Anode electrode structure
Anode electrode structures with lithium-ion conductive films stabilize lithium metal deposition, addressing integration challenges and enhancing the performance and safety of lithium-ion batteries.
Patent Information
- Application Number
- DE202018006949
- Authority / Receiving Office
- DE · DE
- Patent Type
- Utility models
- Current Assignee / Owner
- Priority Date
- 2017-09-21
- Filing Date
- 2018-09-12
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2028-09-30
AI Technical Summary
Conventional lithium-ion batteries face challenges with the integration of lithium metal due to its reactivity and instability, leading to safety issues and processing complexities, which affect the capacity and stability of silicon-mixed graphite anodes.
The development of anode electrode structures that include a current collector with a lithium metal film protected by a lithium-ion conductive film, such as ceramics or ion-conducting polymers, to stabilize lithium metal deposition and enhance electrochemical performance.
This approach stabilizes lithium metal deposition, prevents dendrite formation, and improves the capacity and cycle stability of lithium-ion batteries, reducing manufacturing complexity and enhancing safety.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL BACKGROUND Technical area
[0001] The implementations described herein generally relate to metal electrodes, in particular lithium-containing anodes, high-performance electrochemical devices such as secondary batteries, including the above so-called lithium-containing electrodes. Description of the state of the art
[0002] Rechargeable electrochemical storage systems are gaining importance in many areas of daily life increasingly important. High-capacity electrochemical energy storage devices, such as lithium-ion Batteries (Li-ion batteries) are being used in more and more applications, including portable electronic devices, medicine, transport, grid-connected large energy storage systems, Storage of renewable energy and in uninterruptible power supplies (UPS). Conventional lead- / Sulfuric acid batteries often lack capacity and cycle stability for these increasing applications. However, lithium-ion batteries are considered to have the best chances.
[0003] As a rule, lithium-ion batteries do not contain metallic lithium for safety reasons, but use Anode is a graphitic material. However, the use of graphite, which in the charged state up to the limit composition LiC is chargeable, a significantly lower capacity compared to the use of 6 metallic lithium. Currently, the industry is moving away from graphite-based anodes and towards Silicon-mixed graphite to increase energy cell density. For anodes made of silicon-mixed graphite However, graphite leads to a capacity loss in the first cycle. Therefore, the deposition of of lithium metal to compensate for the capacity loss of silicon-mixed graphite anodes in the first cycle However, there are several challenges to be overcome when integrating lithium metal into devices. get over.
[0004] Lithium is an alkali metal. Lithium, like the heavy element homologues of the first main group, characterized by strong reactivity with a variety of substances. Lithium reacts violently with water, Alcohols and other substances containing protic hydrogen, which often leads to inflammation. Lithium is unstable in the air and reacts with oxygen, nitrogen and carbon dioxide. Lithium is usually used under protective gas atmosphere (noble gases such as argon), and due to the strong reactivity of lithium, it is necessary that other processing operations are also carried out in a protective gas atmosphere. As a result Lithium presents several challenges in terms of processing, storage and transportation.
[0005] Protective surface treatments have been developed for lithium metal. A process for protective Surface treatment of lithium metal consists in coating the lithium metal with a layer of wax, for example Polyethylene wax. However, this usually involves applying a large amount of coating agent, which impairs the subsequent processing of the lithium metal film. For example, EP 1236231 A1 describes Lithium anodes for electrochemical cells. WO 2017 / 131997 A1 describes a lithium deposition process using a tool for a protective layer.
[0006] Another method for protective surface treatment proposes the production of stabilized Lithium metal powder (SLMP) with a continuous carbonate coating, polymer coating, for example Polyurethanes, PTFE, PVC, polystyrene and others. However, these polymer coatings can Pre-lithiation of electrode materials can cause problems.
[0007] Therefore, there is a need for methods and systems for the deposition and processing of lithium metals in Energy storage systems. SUMMARY
[0008] The implementations described herein generally relate to metal electrodes, in particular lithium-containing anodes, high-performance electrochemical devices such as secondary batteries, including the above lithium-containing electrodes, and methods for their production. In one implementation, a Anode electrode structure is provided. The anode electrode structure includes a current collector comprising copper, a lithium metal film formed on the current collector, a copper film formed on the lithium metal film and a protective film formed on the copper film. The protective film is a lithium-ion conductive film selected from the Group comprising lithium-ion conductive ceramic, lithium-ion conductive glass or ion conductive liquid crystal.
[0009] In a further implementation, an anode electrode structure is provided. The anode electrode structure comprises a current collector comprising copper, a silicon graphite anode formed on the current collector, a the silicon graphite anode formed film of lithium metal and a film formed on the lithium metal film Protective film. The protective film is a lithium-ion conductive material selected from the group comprising lithium-ion conductive ceramic, lithium-ion conductive glass, ion-conductive polymer, ion-conductive liquid crystal, composite Combinations thereof or unit layer combinations thereof.
[0010] In yet another implementation, an anode electrode structure is provided. The Anode electrode structure comprises a current collector comprising copper, a lithium metal film deposited on the current collector is formed; a metal film formed on the lithium metal film, the metal film having an upper Surface and sidewalls of the lithium metal film coated, which extend to contact with the current collector; and a protective film formed on the metal film, wherein the protective film is a lithium ion conductive film, and wherein the Metal film is selected from a copper film, a bismuth film, a tin film or combinations thereof.
[0011] In yet another implementation, an anode electrode structure is provided. The Anode electrode structure comprises a current collector comprising copper, a current collector formed on the current collector Lithium metal film and a protective film stack formed on the lithium metal film. The protective film stack comprises a the lithium metal film formed protective film, a first polymer film formed on the protective film, a first polymer film formed on the first polymer film formed ceramic film and a second polymer film formed on the ceramic film. The protective film is from the group of lithium fluoride (LiF), aluminum oxide, bismuth chalcogenide, copper chalcogenide, lithium carbonate (Li CO 2 3 ) and combinations thereof.
[0012] In yet another implementation, an anode electrode structure is provided. The Anode electrode structure comprises a current collector comprising copper, a current collector formed on the current collector Lithium metal film and a protective film stack formed on the lithium metal film. The protective film stack comprises a first polymer film formed on the lithium metal film, a dielectric film formed on the first polymer film and a second polymer film formed on the ceramic film.
[0013] In yet another implementation, an anode electrode structure is provided. The Anode electrode structure comprises a current collector comprising copper, a current collector formed on the current collector Lithium metal film and a protective film stack formed on the lithium metal film. The protective film stack comprises a the lithium metal film, a dielectric film formed on the copper film and a dielectric film formed on the polymer film formed by a dielectric film. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] To understand the details of the above-mentioned features of the present disclosure, a more concrete description of the implementations briefly summarized above based on implementations some of which are illustrated in the attached drawings. However, it should be noted that the The accompanying drawings only illustrate typical implementations of this disclosure and therefore are not to be considered be regarded as a limitation of the scope of protection, since the disclosure of other equally effective can allow implementations. Fig. 1 illustrates a schematic cross-sectional view of an implementation of a Energy storage device including an electrode structure constructed according to the method described herein implementations are formed; Fig. 2 illustrates a cross-sectional view of an implementation of a double-sided Anode electrode structure formed according to implementations described herein; Fig. 3 illustrates a cross-sectional view of another implementation of a double-sided Anode electrode structure formed according to implementations described herein; Fig. 4 illustrates a cross-sectional view of another implementation of a double-sided Anode electrode structure formed according to implementations described herein; Fig. 5 illustrates a cross-sectional view of another implementation of a double-sided Anode electrode structure formed according to implementations described herein; Fig. 6 illustrates a cross-sectional view of another implementation of a double-sided Anode electrode structure formed according to implementations described herein; Fig. 7 illustrates a process flow diagram that shows an implementation of a method for forming a Anode electrode structure ture according to implementations described herein; Fig. 8 illustrates a process flow diagram that shows an implementation of a method for forming a anode electrode structure according to implementations described herein; Fig. 9 illustrates a process flow diagram that shows an implementation of a method for forming a anode electrode structure according to implementations described herein; Fig. 10 illustrates a process flow diagram showing an implementation of a method for forming a anode electrode structure according to implementations described herein; Fig. 11 illustrates a process flow diagram showing an implementation of a method for forming a anode electrode structure according to implementations described herein; and Fig. 12 illustrates a schematic view of an integrated processing tool for forming Anode electrode structures according to implementations described herein.
[0015] To facilitate understanding, the same reference numerals have been used where possible to indicate identical to designate elements that are common to the figures. It is considered that elements and features of a Implementation can be advantageously integrated into other implementations without further mention. DETAILED DESCRIPTION
[0016] The following disclosure describes anode electrodes, high performance electrochemical cells and batteries including the above-mentioned anode electrodes and methods for their manufacture. In the following description and in Figures 1 to 12 certain details are explained to provide a comprehensive understanding of the various implementations of the disclosure. Further details, the well-known structures and systems which are often associated with electrochemical cells and batteries are described in the following Disclosure is not set forth in order not to unnecessarily obscure the description of the various implementations.
[0017] Many of the details, dimensions, angles and other features shown in the figures are for illustrative purposes only. Illustration of particular implementations. Accordingly, other implementations may contain different details, components, dimensions, angles and features without departing from the spirit or scope of this Disclosure. In addition, other implementations of the disclosure may be made without some of the The details described below are implemented in practice.
[0018] The implementations described herein are described below with respect to a coil-to-coil Coating system such as TopMet™, SMARTWEB®, TopBeam™, all manufactured by Applied Materials, Inc. in Santa Clara, California. Other tools that perform physical vapor deposition processes (e.g. high-speed evaporation processes and magnetron sputtering processes) can also be adapted to benefit from the implementations described herein. In addition, any system that supports the The physical vapor deposition processes described here can be used advantageously. The device description described is for illustrative purposes only and should not be construed as a limitation of the scope of protection of the be construed or interpreted in the implementations described herein. It is further understood that the described implementations, although described as a reel-to-reel process, also on separate substrates can be carried out.
[0019] Energy storage devices, such as batteries, usually consist of a positive electrode, an anode electrode separated by a porous separator and an electrolyte which acts as an ion-conducting Matrix is used. Graphite anodes currently represent the state of the art, but the industry is moving from anodes to Graphite-based anodes to silicon-mixed graphite to increase the energy density of the cell. However, with graphite mixed with silicon, an irreversible loss of capacity often occurs during the first cycle. There is therefore a need for methods to compensate for this capacity loss in the first cycle.
[0020] The deposition of lithium metal is one such method to compensate for this capacity loss of a silicon-based mixed graphite anode in the first cycle. Although there are numerous processes for the deposition of Lithium metal (e.g. thermal evaporation, lamination, printing, etc.), the handling of the lithium metal on a coil deposited lithium metal before stacking in the device, especially in a Production environment with large quantities. In an implementation, processes and systems for forming Lithium anode devices provided.
[0021] Using the implementations described herein, the single-sided or double-sided deposited Lithium metal during winding and unwinding of the subsequent coils. The deposition of thin films of Lithium-ion conductive polymers, ion-conductive ceramics or ion-conductive glass have several advantages. Firstly, electrode coils containing lithium metal can be wound and unwound without the lithium metal adjacent electrodes. Secondly, a stable solid electrolyte interface (SEI) is used for better cell performance and high electrochemical utilization of the lithium metal. The protective layer can also help to protect lithium dendrites suppress or eliminate, especially when operating at high current density. In addition, the Use of protective films reduces the complexity of manufacturing systems and is compatible with current manufacturing systems compatible.
[0022] Fig. 1 illustrates a schematic cross-sectional view of an implementation of a Energy storage device 100 including an anode electrode structure constructed according to the method described herein implementations. Although the energy storage device 100 is shown as a planar structure, it may by rolling the layer stack into a cylinder; in addition, other cell configurations (e.g. prismatic cells, button cells or stacked electrode cells). Energy storage device 100 has an anode electrode structure 110 and a cathode electrode structure 120 with a separating film 130 positioned therebetween. The cathode electrode structure 120 has a Cathode current collector 140 and a cathode film 150. The anode electrode structure 110 has a Anode current collector 160, an anode film 170 and at least one protective film 175, a lithium-ion conductive Polymer film 180, a ceramic coating 185 and a binding porous polymer film 190.
[0023] The cathode electrode structure 120 has the cathode current collector 140 with the Cathode film 150 formed by the cathode current collector 140. It is understood that the cathode electrode structure 120 may also contain other elements or films.
[0024] The current collectors 140, 160 on the cathode film 150 and the anode film 170, respectively, may have identical or different electronic conductors. Examples of metals from which the current collectors 140, 160 can be made are close aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), stainless steel, clad Materials, their alloys, and combinations thereof. In one implementation, at least one of the Current collectors 140, 160 are perforated. In one implementation, at least one of the current collectors 140, 160 has a Polyethylene terephthalate polymer substrate (PET) coated with a metallic material. In this implementation, the anode current collector 160 is a copper-coated PET film. In another Implementation, the anode current collector 160 is a multi-metal layer on PET. In the multi-metal layer, These can be combinations of copper, chromium, nickel, etc. In one implementation, the anode current collector 160 a multilayer structure comprising a copper-nickel plating material. In one implementation, the Multi-layer structure a first layer of nickel or chromium, a second layer formed on the first layer of Copper and a third layer formed on the second layer containing nickel, chromium or both. In a In this embodiment, the anode current collector 160 is made of nickel-plated copper. In addition, Current collectors of any form factor (e.g. metal foil, track or plate), shape and micro / macrostructure In prismatic cells, the strips are generally made of the same material as the current collector and can be formed during the production of the stack or added later. In some Implementations, the current collectors extend beyond the stack, and the sections of the current collector, that extend beyond the stack can be used as strips. All components except the current collectors 140 and 160 contain lithium-ion electrolytes. In one implementation, the cathode current collector 140 is made of Aluminum. In another implementation, the cathode current collector 140 comprises deposited on a PET film Aluminum. In one implementation, the cathode current collector 140 has a thickness of about 0.5 µm to about 20 µm (e.g., B. from about 1 µm to about 10 µm; from about 2 µm to about 8 µm; or from about 5 µm to about 10 µm). In a In one implementation, the anode current collector 160 is made of copper. In one implementation, the anode current collector 160 a thickness of about 0.5 µm to about 20 µm (e.g. from about 1 µm to about 10 µm; from about 2 µm to about 8 µm; from about 6 µm to about 12 µm; or from about 5 µm to about 10 µm).
[0025] The cathode film 150 or cathode may be any material compatible with the anode and may comprise a intercalation compound, an insertion compound or an electrochemically active polymer. Suitable Intercalation materials include, for example, lithium-containing metal oxides, MoS , FeS , BiF , Fe OF , MnO , TiS , NbSe , 2 2 3 2 4 2 2 3 LiCoO , LiNiO , LiMnO , LiMn O , VO and VO. Suitable polymers have, for example, 2 2 2 2 4 6 43 2 5 polyacetylene, polypyrrole, polyaniline and polythiophene. The cathode film 150 or the cathode can be made of a layered oxide, such as lithium cobalt oxide, an olivine, such as lithium iron phosphate, or a spinel, such as Lithium manganese oxide. Examples of lithium-containing oxides can be layered, such as lithium cobalt oxide (LiCoO ) or mixed metal oxides, such as LiNi Co MnO , LiNiMnCoO (´´NMG´´), LiNi Mn O , Li(Ni Co Al )O , 2x1 -2x2 2 0.5 1.5 4 0.8 0.15 0.05 2 LiMnO and doped lithium-rich layered materials, where x is zero or a non-zero number. 2 4 Examples of phosphates include iron olivine (LiFePO ) and its variants (such as LiFe Mg PO ), LiMoPO , LiCoPO , LiNiPO 4 ( 1-x) x 4 4 4 4 , Li V (PO ) , LiVOPO , LiMP O or LiFe PO , where x is zero or a number other than zero. 3 2 4 3 4 2 7 1.5 2 7 Examples of fluorophosphates can be LiVPO F, LiAlPO F, Li V(PO ) F , Li Cr(PO ) F , Li CoPO F or Li NiPO F. 4 4 5 4 2 2 5 4 2 2 2 4 2 4 Examples of silicates are LiFeSiO, LiMnSiO, or LiVOSiO. An example of a non-lithium compound is NaV 2 4 2 4 2 4 5 (PO ) F . 2 4 2 3
[0026] The anode electrode structure 110 has the anode current collector 160 with the on the anode current collector 160 formed anode film 170. The anode electrode structure 110 may optionally have at least one of the protective film 175, the lithium-ion conductive polymer film 180, the ceramic coating 185 and the binding porous polymer film 190 In the implementation shown in Fig. 1, the protective film 175 is formed on the anode film 170. The film of the lithium-ion conductive polymer film 180 is formed on the protective film 175. The ceramic coating 185 is on the lithium-ion conductive polymer film 180. Between the separator film 130 and the anode film 170, a binding porous polymer film 190 is formed.
[0027] The anode film 170 may be made of any material that is compatible with the cathode film 150. The Anode film 170 may have an energy capacity greater than or equal to 372 mAh / g, preferably ≥ 700 mAh / g and most preferably ≥ 1000 mAh / g. The anode film 170 may be made of graphite, silicon-containing graphite, Lithium metal, lithium metal foil or a lithium alloy foil (e.g. lithium-aluminium alloys) or a Mixture of a lithium metal and / or a lithium alloy and materials such as carbon (e.g. coke, graphite), Nickel, copper, tin, indium, silicon, oxides thereof, or combinations thereof. The anode film 170 usually includes intercalation compounds containing lithium or insertion compounds containing lithium In some implementations where the anode film 170 comprises lithium metal, the lithium metal deposited using the methods described herein.
[0028] In one implementation, the anode film 170 has a thickness of about 10 µm to about 200 µm (e.g., from about 1 µm to about 100 µm; from about 10 µm to about 30 µm; from about 20 µm to about 30 µm; from about 1 µm to about 20 µm; or from about 50 µm to about 100 µm). In one implementation, the anode film 170 is a lithium metal film.
[0029] In some implementations, the protective film 175 is formed on the anode film 170. The protective film 175 has at least one of lithium fluoride (LiF), a metal film (e.g. copper, bismuth, tin or combinations thereof), a copper chalcogenide (e.g. CuS, CuSe, CuS), a bismuth chalcogenide (e.g. BiTe, BiSe) and a lithium carbonate (Li 2 2 2 3 2 3 2 CO ). In some implementations, the protective film 175 is for at least one of lithium ions and lithium atoms 3 The protective film 175 provides surface protection of the anode film 170, thereby facilitating the handling of the anode film in a dry room. Without being bound to any theory, it is assumed that the protective film 175 can absorb Li-conductive electrolytes during device manufacture to form a gel, which has a positive effect on the formation of a good solid electrolyte interface (SEI) and also contributes to the reduction of resistance. In some implementations where the energy storage device 100 comprises a solid-state Energy storage device, the protective film 175 helps to build a better SEI and the The protective film 175 can be formed by physical vapor deposition (PVD), such as Evaporation or sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating or a three-dimensional lithium printing process directly on the Anode film 170 is deposited. PVD is a preferred method for depositing the protective film 175.
[0030] In some implementations, the protective film 175 is a metal film. The metal film may be an ultra-thin The metal film can be a copper film. The copper film can be an ultrathin copper film.
[0031] The protective film 175 may be a coating or a separate film, each having a thickness in the range of 1 Nanometers to 2000 nanometers (e.g. in the range from 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 50 nanometers to 200 nanometers; in the range from 100 nanometers to 150 nanometers) The protective film 175 may be a separate film having a thickness in the range of 1 micrometer to 50 micrometers (e.g. in the range of 1 micrometer to 25 micrometers).
[0032] The protective film 175 may be porous. In some implementations, the protective film 175 has nanopores. In one Implementation, the protective film 175 has a plurality of nanopores that are sized to form a average pore size or an average pore diameter of less than about 10 nanometers (e.g. from about 1 nanometer to about 10 nanometers; from about 3 nanometers to about 5 nanometers). In another Implementation, the protective film 175 has a plurality of nanopores whose average pore size or whose average pore diameter is less than about 5 nanometers. In one implementation, the protective film 175 a multitude of nanopores with a diameter in the range of about 1 nanometer to about 20 nanometers (e.g. from about 2 nanometers to about 15 nanometers; or from about 5 nanometers to about 10 nanometers).
[0033] In some implementations, a lithium-ion conductive polymer film 180 is formed on the protective film 175. Without To be bound by a theory, it is assumed that the lithium-ion conductive polymer film conducts 180 lithium ions and blocks any dendrites that may originate from the anode film 170. Examples of ion-conducting polymers used for Formation of the lithium-ion conductive polymer film 180 include polyvinylidene difluoride (PVDF), Polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4- 2 4 2 benzoquinone, polyphenylene sulfide, poly(sulphur-random)-triallylamine, polyetheretherketone (PEEK), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof, but are not limited to limited.
[0034] In some implementations, the ceramic coating 185 is deposited on the lithium-ion conductive polymer film 180 The ceramic coating 185 comprises one or more dielectric materials. The dielectric material may be a ceramic material. The ceramic material can be an oxide. The ceramic material can, for example, from aluminum oxide (Al O ), AlO , AlO N , aluminum oxyhydroxide AIO(OH), AIN (in a nitrogen environment 2 3 xxy deposited aluminum), calcium carbonate (CaCO ), titanium dioxide (TiO ), niobium oxide (Nb O ), SiS , SiPO , silicon oxide (SiO 3 2 2 5 2 4 2 ), zirconium oxide (ZrO), MgO, TiO, TaO, NbO, LiAlO, LiNbO, LiTaO, LiNbO, BaTiO, BN, ion-conducting garnet, 2 2 2 5 2 5 2 3 3 2 3 3 Ion-conducting perovskite, ion-conducting anti-perovskite, porous glass ceramics and the like or combinations In one embodiment, the ceramic material is a material selected from the group consisting of: porous aluminum oxide, porous ZrO , porous SiO , porous MgO, porous TiO , porous Ta O , 2 2 2 2 5 porous NbO, porous LiAlO, porous LiNbO, porous LiTaO, porous Li NbO, porous BaTiO, ion conductive 2 5 2 3 3 2 3 3 Garnet, anti-ion conducting perovskites, Li SP S glass, porous glass dielectric or combinations thereof. 2 2 5 Ceramic coating 185 is a binderless dielectric film. In some implementations, the Ceramic coating 185 a porous aluminum oxide film.
[0035] The ceramic coating 185 may be a lithium-ion conductive ceramic or a lithium-ion conductive glass. The Li-ion conductive material can, for example, consist of one or more LiPON, doped variants of either crystalline or amorphous phases of Li La Zr O , doped anti-perovskite compositions, Li SP S , Li S, LiKSO 7 3 2 12 2 2 5 2 4 , Li P, Li BS , Li GeP S , Li PS , LiNH , LiNO , lithium amide borohydride Li(BH ) (NH ) , lithium phosphate glasses, (1-x)LiI- 3 5 7 13 10 2 12 3 4 2 3 4 1-x 2x (x)Li SnS , xLiI-(1-x)Li SnS , mixed sulfide and oxide electrolytes (crystalline LLZO, an amorphous (1-x)LiI-(x)Li SnS - 4 4 4 4 4 4 mixture and amorphous xLiI-(1-x)Li SnS ). In one implementation, x is between 0 and 1 (e.g., 0.1, 0.2, 0.3, 4 4 0.4, 0.5, 0.6, 0.7, 0.8 and 0.9). The lithium-ion conductive material can be either by physical Gas phase deposition (PVD), chemical vapor deposition (CVD), spraying, doctor blade coating, printing or any A number of other coating processes can be used to deposit lithium metal film directly onto it. For some PVD is a suitable process for some implementations. In some implementations, the ceramic coating must be 185 not be ion-conductive; however, once filled with electrolyte (liquid, gel, solid, combination, etc.), the Combination of porous substrate and electrolyte ion conductive.
[0036] In some implementations, the ceramic coating 185 is selected from the group consisting of: Lithium zirconate (LiZrO), LiPON, crystalline or amorphous phases of the garnet type LiLaZrO, LISICON (e.g. LiZn 2 3 7 3 2 12 2+2x 1- GeO , where 0 < x < 1), NASICON (e.g. Na Zr Si PO , where 0 < x < 3), lithium borohydride (LiBH ), doped anti- x 4 1+x 2 x 3-x 12 4 Perovskite compositions, lithium-containing sulfides (e.g. Li S, Li SP S , Li GeP S and Li PS ) and lithium 2 2 2 5 10 2 12 3 4 Argyrodites (e.g. LiPS X, where x is Cl, Br or I). 5
[0037] The ceramic coating 185 may have a thickness in the range of 1 nanometer to 2000 nanometers (e.g. in the range from 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 100 nanometers up to 200 nanometers; in the range of 100 nanometers to 150 nanometers).
[0038] In some implementations, the bonding porous polymer film 190 is between the ceramic coating 185 and the Separating film 130 is formed. Without being bound to any theory, it is assumed that the binding porous polymer film 190 helps to improve the adhesion between the anode electrode structure 110 and the separator film 130, when these are connected to each other.
[0039] The polymer for the binding porous polymer film 190 can be selected from polymers that are currently used in the lithium-ion battery industry. Examples of polymers used to form the Lithium gel polymer film can be used, including polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), Ethylene oxide (EO), polyacrylonitrile (PAN), succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, 2 4 2 Polyphenylene sulfide, polyetheretherketone (PEEK), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. Without being bound to any theory, it is assumed that the binding porous polymer film 190 can accommodate Li-conducting electrolytes during device manufacture to form a gel which has a positive effect on the formation of a good solid electrolyte interface (SEI) and also contributes to the reduction of resistance. In some implementations, the gel electrolyte or the liquid crystal electrolyte is Using a mixture of warm liquids and a lithium-ion conductive salt. The mixture warm liquids are injected into the spirally wound electrodes or stacked electrodes, filling the pores of the network electrodes and the electrolyte forms a solid or a gel at room temperature. The binding porous Polymer film 190 can be formed by dip coating, slot die coating, gravure coating or printing Organic polymers with sulfur ions (e.g. polyphenylene sulfide with Li O mixture) show good results for 2 Lithium metal-based anodes and in some cases form liquid crystal electrolytes.
[0040] The binding porous polymer film 190 may have a thickness in the range of 5 nanometers to 2000 micrometers (e.g., in Range from 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 100 nanometers to 200 nanometers; in the range of 100 nanometers to 150 nanometers).
[0041] The separation film 130 is formed between the anode electrode structure 110 and the cathode electrode structure 120. The separator film 130 comprises a porous (e.g., microporous) polymer substrate capable of trapping ions with pores. conduct (e.g., a separator film). In some implementations, the porous polymer substrate itself does not need to be ion-conductive However, once filled with electrolyte (liquid, gel, solid, combination, etc.), the combination of porous substrate and electrolyte ions conducting. In one implementation, the porous polymer substrate is a multi-film Polymer substrate. In one implementation, the pores are micropores. In some implementations, the porous Polymer substrate made of any commercially available microporous polymer membranes (e.g. single-layer or multi-layer), for example, the products of Polypore (Celgard Inc., Charlotte, North Carolina), Toray Tonen (battery separator film (BSF)), SK Energy (Li-ion battery separator (LiBS), Evonik Industries (SEPARION® ceramic separator membrane), Asahi Kasei (Hipore™ polyolefin flat film membrane), DuPont (Energain®), etc. In some implementations, the porous polymer substrate has a porosity in the range of 20 to 80% (e.g. in the range of 28 to 60%). In some Implementations, the porous polymer substrate has an average pore size in the range of 0.02 to 5 micrometers (e.g., 0.08 to 2 micrometers). In some implementations, the porous polymer substrate has a Gurley Number in the range of 15 to 150 seconds. In some implementations, the porous polymer substrate is polyolefinic. Examples of polyolefins are polypropylene, polyethylene or combinations thereof.
[0042] In some implementations where the energy storage device 100 is a solid-state battery, the separating film 130 is replaced by a lithium-ion conductive glass. The lithium-ion conductive material can be a lithium Ion-conducting ceramic or lithium-ion-conducting glass. The Li-ion conductive material can, for example, be one or more LiPon, doped variants of either crystalline or amorphous phases of Li La Zr O , 7 3 2 12 doped anti-perovskite compositions, Li SP S , Li GeP S and Li PS , lithium phosphate glasses, (1-x)LiI-(x)Li SnS 2 2 5 10 2 12 3 4 4 4 , xLiI-(1-x)Li SnS , mixed sulfide and oxide electrolytes (crystalline LLZO, an amorphous (1-x)LiI-(x)Li SnS mixture 4 4 4 4 and amorphous xLiI-(1-x)Li SnS ). In one implementation, x is between 0 and 1 (e.g., 0.1, 0.2, 0.3, 0.4, 0.5, 4 4 0.6, 0.7, 0.8 and 0.9).
[0043] Introduced into the anode electrode structure 110, the cathode electrode structure 120 and the separating film 130 Electrolytes can consist of a liquid / gel or a solid polymer and can each be different In some implementations, the electrolyte mainly comprises a salt and a medium (e.g., in a In a liquid electrolyte the medium can be called a solvent, in a gel electrolyte the medium can be a polymer matrix). The salt can be a lithium salt. The lithium salt can be used for example LiPF , LiAsF , LiCF SO , LiN(CF SO ) , LiBF and LiClO , BETTE electrolyte (sold by 3M Corp., 6 6 3 3 3 3 3 6 4 Minneapolis, MN) and combinations thereof. Solvents may include, for example, ethylene carbonate (EC), propylene carbonate (PC), EC / PC, 2-MeTHF(2-methyltetrahydrofuran) / EC / PC, EC / DMC (dimethyl carbonate), EC / DME (dimethylethane), EC / DEC (diethyl carbonate), EC / EMC (ethyl methyl carbonate), EC / EMC / DMC / DEC, EC / EMC / DMC / DEC / PE, PC / DME and DME / PC. Polymer matrices can be, for example, PVDF (polyvinylidene fluoride), PVDF:THF (PVDF: Tetrahydrofuran), PVDF:CTFE (PVDF: Chlorotrifluoroethylene), PAN (Polyacrylonitrile) and PEO (Polyethylene oxide). In In one embodiment, the electrolyte is a solvent in salt, wherein the solvent percentage is much lower than the solvent percentage in a typical electrolyte.
[0044] Fig. 2 illustrates a cross-sectional view of an implementation of an anode electrode structure 200, the formed according to implementations described herein. It should be noted in Fig. 2 that the anode current collector 160 is shown as projecting beyond the stack, although it is not necessary that the anode current collector 160 extends beyond the stack, the sections extending beyond the stack can be used as strips. Although the anode electrode structure 200 is shown as a double-sided electrode structure, it is understood that the described implementations also apply to single-sided electrode structures.
[0045] The anode electrode structure 200 comprises the anode current collector 160, anode films 170a, 170b (collectively 170) formed on opposite sides of the anode current collector 160. In one implementation, the Anode film 170 is a lithium metal film. In one implementation, the anode film 170 has a thickness of 20 micrometers or less (e.g., from about 1 micrometer to about 20 micrometers). On each of the anode films 170a, 170b, a Metal film 210a, 210b (collectively 210). In one implementation, the metal film is made of a copper film, a bismuth film or a tin film. In one implementation, the metal film is an ultra-thin metal film with a Thickness of 100 nanometers or less (e.g. from about 5 nanometers to 100 nanometers; from about 5 nanometers to about 40 nanometers; from about 10 nanometers to about 20 nanometers; or from about 50 nanometers to about 100 nanometers). In In some implementations, as shown in Fig. 2, the metal film 210 coats the exposed surfaces (e.g. top and side walls) of the anode film 170 and extends to contact with the anode current collector 160. On each of the metal films 210a, 210b, a protective film 220a, 220b (collectively 220) is formed. In some Implementations, the protective film 220 is permeable to at least lithium ions and lithium atoms. In a In one embodiment, the protective film 220 is selected from the group comprising lithium-ion conductive ceramics, lithium Ion-conducting glass or ion-conducting liquid crystal. The protective film 220 can have a thickness in the range of 5 nanometers up to 2000 micrometers (e.g. in the range from 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 100 nanometers to 200 nanometers; in the range from 100 nanometers to 150 nanometers) have.
[0046] Fig. 3 illustrates a cross-sectional view of another implementation of an anode electrode structure 300 formed according to implementations described herein. It should be noted in Fig. 3 that the Anode current collector 160 is shown extending beyond the stack, although it is not necessary that the Anode current collector 160 projects beyond the stack, the sections projecting beyond the stack can be formed as strips Although the anode electrode structure 300 is shown as a double-sided electrode structure, It is important to note that the implementations described herein also apply to single-sided electrode structures.
[0047] The anode electrode structure 300 comprises the anode current collector 160, anode films 170a, 170b (collectively 170) formed on opposite sides of the anode current collector 160. In one implementation, the Anode film 170 is a silicon-graphite film. In one implementation, the anode film 170 has a thickness of 100 micrometers or less (e.g., from about 1 µm to about 100 µm; from about 10 µm to about 30 µm; from about 20 µm to about 30 µm; from about 3 µm to about 20 µm; or from about 50 µm to about 100 µm). On an upper surface 320a, 320b (collectively 320) each of the anode films 170a, 170b is formed a lithium metal film 310a, 310b (collectively 310). In some implementations, the lithium metal film 310 is formed on the exposed surfaces of the anode film 170, including the top surface 320 and the sidewalls 330a, 330b (collectively 330). The lithium metal film 310 compensates for the capacity loss of graphite anodes mixed with silicon in the first cycle. The lithium metal film 310 is an ultra-thin lithium film with a thickness of 20 nanometers or less (e.g. from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers).
[0048] In some implementations, as shown in Fig. 3, a protective film 340a, 340b (collectively 340) covers the exposed surfaces of the lithium metal film 310 and the exposed surfaces surfaces (e.g. top and side walls) of the anode film 170 and extends to the contact with the Anode current collector 160. In some implementations, the protective film 340 is capable of protecting at least lithium ions and Lithium atoms permeable. In one implementation, the protective film 340 is selected from the group comprising lithium Ion-conductive ceramic, lithium-ion conductive glass, or ion-conductive liquid crystal. The protective film 340 may be a Thickness in the range of 5 nanometers to 2000 micrometers (e.g. in the range of 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 100 nanometers to 200 nanometers; in the range from 100 nanometers up to 150 nanometers).
[0049] Fig. 4 illustrates a cross-sectional view of another implementation of an anode electrode structure 400 formed according to implementations described herein. It should be noted in Fig. 4 that the Anode current collector 160 is shown extending beyond the stack, although it is not necessary that the Anode current collector 160 projects beyond the stack, the sections projecting beyond the stack can be formed as strips Although the anode electrode structure 400 is shown as a double-sided electrode structure, It is important to note that the implementations described herein also apply to single-sided electrode structures.
[0050] The anode electrode structure 400 comprises the anode current collector 160 and anode films 170a, 170b (collectively 170) formed on opposite sides of the anode current collector 160. In one implementation, the Anode film 170 is a silicon-graphite film. In one implementation, the anode film 170 is a lithium metal film. In one Implementation, the anode film 170 has a thickness of 100 micrometers or less (e.g., from about 1 µm to about 100 µm; from about 10 µm to about 30 µm; from about 20 µm to about 30 µm; from about 3 µm to about 20 µm; or from about 50 µm to about 100 µm). A protective film stack 410a, 410b (collectively 410) is formed on the anode film 170. In In some implementations, the protective film stack 410 is formed over the exposed surfaces of the anode film 170, including the upper surface 420a, 420b (collectively 420) and the side walls 430a, 430b (collectively 430) of the anode film 170. The protective film stack 410 comprises a protective film 440a, 440b (collectively 440), a first polymer film 450a, 450b (collectively 450) formed over the protective film stack 410, a ceramic film 460a, 460b (collectively 460) formed over the first polymer film 450, and a second polymer film 470a, 470b (collectively 470) formed over the ceramic film 460.
[0051] The protective film 440 is selected from the group of lithium fluoride (LiF), aluminum oxide, aluminum oxyhydroxide (AlO(OH)), a copper chalcogenide (e.g. CuS, Cu Se, Cu S), bismuth chalcogenide (e.g. Bi Te, Bi Se), lithium carbonate (Li 2 2 2 3 2 3 2 CO ) and combinations thereof. In one implementation, the protective film 440 is a lithium carbonate film (Li CO ). In a 3 2 3 Implementation, the protective film 440 is an ultra-thin film with a thickness of 20 nanometers or less (e.g., about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the protective film 440 is over the exposed surfaces of the anode film 170, including the upper surface 420a, 420b (collectively 420) and the side walls 430a, 430b (collectively 430) of the anode film 170.
[0052] The first polymer film 450 is formed over the protective film 440. The first polymer film 450 functions as connecting layer and improves ionic conduction. In one implementation, the first polymer film 450 is selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), Succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a Implementation, the first polymer film 450 has a thickness of 20 nanometers or less (e.g., about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the first polymer film 450 is deposited over the exposed surfaces of the protective film 440, including the top surface and side walls of the protective film 440.
[0053] The ceramic film 460 is formed over the first polymer film 450. The ceramic film 460 functions as a lithium-ion conductive amplifier and blocks dendrites. In one embodiment, the ceramic film 460 is a porous film. The Ceramic film 460 may be similar to ceramic coating 185. In one embodiment, ceramic film 460 is selected from the group comprising: LiPON, crystalline or amorphous phases of the garnet type LiLaZrO, LISICON (e.g. 7 3 2 12 B. Li Zn GeO , where 0 < x < 1), NASICON (e.g. Na Zr Si PO , where 0 < x < 3), lithium borohydride (LiBH ), 2+2x 1-x 4 1+x 2 x 3-x 12 4 doped anti-perovskite compositions, lithium-containing sulfides (e.g. Li S, Li SP S , Li GeP S and Li PS ) and 2 2 2 5 10 2 12 3 4 Lithium argyrodite (e.g., LiPS X, where x is Cl, Br, or I). In one implementation, the ceramic film 460 has a thickness 5 of 20 nanometers or less (e.g. from about 1 nanometer to about 20 nanometers; from about 1 nanometer ter to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the Ceramic film 460 is formed over the exposed surfaces of the first polymer film 450, including the upper surface and side walls of the first polymer film 450.
[0054] The second polymer film 470 is formed over the ceramic film 460. The second polymer film 470 functions as connecting layer and improves ionic conduction. In one implementation, the second polymer film 470 is selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), Succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a Implementation, the second polymer film 470 has a thickness of 20 nanometers or less (e.g., about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the second polymer film 470 is deposited over the exposed surfaces of the ceramic film 460, including the top surface and sidewalls of the second polymer film 470.
[0055] Fig. 5 illustrates a cross-sectional view of another implementation of an anode electrode structure 500 formed according to implementations described herein. It should be noted in Fig. 5 that the Anode current collector 160 is shown extending beyond the stack, although it is not necessary that the Anode current collector 160 projects beyond the stack, the sections projecting beyond the stack can be formed as strips Although the anode electrode structure 500 is shown as a double-sided electrode structure, It is important to note that the implementations described herein also apply to single-sided electrode structures.
[0056] The anode electrode structure 500 comprises the anode current collector 160 and anode films 170a, 170b (collectively 170) formed on opposite sides of the anode current collector 160. In one implementation, the Anode film 170 is a silicon-graphite film. In one implementation, the anode film 170 has a thickness of 100 micrometers or less (e.g., from about 1 µm to about 100 µm; from about 10 µm to about 30 µm; from about 20 µm to about 30 µm; from about 3 µm to about 20 µm; or from about 50 µm to about 100 µm). In one implementation, the anode film 170 is a Lithium metal film. A protective film stack 510a, 510b (collectively 510) is formed on the anode film 170. In some Implementations, the protective film stack 510 is formed over the exposed surfaces of the anode film 170, including the upper surface 520a, 520b (collectively 520) and the side walls 530a, 530b (collectively 530) of the anode film 170. The protective film stack 510 has a first polymer film 550a, 550b (collectively 550) which is exposed surfaces of the anode film 170, a dielectric film 560a, 560b (collectively 560) which formed over the first polymer film 550, and a second polymer film 570a, 570b (collectively 570) formed over the dielectric film 560 is formed.
[0057] The first polymer film 550 is formed over the anode film 170. The first polymer film 550 functions as connecting layer and improves ionic conduction. In one implementation, the first polymer film 550 is selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), Succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a Implementation, the first polymer film 550 has a thickness of 20 nanometers or less (e.g., about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the first polymer film 550 is deposited over the exposed surfaces of the anode film 170, including the top surface 520 and the sidewalls 530 of the anode film 170.
[0058] The dielectric film 560 is formed over the first polymer film 550. The dielectric film 560 functions as Lithium-ion conductive amplifier and blocks dendrites. In one implementation, the dielectric film 560 is a porous film. The dielectric film 560 may be similar to the ceramic coating 185. In one embodiment, the dielectric film 560 selected from the group comprising: LiPON, crystalline or amorphous phases of the garnet type Li La 7 ZrO, LISICON (e.g. Li Zn GeO, where 0 < x < 1), NASICON (e.g. Na Zr Si PO, where 0 < x < 3), 3 2 12 2+ 2x 1-x 4 1+x 2 x 3-x 12 Lithium borohydride LiBH ), doped anti-perovskite compositions, lithium-containing sulfides (e.g. Li S, Li SP S , Li GeP S 4 2 2 2 5 10 2 and Li PS ) and lithium argyrodite (e.g. LiPS X, where x is Cl, Br or I). In one implementation, the 12 3 4 5 dielectric film 560 has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some Implementations, the dielectric film 560 is formed over the exposed surfaces of the first polymer film 550, including the upper surface and side walls of the first polymer film 550.
[0059] The second polymer film 570 is formed over the dielectric film 560. The second polymer film 570 functions as Connection layer and improves ionic conduction. In one implementation, the second polymer film 570 is selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), Succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a Implementation, the second polymer film 570 has a thickness of 20 nanometers or less (e.g., about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the second polymer film 570 is deposited over the exposed surfaces of the dielectric film 560, including the top surface and sidewalls of the dielectric film 560.
[0060] Fig. 6 illustrates a cross-sectional view of another implementation of an anode electrode structure 600, which was formed according to implementations described herein. It should be noted in Fig. 6 that the Anode current collector 160 is shown extending beyond the stack, although it is not necessary that the Anode current collector 160 projects beyond the stack, the sections projecting beyond the stack can be formed as strips Although the anode electrode structure 600 is shown as a double-sided electrode structure, It is important to note that the implementations described herein also apply to single-sided electrode structures.
[0061] The anode electrode structure 600 comprises the anode current collector 160 and anode films 170a, 170b (collectively 170) formed on opposite sides of the anode current collector 160. In one implementation, the Anode film 170 is a silicon-graphite film. In one implementation, the anode film 170 has a thickness of 100 micrometers or less (e.g., from about 1 µm to about 100 µm; from about 10 µm to about 30 µm; from about 20 µm to about 30 µm; from about 3 µm to about 20 µm; or from about 50 µm to about 100 µm). In one implementation, the anode film 170 is a Lithium metal film. A protective film stack 610a, 610b (collectively 610) is formed on the anode film 170. In some Implementations, the protective film stack 610 is formed over the exposed surfaces of the anode film 170, including the upper surface 620a, 620b (collectively 620) and the side walls 630a, 630b (collectively 630) of the anode film 170. The protective film stack 610 includes a metal film 650a, 650b (collectively 650) that is deposited over the exposed surfaces of the anode film 170, a dielectric film 660a, 660b (collectively 660) which is formed over the Metal film 650 is formed, and a polymer film 670a, 670b (collectively 670) which is formed over the dielectric film 660 is formed.
[0062] The metal film 650 is formed over the anode film 170. The metal film 650 functions as a protective film. The metal film 650 may be similar to the protective film 175. In one implementation, the metal film 650 is an ultra-thin metal seed film. The metal film 650 may be a copper film. The copper film may be an ultra-thin copper film. In one implementation the metal film 650 has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some Implementations, the metal film 650 is formed over the exposed surfaces of the anode film 170, including the top surface 620 and the side walls 630 of the anode film 170.
[0063] The dielectric film 660 is formed over the metal film 650. The dielectric film 660 functions as a lithium-ion conductive amplifier and blocks dendrites. In one implementation, the dielectric film 660 is a porous film. The Dielectric film 660 may be similar to ceramic coating 185. In one implementation, the dielectric film 660 selected from the group comprising: LiPON, crystalline or amorphous phases of the garnet type Li La Zr O , LISICON 7 3 2 12 (e.g. Li Zn GeO , where 0 < x < 1), NASICON (e.g. Na Zr Si PO , where 0 < x < 3), lithium borohydride (LiBH ), 2+ 2x 1-x 4 1+x 2 x 3-x 12 4 doped anti-perovskite compositions, lithium-containing sulfides (e.g. Li S, Li SP S , Li GeP S and Li PS ) and 2 2 2 5 10 2 12 3 4 Lithium argyrodite (e.g., LiPS X, where x is Cl, Br, or I). In one implementation, the dielectric film 660 has a 5 Thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the dielectric film 660 is formed over the exposed surfaces of the metal film 650, including the upper Surface and side walls of the metal film 650.
[0064] The polymer film 670 is formed over the dielectric film 660. The polymer film 670 functions as connection layer and improves ionic conduction. In one implementation, the polymer film 670 is selected from the Group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), Suc cinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a Implementation, the polymer film 670 has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers) In some implementations, the polymer film 670 is over the exposed surfaces of the dielectric film 660 formed, including the top surface and sidewalls of the dielectric film 660.
[0065] Fig. 7 illustrates a process flow diagram illustrating an implementation of a method 700 for forming an anode electrode structure according to implementations described herein. The The anode electrode structure may be the anode electrode structure 200 shown in Fig. 2. In operation 710, a substrate. In one implementation, the substrate is a continuous material web 1250, as shown in Fig. 12 In one implementation, the substrate is the anode current collector 160. Examples of metals from which the Substrate can consist of, include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), Stainless steel, clad materials, their alloys and combinations thereof. In one implementation, the Substrate copper material. In one implementation, the substrate is perforated. In addition, the substrate can have any any form factor (e.g. metal foil, sheet or plate), any shape and micro / macrostructure.
[0066] In some implementations, the substrate is subjected to a pretreatment process that includes at least one Plasma treatment or corona discharge process to remove organic materials from the exposed surfaces of the current collector. The pretreatment process is carried out before film deposition on the substrate carried out.
[0067] In operation 720, a lithium metal film is formed on the substrate. In one embodiment, the Lithium metal film is the anode film 170 and the substrate is the anode current collector 160. In one embodiment, the Lithium metal film is formed on a copper current collector. In some implementations, the lithium metal film is the anode film if an anode film is already present on the substrate. If the anode film 170 is not present, the lithium metal film can be formed directly on the substrate. To deposit the thin Any suitable method for depositing thin lithium metal films can be used. Deposition of the thin film of lithium metal can be done by PVD processes, such as evaporation, a Slot die process, a transfer process or a three-dimensional lithium printing process. The chamber for To deposit the thin film of lithium metal, a PVD system such as an electron beam evaporator, a thermal evaporator or sputtering system, a thin film transfer system (including large area pattern printing systems such as gravure printing systems) or a slot die separation system.
[0068] In operation 730, a metal film is formed on the lithium metal film. In one embodiment, the metal film is a copper film, a bismuth film, or a tin film. Referring to Fig. 2, the metal film may be the metal film 210, and the lithium metal film may be the anode film 170. In one implementation, the metal film is made of a copper film, a bismuth film, a tin film, or combinations thereof. In one implementation, the metal film is a ultra-thin copper film with a thickness of 100 nanometers or less (e.g. from about 5 nanometers to about 100 nanometers; from about 10 nanometers to about 20 nanometers; or from about 50 nanometers to about 100 nanometers). Any suitable copper film deposition process for depositing thin copper films can be used to deposit the thin copper film The deposition of the thin copper film can be done by PVD processes, such as evaporation, a Slot die process, a transfer process or a three-dimensional lithium printing process. The chamber for To deposit the thin film of lithium metal, a PVD system such as an electron beam evaporator, a thermal evaporator or sputtering system, a thin film transfer system (including large area pattern printing systems such as gravure printing systems) or a slot die separation system.
[0069] In operation 740, a protective film may be formed on the metal film. Referring to Fig. 2, the Protective film may be the protective film 220, and the copper film may be the metal film 210. In some implementations, the Protective film 220 permeable to at least lithium ions and lithium atoms. In one embodiment, the protective film 220 selected from the group comprising lithium-ion conductive ceramic, lithium-ion conductive glass, ion conductive Polymer, ion-conducting liquid crystal, composite combinations thereof or unit layer combinations The protective film 220 may have a thickness in the range of 5 nanometers to 2000 micrometers (e.g., in the range from 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 100 nanometers up to 200 nanometers; in the range of 100 nanometers to 150 nanometers). The protective film 220 can be produced using either physical vapor deposition (PVD), chemical vapor deposition (CVD), spraying, doctor blade coating, printing or any number of other plating processes directly onto the copper film. For some PVD is a suitable process. In some implementations, the protective film 220 does not need to be ion conductive; however, once filled with electrolyte (liquid, gel, solid, combination, etc.), the combination of porous substrate and electrolyte ions conductive.
[0070] Fig. 8 illustrates a process flow diagram illustrating an implementation of a method 800 for forming an anode electrode structure according to implementations described herein. The The anode electrode structure may be the anode electrode structure 300 shown in Fig. 3. In operation 810, a substrate. In one implementation, the substrate is a continuous material web 1250. In a Implementation is the substrate of the anode current collector 160. Examples of metals that make up the substrate can include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), stainless steel, plated materials, their alloys, and combinations thereof. In one implementation, the substrate is Copper material. In one implementation, the substrate is perforated. Furthermore, the substrate can have any Form factor (e.g. metal foil, sheet or plate), any shape and micro / macrostructure.
[0071] In some implementations, the substrate is subjected to a pretreatment process that includes at least one Plasma treatment or corona discharge process to remove organic materials from the exposed surfaces of the current collector. The pretreatment process is carried out before film deposition on the substrate carried out.
[0072] In operation 820, a silicon-graphite film is formed on the substrate. In one embodiment, the silicon Graphite film is the anode film 170 and the substrate is the anode current collector 160. In one embodiment, the silicon Graphite film is formed on a copper current collector. The silicon-graphite film can be deposited in a first processing chamber 1210 (see Fig. 12). Any suitable silicon Graphite film deposition process can be used to deposit thin silicon-graphite films. The deposition of the thin silicon-graphite film can be done by PVD processes, such as evaporation, a slot die process, a transfer process, a plating process or a three-dimensional lithium printing process. The chamber for To deposit the thin silicon-graphite film, a PVD system such as an electron beam evaporator, a thermal evaporator or sputtering system, a thin film transfer system (including large area pattern printing systems such as gravure printing systems) or a slot die separation system.
[0073] In operation 830, a lithium metal film is formed on the silicon-graphite film. Referring to Fig. 3, In one implementation, the lithium metal film is the lithium metal film 310, and the silicon graphite film is the anode film 170. Any suitable process for depositing thin lithium metal films may be used to deposit Lithium metal films can be used. The deposition of the thin film of lithium metal can be achieved by PVD processes such as evaporation, a slot die process, a transfer process or a three-dimensional Lithium printing process. The chamber for depositing the thin film of lithium metal can be a PVD system, such as a electron beam evaporator, a thermal evaporator or a sputtering system, a thin film transfer system (including large-area pattern printing systems such as gravure printing systems) or a slot die separation system.
[0074] In operation 840, a protective film may be formed on the lithium metal film. Referring to Fig. 3 the protective film may be the protective film 340, and the lithium metal film may be the lithium metal film 310. In some Implementations, the protective film 340 is permeable to at least lithium ions and lithium atoms. In a Implementation, the protective film 340 is selected from the group comprising lithium-ion conductive ceramics, lithium Ion-conducting glass, ion-conducting polymer, ion-conducting liquid crystal, composite combinations thereof or Unit layer combinations thereof. The protective film 340 may have a thickness in the range of 5 nanometers to 2000 micrometers (e.g. in the range from 10 nanometers to 600 nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 100 nanometers to 200 nanometers; in the range of 100 nanometers to 150 nanometers). The protective film 340 can be deposited using either physical vapor deposition (PVD), chemical vapor deposition (CVD), spraying, doctor blade coating, printing or any number of other coating processes directly onto the Lithium metal film is deposited. For some implementations, PVD is a suitable process. In some Implementations, the protective film 340 does not need to be ion-conductive; however, once it is contacted with electrolyte (liquid, gel, solid, combination, etc.), the combination of porous substrate and electrolyte is ion-conductive.
[0075] Fig. 9 illustrates a process flow diagram illustrating an implementation of a method 900 for forming an anode electrode structure according to implementations described herein. The The anode electrode structure may be the anode electrode structure 400 shown in Fig. 4. At operation 910, a substrate. In one implementation, the substrate is a continuous material web 1250, as shown in Fig. 12 In one implementation, the substrate is the anode current collector 160. Examples of metals from which the Substrate can consist of, include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), Stainless steel, clad materials, their alloys and combinations thereof. In one implementation, the Substrate copper material. In one implementation, the substrate is perforated. In addition, the substrate can have any any form factor (e.g. metal foil, sheet or plate), any shape and micro / macrostructure.
[0076] In some implementations, the substrate is subjected to a pretreatment process that includes at least one Plasma treatment or corona discharge process to remove organic materials from the exposed surfaces of the current collector. The pretreatment process is carried out before film deposition on the substrate carried out.
[0077] In operation 920, a lithium metal film is formed on the substrate. In one embodiment, the Lithium metal film is the anode film 170 and the substrate is the anode current collector 160. In one embodiment, the Lithium metal film is formed on a copper current collector. In some implementations, the lithium metal film is the anode film if an anode film is already present on the substrate. If the anode film 170 is not present, the lithium metal film can be formed directly on the substrate. To deposit the thin Any suitable process for depositing thin lithium metal films can be used. Deposition of the thin film of lithium metal can be done by PVD processes, such as evaporation, a Slot die process, a transfer process or a three-dimensional lithium printing process. The chamber for To deposit the thin film of lithium metal, a PVD system such as an electron beam evaporator, a thermal evaporator or sputtering system, a thin film transfer system (including large area pattern printing systems such as gravure printing systems) or a slot die separation system.
[0078] In operation 930, a protective film is formed on the lithium metal film. Referring to Fig. 4, the Protective film may be the protective film 440, and the lithium metal film may be the anode film 170. In one embodiment The protective film is similar to the protective film 175 as described in relation to Fig. 1. The protective film has at least one of Lithium fluoride (LiF), a metal film (e.g. copper, bismuth, tin or combinations thereof), a copper chalcogenide (e.g. B. CuS, CuSe, CuS), bismuth chalcogenide (e.g. BiTe, BiSe) and a lithium carbonate (LiCO). The protective film 175 2 2 2 3 2 3 2 3 provides surface protection of the anode film 170. The protective film can be deposited by physical vapor deposition (PVD), such as vapor deposition or sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating, comma bar coating, roll coating or a three-dimensional lithium printing process directly onto the anode film 170. PVD is a preferred Method for depositing the protective film. The protective film can be a coating or a separate layer that each have a thickness in the range of 1 nanometer to 2000 nanometers (e.g. in the range of 10 nanometers to 600 Nanometers; in the range from 50 nanometers to 100 nanometers; in the range from 50 nanometers to 200 nanometers; in the range of 100 nanometers to 150 nanometers). The protective film can be a separate film with a thickness in the Range from 5 micrometers to 50 micrometers (e.g. in the range from 6 micrometers to 25 micrometers).
[0079] In operation 940, a first polymer film is formed on the protective film. Referring to Fig. 4, the first polymer film may be the first polymer film 450, and the protective film may be the protective film 440. The first polymer film acts as a connecting layer and improves ionic conduction. In one implementation, the first polymer film selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a embodiment, the first polymer film has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers) In some implementations, the first polymer film is formed over the exposed surfaces of the protective film, including the top surface and side walls of the protective film. The first polymer film can be formed by physical Chemical vapor deposition (PVD), such as evaporation or sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating or a three-dimensional lithium printing process directly on the protective layer is deposited.
[0080] In operation 950, a ceramic film is formed on the first polymer film. Referring to Fig. 4, the Ceramic film may be the ceramic film 460, and the first polymer film may be the first polymer film 450. The ceramic film acts as a lithium-ion conductive amplifier and blocks dendrites. In one embodiment, the ceramic film is a porous film. The ceramic film may be similar to the ceramic coating 185, as described with reference to Fig. 1. In In one embodiment, the ceramic film is selected from the group comprising: LiPON, crystalline or amorphous phases of the garnet type Li La Zr O, LISICON (e.g. Li Zn GeO, where 0 < x < 1), NASICON (e.g. Na Zr Si PO, where 7 3 2 12 2+2x 1-x 4 1 +x 2 x 3-x 12 0 < x < 3), lithium borohydride (LiBH ), doped anti-perovskite compositions, lithium-containing sulfides (e.g. Li S, Li SP S 4 2 2 2 , Li GeP S and Li PS ) and lithium argyrodite (e.g. LiPS X, where x is Cl, Br or I). In one embodiment, 5 10 2 12 3 4 5 the ceramic film has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some Implementations, the ceramic film is formed over the exposed surfaces of the first polymer film, including the top surface and side walls of the first polymer film. The ceramic film can be formed by physical Chemical vapor deposition (PVD), such as evaporation or sputtering, atomic layer deposition (ALD), a slot die process, Dip coating, a thin film transfer process, gravure coating or a three-dimensional Lithium printing process can be deposited directly onto the protective layer.
[0081] In operation 960, a second polymer film is formed on the ceramic film. Referring to Fig. 4, the second polymer film may be the second polymer film 470, and the ceramic film may be the ceramic film 460. The second Polymer film 470 acts as a connecting layer and improves ionic conduction. In one implementation, the second Polymer film selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), Polyacrylonitrile (PAN), succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, 2 4 2 Polyetheretherketone (PEEK), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and Combinations thereof. In one embodiment, the second polymer film has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the second polymer film is placed over the exposed surfaces of the ceramic film, including the top surface and side walls of the second The second polymer film can be deposited by physical vapor deposition (PVD), such as vapor deposition or Sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating or a three-dimensional lithium printing process directly on the protective layer is deposited.
[0082] Fig. 10 illustrates a process flow diagram illustrating an implementation of a method 1000 for forming an anode electrode structure according to implementations described herein. The The anode electrode structure may be the anode electrode structure 500 shown in Fig. 5. In operation 1010, a substrate. In one implementation, the substrate is a continuous material web 1250, as shown in Fig. 12 In one implementation, the substrate is the anode current collector 160. Examples of metals from which the Substrate can consist of, include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), Stainless steel, clad materials, their alloys and combinations thereof. In one implementation, the Substrate copper material. In one implementation, the substrate is perforated. In addition, the substrate can have any any form factor (e.g. metal foil, sheet or plate), any shape and micro / macrostructure.
[0083] In some implementations, the substrate is subjected to a pretreatment process that includes at least one Plasma treatment or corona discharge process to remove organic materials from the exposed surfaces of the current collector. The pretreatment process is carried out before film deposition on the substrate carried out.
[0084] In operation 1020, a lithium metal film is formed on the substrate. In one embodiment, the Lithium metal film is the anode film 170 and the substrate is the anode current collector 160. In one embodiment, the Lithium metal film is formed on a copper current collector. In some implementations, the lithium metal film is the anode film if an anode film is already present on the substrate. If the anode film 170 is not present, the lithium metal film can be formed directly on the substrate. To deposit the thin Lithium metal film, any suitable process for depositing thin Lithium metal films can be used. The deposition of the thin film of lithium metal can be achieved by PVD processes such as evaporation, a slot die process, a transfer process or a three-dimensional Lithium printing process. The chamber for depositing the thin film of lithium metal can be a PVD system, such as a electron beam evaporator, a thermal evaporator or a sputtering system, a thin film transfer system (including large-area pattern printing systems such as gravure printing systems) or a slot die separation system.
[0085] In operation 1030, a first polymer film is formed on the lithium metal film. Referring to Fig. 5 the first polymer film may be the first polymer film 550, and the lithium metal film may be the anode film 170. The The first polymer film acts as a connecting layer and improves ionic conduction. In one implementation, the first Polymer film selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), Polyacrylonitrile (PAN), succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, 2 4 2 Polyetheretherketone (PEEK), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and Combinations thereof. In one embodiment, the first polymer film has a thickness of 20 nanometers or less (e.g., B. from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the first polymer film is deposited over the exposed surfaces of the lithium metal film, including the top surface and sidewalls of the protective film. The first polymer film can be deposited by physical vapor deposition (PVD), such as evaporation or sputtering. Atomic layer deposition (ALD), a slot die process, dip coating, a thin film transfer process, Gravure coating or a three-dimensional lithium printing process deposited directly on the protective layer become.
[0086] In operation 1040, a dielectric film is formed on the first polymer film. Referring to Fig. 5 the dielectric film may be the dielectric film 560, and the first polymer film may be the first polymer film 550. The dielectric film acts as a lithium-ion conductive amplifier and blocks dendrites. In one embodiment, the dielectric film is a porous film. The dielectric film may be similar to the ceramic coating 185, as described in reference described in Fig. 1. In one embodiment, the dielectric film is selected from the group comprising: LiPON, crystalline or amorphous phases of the garnet type Li La Zr O , LISICON (e.g. Li Zn GeO , where 0 < x < 1), NASICON 7 3 2 12 2+2x 1-x 4 (e.g. Na Zr Si PO , where 0 < x < 3), lithium borohydride (LiBH ), doped anti-perovskite compositions, 1 + x 2 x 3 - x 12 4 lithium-containing sulfides (e.g. Li S, Li SP S , Li GeP S and Li PS ) and lithium argyrodites (e.g. LiPS X, where x is Cl, Br 2 2 2 5 10 2 12 3 4 5 or I). In one implementation, the dielectric film has a thickness of 20 nanometers or less (e.g., about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the dielectric film is deposited over the exposed surfaces of the first polymer film, including the top surface and sidewalls of the first polymer film. The dielectric Film can be deposited by chemical vapor deposition (CVD), physical vapor deposition (PVD), such as vapor deposition or sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating or a three-dimensional lithium printing process directly on the protective layer is deposited.
[0087] At operation 1050, a second polymer film is formed on the dielectric film. Referring to Fig. 5 the second polymer film may be the second polymer film 570, and the dielectric film may be the dielectric film 560 The second polymer film 570 acts as a connecting layer and improves ionic conduction. In one implementation the second polymer film is selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), Ethylene oxide (EO), polyacrylonitrile (PAN), succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, 2 4 2 Polyphenylene sulfide, polyetheretherketone (PEEK), carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic Liquids and combinations thereof. In one embodiment, the second polymer film has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In some implementations, the second Polymer film is formed over the exposed surfaces of the ceramic film, including the top surface and the Side walls of the second polymer film. The second polymer film can be deposited by physical vapor deposition (PVD), such as Evaporation or sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating or a three-dimensional lithium printing process directly on the protective layer is deposited.
[0088] Fig. 11 illustrates a process flow diagram showing an implementation of a method rens 1100 for forming an anode electrode structure according to implementations described herein. The The anode electrode structure may be the anode electrode structure 600 shown in Fig. 6. In operation 1110, a substrate. In one implementation, the substrate is a continuous material web 1250, as shown in Fig. 12 In one implementation, the substrate is the anode current collector 160. Examples of metals from which the Substrate can consist of, include aluminum (Al), copper (Cu), zinc (Zn), nickel (Ni), cobalt (Co), manganese (Mn), chromium (Cr), Stainless steel, clad materials, their alloys and combinations thereof. In one implementation, the Substrate copper material. In one implementation, the substrate is perforated. In addition, the substrate can have any any form factor (e.g. metal foil, sheet or plate), any shape and micro / macrostructure.
[0089] In some implementations, the substrate is subjected to a pretreatment process that includes at least one Plasma treatment or corona discharge process to remove organic materials from the exposed surfaces of the current collector. The pretreatment process is carried out before film deposition on the substrate carried out.
[0090] In operation 1120, a lithium metal film is formed on the substrate. In one embodiment, the Lithium metal film is the anode film 170 and the substrate is the anode current collector 160. In one embodiment, the Lithium metal film is formed on a copper current collector. In some implementations, the lithium metal film is the anode film if an anode film is already present on the substrate. If the anode film 170 is not present, the lithium metal film can be formed directly on the substrate. The lithium metal film can be first processing chamber 1210 and / or the second processing chamber 1220. For depositing the Any suitable process for depositing thin lithium metal films can be used. Deposition of the thin film of lithium metal can be done by PVD processes, such as evaporation, a Slot die process, a transfer process or a three-dimensional lithium printing process. The chamber for To deposit the thin film of lithium metal, a PVD system such as an electron beam evaporator, a thermal evaporator or sputtering system, a thin film transfer system (including large area Pattern printing systems such as gravure printing systems, comma bar printing or roll coating) or a Slot nozzle separation system.
[0091] In operation 1130, a metal film is formed on the lithium metal film. Referring to Fig. 6, the Metal film may be the metal film 650, and the lithium metal film may be the anode film 170. In one implementation, the Metal film an ultra-thin metal film with a thickness of 100 nanometers or less (e.g. from about 5 nanometers to 100 nanometers; from about 10 nanometers to about 20 nanometers; or from about 50 nanometers to about 100 nanometers). In In one embodiment, the metal film is a copper film. Any suitable method can be used to deposit the thin metal film. Metal film deposition process can be used to deposit thin metal films. The deposition of the metal film can by PVD processes, such as evaporation, a slot die process, a transfer process or a three-dimensional lithium printing process. The chamber for depositing the metal film can be a PVD system, such as a electron beam evaporator, a thermal evaporator or a sputtering system, a thin film transfer system (including large-scale pattern printing systems such as gravure printing systems, comma-bar printing or roll coating) or have a slot nozzle separation system.
[0092] In operation 1140, a dielectric film is formed on the metal film. Referring to Fig. 6, the dielectric film may be the dielectric film 660, and the metal film may be the metal film 650. The dielectric film acts as a lithium-ion conductive amplifier and blocks dendrites. In one embodiment, the dielectric film a porous film. The dielectric film may be similar to the ceramic coating 185, as shown in Fig. 1 In one embodiment, the dielectric film is selected from the group comprising: LiPON, crystalline or amorphous phases of the garnet type Li La Zr O , LISICON (e.g. Li Zn GeO , where 0 < x < 1), NASICON (e.g. Na 7 3 2 12 2+2x 1-x 4 1+ Zr Si PO , where 0 < x < 3), lithium borohydride (LiBH ), doped anti-perovskite compositions, lithium-containing x 2 x 3-x 12 4 Sulfides (e.g. LiS, LiSPS, LiGePS and LiPS) and lithium argyrodites (e.g. LiPSX, where x is Cl, Br or I). In a 2 2 2 5 10 2 12 3 4 5 Implementation, the dielectric film has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers) In some implementations, the dielectric film is deposited over the exposed surfaces of the first polymer film formed, including the top surface and side walls of the first polymer film. The dielectric film can by chemical vapor deposition (CVD), physical vapor deposition (PVD), such as vapor deposition or Sputtering, atomic layer deposition (ALD), a slot die process, dip coating, a Thin film transfer process, gravure coating or a three-dimensional lithium printing process directly onto the protective layer.
[0093] In operation 1150, a polymer film is formed on the dielectric film. Referring to Fig. 6, the Polymer film may be the polymer film 670, and the dielectric film may be the dielectric film 660. The polymer film 670 acts as a connecting layer and improves ionic conduction. In one implementation, the polymer film is selected from the group comprising polyvinylidene difluoride (PVDF), polyethylene oxide (PEO), ethylene oxide (EO), polyacrylonitrile (PAN), Succinonitrile (CH (CN) ), 2,3-dichloro-5,6-dicyano-1,4-benzoquinone, polyphenylene sulfide, polyether ether ketone (PEEK), 2 4 2 Carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), ionic liquids and combinations thereof. In a In one embodiment, the polymer film has a thickness of 20 nanometers or less (e.g., from about 1 nanometer to about 20 nanometers; from about 1 nanometer to about 10 nanometers; or from about 5 nanometers to about 10 nanometers). In In some implementations, the polymer film is formed over the exposed surfaces of the metal film, including the top surface and side walls of the polymer film. The polymer film can be formed by physical Chemical vapor deposition (PVD), such as evaporation or sputtering, atomic layer deposition (ALD), a slot die process, Dip coating, a thin film transfer process, gravure coating or a three-dimensional Lithium printing process can be deposited directly onto the protective layer.
[0094] Fig. 12 illustrates a schematic view of an integrated processing tool 1200 for forming Anode electrode structures according to implementations described herein. The integrated processing tool 1200 can be a SMARTWEB®, manufactured by Applied Materials, which is used for the production of lithium anode devices according to the implementations described herein. The integrated processing tool 1200 is configured as Reel-to-reel system and comprises an unwinding module 1202, a processing module 1204 and a winding module 1206. In certain implementations, the processing module 1204 includes a plurality of processing modules or chambers 1210, 1220, 1230 and 1240 arranged in series and each configured to form a Processing operation on a continuous material web 1250 or a material layer. In a Embodiment, as shown in Fig. 12, the processing chambers 1210 to 1240 are radially Processing drum 1255. In addition to the radial arrangement, other arrangements are also conceivable. In a Implementation, the processing chambers 1210 to 1240 are standalone modular processing chambers, with each modular processing chamber is structurally separated from the other modular processing chambers. Therefore Each of the stand-alone modular processing chambers can be arranged, rearranged, replaced or serviced without affecting each other. Although four processing chambers 1210 to 1240, it is understood that in the integrated processing tool 1200 any number may be comprised of processing chambers.
[0095] The processing chambers 1210 to 1240 may have any suitable structure, configuration, arrangement and / or Components that enable the integrated processing tool 1200 to Lithium anode device according to implementations of the present disclosure. For example, but not limited to this, the processing chambers may have suitable separation systems, including Coating sources, power sources, individual pressure regulators, deposition control systems and temperature controllers. According to typical implementations, the chambers are equipped with individual gas supplies. For good gas separation, the chambers are usually separated from each other. The integrated processing tool 1200 according to the implementations described herein is not limited in the number of deposition chambers. For example, but not limited to, the integrated processing tool 1200 can be 3, 6 or 12 processing chambers.
[0096] In some implementations, each of the processing chambers 1210 to 1240 of the integrated Processing tool 1200 configured to perform deposition by sputtering, such as magnetron sputtering As used herein, ´´magnetron sputtering´´ refers to sputtering using a magnet arrangement , ie a unit capable of generating a magnetic field. Typically, such a Magnet arrangement has a permanent magnet. This permanent magnet is usually located within a rotating target or coupled to a planar target in a way that the free electrons within the generated magnetic field beneath the surface of the rotating target. Such a magnet arrangement can also be used with arranged coupled to a planar cathode.
[0097] Magnetron sputtering can also be achieved by a double magnetron cathode, such as, but not limited to, a TwinMag™ cathode array. In some implementations, the cathodes can be arranged in the Processing chamber made of This allows a modular design of the facility, which allows for optimization of the facility to special manufacturing requirements. In some implementations, the number of cathodes in a Sputter deposition chamber selected to optimize the productivity of the integrated processing tool 1200.
[0098] In some implementations, one or some of the processing chambers 1210 to 1240 may be used to perform sputtering without a magnetron array. In particular, one or some of the chambers can be Be configured to perform deposition by other methods, such as, but not limited to, chemical Chemical vapor deposition, atomic laser deposition or pulsed laser deposition.
[0099] In certain implementations, the processing chambers 1210 to 1240 are configured to process both sides of the continuous material web 1250. Although the integrated processing tool 1200 is designed to process a horizontally aligned continuous web of material 1250, the integrated processing tool 1200 can be configured to process substrates positioned in different orientations, for example, in a vertically aligned continuous web of material 1250. In certain implementations, the continuous material web 1250 comprises a flexible conductive substrate. In certain implementations, the continuous Material web 1250 comprises a conductive substrate having one or more layers formed thereon. In certain Implementations, the conductive substrate is a copper substrate with one or more Silicon graphite layers.
[0100] In certain implementations, the integrated processing tool 1200 includes a Transmission mechanism 1252. The transmission mechanism 1252 may be any transmission mechanism capable of conveying the continuous material web 1250 through the Processing area of the processing chambers 1210 to 1240. The transmission mechanism 1252 can a common transport architecture. The common transport architecture can be a reel-to-reel system with a common take-up reel 1254 in the winding module 1206, wherein the processing drum 1255 in the processing module 1204 and a feed reel 1256 is positioned in the unwind module 1202. The The take-up reel 1254, the processing drum 1255 and the feed reel 1256 can be heated individually. Take-up reel 1254, processing drum 1255 and feed reel 1256 can be individually wound using a internal heat source positioned on each coil or an external heat source. The common Transport architecture may further comprise one or more auxiliary transmission coils 1253a, 1253b arranged between the take-up reel 1254, processing drum 1255 and feed reel 1256. Although the integrated Although the processing tool 1200 is shown with a single processing area, it can in certain Implementations may be advantageous to have separate or separate processing areas for each Processing chamber 1210 to 1240. For implementations with separate processing areas, modules or chambers, the common transport architecture may be a coil-to-coil system, where each chamber or Each processing area has a single take-up reel and feed reel as well as one or more optional intermediate transfer reels positioned between the take-up reel and the feed reel. Common transport architecture may include a rail system. The rail system extends through the processing areas or separate processing areas. The rail system is configured to either Configure a web substrate or a separate substrate.
[0101] The integrated processing tool 1200 may move the supply reel 1256 and the take-up reel 1254 the continuous material web 1250 through the different processing chambers 1210 to 1240. In a Implementation, the first processing chamber 1210 and the second processing chamber 1220 are each configured to deposit a portion of a lithium metal film. The third processing chamber 1230 is configured to The fourth processing chamber 1240 is configured to deposit over the copper film and the Lithium metal film to deposit a protective coating to protect the lithium metal film from oxidizing agents in the environment In some implementations, the finished negative electrode is not placed on the Take-up coil 1254, but can be directly integrated with the separator and the positive electrodes, etc. to form battery cells.
[0102] In one implementation, the processing chambers 1210 to 1230 are configured to deposit a thin film of Lithium metal on the continuous material web 1250 configured. To deposit the thin film of lithium metal Any suitable lithium deposition process can be used to deposit thin films of lithium metal. Deposition of the thin film of lithium metal can be done by PVD processes, such as evaporation, a Slot die process, a transfer process, a lamination process or a three-dimensional Lithium printing process. The chambers for depositing the thin Lithium metal films can be deposited using a PVD system such as an electron beam evaporator, a Thin film transfer system (including large-area pattern printing systems such as gravure printing systems), a lamination system or a slot die separation system.
[0103] In one implementation, the fourth processing chamber 1240 is configured to form a protective film on the lithium metal film. The fourth processing chamber 1240 is configured to form a protective film on the Lithium metal film configured. The protective film may be an ion-conductive material as described herein. The protective film can be formed by dip coating, slot die coating, gravure coating, laminating or printing In one implementation, the fourth processing chamber 1240 is an evaporation chamber or PVD chamber, which is configured to form a ceramic or dielectric layer over the continuous material web 1250 In one embodiment, the evaporation chamber comprises a processing area that evaporation source which can be placed in a crucible, which for example is a thermal evaporator or an electron beam evaporator (cold) in a vacuum environment.
[0104] In summary, some of the advantages of the present disclosure include the efficient integration of the Lithium metal deposition into currently available processing systems. Currently, the deposition of Lithium metal in a dry room or an argon gas atmosphere. Due to the volatility of Lithium metal, subsequent processing operations are carried out in an argon gas atmosphere. subsequent processing operations in an argon gas atmosphere would require retrofitting existing manufacturing tools. The inventors have discovered that coating the lithium metal with a Protective film before subsequent processing allows subsequent processing either under vacuum or in the atmosphere. The protective film eliminates the need for additional processing in a Inert gas atmosphere and the complexity of the tools is reduced. The protective film also facilitates transport and / or the storage of the negative electrode with the lithium metal film formed on it. In addition, Implementations where the protective film is an ion-conducting film, the ion-conducting film is incorporated into the final battery structure, reducing the complexity of the battery manufacturing process. This reduces the complexity of the tool and consequently lowers operating costs.
[0105] In introducing elements of the present disclosure or exemplary aspects or Implementations of this, the articles ´´ein´´, ´´eine´´, ´´der´´ ´´die´´ and ´´das´´ mean that one or several of the elements are present.
[0106] The terms ´´comprising´´, ´´including´´, ´´having´´ and having are to be understood inclusively and mean that there may be additional elements besides those listed.
[0107] Although the foregoing is directed to implementations of the present disclosure, other and further implementations of the disclosure may be developed without departing from the basic scope of protection thereof to depart from, and the scope of protection thereof is determined by the following claims. QUOTES CONTAINED IN THE DESCRIPTION
[0000] This list of documents submitted by the applicant was generated automatically and is intended solely for This list is not part of the German patent or trademark law. Utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature
[0000] EP 1236231 A1
[0005] WO 2017131997 A1
[0005]
Claims
1. Anode electrode structure (200) comprising: a current collector (160) comprising copper; a lithium metal film (170) formed on the current collector; a metal film (210) formed on the lithium metal film, the metal film having a top surface and side walls of the lithium metal film extending to contact the current collector; and a protective film (175) formed on the metal film, wherein the protective film is a lithium-ion conductive film selected from the group comprising lithium-ion conductive Ceramic, lithium-ion conductive glass, lithium-ion conductive polymer, lithium-ion conductive liquid crystal or Combinations of these.
2. Anode electrode structure (200) comprising: a current collector (160) comprising copper; a lithium metal film (170) formed on the current collector; a metal film (210) formed on the lithium metal film, the metal film having a top surface and side walls of the lithium metal film extending to contact the current collector; and a protective film (175) formed on the metal film, wherein the protective film is a lithium-ion conductive film, and wherein the metal film is selected from a copper film, a bismuth film, a tin film or combinations thereof.
3. Anode electrode structure (200) according to one of claims 1 or 2, wherein the copper film has a thickness between about 5 nanometers and about 40 nanometers, in particular between about 10 nanometers and about 20 nanometers.
4. Anode electrode structure (200) according to any one of claims 1 to 3, wherein the lithium-ion conductive film of one or more several of aluminum oxide (AlO), LiPON, Li La ZrO (LLZO), Li SP S, Li GeP S, Li PS, (1-x)LiI-(x)Li SnS, xLiI-(1- 2 3 7 3 2 12 2 2 5 10 2 12 3 4 4 4 x)Li SnS , (1-x)LiI-(x)Li SnS , (x)LiI-(1-x)Li SnS ), where 0 < x < 1. 4 4 4 4 4 4 5. Anode electrode structure (200) according to any one of claims 1 to 4, wherein the lithium metal film has a thickness between about 1 micrometer and about 20 micrometers.
6. Anode electrode structure (200) according to claim 5, wherein the current collector has a thickness between about 2 micrometers and about 8 micrometers.
7. Anode electrode structure (200) according to any one of claims 1 to 6, wherein the current collector (160) comprises: a first nickel- or chromium-containing film; a copper film formed on the first nickel- or chromium-containing film and having a thickness between about 50 nanometers and about 500 nanometers; and a second nickel- or chromium-containing film formed on the copper film and having a thickness of between about 20 nanometers and about 50 nanometers.
8. Anode electrode structure (200) according to any one of claims 1 to 7, wherein the current collector (160) comprises: a polyethylene terephthalate (PET) polymer substrate; and a copper film formed on the PET polymer substrate.
9. Anode electrode structure (200) according to claim 1, wherein the metal film is selected from a copper film, a bismuth film, a tin film or combinations thereof, and wherein the copper film has a thickness between about 5 nanometers and about 40 nanometers.
10. Anode electrode structure (200) according to claim 1, wherein the lithium-ion conductive film is selected from the group comprising lithium-ion conductive ceramic, lithium-ion conductive glass, lithium-ion conductive polymer, lithium-ion conductive liquid crystal or combinations thereof, and wherein the copper film has a thickness between about 5 nanometers and about 40 nanometers.
11. Anode electrode structure (300) comprising: a current collector (160); a silicon-graphite anode formed on the current collector; a film of lithium metal (310) formed on the silicon-graphite anode; and a protective film (340) formed on the lithium metal film, the protective film comprising a lithium ion conductive film selected from the group comprising lithium-ion conductive ceramic, lithium-ion conductive Glass, lithium-ion conductive polymer, lithium-ion conductive liquid crystal or combinations thereof, wherein the Protective film the exposed surfaces of the lithium metal film and side walls of the silicon graphite anode, which extending to contact with the current collector.
12. Anode electrode structure (300) according to claim 11, wherein the lithium-ion conductive film comprises lithium-ion conductive Ceramics included.
13. The anode electrode structure (300) of claim 11, wherein the lithium-ion conductive film comprises lithium-ion conductive glass includes.
14. Anode electrode structure (300) according to claim 11, wherein the lithium-ion conductive film comprises lithium-ion conductive polymer.
15. Anode electrode structure (300) according to claim 11, wherein the lithium-ion conductive film comprises lithium-ion conductive Liquid crystal.
Citation Information
Patent Citations
Lithium anodes for electrochemical cells
EP1236231A1
Integrated lithium deposition with protective layer tool
WO2017131997A1