were manufactured using these sliding contact materials.
[0044] Each manufactured motor brush was then installed in the same small DC motor as in the first embodiment and subjected to a durability test. Durability against mechanical wear and spark wear was also tested in the present embodiment, but the evaluation was carried out by an accelerated test under stringent test conditions. Table 2 shows the test conditions in the present embodiment. [Table 2] Test conditions 3 Test conditions 4 Tension DC 12.5 V DC 13.5 V Electricity 90 mA 160 mA load 0.78 mN-m 1.96 mN-m Rotational frequency 7000 rpm 7000 rpm commutator AgCuNi-Ta2O5 +ZnO AgCuZnNi mode CCW 6 seconds - OFF 2 seconds CW 6 seconds - OFF 2 seconds Test environment 25°C 65%± 20%RH
[0045] The two sets of test conditions in the present embodiment each simulated a small, low-load DC motor for HVAC applications. “Test Conditions 3” primarily served to evaluate mechanical wear, and the test was an accelerated test in which the rotational frequency was increased compared to “Test Conditions 1” of the first embodiment. “Test Conditions 4” primarily served to evaluate spark resistance under increased electrical load, and the test was an accelerated test in which the rotational frequency and current were increased compared to “Test Conditions 1” of the first embodiment. Table 3 shows the results of the durability test. Also in the present embodiment, a motor brush with a contact material (thickness: 10 µm) containing an Ag-50% Pd alloy was fabricated as a reference example and subjected to the durability test.The results of the shelf-life test are listed in Table 3. [Table 3] composition Test conditions 3 (wear resistance) Test conditions 4 (spark resistance) Example 1 Ag-1.2Ta2O5 -3ZnO 110,000 cycles 20,000 cycles Example 2 Ag-1.8Ta2O5 -3ZnO 159,000 cycles 51000 cycles Example 3 Ag-1.2Ta2O5 -6ZnO 110,000 cycles 83,000 cycles Example 4 Ag-1.8Ta2O5 -6ZnO 151,000 cycles 100,000 cycles Reference example Ag-50Pd 87000 cycles 9600 cycles *Example 1 is the contact material of the first embodiment.
[0046] The results of the durability test in the present embodiment confirmed that the Ag-Ta2O5-ZnO alloys of the examples were superior to the Ag-Pd alloy as a reference example in the accelerated test under all test conditions, both with respect to wear resistance and spark resistance. Accordingly, the Ag-Ta2O5-ZnO alloys of the present embodiment enable the production of sliding contact materials with high durability combined with cost reduction, since they are Pd-free.
[0047] A comparison of the contact materials in Examples 1 to 4 revealed an improvement in spark resistance with increasing the content of either Ta₂O₅ or ZnO. This suggests that both Ta₂O₅ and ZnO each have an effect on improving spark resistance. A comparison of mechanical wear between Example 1 and Example 2 indicates that Ta₂O₅ improves wear resistance. On the other hand, the comparison between Example 2 and Example 4 showed that increasing the ZnO content did not change the number of cycles before failure, suggesting that ZnO has a weaker effect on improving mechanical wear. Nevertheless, an adequate ZnO content is essential for a motor brush contact material to ensure wear resistance in harsh environments, not only with respect to mechanical wear but also to spark wear.
[0048] If the Ag-50%-Pd alloy tested as a reference example in the first and second embodiments has the same thickness of a contact material as the Ag-Ta₂O₅-ZnO alloys of the present embodiment, it is expected that the Ag-50%-Pd alloy will have a longer service life than in the present embodiment. The Ag-Pd alloy exhibits a very large area of solid-solution strengthening. On the other hand, the present Ag-Ta₂O₅-ZnO alloy according to the invention exhibits wear resistance increased by enhanced dispersion with metal oxide particles, but contains Ag, which is relatively soft, as a matrix, and therefore it is concluded that the area of strengthening is narrower than that by solid-solution strengthening. However, the increased price of Pd has resulted in the Ag-Pd alloy having an unbalanced cost-performance ratio, as described above.Since they are Pd-free, motor brush materials comprising the present Ag-Ta2O5-ZnO alloy according to the invention require significantly lower material costs than the Ag-Pd alloy. As shown in the first and second embodiments, it has been confirmed that the Ag-Ta2O. S ZnO alloys of the present embodiment are very useful as an alternative material to the Ag-Pd alloy with regard to material costs.
[0049] Third embodiment: In the present embodiment, an evaluation was carried out simulating a motor brush of a small, general-purpose, low-load DC motor used in shavers, etc. In the present embodiment, the same Ag-Ta₂O₅-ZnO alloys as in Examples 1 to 3 of the second embodiment were produced by powder metallurgy. Subsequently, a sliding contact material in the form of a strip and a base material were bonded together by cladding in the same manner as in the second embodiment, resulting in a composite material (thickness: 30 µm). The base material used was beryllium copper (C₁₇₁₀C₁₄). The produced composite material was processed into a motor brush, which was used to assemble a small DC motor and subjected to a durability test.
[0050] For comparison, a durability test was performed on two commercially available, universal small DC motors. The commercially available small DC motors used for comparison were one for high voltages and one for low voltages. The high-voltage motor incorporated a motor brush material of an Ag-30% Pd alloy with a thickness of 5 µm, and the low-voltage motor incorporated a motor brush material of an Ag-50% Pd alloy with a thickness of 5 µm. In the present embodiment, the thickness of the contact material comprising the Ag-Ta₂O₅-ZnO alloy (30 µm) was also determined such that the material costs correspond to those of the contact materials of the comparison examples. [Table 4] For high voltages For low voltages Tension DC 3.4 V DC 1.1 V Electricity 0.85 A 2A load 1.27 mN-m Rotational frequency 12500 rpm 10000 rpm commutator AgPdCuZnNi AgPdCuZnNi mode CCW 2 minutes - OFF 2 seconds Test environment 25°C 65%± 20%RH [Table 5] Brush material For high voltages For low voltages Example 1 Ag-1.2Ta2O5 -3ZnO 436 hours 342 hours Example 2 Ag-1.8Ta2O5 -3ZnO 525 hours - Example 3 Ag-1.8Ta2O5 -6ZnO 566 hours - Universal motor Ag-30Pd 352 hours - Ag-50Pd - 169 hours
[0051] Table 5 confirmed that the small DC motors, each with a motor brush material made from one of the Ag-Ta2O S The Ag-Pd alloys of Examples 1 to 3 exhibit operating times comparable to or longer than those of the universal motor for high voltage and the universal motor for low voltage as comparative examples, thus demonstrating satisfactory durability. The results of the present embodiment also suggest that, at the same contact material thickness, the Ag-Pd alloy will exhibit a longer service life than the Ag-Ta2O5-ZnO alloys of the examples. However, the evaluation carried out in the present embodiment was based on concerns about material costs and, from this perspective, confirmed that the Ag-Ta2O5-ZnO alloys of the present embodiment are a useful alternative material to the Ag-Pd alloy.
[0052] Fourth embodiment: Here, motor brush materials were produced with other types of oxides to be dispersed in the Ag matrix, and their resistance to spark wear was evaluated. In the present embodiment, contact materials based on Ag-Ta2O were used. S -ZnO alloy of the first embodiment (Example 1) (Ta2O5: 1.2 wt%, ZnO: 3 wt%) with different amounts of Ta2O S and those in which MgO or SnO was dispersed instead of ZnO, and their durability when installed in a small DC motor was evaluated. The contact materials were produced by powder metallurgy as in the first embodiment. For the ZnO and SnO mixtures, ZnO powder and SnO powder with a particle size of 1 µm each were used.
[0053] The contact materials were used to produce composite materials and processed into motor brushes, which were then used to mount small DC motors. A wear test was then carried out under the conditions described below. The test conditions simulated an automatic door lock in a car and were primarily intended to evaluate spark resistance. [Table 6] Tension DC 13.5 V Electricity 3A mode CCW 0.1 seconds - OFF 2.4 seconds CW 0.1 seconds - OFF 2.4 seconds Commutator material AgCuNiMgZn Load 50 g-cm Test environment 298 K, 50% RH
[0054] In the wear test of the present embodiment, each motor that had been operated in this mode for 100,000 cycles was disassembled, the brush was removed, and the wear depth was measured using a contact roughness measuring device (number of tests: 3). Table 7 shows the mean values of the measured wear depth for the motor brush materials. Table 7] Composition (in % of mass) Wear depth AG Ta2O3 ZnO MgO SnO Example 1 balance sheet 1.2 3.0 - - 14 µm Example 2 balance sheet 1.8 3.0 - - 16 µm Example 5 balance sheet 0.6 3.0 - - 16 µm Example 6 balance sheet 0.6 5.0 - - 15 µm Comparative Example 1 balance sheet 1.2 - - - 18 µm Comparative Example 2 balance sheet 1.2 - 2.3 - 22 µm Comparative Example 3 balance sheet 1.8 - 2.3 - 25 µm Comparative Example 4 balance sheet 0.6 - 2.3 - 22 µm Comparative Example 5 balance sheet 1.2 - - 3.0 22 µm Comparative Example 6 balance sheet 1.2 - - 5.0 26 µm Comparative Example 7 balance sheet 1.2 3.0 2.3 - 22 µm Comparative Example 8 balance sheet 1.2 3.0 - 3.0 20 µm
[0055] As confirmed in the second embodiment, Ta2O is assumed to be among the oxides dispersed in the Ag matrix. S The primary function of the contact material is to ensure its resistance to mechanical wear, and ZnO is believed to improve its spark resistance. The results of the present embodiment (Table 7) showed that contact materials containing a non-ZnO oxide (MgO, SnO) dispersed exhibited lower spark resistance than the materials from Example 1, etc. Contact materials containing ZnO but also dispersed MgO or SnO did not have satisfactory spark resistance. This suggests that not all types of metal oxide should be dispersed. The present embodiment demonstrated that ZnO is preferable for improved resistance to mechanical and spark wear. Industrial applicability
[0056] The sliding contact material according to the invention is wear-resistant and spark-resistant, which is advantageous for brushes of small DC motors, and has a long service life combined with a noise-reducing effect. The present invention can preferably be applied to small DC motors in various fields, including automotive applications, precision instruments, and household appliances. In the automotive sector, the present invention can be used for small DC motors in electrical components such as audio equipment, air conditioning flaps, electric folding mirrors, and automatic door locks. In household appliances, the present invention can be used for small motors in razors, electric toothbrushes, small vacuum cleaners, etc. QUOTES INCLUDED IN THE DESCRIPTION
[0000] This list of documents cited by the applicant was automatically generated and is included solely for the reader's convenience. The list is not part of the German patent or utility model application. The DPMA accepts no liability for any errors or omissions. Cited patent literature
[0000] Japanese patent application no. Hei 11-4563
[0006] Japanese patent application no. 2005-176492
[0006] Japanese patent application no. Hei 5-277762
[0006]
Claims
[1] A sliding contact material for a motor brush, the sliding contact material comprising: pure Ag as a matrix; and ZnO particles and Ta2O5 particles dispersed in the matrix, the sliding contact material having a ZnO particle content of 0.1 mass% or more and 12 mass% or less and a Ta2O5 particle content of 0.1 mass% or more and 6.0 mass% or less. [2] The sliding contact material for a motor brush according to claim 1, wherein the pure Ag as a matrix is pure Ag having a total Fe / Cr / Ni content of 0.3 mass% or less. [3] A composite material for a motor brush, the composite material comprising: a base material comprising a Cu-based material; and a sliding contact material bonded to at least a part of the base material, wherein the bonded sliding contact material is the sliding contact material defined in claim 1 or 2. [4] A motor brush for a DC motor, the motor brush comprising the composite material defined in claim 3. [5] A DC motor comprising: a motor brush; and a commutator, wherein the motor brush is the motor brush defined in claim 4.
Citation Information
Patent Citations
JP1977077762U
Carbon brush
JP1999004563A
Brush for DC motor
JP2005176492A